Composite coolant and use thereof in aerosol fire extinguishment
By loading chemical coolants on molecular sieves and utilizing their microchannel pores and large specific surface area, the problem of adsorption and decomposition of aerosol fire extinguishing agents during flame suppression and cooling is solved, achieving more efficient fire extinguishing capabilities and flame suppression effects, and avoiding Fire risk.
Patent Information
- Application Number
- PCT/CN2023/109949
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2023-07-28
- Publication Date
- 2024-10-24
AI Technical Summary
When existing aerosol fire extinguishing agents are used to extinguish flames and cool down, the physical cooling agent is easy to adsorb the aerosol, resulting in weakening the fire extinguishing ability, while the chemical coolant is easy to decompose, resulting in insufficient flame extinguishing and cooling capabilities, and may even cause fire problems.
A composite coolant is used, which is prepared by loading chemical coolants with fire extinguishing capabilities such as phosphates, potassium salts, halogens, etc. on the molecular sieve through a co-impregnation method. The microchannel pores and large specific surface area of the molecular sieve are used to achieve flame control. Effective adsorption and cooling.
It is possible to improve the fire-extinguishing capability and flame-extinguishing and cooling effect while maintaining structural stability, ensuring the effective adsorption and cooling of the aerosol jet flame, and enhancing the overall performance of the fire-extinguishing device.
Smart Images

Figure PCTCN2023109949-FTAPPB-I100001 
Figure PCTCN2023109949-FTAPPB-I100002
Abstract
Description
Composite coolant and its application in aerosol fire extinguishing Technical Field
[0001] The invention belongs to the technical field of fire fighting and extinguishing, and particularly relates to a composite coolant and application thereof in aerosol fire extinguishing. Background Art
[0002] Aerosol fire extinguishing agent is a kind of agent that undergoes a violent redox combustion reaction. The flame released during the reaction is as high as 900℃~1200℃. It needs to be flame-extinguished and cooled during actual use. The current flame-extinguishing and cooling methods mainly adopt physical flame-extinguishing and cooling or chemical flame-extinguishing and cooling methods when aerosol fire extinguishing agent is sprayed. When physical cooling agents such as ceramic balls are used, although they have good flame-extinguishing and cooling effects, the ceramic balls have a high adsorption effect on the sprayed aerosol, which greatly weakens the aerosol fire extinguishing ability. When chemical coolants are used, since chemical coolants are easy to decompose, although the aerosol fire extinguishing ability can be guaranteed to have no obvious decrease, the decomposition of the chemical coolant during spraying leads to poor flame-extinguishing and cooling ability, and even fire spraying problems.
[0003] Summary of the Invention
[0004] The present invention provides a composite coolant and its application in aerosol fire extinguishing, which can achieve effective adsorption of aerosol jet flames, thereby improving the fire extinguishing ability of the device while achieving good temperature reduction and flame extinguishing effects.
[0005] The technical solution of the present invention is a composite coolant comprising a molecular sieve and a chemical coolant loaded in the molecular sieve and having fire extinguishing capability.
[0006] Furthermore, the molecular sieve includes but is not limited to one or more of ZSM-5 molecular sieve, ZSM-11 molecular sieve, ZSM-35 molecular sieve, ZSM-22 molecular sieve, ZSM-23 molecular sieve, SAPO-34 molecular sieve, SAPO-5 molecular sieve, SAPO-11 molecular sieve, SBA-15 molecular sieve, SBA-16 molecular sieve, 10X molecular sieve, 13X molecular sieve, MCN-41 molecular sieve, MCM-22 molecular sieve, MCM-48 molecular sieve, MCM-41 molecular sieve, β molecular sieve, 3A molecular sieve, 4A molecular sieve, 5A molecular sieve, and TS-1 molecular sieve.
[0007] Furthermore, the molecular sieve is preferably ZSM-5 molecular sieve, ZSM-35 molecular sieve, 13X molecular sieve, MCN-41 molecular sieve, or TS-1 molecular sieve.
[0008] Furthermore, the molecular sieve has a diameter of 5-11 mm and a specific surface area of 300-2000 m 2 / g.
[0009] Furthermore, the chemical coolant with fire extinguishing capability includes but is not limited to one or more of phosphorus-containing compounds, potassium salts, and halides.
[0010] Furthermore, the phosphorus-containing compound is one or more of phosphorous acid, hypophosphoric acid, metaphosphoric acid, sodium tripolyphosphate, phosphorus pentanide, hexachlorotriphosphazene, ammonium polyphosphate, and phosphoacetic acid; the potassium salt includes but is not limited to one or more of potassium perfluorobutanesulfonate, potassium chloride, and potassium bromide; the halide includes but is not limited to one or more of 2-bromoethylamine hydrobromide, ammonium fluoride, strontium fluoride, titanium tetrafluoride, tetrabutylammonium fluoride, octafluoronaphthalene, strontium chloride, zinc bromide, strontium bromide, ammonium bromide, hexamethylammonium bromide, tetramethylammonium bromide, and tetraethylammonium bromide.
[0011] Furthermore, the loading amount of the chemical coolant in the composite coolant is 20-40% of the mass of the molecular sieve.
[0012] The present invention also relates to a method for preparing the composite coolant, which comprises the following specific steps:
[0013] A chemical coolant with fire extinguishing ability is dissolved in a solvent to prepare a solution, and then the molecular sieve is added into the solution in proportion for impregnation. After the impregnation is completed, the solution is filtered and dried to obtain the composite coolant.
[0014] Furthermore, the solvent is one or more of water, ethanol or acetone; the immersion time is more than 10 hours; the drying temperature is 50-80° C., and the drying time is 3-10 hours.
[0015] The invention also relates to the application of the composite coolant in aerosol fire extinguishing.
[0016] The present invention has the following beneficial effects:
[0017] The present invention provides a coolant loaded with fire-extinguishing chemicals. Fire-extinguishing chemicals such as phosphates, potassium salts, and halogens (fluorides, chlorides, bromides, etc.) are loaded onto a molecular sieve via a co-impregnation process to produce a novel coolant. During the co-impregnation process, the chemicals adhere to the molecular sieve's pores through interaction with the chemicals, resulting in a uniform distribution. When this coolant is used to extinguish flames and reduce temperature in an aerosol fire extinguishing device, the chemicals decompose during the device's discharge, forming free radicals with strong binding capacity for OH and H radicals generated during combustion. The molecular sieve has excellent thermal stability and maintains structural stability even under the high temperatures of aerosol discharge. Furthermore, due to the molecular sieve's large number of microchannel pores and large specific surface area, the chemicals attached to the molecular sieve surface effectively adsorb aerosol jet flames, thereby achieving excellent cooling and flame-extinguishing effects while improving the device's fire-extinguishing capability. DETAILED DESCRIPTION
[0018] The embodiments of the present invention will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be regarded as limiting the scope of the present invention.
[0019] Example 1
[0020] In parts by weight, 500 parts of tap water were taken, and then 100 parts of sodium tripolyphosphate was weighed and added to the tap water, and the sodium tripolyphosphate was fully stirred until it was completely dissolved. 200 parts of X13 molecular sieves with a diameter of 7 mm to 9 mm were weighed in proportion, and the mixture was impregnated for 24 hours by a co-impregnation method. After the impregnation was completed, the filtered X13 molecular sieve was placed in a drying oven at a temperature of 70°C and dried for 6 hours. The prepared new coolant was weighed, and the impregnation rate was calculated to be 20.8%. The new coolant was combined with a commercially available aerosol fire extinguishing agent for a fire extinguishing test and a temperature test at 5 cm from the nozzle. The weight ratio of the coolant to the aerosol agent was 1:1.4.
[0021] Example 2
[0022] Weigh 500 parts of tap water, then weigh 100 parts of potassium chloride and add it to the tap water, stir thoroughly until the potassium chloride is completely dissolved, weigh 200 parts of ZSM-5 molecular sieve with a diameter of 7mm to 9mm in proportion, adopt the co-impregnation method to impregnate for 24 hours, filter with a filter after impregnation, place the filtered ZSM-5 molecular sieve in a drying oven at a temperature of 70°C and dry for 6 hours, weigh the prepared new coolant, and calculate the impregnation rate to be 25.6%. The new coolant is combined with a commercially available aerosol fire extinguishing agent for fire extinguishing test and temperature test at 5 cm from the nozzle, and the weight ratio of coolant to aerosol agent is 1:1.4.
[0023] Example 2-1
[0024] Based on Example 2, the only difference is that the amount of ZSM-5 molecular sieve used is 100 parts, and the final impregnation rate is 30.5%.
[0025] Example 2-2
[0026] Based on Example 2, the only difference is that the amount of potassium chloride used is 200 parts, and the final impregnation rate is 28.1%.
[0027] Example 2-3
[0028] Based on Example 2, the only difference is that the particle size of the ZSM-5 molecular sieve is 5-7 mm, and the final impregnation rate is 28.4%.
[0029] Examples 2-4
[0030] Based on Example 2, the only difference is that the particle size of the ZSM-5 molecular sieve is 9-10 mm, and the final impregnation rate is 23.7%.
[0031] Examples 2-5
[0032] Based on Example 2, the only difference is that the impregnation time is 30 hours and the final impregnation rate is 26.9%.
[0033] Example 3
[0034] Weigh 500 parts of tap water, then weigh 100 parts of ammonium fluoride and add it to the tap water, stir thoroughly until the ammonium fluoride is completely dissolved, weigh 200 parts of SBA-15 molecular sieve with a diameter of 7 mm to 9 mm in proportion, adopt the co-impregnation method to impregnate for 24 hours, filter with a filter after impregnation, place the filtered SBA-15 molecular sieve in a drying oven at a temperature of 70°C and dry for 6 hours, and weigh the prepared new coolant. The impregnation rate is calculated to be 22.1%. The new coolant is combined with a commercially available aerosol fire extinguishing agent for a fire extinguishing test and a temperature test at 5 cm from the nozzle. The weight ratio of the coolant to the aerosol agent is 1:1.4.
[0035] Example 4
[0036] 500 parts of tap water were weighed, and then 100 parts of hexamethylammonium bromide were weighed and added to the tap water. The mixture was stirred thoroughly until the hexamethylammonium bromide was completely dissolved. 200 parts of SAPO-34 molecular sieves with a diameter of 7 mm to 9 mm were weighed in proportion and impregnated for 24 hours using a co-impregnation method. After impregnation, the filtered SAPO-34 molecular sieve was placed in a drying oven at a temperature of 70°C and dried for 6 hours. The prepared new coolant was weighed, and the impregnation rate was calculated to be 22.3%. The new coolant was combined with a commercially available aerosol fire extinguishing agent for a fire extinguishing test and a temperature test at 5 cm from the nozzle. The weight ratio of the coolant to the aerosol agent was 1:1.4.
[0037] Example 5
[0038] 500 parts of tap water were weighed, and then 100 parts of potassium perfluorobutanesulfonate were weighed and added to the tap water. The potassium perfluorobutanesulfonate was fully stirred until it was completely dissolved. 200 parts of MCM-22 molecular sieves with a diameter of 7 mm to 9 mm were weighed in proportion, and the mixture was impregnated for 24 hours by a co-impregnation method. After impregnation, the filtered MCM-22 molecular sieve was placed in a drying oven at a temperature of 70°C and dried for 6 hours. The prepared new coolant was weighed, and the impregnation rate was calculated to be 22.8%. The new coolant was combined with a commercially available aerosol fire extinguishing agent for a fire extinguishing test and a temperature test at 5 cm from the nozzle. The weight ratio of the coolant to the aerosol agent was 1:1.4.
[0039] Example 6
[0040] 500 parts of tap water were weighed, and then 100 parts of strontium chloride were weighed and added to the tap water. The mixture was stirred thoroughly until potassium perfluorobutanesulfonate was completely dissolved. 200 parts of MCN-41 molecular sieves with a diameter of 7 mm to 9 mm were weighed in proportion and impregnated for 24 hours using a co-impregnation method. After impregnation, the filtered MCM-22 molecular sieves were placed in a drying oven at a temperature of 70°C and dried for 6 hours. The prepared new coolant was weighed, and the impregnation rate was calculated to be 24.0%. The new coolant was combined with a commercially available aerosol fire extinguishing agent for a fire extinguishing test and a temperature test at 5 cm from the nozzle. The weight ratio of the coolant to the aerosol agent was 1:1.4.
[0041] Example 7
[0042] Weigh 500 parts of tap water, then weigh 100 parts of phosphorus pentanitride and add them to the tap water, stir thoroughly until potassium perfluorobutanesulfonate is completely dissolved, weigh 200 parts of β molecular sieve with a diameter of 7 mm to 9 mm in proportion, adopt the co-impregnation method to impregnate for 24 hours, filter with a filter after impregnation, place the filtered MCM-22 molecular sieve in a drying oven at a temperature of 70°C and dry for 6 hours, weigh the prepared new coolant, and calculate the impregnation rate to be 26.4%. The new coolant is combined with a commercially available aerosol fire extinguishing agent for fire extinguishing test and temperature test at 5 cm from the nozzle, and the weight ratio of coolant to aerosol agent is 1:1.4.
[0043] Example 8
[0044] Weigh 500 parts of tap water, then weigh 100 parts of 2-bromoethylamine hydrobromide and add them to the tap water, stir thoroughly until potassium perfluorobutanesulfonate is completely dissolved, weigh 200 parts of TS-1 molecular sieve with a diameter of 7 mm to 9 mm in proportion, adopt the co-impregnation method to impregnate for 24 hours, filter with a filter after impregnation, place the filtered MCM-22 molecular sieve in a drying oven at a temperature of 70°C and dry for 6 hours, weigh the prepared new coolant, and calculate the impregnation rate to be 25.1%. The new coolant is combined with a commercially available aerosol fire extinguishing agent for a fire extinguishing test and a temperature test 5 cm away from the nozzle. The weight ratio of the coolant to the aerosol agent is 1:1.4.
[0045] Comparative Example 1
[0046] Commercially available ceramic balls (7mm-9mm) were combined with commercially available aerosol fire extinguishing agents to conduct fire extinguishing tests and temperature tests at a distance of 5 cm from the nozzle. The weight ratio of coolant to aerosol agent was 1:1.4.
[0047] Comparative Example 2
[0048] Commercially available 13X molecular sieve was used as a coolant in combination with a commercial aerosol fire extinguishing agent to conduct fire extinguishing tests and temperature tests at a distance of 5 cm from the nozzle. The weight ratio of coolant to aerosol agent was 1:1.4.
[0049] Comparative Example 3
[0050] Without adding any coolant, a commercially available aerosol fire extinguishing agent was subjected to a fire extinguishing test and a temperature test at a distance of 5 cm from the nozzle.
[0051] Comparative Example 4
[0052] Based on Example 2, the difference is that the TS-1 molecular sieve is replaced by ceramic balls.
[0053] Weigh 500 parts of tap water, then weigh 100 parts of potassium chloride and add it to the tap water, stir thoroughly until the potassium chloride is completely dissolved, weigh 200 parts of ceramic balls with a diameter of 7mm to 9mm in proportion, adopt the co-impregnation method to impregnate for 24 hours, filter with a filter after impregnation, place the filtered ceramic balls in a drying oven at a temperature of 70°C and dry for 6 hours, weigh the prepared coolant, and calculate its impregnation rate to be 3.2%. The coolant is combined with a commercially available aerosol fire extinguishing agent for a fire extinguishing test and a temperature test at 5 cm from the nozzle. The weight ratio of the coolant to the aerosol agent is 1:1.4.
[0054] The commercially available aerosol fire extinguishing agent may be a K-type aerosol fire extinguishing agent or an S-type aerosol fire extinguishing agent. The K-type aerosol fire extinguishing agent is used in the above embodiments and comparative examples.
[0055] The performance characterization data and effect data of the products obtained in the above examples and comparative examples are shown in Table 1.
[0056] Table 1
[0057] The above-mentioned embodiments are only preferred technical solutions of the present invention, but the scope of protection of the present invention is not limited thereto. The embodiments of the present invention and the features in the embodiments can be arbitrarily combined with each other without conflict. The scope of protection of the present invention shall be the technical solutions described in the claims, including equivalent replacement solutions of the technical features in the technical solutions described in the claims. Any changes or replacement improvements that can be easily thought of by any technician familiar with the field within the technical scope disclosed in the present invention are also covered by the scope of protection of the present invention.
Claims
1. A composite coolant, characterized in that: The invention comprises a molecular sieve and a chemical coolant loaded in the molecular sieve and having fire extinguishing capability.
2. The composite coolant according to claim 1, characterized in that: The molecular sieves include, but are not limited to, one or more of ZSM-5 molecular sieve, ZSM-11 molecular sieve, ZSM-35 molecular sieve, ZSM-22 molecular sieve, ZSM-23 molecular sieve, SAPO-34 molecular sieve, SAPO-5 molecular sieve, SAPO-11 molecular sieve, SBA-15 molecular sieve, SBA-16 molecular sieve, 10X molecular sieve, 13X molecular sieve, MCN-41 molecular sieve, MCM-22 molecular sieve, MCM-48 molecular sieve, MCM-41 molecular sieve, β molecular sieve, 3A molecular sieve, 4A molecular sieve, 5A molecular sieve, and TS-1 molecular sieve.
3. The composite coolant according to claim 2, characterized in that: The molecular sieve is one or more of ZSM-5 molecular sieve, ZSM-35 molecular sieve, 13X molecular sieve, MCN-41 molecular sieve or TS-1 molecular sieve.
4. The composite coolant according to claim 1, characterized in that: The molecular sieve has a diameter of 5-11 mm and a specific surface area of 300-2000 m 2 / g.
5. The composite coolant according to claim 1, characterized in that: The chemical coolant with fire extinguishing capability includes, but is not limited to, one or more of phosphorus-containing compounds, potassium salts, and halides.
6. The composite coolant according to claim 1, characterized in that: The phosphorus-containing compound is one or more of phosphorous acid, hypophosphoric acid, metaphosphoric acid, sodium tripolyphosphate, phosphorus pentanide, hexachlorotripolyphosphazene, ammonium polyphosphate, and phosphoacetic acid; the potassium salt includes but is not limited to one or more of potassium perfluorobutylsulfonate, potassium chloride, and potassium bromide; the halide includes but is not limited to one or more of 2-bromoethylamine hydrobromide, ammonium fluoride, strontium fluoride, titanium tetrafluoride, tetrabutylammonium fluoride, octafluoronaphthalene, strontium chloride, zinc bromide, strontium bromide, ammonium bromide, hexamethylammonium bromide, tetramethylammonium bromide, and tetraethylammonium bromide.
7. The composite coolant according to any one of claims 1 to 6, characterized in that: The loading amount of the chemical coolant in the composite coolant is 20-40% of the mass of the molecular sieve.
8. The method for preparing the composite coolant according to any one of claims 1 to 7, characterized in that: The specific steps are: The chemical coolant with fire extinguishing ability is dissolved in a solvent to prepare a solution, and then the molecular sieve is added into the solution in proportion for impregnation. After the impregnation is completed, the solution is filtered and dried to obtain the composite coolant.
9. The preparation method according to claim 8, characterized in that: The solvent is one or more of water, ethanol or acetone; the immersion time is more than 10 hours; the drying temperature is 50-80° C., and the drying time is 3-10 hours.
10. Use of the composite coolant according to any one of claims 1 to 7 in aerosol fire extinguishing.
Citation Information
Patent Citations
Molecular sieve coolant processing and preparing method
CN108424750A
Cooling ball and preparation method and application thereof
CN109603039A
Cooling ball
CN209500583U
Catalytic chemical coolant for hot aerosol and making process thereof
WO2011088666A1
Aerosol fire extinguishing device
WO2017187792A1
Cited By
Low-toxicity high-efficiency aerosol fire extinguishing agent composition and preparation method thereof
CN122297965A
A low-toxicity and high-efficiency aerosol fire extinguishing agent composition and a preparation method thereof
CN122297965B