Method for producing water-absorbing resin particles, water-absorbing resin particles, absorber, and absorbent article

The method of reverse-phase suspension polymerization with controlled crosslinking agents enhances water-absorbing resin particles' performance, addressing the challenge of maintaining high water retention and absorption in absorbent articles with reduced fiber usage.

WO2024214752A1PCT designated stage expired Publication Date: 2024-10-17SUMITOMO SEIKA CHEM CO LTD

Patent Information

Application Number
PCT/JP2024/014596
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-04-10
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Current water-absorbing resin particles in absorbent articles, such as disposable diapers and sanitary napkins, face challenges in maintaining high water retention capacity while minimizing the amount of absorbent fibers, which can lead to reduced performance in penetration rate, reversion, and liquid leakage.

Method used

A method for producing water-absorbing resin particles through reverse-phase suspension polymerization using a radical polymerization initiator, specifically an azo compound, in multiple stages with controlled amounts of internal and surface crosslinking agents, enhancing the particles' water retention and absorption capabilities under load.

Benefits of technology

The method produces water-absorbing resin particles with improved physiological saline water retention and absorption performance, specifically under a load of 4.14 kPa, and increased 5-minute unpressurized wettability, allowing for reduced fiber usage in absorbent articles while maintaining performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000052_0000
    Figure 00000052_0000
  • Figure 00000052_0001
    Figure 00000052_0001
Patent Text Reader

Abstract

Provided is a novel method for producing water-absorbing resin particles the method being capable of obtaining water-absorbing resin particles having high absorption performance (in particular, in terms of the physiological-saline-solution retention amount, the physiological-saline-solution absorption amount under a 4.14 kPa load, and the 5-minute value of the non-pressurization DW). The present invention provides a method for producing water-absorbing resin particles by performing reverse-phase suspension polymerization of a water-soluble ethylenically unsaturated monomer using radical polymerization initiators, wherein: at least one of the radical polymerization initiators is an azo-based compound; the reverse-phase suspension polymerization comprises two or more stages of polymerization steps; in the first-stage polymerization step, (a) 0.01-0.11 mmol of an internal crosslinking agent is used per 1 mol of the water-soluble ethylenically unsaturated monomer used when the first-stage polymerization is performed; in the second-stage polymerization step, (b) 0-0.042 mmol of an internal crosslinking agent is used per 1 mol of the water-soluble ethylenically unsaturated monomer used when the second-stage polymerization is performed, and (c) 0.38 mmol or less of the azo-based compound is used per 1 mol of the water-soluble ethylenically unsaturated monomer used when the second-stage polymerization is performed; and, in the polymerization steps after the second stage, a surface crosslinking step is included.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing water-absorbent resin particles, water-absorbent resin particles, absorbent body, and absorbent article

[0001] The present invention relates to a method for producing water-absorbent resin particles, water-absorbent resin particles, an absorbent body, and an absorbent article, and more particularly to a method for producing a water-absorbent resin constituting an absorbent body suitably used in hygiene materials such as disposable diapers, sanitary napkins, and incontinence pads, water-absorbent resin particles, an absorbent body using the water-absorbent resin particles, and an absorbent article.

[0002] BACKGROUND ART In recent years, water-absorbent resins have been widely used in the field of sanitary materials such as disposable diapers, sanitary napkins, and incontinence pads.

[0003] As such water-absorbent resin particles, a crosslinked product of a polymer of a water-soluble ethylenically unsaturated monomer, more specifically a crosslinked product of a polymer of a partially neutralized polyacrylic acid, has excellent water-absorbing ability, and since acrylic acid, which is a raw material thereof, is easily available industrially, it can be produced at low cost with constant quality, and is less susceptible to putrefaction and deterioration, and therefore, it is considered to be a preferable water-absorbent resin particle (see, for example, Patent Document 1).

[0004] Absorbent articles such as disposable diapers, sanitary napkins, and incontinence pads are mainly composed of an absorbent core located in the center for absorbing and retaining body fluids such as urine and menstrual blood excreted from the body, a liquid-permeable surface sheet (top sheet) located on the side that comes into contact with the body, and a liquid-impermeable back sheet (back sheet) located on the opposite side that comes into contact with the body. The absorbent core is usually composed of hydrophilic fibers such as pulp and water-absorbent resin particles.

[0005] Japanese Patent Application Publication No. 3-227301

[0006] In such absorbent articles, the water-absorbent resin particles contained in the absorbent core are required to have a higher water retention capacity. By using water-absorbent resin particles with a high water retention capacity in an absorbent article, it becomes possible to reduce the amount of water-absorbent resin particles and the amount of hydrophilic fibers such as pulp used in the absorbent article from the viewpoint of maintaining the water retention capacity of the entire absorbent article, for example. However, this may result in a decrease in other performance properties of the absorbent article (e.g., permeation rate, backflow, and liquid leakage). Therefore, by improving the absorption performance of the water-absorbent resin particles, it becomes possible to reduce the amount of water-absorbent resin particles and the amount of hydrophilic fibers such as pulp used in the absorbent article while maintaining the performance of the absorbent article.

[0007] From the viewpoint of improving the absorption performance of water-absorbent resin particles used in absorbent articles, the inventors of the present invention focused on the saline water retention capacity, the saline water absorption capacity under a load of 4.14 kPa, and the 5-minute value of no-pressure Demand Wettability (hereinafter, no-pressure DW).

[0008] Under these circumstances, a main object of the present invention is to provide a novel method for producing water-absorbent resin particles, which can provide water-absorbent resin particles excellent in high absorption performance (particularly, properties of water retention capacity of saline solution, water absorption capacity of saline solution under a load of 4.14 kPa, and 5-minute value of DW without pressure). Another object of the present invention is to provide water-absorbent resin particles excellent in high absorption performance (particularly, properties of water retention capacity of saline solution, water absorption capacity of saline solution under a load of 4.14 kPa, and 5-minute value of DW without pressure), and an absorbent body and an absorbent article using the water-absorbent resin particles.

[0009] The present inventors have conducted extensive studies to solve the above-mentioned problems. As a result, they have found that, in a method for producing water-absorbent resin particles by reverse-phase suspension polymerization of a water-soluble ethylenically unsaturated monomer using a radical polymerization initiator, an azo-based compound is used as the radical polymerization initiator, the reverse-phase suspension polymerization is carried out in two or more stages, and the amounts of the internal crosslinking agent used in the first-stage polymerization, the internal crosslinking agent used in the second-stage polymerization, and the azo-based compound used in the second-stage polymerization are set within predetermined ranges, and a surface crosslinking step is further performed after the polymerization, thereby obtaining water-absorbent resin particles having excellent absorption performance (particularly, saline water retention capacity, saline water absorption capacity under a load of 4.14 kPa, and 5-minute value of unpressurized DW). The present invention has been completed based on this finding and through further extensive studies.

[0010] That is, the present invention provides the invention having the following features: Item 1. A method for producing water-absorbent resin particles by reverse-phase suspension polymerization of a water-soluble ethylenically unsaturated monomer using a radical polymerization initiator, wherein at least one of the radical polymerization initiators is an azo-based compound, and the reverse-phase suspension polymerization comprises two or more polymerization stages, wherein in a first polymerization stage, (a) 0.01 mmol or more and 0.11 mmol or less of an internal crosslinking agent is used per mole of the water-soluble ethylenically unsaturated monomer used in the first polymerization stage, and in a second polymerization stage, (b) 0 mmol or more and 0.042 mmol or less of an internal crosslinking agent is used per mole of the water-soluble ethylenically unsaturated monomer used in the second polymerization stage, and (c) 0.38 mmol or less of an azo-based compound is used per mole of the water-soluble ethylenically unsaturated monomer used in the second polymerization stage, and a surface crosslinking step is comprised after the second or subsequent polymerization stages. Item 2. Item 1 is a method for producing water-absorbent resin particles according to Item 1, wherein the primary particles obtained in the first polymerization step have a storage modulus of 10 Pa or more and 200 Pa or less when swollen 40 times with ion-exchanged water, and the secondary particles obtained in the second or subsequent polymerization steps have a storage modulus of 5 Pa or more and 200 Pa or less when swollen 40 times with ion-exchanged water. Item 3 is a method for producing water-absorbent resin particles according to Item 1 or 2, wherein the water-absorbent resin particles have the following properties (A) to (C): (A) A saline water retention capacity of 50 g / g or more and 80 g / g or less. (B) A saline water absorption capacity under a load of 4.14 kPa of 15 g / g or more and 40 g / g or less. (C) A 5-minute value of unpressurized DW of 50 mL / g or more and 80 mL / g or less. Item 4. Item 5. Water-absorbent resin particles which are a crosslinked product of a polymer of a water-soluble ethylenically unsaturated monomer, the water-absorbent resin particles having the following properties (A) to (C): (A) a saline water retention capacity of 50 g / g or more and 80 g / g or less; (B) a saline water absorption capacity under a load of 4.14 kPa of 15 g / g or more and 40 g / g or less; (C) a 5-minute no-pressure DW value of 50 mL / g or more and 80 mL / g or less. Item 5. An absorbent body comprising the water-absorbent resin particles according to Item 4. Item 6. An absorbent article comprising the absorbent body according to Item 5.

[0011] According to the present invention, it is possible to provide a novel method for producing water-absorbent resin particles, which can obtain water-absorbent resin particles excellent in absorption performance (particularly, characteristics of water retention capacity of physiological saline solution, water absorption capacity of physiological saline solution under a load of 4.14 kPa, and 5-minute value of DW without pressure). Furthermore, according to the present invention, it is also possible to provide water-absorbent resin particles excellent in absorption performance (particularly, characteristics of water retention capacity of physiological saline solution, water absorption capacity of physiological saline solution under a load of 4.14 kPa, and 5-minute value of DW without pressure), an absorbent body using the water-absorbent resin particles, and an absorbent article.

[0012] 1 is a schematic diagram of a measuring device used to measure the unloaded DW of a water-absorbent resin particle, and FIG. 2 is a schematic diagram of a measuring device used to measure the amount of saline solution absorbed by a water-absorbent resin particle under a load of 4.14 kPa.

[0013] As used herein, the term "comprising" includes "consisting essentially of" and "consisting of." Furthermore, as used herein, "(meth)acrylic" means "acrylic or methacrylic," "(meth)acrylate" means "acrylate or methacrylate," and "(poly)" refers to the presence or absence of the prefix "poly." Furthermore, as used herein, "water-soluble" means exhibiting a solubility of 5% by mass or more in water at 25°C.

[0014] In this specification, a numerical value connected with "~" means a numerical range that includes the numerical values ​​before and after "~" as the lower limit and upper limit. When multiple lower limit values ​​and multiple upper limit values ​​are listed separately, any lower limit value and upper limit value can be selected and connected with "~".

[0015] 1. Method for Producing Water-Absorbent Resin Particles The method for producing water-absorbent resin particles of the present invention is a method for producing water-absorbent resin particles by reverse-phase suspension polymerization of a water-soluble ethylenically unsaturated monomer using a radical polymerization initiator. At least one of the radical polymerization initiators is an azo-based compound. In the method for producing water-absorbent resin particles of the present invention, the reverse-phase suspension polymerization comprises two or more polymerization stages.

[0016] The method for producing water-absorbent resin particles of the present invention uses, in the first-stage polymerization step of reversed-phase suspension polymerization, (a) 0.01 to 0.11 millimoles of an internal crosslinking agent per mole of the water-soluble ethylenically unsaturated monomer used in the first-stage polymerization. Furthermore, in the second-stage polymerization step, (b) 0 to 0.042 millimoles of an internal crosslinking agent per mole of the water-soluble ethylenically unsaturated monomer used in the second-stage polymerization, and (c) 0.38 millimoles or less of an azo compound per mole of the water-soluble ethylenically unsaturated monomer used in the second-stage polymerization. Furthermore, the method for producing water-absorbent resin particles of the present invention includes a surface crosslinking step after the second-stage or later polymerization steps.

[0017]

[0033] The method for producing water-absorbent resin particles of the present invention has these configurations, and thereby can suitably produce water-absorbent resin particles excellent in absorption performance (particularly, properties of saline water retention capacity, saline water absorption capacity under a load of 4.14 kPa, and 5-minute value of unpressurized DW). Hereinafter, the method for producing water-absorbent resin particles of the present invention will be described in detail.

[0018] [Reverse-phase suspension polymerization] When performing reverse-phase suspension polymerization, for example, an aqueous monomer solution containing a water-soluble ethylenically unsaturated monomer is dispersed in a dispersion medium in the presence of a dispersion stabilizer. As described later, the dispersion medium is preferably, for example, a hydrocarbon dispersion medium.

[0019]

[0023] Conventionally, when water-soluble ethylenically unsaturated monomers are subjected to reverse phase suspension polymerization to obtain water-absorbent resin particles, the reverse phase suspension polymerization can be carried out in only one polymerization step, but the reverse phase suspension polymerization in the present invention is carried out in two or more polymerization steps. From the viewpoint of enhancing the productivity of water-absorbent resin particles while suitably exhibiting the effects of the present invention, the reverse phase suspension polymerization is preferably carried out in two to three polymerization steps.

[0020] In reversed-phase suspension polymerization, after carrying out the first-stage polymerization step (first-stage reversed-phase suspension polymerization), a water-soluble ethylenically unsaturated monomer is added to the reaction mixture obtained in the first-stage polymerization reaction and mixed, and the second-stage and subsequent polymerization steps (first-stage reversed-phase suspension polymerization) can be carried out in the same manner as in the first stage.In the reversed-phase suspension polymerization in each stage from the second stage onwards, it is preferable to carry out the reversed-phase suspension polymerization by adding a predetermined amount of a polymerization initiator in addition to the water-soluble ethylenically unsaturated monomer, based on the amount of the water-soluble ethylenically unsaturated monomer added during the reversed-phase suspension polymerization in each stage from the second stage onwards.In addition, in the polymerization in the second stage and subsequent stages, an internal crosslinking agent may be added to the water-soluble ethylenically unsaturated monomer, if necessary.

[0021] As will be described later, it is also preferable to use a dispersion stabilizer (a surfactant or a polymeric dispersant) in the reversed-phase suspension polymerization. The dispersion stabilizer may be added either before or after the addition of the aqueous monomer solution, as long as it is added before the start of the polymerization reaction.

[0022]

[0123] From the viewpoint of easily reducing the amount of hydrocarbon dispersion medium remaining in the obtained water absorbent resin particles, it is preferable to disperse an aqueous monomer solution in a hydrocarbon dispersion medium having a polymeric dispersant dispersed therein, and then further disperse a surfactant therein, and then carry out polymerization.

[0023] The reaction temperature of the polymerization reaction is preferably 20 to 110°C, more preferably 40 to 90°C, from the viewpoints of rapidly progressing the polymerization, shortening the polymerization time, thereby improving economic efficiency, and easily removing the heat of polymerization to smoothly carry out the reaction.

[0024] <Polymerization Step> In each of the first and second and subsequent polymerization steps, the water-soluble ethylenically unsaturated monomer is polymerized by reversed-phase suspension polymerization using a radical polymerization initiator. Specifically, an aqueous solution containing the water-soluble ethylenically unsaturated monomer, a hydrocarbon dispersion medium, a radical polymerization initiator, and an internal crosslinking agent are mixed, and the polymerization reaction of the water-soluble ethylenically unsaturated monomer is allowed to proceed.

[0025] In the present invention, in the first-stage polymerization step, (a) 0.01 to 0.11 millimoles of an internal crosslinking agent are used per mole of the water-soluble ethylenically unsaturated monomer used in the first-stage polymerization. Furthermore, in the present invention, in the second-stage polymerization step, (b) 0 to 0.042 millimoles of an internal crosslinking agent are used per mole of the water-soluble ethylenically unsaturated monomer used in the second-stage polymerization, and (c) 0.38 millimoles or less of an azo compound are used per mole of the water-soluble ethylenically unsaturated monomer used in the second-stage polymerization.

[0026] The first and second and subsequent polymerization steps will be described in detail below.

[0027] [Water-Soluble Ethylenically Unsaturated Monomer] Examples of water-soluble ethylenically unsaturated monomers include (meth)acrylic acid and salts thereof; 2-(meth)acrylamido-2-methylpropanesulfonic acid and salts thereof; nonionic monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, 2-hydroxyethyl(meth)acrylate, N-methylol(meth)acrylamide, and polyethylene glycol mono(meth)acrylate; and amino group-containing unsaturated monomers and quaternized products thereof such as N,N-diethylaminoethyl(meth)acrylate, N,N-diethylaminopropyl(meth)acrylate, and diethylaminopropyl(meth)acrylamide. Among these water-soluble ethylenically unsaturated monomers, (meth)acrylic acid or salts thereof, (meth)acrylamide, and N,N-dimethylacrylamide are preferred, and (meth)acrylic acid and salts thereof are more preferred, from the viewpoint of industrial ease of availability. These water-soluble ethylenically unsaturated monomers may be used alone or in combination of two or more.

[0028] Among these, acrylic acid and its salts are widely used as raw materials for water-absorbent resin particles, and these acrylic acid and / or salts thereof may be copolymerized with the other water-soluble ethylenically unsaturated monomers described above for use. In the present invention, the content of acrylic acid and its salts in the water-soluble ethylenically unsaturated monomers is 70 to 100 mol %. That is, the proportion of acrylic acid and its salts in the total water-soluble ethylenically unsaturated monomers is 70 to 100 mol %.

[0029] The water-soluble ethylenically unsaturated monomer is dispersed in a hydrocarbon dispersion medium in the form of an aqueous solution and subjected to reversed-phase suspension polymerization. By forming the water-soluble ethylenically unsaturated monomer into an aqueous solution, the dispersion efficiency in the hydrocarbon dispersion medium can be increased. The concentration of the water-soluble ethylenically unsaturated monomer in this aqueous solution is preferably in the range of 20% by mass to the saturated concentration.

[0030] The concentration of the water-soluble ethylenically unsaturated monomer during the first-stage polymerization is preferably 55% by mass or less, more preferably 50% by mass or less, and even more preferably 45% by mass or less, from the viewpoints of improving the water retention capacity of saline solution, the water absorption capacity of saline solution under a load of 4.14 kPa, and the 5-minute value of DW without pressure. On the other hand, the concentration of the water-soluble ethylenically unsaturated monomer is preferably 25% by mass or more, more preferably 30% by mass or more, and even more preferably 35% by mass or more, from the viewpoints of improving the water retention capacity of saline solution, the water absorption capacity of saline solution under a load of 4.14 kPa, and the 5-minute value of DW without pressure.

[0031] The concentration of the water-soluble ethylenically unsaturated monomer during the second-stage polymerization is preferably 55% by mass or less, more preferably 50% by mass or less, and even more preferably 45% by mass or less, from the viewpoints of improving the water retention capacity of saline solution, the water absorption capacity of saline solution under a load of 4.14 kPa, and the 5-minute value of DW without pressure. On the other hand, the concentration of the water-soluble ethylenically unsaturated monomer is preferably 30% by mass or more, more preferably 35% by mass or more, and even more preferably 40% by mass or more, from the viewpoints of improving the water retention capacity of saline solution, the water absorption capacity of saline solution under a load of 4.14 kPa, and the 5-minute value of DW without pressure.

[0032] The ratio of the amount of the water-soluble ethylenically unsaturated monomer used in the second-stage polymerization to the amount of the water-soluble ethylenically unsaturated monomer used in the first-stage polymerization (amount used in the second stage / amount used in the first stage) is preferably 0.1 to 3.0, more preferably 0.5 to 2.5, even more preferably 1.0 to 2.0, and even more preferably 1.3 to 1.5, from the viewpoint of improving the saline water retention capacity, the saline water absorption capacity under a load of 4.14 kPa, and the 5-minute value of the no-pressure DW.

[0033] The water-soluble ethylenically unsaturated monomer may be used in which the acid group (acid group of acrylic acid) has been neutralized in advance with an alkaline neutralizing agent, as necessary. Examples of such alkaline neutralizing agents include alkali metal salts such as sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, and potassium carbonate; and ammonia. These alkaline neutralizing agents may be used in the form of an aqueous solution to simplify the neutralization operation. The alkaline neutralizing agents described above may be used alone or in combination of two or more.

[0034] From the viewpoint of improving the physiological saline water retention capacity, the physiological saline water absorption capacity under a load of 4.14 kPa, and the 5-minute value of non-pressurized DW, the degree of neutralization of the water-soluble ethylenically unsaturated monomer with the alkaline neutralizing agent is preferably 10 to 100 mol%, more preferably 30 to 90 mol%, even more preferably 50 to 85 mol%, and even more preferably 70 to 80 mol%, as the degree of neutralization of all acid groups possessed by the water-soluble ethylenically unsaturated monomer.

[0035] [Polymerization Initiator] The polymerization initiator mixed in the polymerization step is a radical polymerization initiator, and at least one of the initiators is an azo compound.

[0036] The radical polymerization initiator may be an azo compound alone, but it is preferable to use an azo compound in combination with a peroxide from the viewpoint of improving the saline water retention capacity, the saline water absorption capacity under a load of 4.14 kPa, and the 5-minute value of the no-pressure DW.

[0037] When a peroxide and an azo compound are used in combination, the azo compound and the peroxide do not necessarily need to coexist at the start of the polymerization reaction, but rather refer to a state in which one compound is present while the monomer conversion rate due to radical cleavage of the other compound is less than 10%, but it is preferable that both of them coexist in an aqueous solution containing a water-soluble ethylenically unsaturated monomer before the start of the polymerization reaction. Furthermore, the azo compound and the peroxide may be added to the polymerization reaction system through separate flow paths, or may be added to the polymerization reaction system sequentially through the same flow path.

[0038] The azo compound and peroxide used may be in the form of a powder or an aqueous solution.

[0039] Examples of peroxides include persulfates such as potassium persulfate, ammonium persulfate, and sodium persulfate, as well as peroxides such as methyl ethyl ketone peroxide, methyl isobutyl ketone peroxide, di-t-butyl peroxide, t-butylcumyl peroxide, t-butyl peroxyacetate, t-butyl peroxyisobutyrate, t-butyl peroxypivalate, and hydrogen peroxide. Among these peroxides, potassium persulfate, ammonium persulfate, and sodium persulfate are preferred from the viewpoints of easy availability and ease of handling.

[0040] The amount of peroxide used in the first-stage polymerization is, from the viewpoint of improving the water retention capacity of physiological saline, the water absorption capacity of physiological saline under a load of 4.14 kPa, and the 5-minute value of non-pressurized DW, preferably 0.001 to 1.0 mmol, more preferably 0.01 to 0.50 mmol, even more preferably 0.05 to 0.30 mmol, and still more preferably 0.075 to 0.15 mmol, relative to 1 mole of the water-soluble ethylenically unsaturated monomer used in the first-stage polymerization.

[0041] The amount of peroxide used in the second-stage polymerization is, from the viewpoint of improving the water retention capacity of physiological saline, the water absorption capacity of physiological saline under a load of 4.14 kPa, and the 5-minute value of non-pressurized DW, preferably 0.001 to 1.0 mmol, more preferably 0.01 to 0.50 mmol, even more preferably 0.05 to 0.20 mmol, and still more preferably 0.075 to 0.15 mmol, relative to 1 mole of the water-soluble ethylenically unsaturated monomer used in the second-stage polymerization.

[0042] Examples of azo compounds include 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(N-phenylamidino)propane] dihydrochloride, 2,2'-azobis[2-(N-allylamidino)propane] dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], and 4,4'-azobis(4-cyanovaleric acid). Among these azo compounds, 2,2'-azobis(2-amidinopropane) dihydrochloride is preferred from the viewpoint of easy availability and ease of handling.

[0043] The amount of the azo compound used in the first-stage polymerization is preferably 0 to 1.0 mmol, more preferably 0 to 0.50 mmol, even more preferably 0.10 to 0.38 mmol, and still more preferably 0.20 to 0.35 mmol, relative to 1 mole of the water-soluble ethylenically unsaturated monomer used in the first-stage polymerization, from the viewpoint of improving the water retention capacity of physiological saline, the water absorption capacity of physiological saline under a load of 4.14 kPa, and the 5-minute value of DW without pressure.

[0044] In the production method of the present invention, (c) an azo compound is used in an amount of 0.38 mmol or less per mole of the water-soluble ethylenically unsaturated monomer used in the second-stage polymerization. From the viewpoint of improving the saline water retention capacity, the saline water absorption capacity under a load of 4.14 kPa, and the 5-minute value of the no-pressure DW, the amount of the azo compound used in the second-stage polymerization is preferably 0 to 0.35 mmol, more preferably 0.05 to 0.35 mmol, and even more preferably 0.10 to 0.35 mmol, per mole of the water-soluble ethylenically unsaturated monomer used in the second-stage polymerization.

[0045] The polymerization initiator can also be used as a redox polymerization initiator in combination with a reducing agent such as sodium sulfite, sodium hydrogen sulfite, ferrous sulfate, or L-ascorbic acid.

[0046] From the viewpoint of improving the saline water retention capacity, the saline water absorption capacity under a load of 4.14 kPa, and the 5-minute value of the no-pressure DW, the molar ratio of peroxide to azo compound (peroxide / azo compound) in the first-stage polymerization is preferably in the range of 0.1 to 1.0, more preferably in the range of 0.2 to 0.5, and even more preferably in the range of 0.3 to 0.4.

[0047] From the viewpoint of improving the saline water retention capacity, the saline water absorption capacity under a load of 4.14 kPa, and the 5-minute value of the no-pressure DW, the molar ratio of peroxide to azo compound (peroxide / azo compound) in the second-stage polymerization is preferably in the range of 0.1 to 1.5, more preferably in the range of 0.2 to 1.0, and even more preferably in the range of 0.3 to 0.7.

[0048] [Internal Crosslinking Agent] Examples of the internal crosslinking agent include those capable of crosslinking a polymer of a water-soluble ethylenically unsaturated monomer used, such as unsaturated polyesters obtained by reacting polyols such as diols and triols, such as (poly)ethylene glycol, (poly)propylene glycol, 1,4-butanediol, trimethylolpropane, and (poly)glycerin, with unsaturated acids, such as (meth)acrylic acid, maleic acid, and fumaric acid; bisacrylamides such as N,N-methylenebisacrylamide; di(meth)acrylic acid esters or tri(meth)acrylic acid esters obtained by reacting polyepoxides with (meth)acrylic acid; di(meth)acrylic acid carbamyl esters obtained by reacting polyisocyanates, such as tolylene diisocyanate and hexamethylene diisocyanate, with hydroxyethyl (meth)acrylate; allylated starch, allylated cellulose, diallyl phthalate, N,N' ,N''-triallyl isocyanurate, divinylbenzene, and other compounds having two or more polymerizable unsaturated groups; diglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, and other polyglycidyl compounds, and triglycidyl compounds; epihalohydrin compounds such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin; compounds having two or more reactive functional groups, such as isocyanate compounds such as 2,4-tolylene diisocyanate and hexamethylene diisocyanate; and oxetane compounds such as 3-methyl-3-oxetanemethanol, 3-ethyl-3-oxetanemethanol, 3-butyl-3-oxetanemethanol, 3-methyl-3-oxetaneethanol, 3-ethyl-3-oxetaneethanol, and 3-butyl-3-oxetaneethanol. Among these internal cross-linking agents, it is preferable to use unsaturated polyesters or polyglycidyl compounds, it is more preferable to use diglycidyl ether compounds, and it is preferable to use (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, or (poly)glycerin diglycidyl ether. These internal cross-linking agents may be used alone or in combination of two or more.

[0049] In the present invention, in the first-stage polymerization step, (a) 0.01 to 0.11 millimoles of an internal crosslinking agent are used per mole of the water-soluble ethylenically unsaturated monomer used in the first-stage polymerization. From the viewpoint of improving the saline water retention capacity, the saline water absorption capacity under a load of 4.14 kPa, and the 5-minute value of the no-pressure DW, the amount of the internal crosslinking agent used in the first-stage polymerization is preferably 0.02 to 0.09 millimoles, more preferably 0.03 to 0.075 millimoles, and even more preferably 0.04 to 0.06 millimoles, per mole of the water-soluble ethylenically unsaturated monomer used in the first-stage polymerization.

[0050] In the present invention, in the second-stage polymerization step, (b) an internal crosslinking agent is used in an amount of 0 to 0.042 mmol per mole of the water-soluble ethylenically unsaturated monomer used in the second-stage polymerization. From the viewpoint of improving the saline water retention capacity, the saline water absorption capacity under a load of 4.14 kPa, and the 5-minute value of the no-pressure DW, the amount of the internal crosslinking agent used in the second-stage polymerization is preferably 0 to 0.038 mmol, more preferably 0 to 0.032 mmol, even more preferably 0 to 0.030 mmol, and particularly preferably 0 to 0.025 mmol, per mole of the water-soluble ethylenically unsaturated monomer used in the second-stage polymerization.

[0051] [Hydrocarbon Dispersion Medium] Examples of hydrocarbon dispersion media include aliphatic hydrocarbons having 6 to 8 carbon atoms, such as n-hexane, n-heptane, 2-methylhexane, 3-methylhexane, 2,3-dimethylpentane, 3-ethylpentane, and n-octane; alicyclic hydrocarbons, such as cyclohexane, methylcyclohexane, cyclopentane, methylcyclopentane, trans-1,2-dimethylcyclopentane, cis-1,3-dimethylcyclopentane, and trans-1,3-dimethylcyclopentane; and aromatic hydrocarbons, such as benzene, toluene, and xylene. Among these hydrocarbon dispersion media, n-hexane, n-heptane, and cyclohexane are particularly preferred because they are easily available industrially, have stable quality, and are inexpensive. These hydrocarbon dispersion media may be used alone or in combination of two or more. As an example of a mixture of hydrocarbon dispersion media, a commercially available product such as Exxol Heptane (manufactured by ExxonMobil Corporation; contains 75 to 85% by mass of hydrocarbons such as heptane and its isomers) can also be used to obtain favorable results.

[0052] The amount of the hydrocarbon dispersion medium used is preferably 100 to 1,500 parts by mass, more preferably 150 to 1,000 parts by mass, even more preferably 200 to 500 parts by mass, and even more preferably 300 to 400 parts by mass, relative to 100 parts by mass of the first-stage water-soluble ethylenically unsaturated monomer, from the viewpoints of uniformly dispersing the water-soluble ethylenically unsaturated monomer and facilitating control of the polymerization temperature.

[0053] [Dispersion stabilizer] (Surfactant) In the reversed-phase suspension polymerization, a dispersion stabilizer can be used as needed to improve the dispersion stability of the water-soluble ethylenically unsaturated monomer in the hydrocarbon dispersion medium. As the dispersion stabilizer, a surfactant can be used.

[0054] Examples of surfactants that can be used include sucrose fatty acid esters, polyglycerin fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene glycerin fatty acid esters, sorbitol fatty acid esters, polyoxyethylene sorbitol fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, alkylallyl formaldehyde condensed polyoxyethylene ethers, polyoxyethylene polyoxypropylene block copolymers, polyoxyethylene polyoxypropyl alkyl ethers, polyethylene glycol fatty acid esters, alkyl glucosides, N-alkyl gluconamides, polyoxyethylene fatty acid amides, polyoxyethylene alkylamines, phosphate esters of polyoxyethylene alkyl ethers, and phosphate esters of polyoxyethylene alkyl allyl ethers. Among these surfactants, sorbitan fatty acid esters, polyglycerin fatty acid esters, and sucrose fatty acid esters are particularly preferred from the standpoint of dispersion stability of the monomer. These surfactants may be used alone or in combination of two or more.

[0055] The amount of the surfactant used is preferably 0.1 to 30 parts by mass, more preferably 0.3 to 10 parts by mass, even more preferably 0.5 to 1 part by mass, and even more preferably 0.6 to 0.9 parts by mass, relative to 100 parts by mass of the first-stage water-soluble ethylenically unsaturated monomer.

[0056] (Polymer-Based Dispersant) As a dispersion stabilizer used in reversed-phase suspension polymerization, a polymer-based dispersant may be used in combination with the surfactant described above.

[0057] Examples of polymeric dispersants include maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-propylene copolymer, maleic anhydride-modified EPDM (ethylene-propylene-diene terpolymer), maleic anhydride-modified polybutadiene, maleic anhydride-ethylene copolymer, maleic anhydride-propylene copolymer, maleic anhydride-ethylene-propylene copolymer, maleic anhydride-butadiene copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, oxidized polyethylene, oxidized polypropylene, oxidized ethylene-propylene copolymer, ethylene-acrylic acid copolymer, ethyl cellulose, and ethylhydroxyethyl cellulose. Among these polymeric dispersants, it is particularly preferable to use maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-propylene copolymer, maleic anhydride-ethylene copolymer, maleic anhydride-propylene copolymer, maleic anhydride-ethylene-propylene copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, oxidized polyethylene, oxidized polypropylene, and oxidized ethylene-propylene copolymer from the viewpoint of dispersion stability of the monomer. These polymeric dispersants may be used alone or in combination of two or more.

[0058] The amount of the polymeric dispersant used is preferably 0.1 to 30 parts by mass, more preferably 0.3 to 10 parts by mass, even more preferably 0.5 to 1 part by mass, and even more preferably 0.6 to 0.9 parts by mass, relative to 100 parts by mass of the first-stage water-soluble ethylenically unsaturated monomer.

[0059] [Other Components] In the method for producing water-absorbent resin particles, if desired, other components may be added to an aqueous solution containing a water-soluble ethylenically unsaturated monomer to carry out reverse phase suspension polymerization. As the other components, various additives such as a thickener and a chain transfer agent can be added.

[0060] (Thickener) For example, a thickener may be added to an aqueous solution containing a water-soluble ethylenically unsaturated monomer to carry out reversed-phase suspension polymerization. By adding a thickener to adjust the viscosity of the aqueous solution in this way, it is possible to control the median particle size obtained in the reversed-phase suspension polymerization.

[0061] Examples of usable thickeners include hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, carboxymethyl cellulose, polyacrylic acid, (partially) neutralized polyacrylic acid, polyethylene glycol, polyacrylamide, polyethyleneimine, dextrin, sodium alginate, polyvinyl alcohol, polyvinylpyrrolidone, polyethylene oxide, etc. If the stirring speed during polymerization is the same, the higher the viscosity of the water-soluble ethylenically unsaturated monomer aqueous solution, the larger the primary particles and / or secondary particles of the resulting particles tend to be.

[0062] (Chain Transfer Agent) For example, from the viewpoint of improving the saline water retention capacity, the saline water absorption capacity under a load of 4.14 kPa, and the 5-minute value of the no-pressure DW, the polymerization of the water-soluble ethylenically unsaturated monomer may be carried out in the presence of a chain transfer agent.

[0063] Examples of chain transfer agents include thiols such as ethanethiol, propanethiol, and dodecanethiol; thiolic acids such as thioglycolic acid, thiomalic acid, dimethyldithiocarbamic acid, diethyldithiocarbamic acid, and salts thereof; secondary alcohols such as isopropanol; phosphite compounds such as phosphorous acid, normal salts of phosphorous acid such as disodium phosphite, dipotassium phosphite, and diammonium phosphite, and acidic salts of phosphorous acid such as sodium hydrogen phosphite, potassium hydrogen phosphite, and ammonium hydrogen phosphite; phosphate compounds such as phosphoric acid, normal salts of phosphoric acid such as sodium phosphate, potassium phosphate, and ammonium phosphate, and acidic salts of phosphoric acid such as sodium dihydrogen phosphate, potassium dihydrogen phosphate, ammonium dihydrogen phosphate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, and diammonium hydrogen phosphate; hypophosphite compounds such as hypophosphorous acid, and hypophosphites such as sodium hypophosphite, potassium hypophosphite, and ammonium hypophosphite; pyrophosphoric acid, tripolyphosphoric acid, polyphosphoric acid, and salts thereof; trimethyl phosphate, nitrilotrimethylenetriphosphonic acid, and the like. These chain transfer agents may be used alone or in combination of two or more. Furthermore, hydrates of the chain transfer agents may also be used.

[0064] The amount of chain transfer agent used in the second-stage polymerization is preferably 0 to 0.0005 mol, more preferably 0 to 0.0003 mol, even more preferably 0 to 0.0002 mol, and still more preferably 0 to 0.0001 mol, relative to 1 mol of the water-soluble ethylenically unsaturated monomer, from the viewpoint of improving the water retention capacity of physiological saline solution, the water absorption capacity of physiological saline solution under a load of 4.14 kPa, and the 5-minute value of DW without pressure.

[0065] As described above, the inventors of the present invention focused on the saline water retention capacity, saline water absorption capacity under a load of 4.14 kPa, and the 5-minute no-pressure DW value in order to improve the absorption performance of water-absorbent resin particles used in absorbent articles. In order to increase the 5-minute no-pressure DW value, it is necessary to increase the surface area of ​​the water-absorbent resin particles. To increase the surface area of ​​water-absorbent resin particles, the inventors of the present invention discovered that in a method for producing water-absorbent resin particles by reverse-phase suspension polymerization of a water-soluble ethylenically unsaturated monomer, the reverse-phase suspension polymerization is carried out in two or more polymerization stages. By increasing the storage modulus of the primary particles obtained in the first polymerization stage and suppressing the aggregation of the secondary particles obtained in the second and subsequent polymerization stages, the surface area of ​​the water-absorbent resin particles obtained by surface-crosslinking the secondary particles is increased, thereby increasing the 5-minute no-pressure DW value. In order to increase the storage modulus of the primary particles obtained in the first polymerization stage, it is necessary to increase the degree of crosslinking of the primary particles. However, as the degree of crosslinking of the primary particles increases, there arises a problem that the saline water retention capacity and the saline water absorption capacity under a load of 4.14 kPa decrease.

[0066] From the above viewpoints, in the present invention, the storage modulus of the gel of the primary particles obtained in the first-stage polymerization step swollen 40 times with ion-exchanged water is preferably set in the range of 10 Pa or more and 200 Pa or less. From the viewpoint of improving the 5-minute value of DW without pressure, the storage modulus is preferably 10 Pa or more, more preferably 15 Pa or more, and even more preferably 20 Pa or more. Furthermore, from the viewpoint of improving the water retention capacity of saline solution and the water absorption capacity of saline solution under a load of 4.14 kPa, the storage modulus is preferably 200 Pa or less, more preferably 150 Pa or less, and even more preferably 100 Pa or less. From the viewpoint of improving the water retention capacity of saline solution, the water absorption capacity of saline solution under a load of 4.14 kPa, and the 5-minute value of DW without pressure, the storage modulus is preferably in the range of 15 to 150 Pa, and more preferably in the range of about 20 to 100 Pa. The storage modulus can be adjusted, for example, in the first-stage polymerization step by adjusting the amount of the internal crosslinking agent used, the concentration of the water-soluble ethylenically unsaturated monomer, the degree of neutralization of the water-soluble ethylenically unsaturated monomer, the amount of the polymerization initiator used, etc. The storage modulus is the storage modulus measured in an environment of 25°C using a stress-controlled rheometer for the primary particles obtained in the first-stage polymerization step, which are dried and then swollen 40 times with ion-exchanged water to form a 40-fold swollen gel. The specific measurement of the storage modulus is performed by the measurement method described in the Examples.

[0067] In the present invention, the secondary particles obtained in the second or subsequent polymerization steps preferably have a storage modulus of a gel swollen 40 times with ion-exchanged water set to a range of 5 Pa or more and 200 Pa or less. From the viewpoint of improving the saline water retention capacity, the saline water absorption capacity under a load of 4.14 kPa, and the 5-minute value of the no-pressure DW, the storage modulus is preferably 5 Pa or more, more preferably 20 Pa or more, even more preferably 30 Pa or more, and is preferably 200 Pa or less, more preferably 190 Pa or less, even more preferably 170 Pa or less, still more preferably 150 Pa or less, and particularly preferably 100 Pa or less, with a preferred range being 20 to 190 Pa, a more preferred range being 20 to 170 Pa, an even more preferred range being 30 to 150 Pa, and an even more preferred range being about 30 to 100 Pa. The storage modulus can be adjusted, for example, in the second or subsequent polymerization steps by adjusting the amount of the internal crosslinking agent used, the concentration of the water-soluble ethylenically unsaturated monomer, the ratio of the amount of the water-soluble ethylenically unsaturated monomer used in the second polymerization step to the amount of the water-soluble ethylenically unsaturated monomer used in the first polymerization step, the degree of neutralization of the water-soluble ethylenically unsaturated monomer, the amount of the polymerization initiator used, the amount of the chain transfer agent used, etc. The storage modulus is the storage modulus measured in an environment of 25°C using a stress-controlled rheometer on the secondary particles obtained in the second polymerization step, which are dried and then swollen 40 times with ion-exchanged water to form a 40-fold swollen gel. Specific measurements of the storage modulus are performed by the measurement method described in the Examples.

[0068] From the viewpoint of more suitably exerting the effects of the present invention, the ratio of the storage elastic modulus of the secondary particles to the storage elastic modulus of the primary particles (storage elastic modulus of the secondary particles / storage elastic modulus of the primary particles) is preferably 10 times or less, more preferably 5 times or less, and even more preferably 3 times or less, and a preferred range is 0.1 to 5 times, and a more preferred range is 0.5 to 3 times, etc.

[0069] As described above, in order to increase the 5-minute value of the no-pressure DW, it is necessary to increase the surface area of ​​the water-absorbent resin particles. To increase the surface area of ​​the water-absorbent resin particles, the inventors of the present invention discovered that in a method for producing water-absorbent resin particles by reverse-phase suspension polymerization of a water-soluble ethylenically unsaturated monomer, the reverse-phase suspension polymerization is carried out in two or more polymerization stages, and the storage modulus of the primary particles obtained in the first polymerization stage is increased, while the aggregation of the secondary particles obtained in the second and subsequent polymerization stages is suppressed. This increases the surface area of ​​the water-absorbent resin particles obtained by surface-crosslinking the secondary particles, thereby increasing the 5-minute value of the no-pressure DW. However, in order to increase the storage modulus of the primary particles obtained in the first polymerization stage, it is necessary to increase the degree of crosslinking of the primary particles. As the degree of crosslinking of the primary particles increases, the problem of a decrease in the saline water retention capacity and the saline water absorption capacity under a load of 4.14 kPa arises. On the other hand, in the method for producing a water-absorbent resin particle of the present invention, it can be considered that by lowering the degree of internal crosslinking formed during second-stage or later polymerization, the storage modulus of secondary particles before being subjected to surface crosslinking is lowered and the contribution of surface crosslinking is enhanced, thereby water-absorbent resin particles excellent in properties of water retention capacity of physiological saline solution, water absorption capacity of physiological saline solution under a load of 4.14 kPa, and 5-minute value of no-pressure DW are obtained.

[0070] <Surface Cross-Linking (Post-Cross-Linking) Step> The surface cross-linking step is a step of surface-cross-linking secondary particles (a hydrogel-like substance having an internally cross-linked structure) obtained by polymerizing a water-soluble ethylenically unsaturated monomer in the second or subsequent polymerization step of reversed-phase suspension polymerization. The water-absorbent resin particles of the present invention are obtained by mixing the secondary particles obtained in the polymerization step with a surface cross-linking agent and cross-linking the secondary particles (surface cross-linking reaction). This surface cross-linking reaction is preferably carried out in the presence of a surface cross-linking agent after the polymerization of the water-soluble ethylenically unsaturated monomer. In the present invention, primary particles and secondary particles are prepared, and then the secondary particles are subjected to a surface cross-linking reaction, thereby obtaining water-absorbent resin particles having improved properties such as saline water retention capacity, saline water absorption capacity under a load of 4.14 kPa, and 5-minute value of unpressurized DW.

[0071] From the viewpoint of improving the water retention capacity of physiological saline, the water absorption capacity of physiological saline under a load of 4.14 kPa, and the 5-minute value of no-pressure DW, in the surface crosslinking step, the molar ratio of the surface crosslinking agent to the water-soluble ethylenically unsaturated monomer (surface crosslinking agent / water-soluble ethylenically unsaturated monomer) is preferably in the range of 0.00001 to 0.001, more preferably in the range of 0.00005 to 0.00080, even more preferably in the range of 0.00010 to 0.00060, and still more preferably in the range of 0.00020 to 0.00040.

[0072] Examples of the surface cross-linking agent include compounds having two or more reactive functional groups. For example, polyols such as ethylene glycol, propylene glycol, 1,4-butanediol, trimethylolpropane, glycerin, polyoxyethylene glycol, polyoxypropylene glycol, and polyglycerin; polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, trimethylolpropane triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and (poly)glycerol polyglycidyl ether; epichlorohydrin, epibromohydrin, α-methylepichlorohydrin, isocyanate compounds such as 2,4-tolylene diisocyanate and hexamethylene diisocyanate; oxetane compounds such as 3-methyl-3-oxetanemethanol, 3-ethyl-3-oxetanemethanol, 3-butyl-3-oxetanemethanol, 3-methyl-3-oxetaneethanol, 3-ethyl-3-oxetaneethanol and 3-butyl-3-oxetaneethanol; oxazoline compounds such as 1,2-ethylenebisoxazoline; carbonate compounds such as ethylene carbonate; and hydroxyalkylamide compounds such as bis[N,N-di(β-hydroxyethyl)]adipamide. Among these surface cross-linking agents, preferred are polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, trimethylolpropane triglycidyl ether, (poly)propylene glycol polyglycidyl ether, (poly)glycerol polyglycidyl ether, etc. These surface cross-linking agents may be used alone or in combination of two or more.

[0073] As a method for adding the surface crosslinking agent, the surface crosslinking agent may be added as it is or as an aqueous solution, or, if necessary, may be added as a solution using a hydrophilic organic solvent as a solvent. Examples of the hydrophilic organic solvent include lower alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, etc.; ketones such as acetone, methyl ethyl ketone, etc.; ethers such as diethyl ether, dioxane, tetrahydrofuran, etc.; amides such as N,N-dimethylformamide, etc.; sulfoxides such as dimethyl sulfoxide, etc. These hydrophilic organic solvents may be used alone, or two or more types may be used in combination, or as a mixed solvent with water.

[0074] The timing of addition of the surface crosslinking agent may be after the polymerization reaction of the water-soluble ethylenically unsaturated monomer has almost completely finished, and the surface crosslinking agent is added in the presence of water in a range of preferably 1 to 400 parts by mass, more preferably 5 to 100 parts by mass, further preferably 10 to 50 parts by mass, and still further preferably 15 to 35 parts by mass, relative to 100 parts by mass of the water-soluble ethylenically unsaturated monomer. Note that the amount of water means the total amount of water contained in the reaction system and water used as necessary when adding the surface crosslinking agent.

[0075] The reaction temperature in the surface crosslinking reaction is preferably 50 to 250° C., more preferably 60 to 180° C., further preferably 60 to 140° C., and even more preferably 70 to 120° C. The reaction time of the surface crosslinking reaction is preferably 1 to 300 minutes, and more preferably 5 to 200 minutes.

[0076] <Drying Step> After the above-described reversed-phase suspension polymerization is performed, a drying step may be included in which water, hydrocarbon dispersion medium, and the like are removed by distillation by applying energy such as heat from the outside. When dehydrating the hydrogel after reversed-phase suspension polymerization, the system in which the hydrogel is dispersed in the hydrocarbon dispersion medium is heated, and the water and hydrocarbon dispersion medium are temporarily distilled out of the system by azeotropic distillation. At this time, if only the distilled hydrocarbon dispersion medium is returned to the system, continuous azeotropic distillation becomes possible. In this case, the temperature in the system during drying is maintained below the azeotropic temperature with the hydrocarbon dispersion medium, which is preferable from the viewpoint of preventing deterioration of the resin. Subsequently, water and hydrocarbon dispersion medium are distilled off to obtain water-absorbent resin particles. By controlling the processing conditions of this drying step after polymerization to adjust the amount of dehydration, it is possible to control the various properties of the obtained water-absorbent resin particles.

[0077] In the drying step, the drying treatment by distillation may be carried out under normal pressure or under reduced pressure. Moreover, from the viewpoint of increasing the drying efficiency, it may be carried out under a gas flow such as nitrogen. When the drying treatment is carried out under normal pressure, the drying temperature is preferably 70 to 250°C, more preferably 80 to 180°C, even more preferably 80 to 140°C, and even more preferably 90 to 130°C. Moreover, when the drying treatment is carried out under reduced pressure, the drying temperature is preferably 40 to 160°C, more preferably 50 to 110°C.

[0078] In addition, when the surface cross-linking step using a surface cross-linking agent is carried out after the polymerization of monomers by reverse phase suspension polymerization, the drying step by distillation described above is carried out after the surface cross-linking step is completed. Alternatively, the surface cross-linking step and the drying step may be carried out simultaneously.

[0079] The water-absorbent resin particles obtained by the production method of the present invention may contain additives according to the purpose. Examples of such additives include inorganic powders, surfactants, oxidizing agents, reducing agents, metal chelating agents, radical chain inhibitors, antioxidants, antibacterial agents, and the like. For example, inorganic powders may be used to further improve the fluidity of the water-absorbent resin particles. The amount of inorganic powder used is preferably in the range of 0.01 to 5 parts by mass, more preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the water-absorbent resin particles.

[0080] 2. Water-absorbent resin particles Among the methods for producing water-absorbent resin particles of the present invention described above, by adopting preferable conditions from the viewpoint of improving the water retention capacity of physiological saline solution, the water absorption capacity of physiological saline solution under a load of 4.14 kPa, and the 5-minute value of no-pressure DW, it becomes possible to suitably produce water-absorbent resin particles having, for example, the following properties (A) to (C). For example, in the method for producing water-absorbent resin particles, it is preferable to satisfy the preferable storage moduli in the first and second stages described above.

[0081] (A) The saline water retention capacity is 50 g / g or more and 80 g / g or less. (B) The saline water absorption capacity under a load of 4.14 kPa is 15 g / g or more and 40 g / g or less. (C) The 5-minute value of the non-pressurized DW is 50 mL / g or more and 80 mL / g or less.

[0082]

[0113] The (A) physiological saline water retention capacity of the water-absorbent resin particles of the present invention is preferably 50 g / g or more, and is also preferably 80 g / g or less, more preferably 70 g / g or less, and further preferably 60 g / g or less, and a preferred range is 50 to 70 g / g, and a more preferred range is 50 to 60 g / g, etc.

[0083]

[0113] Furthermore, (B) the water absorption amount of physiological saline solution under a load of 4.14 kPa of the water-absorbent resin particle of the present invention is preferably 15 g / g or more, more preferably 17 g / g or more, even more preferably 19 g / g or more, and is preferably 29 g / g or less, more preferably 27 g / g or less, even more preferably 25 g / g or less, and still more preferably 23 g / g or less, and a preferred range is 15 to 29 g / g, and a more preferred range is 17 to 25 g / g, etc.

[0084] The 5-minute value of the (C) no-pressure DW of the present invention is preferably 50 mL / g or more, more preferably 53 mL / g or more, even more preferably 55 mL / g or more, and particularly preferably 58 mL / g or more, and is preferably 78 mL / g or less, more preferably 73 mL / g or less, and even more preferably 68 mL / g or less, and is preferably in the range of 50 to 78 mL / g, and more preferably 58 to 68 mL / g, etc.

[0085] The water retention capacity of the water-absorbent resin particles in physiological saline, the water absorption capacity of physiological saline under a load of 4.14 kPa, and the 5-minute value of the DW without pressure are measured by the measurement methods described in the Examples.

[0086] The physiological saline water absorption capacity of the water-absorbent resin particles is preferably in the following ranges. The physiological saline water absorption capacity is, for example, preferably 30 g / g or more, 35 g / g or more, 40 g / g or more, 45 g / g or more, 50 g / g or more, 55 g / g or more, or 60 g / g or more. The physiological saline water absorption capacity is, for example, preferably 90 g / g or less, 85 g / g or less, 80 g / g or less, or 75 g / g or less. The physiological saline water absorption capacity is preferably 30 to 90 g / g, more preferably 40 to 80 g / g, and even more preferably 60 to 75 g / g. The method for measuring the physiological saline water absorption capacity will be described in detail in the examples below.

[0087] The water absorption rate of the water-absorbent resin particles for physiological saline is preferably in the following ranges. The water absorption rate is, for example, preferably 70 seconds or less, 60 seconds or less, 50 seconds or less, 45 seconds or less, or 40 seconds or less. The water absorption rate is, for example, preferably 20 seconds or more, 25 seconds or more, or 30 seconds or more. The water absorption rate is preferably 20 to 70 seconds, more preferably 25 to 60 seconds, and even more preferably 30 to 50 seconds. The water absorption rate can be measured at room temperature (25±2°C). The method for measuring the water absorption rate will be described in detail in the examples below.

[0088] The water-absorbent resin particles of the present invention are constituted by crosslinking a polymer of a water-soluble ethylenically unsaturated monomer, that is, by a crosslinked polymer having structural units derived from a water-soluble ethylenically unsaturated monomer.

[0089] The water-absorbent resin particles of the present invention are in the form (secondary particles) of aggregates of fine particles (primary particles). Examples of the shape of the primary particles include substantially spherical, irregularly crushed, and plate-like shapes. The water-absorbent resin particles of the present invention, which are secondary particles, may have various shapes. Examples of the shape of the water-absorbent resin particles include granular, substantially spherical, irregularly crushed, plate-like, fibrous, flake-like shapes, and shapes obtained by aggregating these resins. The water-absorbent resin particles are preferably granular, substantially spherical, irregularly crushed, fibrous, or shapes obtained by aggregating these resins.

[0090] The median particle diameter of the water-absorbent resin particles is preferably 200 μm or more, 250 μm or more, 280 μm or more, 300 μm or more, or 320 μm or more. From the same viewpoint, the median particle diameter is preferably 700 μm or less, 600 μm or less, 550 μm or less, 500 μm or less, 450 μm or less, or 400 μm or less. That is, the median particle diameter is preferably 200 to 700 μm, preferably 200 to 600 μm, more preferably 250 to 500 μm, even more preferably 300 to 450 μm, and even more preferably 320 to 400 μm.

[0091] The median particle size of the water-absorbent resin particles can be measured using a JIS standard sieve, and specifically, it is a value measured by the method described in the examples.

[0092] 3. Absorbent Material, Absorbent Articles The water-absorbing resin particles of the present invention constitute an absorbent material used in hygiene materials such as sanitary products and disposable diapers, and are suitably used in absorbent articles containing the absorbent material.

[0093] The absorbent of the present invention contains the water-absorbent resin particles of the present invention. The absorbent may further contain hydrophilic fibers. Examples of the absorbent's configuration include a sheet-like structure in which water-absorbent resin particles are fixed on a nonwoven fabric or between multiple nonwoven fabrics, a mixed dispersion obtained by mixing water-absorbent resin particles and hydrophilic fibers to form a uniform composition, a sandwich structure in which water-absorbent resin particles are sandwiched between layered hydrophilic fibers, and a structure in which water-absorbent resin particles and hydrophilic fibers are wrapped in tissue. The absorbent may also contain other components, such as adhesive binders such as heat-fusible synthetic fibers, hot-melt adhesives, and adhesive emulsions, to improve the shape retention of the absorbent.

[0094] The basis weight of the water-absorbent resin particles in the absorbent body of the present invention is 50 g / m 2 More than 400g / m 2 The basis weight is preferably 100 g / m or less. 2 More preferably, 120 g / m 2 More preferably, 140 g / m 2 or more, and preferably 300 g / m 2 or less, more preferably 250 g / m 2 More preferably 200 g / m or less 2 The following is the result.

[0095] The hydrophilic fiber may be at least one selected from the group consisting of finely ground wood pulp, cotton, cotton linter, rayon, cellulose acetate, polyamide, polyester, and polyolefin. Examples include cellulose fibers such as cotton-like pulp obtained from wood, mechanical pulp, chemical pulp, and semi-chemical pulp; artificial cellulose fibers such as rayon and acetate; and fibers made of synthetic resins such as hydrophilically treated polyamide, polyester, and polyolefin. The average fiber length of the hydrophilic fiber is usually 0.1 to 10 mm, or may be 0.5 to 5 mm.

[0096] The basis weight of the hydrophilic fiber in the absorbent body of the present invention is 50 g / m 2 800g / m or more 2 The basis weight is preferably 100 g / m or less. 2More preferably, 120 g / m 2 More preferably, 140 g / m 2 and preferably 700 g / m 2 or less, more preferably 600 g / m 2 More preferably 500 g / m or less 2 The following is the result.

[0097] The content of the water-absorbent resin particles in the absorbent body is preferably 5 to 100% by mass, more preferably 10 to 95% by mass, even more preferably 20 to 90% by mass, and even more preferably 30 to 80% by mass.

[0098] The absorbent article of the present invention can be produced by holding an absorbent body using the water-absorbent resin particles of the present invention between a liquid-permeable sheet (top sheet) through which liquid can pass and a liquid-impermeable sheet (back sheet) through which liquid cannot pass. The liquid-permeable sheet is arranged on the side that comes into contact with the body, and the liquid-impermeable sheet is arranged on the opposite side that comes into contact with the body.

[0099] Examples of liquid-permeable sheets include air-through, spunbond, chemical-bond, and needle-punched nonwoven fabrics made of fibers such as polyethylene, polypropylene, and polyester, as well as porous synthetic resin sheets. Examples of liquid-impermeable sheets include synthetic resin films made of resins such as polyethylene, polypropylene, and polyvinyl chloride. The liquid-permeable sheet is preferably at least one selected from the group consisting of thermal-bonded nonwoven fabrics, air-through nonwoven fabrics, spunbonded nonwoven fabrics, and spunbonded / meltblown / spunbonded nonwoven fabrics.

[0100] The basis weight of the liquid permeable sheet is 5 g / m 2 More than 100g / m 2 Preferably, it is 10 g / m or less. 2 60g / m or more 2It is more preferable that the liquid-permeable sheet has a surface embossed or perforated to improve the liquid diffusibility. The embossing or perforation can be carried out by a known method.

[0101] Examples of liquid-impermeable sheets include sheets made of synthetic resins such as polyethylene, polypropylene, and polyvinyl chloride; sheets made of nonwoven fabrics such as spunbond / meltblown / spunbond (SMS) nonwoven fabrics in which a water-resistant meltblown nonwoven fabric is sandwiched between high-strength spunbond nonwoven fabrics; and sheets made of composite materials of these synthetic resins and nonwoven fabrics (for example, spunbond nonwoven fabrics, spunlace nonwoven fabrics). As the liquid-impermeable sheet, a sheet made of a synthetic resin mainly composed of low-density polyethylene (LDPE) resin can also be used. The liquid-impermeable sheet has, for example, a basis weight of 10 to 50 g / m. 2 The sheet may be made of a synthetic resin.

[0102] The absorbent article preferably comprises a laminate having an absorbent body containing water-absorbent resin particles and a core wrap sandwiching the absorbent body from above and below, a liquid-permeable sheet disposed on the upper surface of the laminate, and a liquid-impermeable sheet disposed on the surface of the laminate opposite to the liquid-permeable sheet side.

[0103] 4. Additional Notes This specification includes at least the inventions shown in (1) to (14) below: (1) A method for producing water-absorbent resin particles by reverse-phase suspension polymerization of a water-soluble ethylenically unsaturated monomer using a radical polymerization initiator, wherein at least one of the radical polymerization initiators is an azo-based compound, and the reverse-phase suspension polymerization comprises two or more polymerization stages, wherein in a first polymerization stage, (a) an internal crosslinking agent is used in an amount of 0.01 millimol or more and 0.11 millimol or less per mole of the water-soluble ethylenically unsaturated monomer used in the first polymerization stage, and in a second polymerization stage, (b) an internal crosslinking agent is used in an amount of 0 millimol or more and 0.042 millimol or less per mole of the water-soluble ethylenically unsaturated monomer used in the second polymerization stage, and (c) an azo-based compound of 0.38 millimol or less per mole of the water-soluble ethylenically unsaturated monomer used in the second polymerization stage, and the method for producing water-absorbent resin particles comprises a surface crosslinking step after the second or subsequent polymerization stages. (2) The method for producing water-absorbent resin particles according to the above (1), wherein the amount of the internal crosslinking agent used in the first-stage polymerization step is 0.01 to 0.11 millimoles, 0.02 to 0.09 millimoles, 0.03 to 0.075 millimoles, or 0.04 to 0.06 millimoles relative to 1 mole of the water-soluble ethylenically unsaturated monomer used in the first-stage polymerization. (3) The method for producing water-absorbent resin particles according to the above (1) or (2), wherein at least one of the radical polymerization initiators used in the first-stage polymerization step is an azo compound, and the amount of the azo compound used is 0 to 1.0 millimoles, 0 to 0.50 millimoles, 0.10 to 0.38 millimoles, or 0.20 to 0.35 millimoles relative to 1 mole of the water-soluble ethylenically unsaturated monomer used in the first-stage polymerization. (4) The method for producing water-absorbent resin particles according to any one of the above (1) to (3), wherein in the second-stage polymerization step, an amount of the internal crosslinking agent used is 0 to 0.042 millimoles, 0 to 0.038 millimoles, 0 to 0.032 millimoles, 0 to 0.030 millimoles, or 0 to 0.025 millimoles relative to 1 mole of the water-soluble ethylenically unsaturated monomer used in the second-stage polymerization.(5) The method for producing water-absorbent resin particles according to any one of (1) to (4), wherein in the second-stage polymerization step, the amount of the azo compound used is 0 to 0.38 millimoles, 0 to 0.35 millimoles, 0.05 to 0.35 millimoles, or 0.10 to 0.35 millimoles relative to 1 mole of the water-soluble ethylenically unsaturated monomer used in the second-stage polymerization. (6) The method for producing water-absorbent resin particles according to any one of (1) to (5), wherein the primary particles obtained in the first-stage polymerization step have a storage modulus of 10 Pa or more and 200 Pa or less when swollen 40 times with ion-exchanged water, and the secondary particles obtained in the second or subsequent polymerization steps have a storage modulus of 5 Pa or more and 200 Pa or less when swollen 40 times with ion-exchanged water. (7) A method for producing water-absorbent resin particles according to any one of (1) to (6) above, wherein the storage modulus of a gel of the primary particles obtained in the first-stage polymerization step when swollen 40 times with ion-exchanged water is 15 to 150 Pa, or 20 to 100 Pa. (8) A method for producing water-absorbent resin particles according to any one of (1) to (7) above, wherein the storage modulus of a gel of the secondary particles obtained in the second-stage polymerization step when swollen 40 times with ion-exchanged water is 20 to 190 Pa, 20 to 170 Pa, 30 to 150 Pa, or 30 to 100 Pa. (9) Water-absorbent resin particles which are crosslinked polymers of water-soluble ethylenically unsaturated monomers, the water-absorbent resin particles having the following properties (A) to (C): (A) A water retention capacity of physiological saline is 50 g / g or more and 80 g / g or less. (B) The physiological saline water absorption capacity under a load of 4.14 kPa is 15 g / g or more and 40 g / g or less. (C) The 5-minute value of DW without pressure is 50 mL / g or more and 80 mL / g or less. (10) The water-absorbent resin particles according to (9) above, wherein the physiological saline water retention capacity of the water-absorbent resin particles is 50 to 70 g / g, or 50 to 60 g / g. (11) The water-absorbent resin particles according to (9) or (10) above, wherein the physiological saline water absorption capacity of the water-absorbent resin particles under a load of 4.14 kPa is 15 to 29 g / g, or 17 to 25 g / g. (12) The water-absorbent resin particles according to any of (9) to (11) above, wherein the 5-minute value of DW without pressure of the water-absorbent resin particles is 50 to 78 mL / g, or 58 to 68 mL / g.(13) The water-absorbent resin particles according to any one of (9) to (12) above, wherein the water-absorbent resin particles have a saline water absorption capacity of 40 to 80 g / g or 60 to 75 g / g. (14) The water-absorbent resin particles according to any one of (9) to (13) above, wherein the water-absorbent resin particles have a saline water absorption speed of 20 to 70 seconds, 25 to 60 seconds, or 30 to 50 seconds.

[0104] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0105] <Production of water-absorbent resin particles> (Example 1) [First-stage polymerization step] A round-bottomed cylindrical separable flask with an inner diameter of 11 cm and a capacity of 2 L was prepared, equipped with a reflux condenser, a dropping funnel, a nitrogen gas inlet tube, and a stirring blade having two stages of four inclined paddle blades with a blade diameter of 5 cm as a stirrer. 293 g of n-heptane was added to this flask as a hydrocarbon dispersion medium, and 0.782 g of maleic anhydride-modified ethylene-propylene copolymer (Hiwax 1105A, Mitsui Chemicals, Inc.) was added as a polymer dispersant. The mixture was heated to 80 ° C. with stirring to dissolve the dispersant, and then cooled to 50 ° C.

[0106] In a 300 mL beaker was placed 92.0 g (1.03 mol) of an 80.5 mass % aqueous acrylic acid solution as a water-soluble ethylenically unsaturated monomer, and while cooling from the outside, 110.1 g of a 28 mass % aqueous sodium hydroxide solution was added dropwise to carry out 75 mol % neutralization, followed by adding and dissolving 0.092 g (0.339 mmol) of 2,2′-azobis(2-amidinopropane) dihydrochloride and 0.028 g (0.102 mmol) of potassium persulfate as water-soluble radical polymerization initiators, 0.0101 g (0.058 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent, and 37.2 g of ion-exchanged water, to prepare a first-stage aqueous monomer solution.

[0107] The aqueous solution prepared above was then added to a separable flask and stirred for 10 minutes, after which a surfactant solution prepared by heating and dissolving 0.828 g of a sucrose stearate ester with an HLB of 3 (Ryoto Sugar Ester S-370, Mitsubishi-Kagaku Foods Corporation) as a surfactant in 7.45 g of n-heptane was further added, and the system was thoroughly purged with nitrogen while stirring at a stirrer rotation speed of 500 rpm.The flask was then immersed in a water bath at 70°C to raise the temperature, and polymerization was carried out for 60 minutes, thereby obtaining a first-stage polymerization slurry liquid containing primary particles.

[0108] [Second-Stage Polymerization Step] In a 500 mL beaker was placed 128.8 g (1.44 mol) of an 80.5 mass % aqueous acrylic acid solution as a water-soluble ethylenically unsaturated monomer, and while cooling from the outside, 154.2 g of a 28 mass % aqueous sodium hydroxide solution was added dropwise to carry out 75 mol % neutralization. Thereafter, 0.064 g (0.237 mmol) of 2,2′-azobis(2-amidinopropane) dihydrochloride as a water-soluble radical polymerization initiator, 0.039 g (0.143 mmol) of potassium persulfate, and 6.49 g of ion-exchanged water were added and dissolved to prepare a second-stage aqueous monomer solution.

[0109] The contents of the separable flask were cooled to 25°C while stirring at a stirrer speed of 1000 rpm, and then the entire amount of the second-stage aqueous solution was added to the first-stage polymerization slurry. The atmosphere in the system was replaced with nitrogen for 30 minutes, and the flask was again immersed in a water bath at 70°C to raise the temperature, and the polymerization reaction was carried out for 60 minutes. By the above operations, a hydrogel after second-stage polymerization was obtained.

[0110] [Surface Crosslinking] The flask was then immersed in an oil bath set at 125°C, and 176.6 g of water was extracted from the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Then, 0.491 g of a 45 mass% aqueous solution of pentasodium diethylenetriaminepentaacetate and 2.58 g of a 3 mass% aqueous solution of sodium sulfite were added to the flask with stirring to obtain a second-stage polymerization slurry containing secondary particles.

[0111] Thereafter, the flask was again immersed in the oil bath set to 125°C, and 80.5 g (257.1 g in total) of water was further extracted from the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Thereafter, 5.52 g (0.634 mmol) of a 2 mass% aqueous solution of ethylene glycol diglycidyl ether was added as a surface crosslinking agent to the flask, and the mixture was maintained at 83°C for 2 hours.

[0112] Thereafter, n-heptane was evaporated at 125°C to dry the product, thereby obtaining a dried product. This dried product was passed through a sieve with an opening of 850 µm, and 0.2 mass% of amorphous silica (Toxil NP-S, Oriental Silicas Corporation) was mixed with the dried product, thereby obtaining 235.2 g of water-absorbent resin particles. The median particle diameter of the water-absorbent resin particles was 347 µm.

[0113] The amount of saline solution absorbed by the water-absorbent resin particles of Example 1 was 64 g / g, and the water-absorption speed of the water-absorbent resin particles was 35 seconds.

[0114] (Example 2) Except for changing the amount of water extracted to outside the system by the second azeotropic distillation to 90.2 g (total 266.8 g), the same procedure as in Example 1 was carried out to obtain 223.4 g of water-absorbent resin particles. The median particle diameter of the water-absorbent resin particles was 339 μm.

[0115] The amount of saline solution absorbed by the water-absorbent resin particles of Example 2 was 72 g / g, and the water-absorption speed of the water-absorbent resin particles was 33 seconds.

[0116] (Example 3) The amount of 2,2'-azobis(2-amidinopropane) dihydrochloride added to the second-stage aqueous monomer solution was changed to 0.129 g (0.475 mmol), the amount of ion-exchanged water added was changed to 6.42 g, and the amount of water extracted from the system by the second azeotropic distillation was changed to 80.3 g (total 256.9 g), in the same manner as in Example 1, to obtain 226.0 g of water-absorbent resin particles. The median particle diameter of the water-absorbent resin particles was 353 μm.

[0117] The amount of saline solution absorbed by the water-absorbent resin particles of Example 3 was 71 g / g, and the water-absorption speed of the water-absorbent resin particles was 39 seconds.

[0118] (Example 4) 224.3 g of water-absorbent resin particles were obtained in the same manner as in Example 1, except that 0.0052 g (0.030 mmol) of ethylene glycol diglycidyl ether was added as an internal cross-linking agent to the second-stage aqueous monomer solution, the amount of ion-exchanged water added to the second-stage aqueous monomer solution was changed to 6.48 g, and the amount of water extracted to the outside of the system by the second azeotropic distillation was changed to 83.9 g (total 260.6 g). The median particle diameter of the water-absorbent resin particles was 361 μm.

[0119] The amount of saline solution absorbed by the water-absorbent resin particles of Example 4 was 68 g / g, and the water-absorption speed of the water-absorbent resin particles was 39 seconds.

[0120] (Example 5) Except for changing the amount of water extracted to outside the system by the second azeotropic distillation to 89.9 g (total 266.5 g) and changing the amount of 2 mass % ethylene glycol diglycidyl ether aqueous solution added to 8.28 g (0.951 mmol), the same procedure as in Example 1 was carried out to obtain 225.7 g of water-absorbent resin particles. The median particle diameter of the water-absorbent resin particles was 360 μm.

[0121] The amount of saline solution absorbed by the water-absorbent resin particles of Example 5 was 72 g / g, and the water-absorption speed of the water-absorbent resin particles was 40 seconds.

[0122] (Example 6) 221.5 g of water-absorbent resin particles were obtained in the same manner as in Example 1, except that 0.0129 g (0.122 mmol) of sodium hypophosphite was added as a chain transfer agent to the second-stage aqueous monomer solution, the amount of ion-exchanged water added to the second-stage aqueous monomer solution was changed to 6.47 g, and the amount of water extracted to the outside of the system by the second azeotropic distillation was changed to 82.9 g (total 259.5 g). The median particle diameter of the water-absorbent resin particles was 369 μm.

[0123] The amount of saline solution absorbed by the water-absorbent resin particles of Example 6 was 64 g / g, and the water-absorption speed of the water-absorbent resin particles was 37 seconds.

[0124] (Example 7) Except for changing the amount of ethylene glycol diglycidyl ether added to the first-stage aqueous monomer solution to 0.0184 g (0.106 mmol) and changing the amount of water extracted to the outside of the system by the second azeotropic distillation to 84.7 g (total 261.4 g), the same procedure as in Example 1 was carried out to obtain 220.1 g of water-absorbent resin particles. The median particle diameter of the water-absorbent resin particles was 423 μm.

[0125] The amount of saline solution absorbed by the water-absorbent resin particles of Example 7 was 67 g / g, and the water-absorption speed of the water-absorbent resin particles was 48 seconds.

[0126] Example 8 [First-stage polymerization step] A round-bottomed cylindrical separable flask with an inner diameter of 11 cm and a capacity of 2 L was prepared, equipped with a reflux condenser, a dropping funnel, a nitrogen gas inlet tube, and a stirrer with a stirring blade having two stages of four inclined paddle blades with a blade diameter of 5 cm. 294 g of n-heptane was added to this flask as a hydrocarbon dispersion medium, and 0.644 g of maleic anhydride-modified ethylene-propylene copolymer (Mitsui Chemicals, Inc., Hiwax 1105A) was added as a polymeric dispersant. The mixture was heated to 80 ° C. with stirring to dissolve the dispersant, and then cooled to 50 ° C.

[0127] In a 300 mL beaker was placed 92.0 g (1.03 mol) of an 80.5 mass % aqueous acrylic acid solution as a water-soluble ethylenically unsaturated monomer, and while cooling from the outside, 110.1 g of a 28 mass % aqueous sodium hydroxide solution was added dropwise to carry out 75 mol % neutralization, followed by adding and dissolving 0.074 g (0.272 mmol) of potassium persulfate as a water-soluble radical polymerization initiator, 0.0046 g (0.026 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent, and 37.3 g of ion-exchanged water, to prepare a first-stage aqueous monomer solution.

[0128] The aqueous solution prepared above was then added to a separable flask and stirred for 10 minutes, after which a surfactant solution prepared by heating and dissolving 0.644 g of a sucrose stearate ester with an HLB of 3 (Ryoto Sugar Ester S-370, Mitsubishi-Kagaku Foods Corporation) as a surfactant in 5.8 g of n-heptane was further added, and the system was thoroughly purged with nitrogen while stirring at a stirrer rotation speed of 500 rpm.The flask was then immersed in a water bath at 70°C to raise the temperature, and polymerization was carried out for 60 minutes, thereby obtaining a first-stage polymerization slurry liquid containing primary particles.

[0129] [Second-Stage Polymerization Step] In a 500 mL beaker was placed 128.8 g (1.44 mol) of an 80.5 mass % aqueous acrylic acid solution as a water-soluble ethylenically unsaturated monomer, and while cooling from the outside, 154.2 g of a 28 mass % aqueous sodium hydroxide solution was added dropwise to carry out 75 mol % neutralization. Thereafter, 0.064 g (0.237 mmol) of 2,2′-azobis(2-amidinopropane) dihydrochloride as a water-soluble radical polymerization initiator, 0.039 g (0.143 mmol) of potassium persulfate, and 6.49 g of ion-exchanged water were added and dissolved to prepare a second-stage aqueous monomer solution.

[0130] The contents of the separable flask were cooled to 25°C while stirring at a stirrer speed of 1000 rpm, and then the entire amount of the second-stage aqueous solution was added to the first-stage polymerization slurry. The atmosphere in the system was replaced with nitrogen for 30 minutes, and the flask was again immersed in a water bath at 70°C to raise the temperature, and the polymerization reaction was carried out for 60 minutes. By the above operations, a hydrogel after second-stage polymerization was obtained.

[0131] [Surface Crosslinking] The flask was then immersed in an oil bath set at 125°C, and 176.6 g of water was extracted from the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Then, 0.491 g of a 45 mass% aqueous solution of pentasodium diethylenetriaminepentaacetate and 2.58 g of a 3 mass% aqueous solution of sodium sulfite were added to the flask with stirring to obtain a second-stage polymerization slurry containing secondary particles.

[0132] Thereafter, the flask was again immersed in the oil bath set to 125°C, and 79.7 g (total 256.4 g) of water was further extracted from the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Thereafter, 5.52 g (0.634 mmol) of a 2 mass% aqueous solution of ethylene glycol diglycidyl ether was added as a surface crosslinking agent to the flask, and the mixture was maintained at 83°C for 2 hours.

[0133] Thereafter, n-heptane was evaporated at 125°C to dry the product, thereby obtaining a dried product. This dried product was passed through a sieve with an opening of 850 µm, and 0.2 mass% of amorphous silica (Toxil NP-S, Oriental Silicas Corporation) was mixed with the dried product, thereby obtaining 214.9 g of water-absorbent resin particles. The median particle diameter of the water-absorbent resin particles was 372 µm.

[0134] The amount of saline solution absorbed by the water-absorbent resin particles of Example 8 was 73 g / g, and the water-absorption speed of the water-absorbent resin particles was 41 seconds.

[0135] Comparative Example 1 224.4 g of water-absorbent resin particles were obtained in the same manner as in Example 8, except that 2,2'-azobis(2-amidinopropane) dihydrochloride was not added to the second-stage aqueous monomer solution, the amount of potassium persulfate added to the second-stage aqueous monomer solution was changed to 0.090 g (0.334 mmol), 0.0116 g (0.067 mmol) of ethylene glycol diglycidyl ether was added to the second-stage aqueous monomer solution, and the amount of water extracted to the outside of the system by the second azeotropic distillation was changed to 95.4 g (total 272.0 g). The median particle diameter of the water-absorbent resin particles was 347 μm.

[0136] The amount of saline solution absorbed by the water-absorbent resin particles of Comparative Example 1 was 67 g / g, and the water-absorption speed of the water-absorbent resin particles was 39 seconds.

[0137] (Comparative Example 2) [First-stage polymerization step] A round-bottomed cylindrical separable flask with an inner diameter of 11 cm and a capacity of 2 L was prepared, equipped with a reflux condenser, a dropping funnel, a nitrogen gas inlet tube, and a stirrer with a stirring blade having two stages of four inclined paddle blades with a blade diameter of 5 cm. 265 g of n-heptane was added to this flask as a hydrocarbon dispersion medium, and 0.736 g of maleic anhydride-modified ethylene-propylene copolymer (Mitsui Chemicals, Inc., Hiwax 1105A) was added as a polymeric dispersant. The mixture was heated to 80 ° C. with stirring to dissolve the dispersant, and then cooled to 50 ° C.

[0138] In a 300 mL beaker was placed 92.0 g (1.03 mol) of an 80.5 mass% aqueous acrylic acid solution as a water-soluble ethylenically unsaturated monomer, and while cooling from the outside, 110.1 g of a 28 mass% aqueous sodium hydroxide solution was added dropwise to carry out 75 mol% neutralization. Thereafter, 0.092 g of hydroxyl ethyl cellulose (Sumitomo Seika Chemicals Co., Ltd., HECAW-15F) as a thickener, 0.092 g (0.339 mmol) of 2,2′-azobis(2-amidinopropane) dihydrochloride as a water-soluble radical polymerization initiator, 0.028 g (0.102 mmol) of potassium persulfate, 0.0046 g (0.026 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent, and 14.3 g of ion-exchanged water were added and dissolved to prepare a first-stage aqueous monomer solution.

[0139] The aqueous solution prepared above was then added to a separable flask and stirred for 10 minutes, after which a surfactant solution prepared by heating and dissolving 0.736 g of a sucrose stearate ester with an HLB of 3 (Ryoto Sugar Ester S-370, Mitsubishi-Kagaku Foods Corporation) as a surfactant in 6.62 g of n-heptane was further added, and the system was thoroughly purged with nitrogen while stirring at a stirrer rotation speed of 600 rpm.The flask was then immersed in a water bath at 70°C to raise the temperature, and polymerization was carried out for 60 minutes, thereby obtaining a first-stage polymerization slurry liquid containing primary particles.

[0140] [Second-Stage Polymerization Step] In a 500 mL beaker was placed 128.8 g (1.44 mol) of an 80.5 mass% aqueous acrylic acid solution as a water-soluble ethylenically unsaturated monomer, and while cooling from the outside, 154.2 g of a 28 mass% aqueous sodium hydroxide solution was added dropwise to carry out 75 mol% neutralization. Thereafter, 0.129 g (0.475 mmol) of 2,2′-azobis(2-amidinopropane) dihydrochloride and 0.039 g (0.143 mmol) of potassium persulfate as water-soluble radical polymerization initiators, 0.0116 g (0.067 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent, and 6.41 g of ion-exchanged water were added and dissolved to prepare a second-stage aqueous monomer solution.

[0141] The contents of the separable flask were cooled to 25°C while stirring at a stirrer speed of 1000 rpm, and then the entire amount of the second-stage aqueous solution was added to the first-stage polymerization slurry. The atmosphere in the system was replaced with nitrogen for 30 minutes, and the flask was again immersed in a water bath at 70°C to raise the temperature, and the polymerization reaction was carried out for 60 minutes. By the above operations, a hydrogel after second-stage polymerization was obtained.

[0142] [Surface Crosslinking] The flask was then immersed in an oil bath set at 125°C, and 176.6 g of water was extracted from the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Then, 0.393 g of a 45 mass% aqueous solution of pentasodium diethylenetriaminepentaacetate and 4.42 g of a 3 mass% aqueous solution of sodium sulfite were added to the flask with stirring to obtain a second-stage polymerization slurry containing secondary particles.

[0143] Thereafter, the flask was again immersed in the oil bath set to 125°C, and 49.3 g (total 226.0 g) of water was further extracted from the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Thereafter, 4.42 g (0.507 mmol) of a 2 mass% aqueous solution of ethylene glycol diglycidyl ether was added as a surface crosslinking agent to the flask, and the mixture was maintained at 83°C for 2 hours.

[0144] Thereafter, n-heptane was evaporated at 125°C to dry the product, thereby obtaining a dried product. This dried product was passed through a sieve with an opening of 850 µm, and 0.2 mass% of amorphous silica (Toxil NP-S, Oriental Silicas Corporation) was mixed with the dried product, thereby obtaining 229.4 g of water-absorbent resin particles. The median particle diameter of the water-absorbent resin particles was 352 µm.

[0145] The amount of saline solution absorbed by the water-absorbent resin particles of Comparative Example 2 was 66 g / g, and the water-absorption speed of the water-absorbent resin particles was 36 seconds.

[0146] [Measurement of storage modulus of primary particles (gel swollen 40 times with ion-exchanged water)] In the production of water-absorbent resin particles, a first-stage polymerization slurry liquid was obtained. Thereafter, the reaction liquid was heated in an oil bath at 125°C, and water was extracted from the system by azeotropic distillation of n-heptane and water while refluxing n-heptane until the temperature inside the system reached 88°C. Thereafter, n-heptane was evaporated at 125°C to dry the product, thereby obtaining a dried product. This dried product was passed through a sieve with an opening of 850 μm, and 0.2% by mass of amorphous silica (Toxil NP-S, Oriental Silicas Corporation) was mixed with the dried product to obtain primary particles.

[0147] Next, the primary particles were swelled 40 times in ion-exchanged water to prepare a 40-fold swollen gel. Specifically, 195.0 g of ion-exchanged water was weighed into a 500 mL beaker. Next, the beaker containing the ion-exchanged water was placed in a MIYAMOTO CORPORATION jar tester (MJS-8S). A stirring blade with a stainless steel flat blade (7 cm horizontal length × 2.5 cm vertical length × 0.1 cm thickness) was attached and placed 0.5 cm above the bottom of the beaker, and the mixture was rotated at 500 rpm. Next, 5.0 g of the primary particles were added to the beaker while stirring to avoid the formation of lumps. One minute after addition, the rotation speed was changed to 300 rpm. Stirring was continued for one hour after addition to prepare a 40-fold swollen gel. This 40-fold swollen gel was transferred to a centrifuge tube and degassed by centrifugation at 2000 rpm for 10 minutes in a centrifuge (Kokusan Centrifuge Co., Ltd., product number H-36), and used as a measurement sample.

[0148] The storage modulus was measured by creep measurement using a stress-controlled rheometer (TA Instruments Ltd., product number AR2000ex). The measurement temperature was 25°C, and the jig used was an aluminum parallel plate with a diameter of 60 mm (TA Instruments Ltd., product number 513600.901). The shear stress was measured at 0.7 Pa.

[0149] The measurement sample was measured using a 15 mL spoon and placed on the sample stage, taking care not to introduce air bubbles. The jig was then lowered so that the bottom of the jig was filled with the measurement sample, leaving a gap of 4000 μm between the jig and the sample stage. Any sample that protruded outside the jig was removed. Creep measurements were performed, and the storage modulus was calculated using Jeffreys underdamped ringing analysis. The results are shown in Table 1.

[0150] [Measurement of Storage Modulus of Secondary Particles (Gel Swelled 40 Times with Ion-Exchanged Water)] In the production of water-absorbent resin particles, a second-stage polymerization slurry was obtained. Thereafter, the reaction solution was heated in an oil bath at 125°C, and water was extracted from the system by azeotropic distillation of n-heptane and water while refluxing n-heptane until the temperature inside the system reached 88°C. The n-heptane was then evaporated at 125°C to dry the system, thereby obtaining a dried product. This dried product was passed through a sieve with an opening of 850 μm, and 0.2% by mass of amorphous silica (Toxil NP-S, Oriental Silicas Corporation) was mixed with the dried product to obtain secondary particles. The storage modulus was measured using the same procedures as in the storage modulus measurement method for primary particles. The results are shown in Table 1.

[0151] [Saline Water Retention Capacity] A cotton bag (membrane broadcloth No. 60, 100 mm wide x 200 mm long) containing 2.0 g of water-absorbent resin particles was placed in a 500 mL beaker. 500 g of a 0.9% by mass aqueous sodium chloride solution (saline) was poured into the cotton bag containing the water-absorbent resin particles all at once, taking care not to allow the bag to swell. The top of the cotton bag was tied with a rubber band and allowed to stand for 30 minutes to allow the water-absorbent resin particles to swell. After 30 minutes, the cotton bag was dehydrated for 1 minute using a dehydrator (manufactured by Kokusan Co., Ltd., product number: H-122) set to a centrifugal force of 167 G, and the mass Wa (g) of the cotton bag containing the swollen gel after dehydration was measured. The same procedure was performed without adding water-absorbent resin particles, and the empty mass Wb (g) of the cotton bag when wet was measured. The saline water retention capacity was calculated using the following formula. The results are shown in Table 1. Saline water retention capacity (g / g) = [Wa - Wb] / 2.0

[0152] [Five-minute value of DW without pressure] The five-minute value of DW without pressure of a water-absorbent resin particle was measured using a measuring device shown in Fig. 1. The measurement was carried out five times for one type of water-absorbent resin particle, and an average value of three measurement values ​​excluding the minimum value and the maximum value was calculated.

[0153] The measuring device comprises a burette unit 1, a conduit 5, a measurement table 13, a nylon mesh sheet 15, a stand 11, and a clamp 3. The burette unit 1 comprises a burette tube 21 with a scale, a rubber stopper 23 that seals the upper opening of the burette tube 21, a cock 22 connected to the lower tip of the burette tube 21, and an air introduction tube 25 and a cock 24 connected to the lower part of the burette tube 21. The burette unit 1 is fixed with the clamp 3. The flat measurement table 13 has a through-hole 13a with a diameter of 2 mm formed in its center and is supported by the height-adjustable stand 11. The through-hole 13a of the measurement table 13 and the cock 22 of the burette unit 1 are connected by a conduit 5. The inner diameter of the conduit 5 is 6 mm.

[0154] First, the stopcocks 22 and 24 of the burette part 1 were closed, and 0.9% by mass saline solution 50 adjusted to 25°C was poured into the burette tube 21 through the opening at the top of the burette tube 21. The concentration of the saline solution, 0.9% by mass, is based on the mass of the saline solution. After sealing the opening of the burette tube 21 with a rubber stopper 23, the stopcocks 22 and 24 were opened. The inside of the conduit 5 was filled with 0.9% by mass saline solution 50 while preventing air bubbles from entering. The height of the measurement table 13 was adjusted so that the height of the water surface of the 0.9% by mass saline solution 50 that had reached the through-hole 13a was the same as the height of the upper surface of the measurement table 13. After adjustment, the height of the water surface of the 0.9% by mass saline solution 50 in the burette tube 21 was read on the scale of the burette tube 21, and this position was designated as the zero point (the reading at 0 seconds).

[0155] A nylon mesh sheet 15 (100 mm x 100 mm, 250 mesh, approximately 50 μm thick) was laid near the through-hole 13 a on the measurement table 13, and a cylinder with an inner diameter of 30 mm and a height of 20 mm was placed in the center of the sheet. 1.00 g of water-absorbent resin particles 10 a was uniformly dispersed in the cylinder. Thereafter, the cylinder was carefully removed, and a sample in which the water-absorbent resin particles 10 a were dispersed in a circular pattern was obtained in the center of the nylon mesh sheet 15. Next, the nylon mesh sheet 15 on which the water-absorbent resin particles 10 a were placed was quickly moved so that its center was positioned at the position of the through-hole 13 a, without dissipating the water-absorbent resin particles 10 a, and measurement was started. The time when air bubbles were first introduced into the burette tube 21 from the air inlet tube 25 was defined as the start of water absorption (0 seconds).

[0156] The amount of 0.9% by mass saline solution 50 lost in the burette tube 21 (i.e., the amount of 0.9% by mass saline solution absorbed by the water-absorbent resin particles 10a) was sequentially read in 0.1 mL increments, and the amount of lost weight Wc (mL) of 0.9% by mass saline solution 50 5 minutes after the start of water absorption by the water-absorbent resin particles 10a was read. From Wc, the 5-minute value of the no-pressure DW was calculated using the following formula. The no-pressure DW is the amount of water absorbed per 1.00 g of the water-absorbent resin particles 10a. The results are shown in Table 1. 5-minute value of no-pressure DW (mL / g) = Wc / 1.00

[0157] [Water absorption under a load of 4.14 kPa] The water absorption of water-absorbent resin particles in physiological saline under a load of 4.14 kPa (water absorption under a load of 4.14 kPa) was measured using an apparatus outlined in FIG. 2. The water absorption under load was measured twice for one type of water-absorbent resin particle, and the average of the measured values ​​was calculated. The apparatus in FIG. 2 includes a burette unit 1, a clamp 3, a conduit 5, a stand 11, a measurement table 13, and a measurement unit 4 placed on the measurement table 13. The burette unit 1 includes a burette tube 21 having a scale, a rubber stopper 23 that seals the opening at the top of the burette tube 21, a cock 22 connected to the tip of the bottom of the burette tube 21, and an air introduction tube 25 and a cock 24 connected to the bottom of the burette tube 21. The burette unit 1 is fixed with a clamp 3. The flat measuring table 13 has a through-hole 13a with a diameter of 2 mm formed in its center, and is supported by a height-adjustable stand 11. The through-hole 13a of the measuring table 13 and the cock 22 of the burette part 1 are connected by a conduit 5. The inner diameter of the conduit 5 is 6 mm.

[0158] The measurement unit 4 has a cylinder 31 made of acrylic resin, a polyamide mesh 32 adhered to one opening of the cylinder 31, and a weight 33 that is movable up and down within the cylinder 31. The cylinder 31 is placed on the measurement table 13 via the polyamide mesh 32. The inner diameter of the cylinder 31 is 20 mm. The opening of the polyamide mesh 32 is 75 μm (200 mesh). The weight 33 has a diameter of 19 mm and a mass of 119.6 g, and can apply a load of 4.14 kPa to the water-absorbent resin particles 10a uniformly arranged on the polyamide mesh 32, as will be described later.

[0159] First, the stopcocks 22 and 24 of the burette part 1 were closed, and 0.9% by mass saline solution adjusted to 25°C was poured into the burette tube 21 through the opening at the top of the burette tube 21. Next, the top opening of the burette tube 21 was sealed with a rubber stopper 23, and then the stopcocks 22 and 24 were opened. The inside of the conduit 5 was filled with 0.9% by mass saline solution 50 while preventing air bubbles from entering. The height of the measurement table 13 was adjusted so that the height of the water surface of the 0.9% by mass saline solution 50 that had reached the through-hole 13a was the same as the height of the upper surface of the measurement table 13. After the adjustment, the height of the water surface of the 0.9% by mass saline solution 50 in the burette tube 21 was read on the scale of the burette tube 21, and this position was designated as the zero point (the reading at 0 seconds).

[0160] In the measurement unit 4, 0.10 g of water-absorbent resin particles 10a were uniformly arranged on the polyamide mesh 32 in the cylinder 31, a weight 33 was placed on the water-absorbent resin particles 10a, and the cylinder 31 was installed so that its center coincided with the conduit opening at the center of the measurement table 13. The amount of saline solution lost in the burette tube 21 (i.e., the amount of saline solution absorbed by the water-absorbent resin particles 10a) Wd (mL) 60 minutes after the water-absorbent resin particles 10a began to absorb saline solution from the conduit 5 was read, and the amount of saline solution absorbed by the water-absorbent resin particles 10a under a load of 4.14 kPa was calculated using the following formula. The results are shown in Table 1. Amount of saline solution absorbed under a load of 4.14 kPa (g / g) = Wd (mL) × 1.0028 [g / mL] (specific gravity of saline solution) / 0.10

[0161] [Saline Water Absorption] 500 g of 0.9% saline was weighed into a 500 mL beaker. Next, 2.0 g of water-absorbent resin particles were dispersed in the saline solution while stirring at 600 rpm using a magnetic stir bar (8 mm diameter x 30 mm length, no ring) to prevent lumps from forming. The mixture was left to stand for 60 minutes while stirring to allow the particles to swell sufficiently, yielding a dispersion containing a swollen gel. Next, the mass We [g] of a 75 μm standard sieve was measured, and the dispersion was passed through the standard sieve. The sieve was then tilted at an angle of approximately 30 degrees relative to the horizontal and left for 30 minutes to remove excess water. The mass Wf [g] of the sieve with the swollen gel remaining was measured, and the saline water absorption Wg [g / g] was calculated using the following formula: Saline Water Absorption Wg [g / g] = (Wf - We) / 2.0

[0162] [Median particle size] 50 g of water-absorbent resin particles were used for measuring the median particle size. JIS standard sieves were combined in the following order from top to bottom: a sieve with a mesh size of 710 μm, a sieve with a mesh size of 600 μm, a sieve with a mesh size of 500 μm, a sieve with a mesh size of 425 μm, a sieve with a mesh size of 300 μm, a sieve with a mesh size of 250 μm, a sieve with a mesh size of 150 μm, and a tray. The water-absorbent resin particles were placed on the top sieve and shaken for 10 minutes using a rotary shaker to classify them. After classification, the mass of the water-absorbent resin particles remaining on each sieve was calculated as a mass percentage relative to the total amount to determine the particle size distribution. With regard to this particle size distribution, the particles remaining on the sieve were integrated in order from the largest particle diameter, and the relationship between the sieve opening and the integrated value of the mass percentage of the water absorbent resin particles remaining on the sieve was plotted on a logarithmic probability paper. By connecting the plots on the probability paper with a straight line, the particle diameter corresponding to an integrated mass percentage of 50 mass% was determined to be the median particle diameter.

[0163] [Water Absorption Rate (Vortex Method)] The water absorption rate of water-absorbent resin particles in physiological saline was measured by the Vortex method using the following procedure. First, 50±0.1 g of physiological saline adjusted to a temperature of 25±0.2°C in a thermostatic water bath was weighed into a 100 mL beaker. Next, a vortex was generated by stirring at 600 rpm using a magnetic stir bar (8 mmφ×30 mm, without ring). 2.0±0.002 g of water-absorbent resin particles were added to the physiological saline all at once. The time [seconds] from the addition of the water-absorbent resin particles to the point at which the vortex on the liquid surface converged was measured, and this time was recorded as the water absorption rate of the water-absorbent resin particles.

[0164]

[0165] REFERENCE SIGNS LIST 1 burette part 3 clamp 4 measuring part 5 conduit 10a water-absorbent resin particles 11 stand 13 measuring table 13a through-hole 15 nylon mesh sheet 21 burette tube 22 cock 23 rubber stopper 24 cock 25 air introduction tube 31 cylinder 32 polyamide mesh 33 weight 50 saline solution

Claims

1. A method for producing water-absorbent resin particles by reversed-phase suspension polymerization of a water-soluble ethylenically unsaturated monomer using a radical polymerization initiator, wherein at least one of the radical polymerization initiators is an azo compound, and the reversed-phase suspension polymerization comprises two or more polymerization steps, and in the first polymerization step, (a) an internal crosslinking agent is used in an amount of 0.01 millimol or more and 0.11 millimol or less per mole of the water-soluble ethylenically unsaturated monomer used in the first polymerization step, and in the second polymerization step, (b) an internal crosslinking agent is used in an amount of 0 millimol or more and 0.042 millimol or less per mole of the water-soluble ethylenically unsaturated monomer used in the second polymerization step, and (c) an azo compound of 0.38 millimol or less per mole of the water-soluble ethylenically unsaturated monomer used in the second polymerization step, and a surface crosslinking step is provided after the second or subsequent polymerization steps.

2. The method for producing water-absorbent resin particles according to claim 1, wherein the primary particles obtained in the first polymerization step have a storage modulus of a gel swollen 40 times with ion-exchanged water of 10 Pa or more and 200 Pa or less, and the secondary particles obtained in the second or subsequent polymerization steps have a storage modulus of a gel swollen 40 times with ion-exchanged water of 5 Pa or more and 200 Pa or less.

3. The method for producing water-absorbent resin particles according to claim 1 or 2, wherein the water-absorbent resin particles have the following characteristics (A) to (C): (A) physiological saline water retention capacity is 50 g / g or more and 80 g / g or less. (B) physiological saline water absorption capacity under a load of 4.14 kPa is 15 g / g or more and 40 g / g or less. (C) 5-minute value of unpressurized DW is 50 mL / g or more and 80 mL / g or less.

4. A water-absorbent resin particle which is a crosslinked polymer of a water-soluble ethylenically unsaturated monomer, the water-absorbent resin particle having the following characteristics (A) to (C): (A) a saline water retention capacity of 50 g / g or more and 80 g / g or less; (B) a saline water absorption capacity under a load of 4.14 kPa of 15 g / g or more and 40 g / g or less; (C) a 5-minute value of unpressurized DW of 50 mL / g or more and 80 mL / g or less.

5. An absorbent comprising the water-absorbent resin particles according to claim 4.

6. An absorbent article comprising the absorbent body according to claim 5.

Citation Information

Patent Citations

  • Production of water absorbing resin

    JP1991227301A

  • Water-absorbing resin particle, absorber and absorptive article

    JP2020121297A

  • Water-absorbent resin particles, absorbent body, absorbent article, and liquid suction force measuring method

    JP7129490B2

  • Method for producing polyacrylic acid (SALT)-based water-absorbent resin

    WO2015163438A1

  • Water-absorbent resin and absorbent article

    WO2016006134A1

Cited By

  • Water absorbent resin particles, absorber, and absorbent article

    WO2025164342A1

  • Water-absorbent resin particles and method for producing same, absorbent body, and absorbent article

    WO2026211453A1

  • Method for producing water-absorbing resin particles

    WO2026211454A1