Polyacrylonitrile-based carbon fiber, stock solution, and preparation methods therefor
By introducing gel particles with high equilibrium swelling degree into the polyacrylonitrile spinning solution and a three-stage temperature-controlled polymerization process, the problem of fiber defects caused by gel particles is solved and the mechanical properties and production of polyacrylonitrile-based carbon fibers are improved. efficiency.
Patent Information
- Application Number
- PCT/CN2023/142998
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2023-12-29
- Publication Date
- 2024-10-24
AI Technical Summary
When preparing polyacrylonitrile-based carbon fibers, it is difficult to effectively remove gel particles with the existing technology, resulting in an increase in internal defects in the fiber, a decrease in mechanical properties, and high filtration precision and pressure requirements, resulting in low production costs and efficiency.
The gel particles in the polyacrylonitrile spinning solution have a high equilibrium swelling degree and are prepared through a three-stage temperature-controlled polymerization process to form carbon fibers with long and narrow micropores, which reduces the negative impact of the gel particles on the fiber and improves the fiber's strength. mechanical properties.
The mechanical properties of polyacrylonitrile-based carbon fiber are improved, the negative impact of micropores on fiber properties is reduced, and production efficiency and cost-effectiveness are improved.
Smart Images

Figure PCTCN2023142998-FTAPPB-I100001 
Figure PCTCN2023142998-FTAPPB-I100002 
Figure PCTCN2023142998-FTAPPB-I100003
Abstract
Description
Polyacrylonitrile-based carbon fiber, stock solution and preparation method thereof Technical Field
[0001] The invention relates to a polyacrylonitrile-based carbon fiber, a stock solution and a preparation method thereof. Background Art
[0002] Polyacrylonitrile-based carbon fibers have excellent properties such as high specific strength and high specific modulus. As reinforcing fibers, they are widely used in composite materials in aerospace, new energy, and other fields. As the application of carbon fibers expands, the requirements for the performance of polyacrylonitrile-based carbon fibers are further improved.
[0003] The spun fiber is the basis of the structure of polyacrylonitrile fiber (precursor). Polyacrylonitrile fiber is prepared by coagulating a spinning stream to obtain a spun fiber, and then the spun fiber undergoes a post-processing process and other processes. More specifically, the spun fiber is obtained by slowly forming a fiber morphology from the spinning stream in a coagulation bath. The fiber forming process of the spinning stream in the coagulation bath directly determines the structure of the spun fiber. Therefore, the coagulation forming state of the spun fiber plays a decisive role in the performance of the polyacrylonitrile-based precursor and the carbon fiber. Whether it is a wet spinning process for polyacrylonitrile-based precursor or a dry-jet wet spinning process, the coagulation forming of the stock solution after it is extruded from the spinneret is a particularly critical link, among which the smoothness of the stock solution extrusion is related to the stability of the extrusion coagulation process, the quality of the spun fiber, the replacement cycle of the spinneret, etc.
[0004] The most significant factor affecting the quality of polyacrylonitrile-based carbon fibers is the quality of the precursor. Defects in the precursor can be inherited by the carbon fibers and even amplified during the pre-oxidation and carbonization stages. The primary requirement for producing high-quality polyacrylonitrile precursor is the preparation of a high-quality polyacrylonitrile solution. A high-quality polyacrylonitrile solution must possess not only long-term stable molecular weight, solids content, viscosity, and copolymer composition, but also sufficiently low impurity levels. Impurities in the polyacrylonitrile solution typically include mechanical impurities introduced from the external environment, non-solvent impurities, and gel particles generated during equipment operation. These impurities negatively impact the filtration and extrusion processes of the polyacrylonitrile solution. In severe cases, they can lead to spinneret blockage, causing a series of spinning anomalies such as fuzzy and broken fibers in the nascent fibers, necessitating shutdown and cleaning, severely impacting production efficiency and precursor quality. Furthermore, when impurities such as gel particles in the polyacrylonitrile solution penetrate the filter and enter the spinneret, they can disrupt extrusion. Furthermore, after the nascent fibers undergo multi-stage drafting and diameter reduction, the mechanical properties of the polyacrylonitrile precursor and carbon fibers decrease, resulting in a high coefficient of variation. In addition, the stretchability of the microgel particles that enter the precursor is very different from that of the fiber body. After the primary fiber is dried, densified and multi-stage stretched, the microgel particles are retained as defects inside the fiber, deteriorating the microscopic orientation structure and mechanical properties of the polyacrylonitrile precursor. Furthermore, for the gel particles inside the precursor, compared with the polyacrylonitrile fiber body, the gel particles with low swelling degree and difficult to stretch are more likely to release heat and collapse in a concentrated manner during the thermal stabilization process, thereby generating micropores with larger radial defects, further deteriorating the performance of polyacrylonitrile-based carbon fibers. Therefore, the preparation of high-quality polyacrylonitrile solution is particularly important for improving the performance and uniformity of polyacrylonitrile-based precursors and carbon fibers.
[0005] JP2017128838A, JP2018141251A, WO2019012999A1, JP2019112730A and CN110832127A disclose that a spinning solution is prepared by dissolving a polyacrylonitrile copolymer (Mz / Mw is 1.5-6.0) in a solvent, filtering the spinning solution under certain conditions of filtration speed, filtration accuracy (≥3μm) and filter material thickness, spinning the filtered spinning solution to obtain a carbon fiber precursor fiber bundle, and after oxidation and carbonization of the carbon fiber precursor fiber bundle, a carbon fiber bundle with fewer defects on the fiber fracture surface can be obtained.
[0006] JP2008248219A5 proposes a polyacrylonitrile (PAN) based polymer, wherein the content of components having a molecular weight exceeding 3 million or higher (10 million) as measured by gel permeation chromatography (GPC) is 1 to 10%, and the polydispersity (M Z / M W) is 3.0-10.0; the polymer can increase spinning speed and improve spinning draft ratio; and it also provides a method for producing high-quality carbon fiber precursor fibers with low fuzziness without compromising productivity. However, it is worth noting that such a high weight-average molecular weight will place very high pressure on the precision filtration of the polyacrylonitrile solution, placing higher requirements on the pressure resistance and replacement cycle of the filter and spinneret.
[0007] JP4924484B2 points out that the weight average molecular weight of polyacrylonitrile polymer is 300,000-500,000, the molecular weight distribution Mz / Mw is 2.5-10.0, the filtration rate or processing capacity per unit area is 1-150L / m 2 h and the filtration residence time V / W (V is the effective volume of the filter L, W is the polymer flow rate L / min) (min) is 0.01-10. If the filtration processing capacity exceeds the limit or the filtration residence time is too long, the high molecular weight part of the polymer will be trapped or the gel impurities will be squeezed out, resulting in a significant reduction in the strength of the carbon fiber. JP5141598B2 points out that the unit area weight A of the filtration guarantee layer before spinning the spinning solution, the material density B (where 0.01≤A / B×1000≤0.06), the filtration resistance coefficient 5×10 5 ~30×10 5 centimeter -1 , the thickness of the filtration guarantee layer (0.033-0.25mm) meets certain conditions, which can not only accurately filter out gel-like substances and other foreign matter from the spinning solution before filtration, but also eliminate the blockage of the filter medium.
[0008] CN1417393A proposes filtering the spinning solution through a 0.5-5 μm filter material, preferably a 0.5-3 μm filter material. This precision filtration effectively reduces the gel particles in the spinning solution. The number of particles larger than 0.2 μm in the filtered spinning solution is reduced from 1,000 particles / L before filtration to 50 particles / L after filtration. The strength of fibers spun from the filtered solution is increased from 5.2 g / d to 7.5 g / d compared to unfiltered solution. It is worth noting that the application does not mention a method for testing the number of gel particles. Furthermore, achieving such a low gel particle content in the spinning solution requires extremely precise filtration or extremely low filtration pressure differentials, which would inevitably lead to a significant increase in production costs and a significant decrease in production efficiency.
[0009] Based on polyacrylonitrile molecular weight and solution filtration, the aforementioned literature establishes a reasonable operating range for stable production of polyacrylonitrile-based carbon fiber precursors, targeting filtration accuracy, filtration throughput, filtration residence time, and polyacrylonitrile molecular weight. However, high-precision filters are not only expensive but also have a short service life. Furthermore, the high filtration pressure drop places high demands on the pressure resistance of the spinneret during the stock solution extrusion process.
[0010] In view of this, the present invention provides a polyacrylonitrile solution that can overcome at least one problem existing in the prior art and meet the requirements of long-term stable production. The polyacrylonitrile solution of the present invention can be spun to produce polyacrylonitrile-based carbon fiber precursor; the precursor can be subjected to pre-oxidation, carbonization, and other processes to produce polyacrylonitrile-based carbon fibers.
[0011] Summary of the Invention
[0012] The inventors found in their in-depth research that polyacrylonitrile gel particles are almost unavoidable during the production process, and further found in their in-depth research that the properties of polyacrylonitrile gel particles are closely related to the temperature of their formation process, and are also related to the concentration of oxygen in the atmosphere during the polymerization process. A polyacrylonitrile solution left in a medium-to-high temperature atmosphere containing oxygen for a long time will easily lead to the formation of gel particles. The chemical structure of the gel particles has undergone a huge change compared to that of polyacrylonitrile, in which a large number of crosslinks are generated between the polyacrylonitrile polymer chains under the dual promotion of oxygen and high temperature. When the molecular chains between the crosslinking points are shorter, the gel particles have a lower equilibrium swelling degree, higher rigidity, and poor tensile properties; during the fiber drawing process, the gel particles retain the gel particle morphology, resulting in an increase in internal defects in the fiber, and thus a significant decrease in mechanical properties. Conversely, gel particles with a high equilibrium swelling degree have longer molecular chains between their crosslinking points and exhibit better tensile properties. Even when entering the fiber under a higher filtration pressure difference, the gel particles with a high equilibrium swelling degree will undergo axial tensile deformation along with the fiber body, thereby producing narrow axial micropores in the final carbon fiber; this can reduce the negative impact on the mechanical properties and make the carbon fiber have better mechanical properties.
[0013] In view of this, one of the objects of the present invention is to provide a polyacrylonitrile-based carbon fiber having long and narrow micropores along the axial direction.
[0014] A second object of the present invention is to provide a polyacrylonitrile spinning solution containing gel particles having a high equilibrium swelling degree, for example, an equilibrium swelling degree of the gel particles of 250 to 5000%. The polyacrylonitrile spinning solution can be used to prepare the above-mentioned polyacrylonitrile-based carbon fibers.
[0015] A third object of the present invention is to provide a method for preparing polyacrylonitrile spinning solution, wherein the solution prepared by the method contains gel particles, and the gel particles have a high equilibrium swelling degree, for example, the equilibrium swelling degree of the gel particles is 250 to 5000%.
[0016] A fourth object of the present invention is to provide a method for preparing polyacrylonitrile-based carbon fibers, such as the above-mentioned polyacrylonitrile-based carbon fibers, wherein the carbon fibers prepared by the method have narrow and long micropores along the axial direction.
[0017] One aspect of the present invention relates to a polyacrylonitrile-based carbon fiber containing micropores, wherein the average radial size L of the micropores is P is less than or equal to 2.0 nm, and the micropore aspect ratio L / L P The ratio of the volume of micropores having an average diameter of greater than or equal to 50 and less than or equal to 100 and a radial dimension greater than 15 nm to the total micropore volume is greater than 0 and less than 10%.
[0018] In some embodiments, the average radial size L of the micropores is P is less than or equal to 1.5nm, and the micropore aspect ratio L / L P is greater than or equal to 60 and less than or equal to 100, and the ratio of the volume of micropores having a radial dimension greater than 15 nm to the total micropore volume is greater than 0 and less than 5%.
[0019] In some embodiments, the diameter C of the carbon fiber V Value is less than or equal to 3%.
[0020] In some embodiments, the polyacrylonitrile-based carbon fibers have a fiber count of 3,000 to 24,000.
[0021] In some embodiments, the diameter of the polyacrylonitrile-based carbon fiber is 5-7 μm; the tensile strength is 4.9-5.8 GPa, and the tensile strength C V Value less than 5%; and / or tensile modulus of 282-323GPa, and tensile modulus C V The value is less than 5%.
[0022] Another aspect of the present invention relates to a polyacrylonitrile spinning solution containing gel particles, wherein the total number of gel particles with a particle size greater than 0.15 μm is less than or equal to 1×10 5 / mL, and the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles is less than or equal to 0.3%; wherein the equilibrium swelling degree of the gel particles is 250-5000%.
[0023] In some embodiments, the polyacrylonitrile spinning solution includes a polyacrylonitrile polymer and a solvent, and the weight ratio of the polyacrylonitrile to the solvent is (15-30):(85-70), preferably (18-22):(82-78).
[0024] In some embodiments, the solvent is at least one of dimethyl sulfoxide, dimethylformamide, dimethylacetamide, and mixtures thereof.
[0025] In some embodiments, the zero shear viscosity of the polyacrylonitrile spinning solution is 50-150 Pa·s, wherein the viscosity test temperature is 50°C.
[0026] In some embodiments, the polyacrylonitrile spinning solution is used to prepare the polyacrylonitrile-based carbon fiber of the present invention.
[0027] Another aspect of the present invention relates to a method for preparing a polyacrylonitrile spinning solution, which includes solution polymerization, wherein the solution polymerization adopts a three-stage temperature control, wherein the temperature of the first initial initiation stage is T1°C, the temperature of the second constant temperature polymerization stage is T2°C, and the temperature of the third cooling polymerization stage is T3°C; wherein T1, T2, and T3 satisfy the following relationship:
[0028] T1 = (0.5-1.4) * T2 and 35 ≤ T1 ≤ 80; and
[0029] T3=T2-(5~50) and 50≥T3≥25.
[0030] In some embodiments, the method for preparing the polyacrylonitrile spinning solution is used to prepare the polyacrylonitrile spinning solution of the present invention.
[0031] In some embodiments, 35°C≤T1≤80°C, preferably 40°C≤T1≤70°C; 40°C≤T2≤90°C, preferably 50°C≤T2≤80°C; and 25°C≤T3≤50°C, preferably 25°C≤T3≤45°C, more preferably 30°C≤T3≤45°C.
[0032] In some embodiments, 50°C≤T2≤80°C, 40°C≤T1≤70°C, and 30°C≤T3≤45°C.
[0033] In some embodiments, T3 = T2-(15-50), preferably T3 = T2-(15-40), more preferably T3 = T2-(20-35).
[0034] In some embodiments, the polymerization time of the first initial initiation section is 20-150 minutes, preferably 30-120 minutes, more preferably 30-80 minutes; the polymerization time of the second constant temperature polymerization section is 300-900 minutes, preferably 400-800 minutes, preferably 400-700 minutes, more preferably 500-600 minutes; and the polymerization time of the third cooling polymerization section is 80-300 minutes, preferably 80-250 minutes, preferably 100-250 minutes, more preferably 120-200 minutes.
[0035] In some embodiments, the monomer conversion rate of the second constant temperature polymerization section is X, the monomer conversion rate of the first initial initiation section is (0.125-0.215)*X, and the monomer conversion rate of the third cooling polymerization section is (0.007-0.0715)*X, wherein the monomer conversion rate X of the second constant temperature polymerization section is 60%-85%, preferably 65%-85%, and more preferably 70%-80% or 70%-79%. In the present invention, the monomer conversion rate of the first, second, and third sections refers to the ratio of the weight of the monomer undergoing polymerization reaction in each section to the total weight of the monomers.
[0036] In some embodiments, the solution polymerization is carried out under an inert gas protection. In some embodiments, preferably, the solution polymerization is carried out under an inert gas protection and the oxygen content is less than 1000 ppm. In some embodiments, the solution polymerization is carried out in a polymerization kettle.
[0037] Another aspect of the present invention relates to a method for preparing polyacrylonitrile-based carbon fibers, preferably the polyacrylonitrile-based carbon fibers of the present invention, comprising the steps of preparing a polyacrylonitrile spinning solution into a precursor, and pre-oxidizing and carbonizing the precursor to obtain the polyacrylonitrile-based carbon fibers; wherein the polyacrylonitrile spinning solution is the polyacrylonitrile spinning solution of the present invention or the polyacrylonitrile spinning solution obtained by the method for preparing the polyacrylonitrile spinning solution of the present invention.
[0038] In some embodiments, the raw silk preparation steps include: (1) coagulation of nascent fibers, (2) hot water drawing, (3) hot water washing, (4) oiling, (5) drying and densification, (6) steam drawing, and (7) heat setting.
[0039] In some embodiments, the pre-oxidation temperature is 180-300°C, preferably divided into 4-6 temperature zones; the carbonization includes low-temperature carbonization and high-temperature carbonization, preferably, the low-temperature carbonization temperature is 300-700°C, and the high-temperature carbonization temperature is 1000-1500°C.
[0040] In some embodiments, the preparation method further comprises the steps of surface treatment and gluing. DETAILED DESCRIPTION
[0041] For one of the above-mentioned purposes, the present invention provides a polyacrylonitrile-based carbon fiber containing micropores, wherein the average radial size L of the micropores is P is less than or equal to 2.0 nm, and the aspect ratio of the micropore is L / L P is greater than or equal to 50 and less than or equal to 100, and the ratio of the volume of micropores having a radial dimension greater than 15 nm to the total micropore volume is greater than 0 and less than 10%.
[0042] In the present invention, L refers to the average size (length) of the micropores along the fiber axis (i.e., the length direction of the fiber), and L P It refers to the average radial size of the micropores in the transverse direction of the fiber (ie perpendicular to the length of the fiber).
[0043] In the present invention, L and L P It is obtained by using small angle X-ray scattering (SAXS) testing and the following double-model Debye-Bueche analysis method:
[0044] In the present invention, according to the obtained L and L P The micropore aspect ratio L / L can be calculated P .
[0045] In the present invention, the scattering curves of two types of micropores (i.e., micropores with radial dimensions greater than 15 nm and all micropores) are fitted by the Debye-Bueche method, and the relative volumes of the two types of micropores are calculated according to the following formula to obtain the volume ratio of the two types of micropores.
[0046] L, L P The specific measurement and analysis methods of the micropore volume are described in detail below.
[0047] In the present invention, the average radial size L of the micropores is P It may be less than or equal to 2.0 nm and greater than or equal to 0 nm, for example, less than or equal to 2.0 nm and greater than or equal to 0.1 nm, less than or equal to 2.0 nm and greater than or equal to 0.5 nm, or less than or equal to 2.0 nm and greater than or equal to 1.0 nm.
[0048] In the present invention, the aspect ratio of the micropores is L / L P It may be greater than or equal to 50 and less than or equal to 100, for example, greater than or equal to 50 and less than or equal to 90, or greater than or equal to 50 and less than or equal to 80, or greater than or equal to 50 and less than or equal to 70.
[0049] In the present invention, the ratio of the volume of micropores with a radial dimension greater than 15 nm to the total micropore volume may be greater than 0 and less than 10%, for example, greater than 0.1% and less than 10%, or greater than 3% and less than 10%. In the present invention, the volume of micropores with a radial dimension greater than 15 nm refers to the total volume of all micropores with a radial dimension greater than 15 nm. In the present invention, the total micropore volume refers to the total volume of all micropores.
[0050] In some embodiments, preferably, the average radial size L of the micropores is PIt can be less than or equal to 1.5nm, and the micropore aspect ratio L / L P The average radial size L of the micropores may be greater than or equal to 60 and less than or equal to 100, and the ratio of the volume of micropores with radial dimensions greater than 15 nm to the total micropore volume may be greater than 0 and less than 5%. P It can be less than or equal to 1.5 nm and greater than or equal to 0 nm, for example, it can be less than or equal to 1.5 nm and greater than or equal to 0.1 nm, or less than or equal to 1.5 nm and greater than or equal to 1.0 nm. In the present invention, the aspect ratio L / L of the micropores is P It may be greater than or equal to 60 and less than or equal to 100, for example, greater than or equal to 60 and less than or equal to 90, or greater than or equal to 60 and less than or equal to 80, or greater than or equal to 60 and less than or equal to 70. In the present invention, the ratio of the volume of micropores with a radial dimension greater than 15 nm to the total micropore volume may be greater than 0 and less than 5%, for example, greater than 0.1% and less than 5%, greater than 3% and less than 5%, or greater than 4% and less than 5%.
[0051] In some embodiments, the diameter of the carbon fiber C V The value is less than 3%. In the present invention, C V The calculation of the value is described in detail below.
[0052] In the present invention, there is no particular limitation on the number of fibers of the carbon fibers. For example, the number of fibers commonly known in the field of carbon fibers can be used. In some embodiments, preferably, the number of fibers of the polyacrylonitrile-based carbon fibers is 3,000 to 24,000.
[0053] In the present invention, the diameter of the carbon fibers is not particularly limited and may have a diameter commonly used in the art. In some embodiments, the diameter of the polyacrylonitrile-based carbon fibers may be 1-10 μm, for example, 2-10 μm. In some embodiments, the diameter of the polyacrylonitrile-based carbon fibers may be 5-7 μm.
[0054] In the present invention, the tensile strength of the polyacrylonitrile-based carbon fiber may be 4.5-6.1 GPa, for example, 4.7-6.0 GPa or 4.9-5.8 GPa. V The value is lower than 10%, for example, lower than 7% or lower than 5%.
[0055] In the present invention, the tensile modulus of the polyacrylonitrile-based carbon fiber is 260-340 GPa, for example, 270-330 GPa or 282-323 GPa.V The value is lower than 10%, for example, lower than 7% or lower than 5%.
[0056] In some embodiments, preferably, the diameter of the polyacrylonitrile-based carbon fiber is 5-7 μm, the tensile strength is 4.9-5.8 GPa, and the tensile strength of C V The value is less than 5%, the tensile modulus is 282-323GPa, and the tensile modulus C V The value is less than 5%.
[0057] In the present invention, the number and diameter of polyacrylonitrile precursor and carbon fiber are measured by microscopy according to GB / T3364-2008.
[0058] In the present invention, the tensile strength and tensile modulus of carbon fibers are measured using a mechanical tensile method according to GB / T3362-2005.
[0059] For the second purpose of the above invention, the present invention provides a polyacrylonitrile spinning solution, which contains gel particles, wherein the total number of gel particles with a particle size greater than 0.15 μm is less than or equal to 1×10 5 / mL, and the ratio of the number of gel particles with a particle size greater than 5 μm to the total number of gel particles (that is, the ratio of the number of gel particles with a particle size greater than 5 μm to the total number of gel particles) is less than or equal to 0.3%; wherein the equilibrium swelling degree of the gel particles is 250 to 5000%.
[0060] In this invention, the particle size and number of agglomerated particles are measured using single-particle optical sensing technology. When a single particle passes through a narrow photosensitive area, it blocks a portion of the incident light, causing the intensity of the incident light reaching the detector to drop momentarily. The attenuation of the intensity signal is theoretically proportional to the particle's cross-section, or the square of its diameter. A calibration curve is established using standard particles to compare particle size and intensity signal magnitude. The particle size is calculated based on this calibration curve, and the number of particles is counted. The specific method for measuring the particle size and number of agglomerated particles is described below.
[0061] As understood by those skilled in the art, equilibrium swelling refers to the ratio of the weight of the gel particles at swelling equilibrium to the weight after solvent removal. The specific method for measuring equilibrium swelling is described below.
[0062] The total number of gel particles with a particle size greater than 0.15 μm contained in the polyacrylonitrile spinning solution of the present invention is less than or equal to 1×10 5 In some embodiments, the total number of gel particles with a particle size greater than 0.15 μm may be less than 9.8×10 4 / mL, less than 9.7×10 4 / mL, less than 9.5×104 / mL, less than 9.3×10 4 / mL, less than 9.1×10 4 / mL, less than 9.0×10 4 / mL, less than 8.8×10 4 / mL, less than 8.6×10 4 / mL, less than 8.4×10 4 / mL, less than 8.2×10 4 / mL, less than 8.0×10 4 / mL, less than 7.8×10 4 / mL, less than 7.6×10 4 / mL, less than 7.4×10 4 / mL, less than 7.2×10 4 / mL, or less than 7.0×10 4 The total number of gel particles with a particle size greater than 0.15 μm contained in the polyacrylonitrile spinning solution of the present invention is less than 1×10 5 In some embodiments, the total number of gel particles with a particle size greater than 0.15 μm contained in the polyacrylonitrile spinning solution of the present invention is less than or equal to 1×10 5 cells / mL and higher than or equal to 10, or lower than or equal to 1×10 5 pc / mL and higher than or equal to 100, or lower than or equal to 1×10 5 pc / mL and higher than or equal to 1000, or lower than or equal to 1×10 5 pcs / mL and higher than or equal to 10,000, or lower than or equal to 1×10 5 cells / mL and higher than or equal to 20,000, or lower than or equal to 1×10 5 pc / mL and higher than or equal to 30,000, or lower than or equal to 1×10 5 cells / mL and higher than or equal to 40,000, or lower than or equal to 1×10 5 pcs / mL and higher than or equal to 50,000 pcs / mL.
[0063] In the present invention, the equilibrium swelling degree of the gel particles can be 250-5000%, for example, 260-5000%, 270-5000%, 280-5000%, 290-5000%, 300-5000%, 310-5000%, 320-5000%, 330-5000%, 340-5000%, 350-5000%, 360-5000%, 370-5000%, 380-5000%, 390-5000%, or 400-5000%. In some embodiments, the equilibrium swelling degree of the gel particles in the spinning solution may be 250-4000%, 250-3000%, 250-2000%, 250-1500%, 260-4000%, 260-3000%, 260-2000%, 260-1500%, 270-4000%, 270-3000%, 270-2000%, 270-1500%, 280-4000%, 280-3000%, 280-2000%, 280-1500%, 290-4000%, 290-3000%, 290-2000%, 290-1500%, 300-4000%, 300-3000%, 300-2 000%, 300-1500%, 310-4000%, 310-3000%, 310-2000%, 310-1500%, 320-4000%, 320-3000%, 320-2000%, 320-1500%, 330-4000%, 330-3000%, 330-2000%, 330-1500%, 340-4000%, 340-3000%, 340-2000%, 340-1500%, 350-4000%, 350-3000%, 350-2000%, 350-1500%, 400-4000%, 400-3000%, 400-2000%, or 400-1500%.
[0064] The proportion of the number of gel particles with a particle size greater than 5 μm in the polyacrylonitrile spinning solution of the present invention to the total number of gel particles may be less than or equal to 0.3%; preferably less than or equal to 0.25%, more preferably less than or equal to 0.20%, and even more preferably less than or equal to 0.15%. In some embodiments, the proportion of the number of gel particles with a particle size greater than 5 μm in the polyacrylonitrile spinning solution to the total number of gel particles may be less than 0.3%, less than 0.29%, less than 0.28%, less than 0.27%, less than 0.26%, less than 0.25%, less than 0.24%, less than 0.23%, less than 0.22%, less than 0.21%, less than 0.20%, less than 0.29%, less than 0.19%, less than 0.18%, less than 0.17%, less than 0.16%, less than 0.15%, or less than 0.14%.
[0065] The ratio of the number of gel particles having a particle size greater than 5 μm in the polyacrylonitrile spinning solution of the present invention to the total number of gel particles may be less than 0.3% and greater than or equal to 0. In some embodiments, the ratio of the number of gel particles having a particle size greater than 5 μm in the polyacrylonitrile spinning solution of the present invention to the total number of gel particles may be less than 0.3% and greater than or equal to 0.01%, or less than 0.3% and greater than or equal to 0.05%.
[0066] In some embodiments, preferably, the total number of the gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile spinning solution of the present invention is less than 9.8×10 4 / mL, preferably less than 7.8×10 4 / mL, more preferably less than 7.0×10 4 / mL; the proportion of gel particles with an average particle size greater than 5μm in the total gel particles is less than 0.25%, preferably less than 0.21%, and more preferably less than 0.15%; and the equilibrium swelling degree of the gel particles is 300-4000%, 300-2000%, 400-2000%, preferably 500-2000% or 500-1000%.
[0067] The polyacrylonitrile spinning solution comprises a polyacrylonitrile polymer and a solvent.
[0068] As the polyacrylonitrile polymer, a polyacrylonitrile homopolymer, a polyacrylonitrile copolymer, or a mixture thereof can be used. Specifically, the polyacrylonitrile polymer can contain 90-100% by mass of monomer units derived from acrylonitrile and 0-10% by mass of structural units derived from monomers copolymerizable with acrylonitrile. As monomers copolymerizable with acrylonitrile, various comonomers commonly known in the art can be used, including, for example, acrylic acid, methacrylic acid, itaconic acid, and their alkali metal salts, ammonium salts, and lower alkyl esters; acrylamide and its derivatives; allyl sulfonic acid, methallyl sulfonic acid, and their salts or alkyl esters; and the like.
[0069] There is no particular limitation on the concentration of the polyacrylonitrile polymer in the polyacrylonitrile spinning solution, and any suitable concentration commonly known in the art for polyacrylonitrile spinning solutions can be used. In the present invention, for example, the concentration of the polyacrylonitrile polymer in the polyacrylonitrile spinning solution can be 15 to 30% by weight. In some embodiments, preferably, the weight ratio of the polyacrylonitrile polymer to the solvent in the polyacrylonitrile spinning solution can be (18 to 22): (82 to 78).
[0070] There is no particular limitation on the solvent in the polyacrylonitrile spinning solution, and any suitable solvent commonly known in the art for polyacrylonitrile spinning solution can be used. The solvent can be at least one of dimethyl sulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMAC), and mixtures thereof.
[0071] In the present invention, the zero-shear viscosity of the polyacrylonitrile spinning solution is 30-200 Pa·s, preferably 50-150 Pa·s, wherein the viscosity is tested at a temperature of 50°C. In the present invention, the zero-shear viscosity is tested using a rotational rheometer, wherein the test temperature is 50±0.01°C, the rotor diameter is 25 mm, and the pitch is 1 mm; and the zero-shear viscosity of the polyacrylonitrile polymer solution is obtained by extrapolation. The specific method for determining the zero-shear viscosity is described below.
[0072] For the third purpose of the above invention, the present invention provides a method for preparing a polyacrylonitrile stock solution, which is preferably used to prepare the polyacrylonitrile stock solution described in the second purpose of the above invention. The method for preparing the polyacrylonitrile stock solution of the present invention comprises solution polymerization, wherein the solution polymerization adopts a three-stage temperature control, wherein the temperature of the first stage (i.e., the initial initiation stage) is T1°C, the temperature of the second stage (constant temperature polymerization stage) is T2°C, and the temperature of the third stage (cooling polymerization stage) is T3°C; wherein T1, T2, and T3 satisfy the following relationship:
[0073] T1 = (0.5-1.4) * T2 and 35 ≤ T1 ≤ 80; and
[0074] T3=T2-(5~50) and 50≥T3≥25.
[0075] In the method for preparing the polyacrylonitrile stock solution of the present invention, the polymerization process of solution polymerization is divided into three stages according to the polymerization temperature as described above: the first stage (i.e., the initial initiation stage), the second stage (constant temperature polymerization stage) and the third stage (cooling polymerization stage), wherein the temperatures of these three stages are T1, T2 and T3, respectively.
[0076] The desired temperatures T1, T2, and T3 can be achieved by temperature detection and control methods commonly known in the art. For example, a temperature detection device such as a thermometer, thermocouple, or the like can be provided to detect the temperature. For example, the desired polymerization temperature can be provided by a heating device and a cooling device commonly used in the art. For example, a control device can be provided to heat or cool the polymerization mixture according to the detected temperature to provide the desired temperature. In some embodiments, a jacketed reactor can be used to achieve temperature control.
[0077] In the present invention, T2 may be in the range of 40° C. ≤ T2 ≤ 90° C., preferably 50° C. ≤ T2 ≤ 80° C. In some embodiments, preferably, T2 is in the range of 50-80° C.; for example, T2 may be 50° C., 55° C., 60° C., 65° C., 70° C., 75° C., 80° C., or a range consisting of any two of the foregoing values.
[0078] In the present invention, T1 may be in the range of 35°C ≤ T1 ≤ 80°C, preferably 40°C ≤ T1 ≤ 70°C. In some embodiments, preferably, T1 is in the range of 40-70°C; for example, T1 may be 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, or a range consisting of any two of the above values.
[0079] In the present invention, T3 may be in the range of 25°C ≤ T3 ≤ 50°C, preferably 25°C ≤ T3 ≤ 45°C, more preferably 30°C ≤ T3 ≤ 45°C. In some embodiments, T3 is preferably in the range of 30-45°C; for example, T3 may be 30°C, 35°C, 40°C, 45°C, or a range consisting of any two of the above values.
[0080] In some embodiments, preferably, 50°C≤T2≤80°C, 40°C≤T1≤70°C and 30°C≤T3≤45°C.
[0081] In some embodiments, T3 = T2 - (15-50), preferably T3 = T2 - (15-40), more preferably T3 = T2 - (20-35), and 50°C ≥ T3 ≥ 25°C.
[0082] The method of the present invention uses solution polymerization to prepare a polyacrylonitrile polymer to obtain a polyacrylonitrile spinning solution. The use of solution polymerization to prepare polyacrylonitrile polymers is known in the art. For example, in the method of preparing a polyacrylonitrile stock solution of the present invention, a solution polymerization process known in the art can be used to obtain the spinning solution, provided that the solution polymerization utilizes the three-stage programmed temperature control of the present invention.
[0083] For the solution polymerization in the present invention, initiators commonly used in the art can be used. In some embodiments, the initiator can be a free radical initiator, including, for example, peroxide initiators, azo initiators, and redox initiators.
[0084] The monomers and solvents used for solution polymerization may be as described above in the section on polyacrylonitrile spinning solution.
[0085] In some embodiments, in the solution polymerization, the monomer conversion rate of the second section is X, then: the monomer conversion rate of the first section is (0.125-0.215)*X, and the monomer conversion rate of the third section is (0.007-0.0715)*X; wherein the monomer conversion rate X of the second section (constant temperature polymerization section) is 60%-85%, preferably 65%-85%, more preferably 70%-80% or 70%-79%.
[0086] In the present invention, the polymerization time of the first initial initiation section can be 20-150 minutes, preferably 30-120 minutes, more preferably 30-80 minutes; the polymerization time of the second constant temperature polymerization section can be 300-900 minutes, preferably 400-800 minutes, preferably 400-700 minutes, more preferably 500-600 minutes; and the polymerization time of the third cooling polymerization section can be 80-300 minutes, preferably 80-250 minutes, preferably 100-250 minutes, more preferably 120-200 minutes. In some embodiments, preferably, the polymerization time of the first section (initial initiation section) is 30-80 minutes, the second section (constant temperature polymerization section) time is 500-600 minutes, and the third section (cooling polymerization section) time is 120-200 minutes.
[0087] In the present invention, the monomer conversion rate of the first initial initiation section can be 8-25%, preferably 8-20%, more preferably 10-18%; the monomer conversion rate of the second constant temperature polymerization section can be 60%-85%, preferably 65%-85%, more preferably 70%-80% or 70%-79%; and the monomer conversion rate of the third cooling polymerization section can be 0.2-8%, preferably 0.4-7%, more preferably 0.5-5% or 1-5%.
[0088] In some embodiments, preferably, the monomer conversion rate of the first stage may be 10-18%, and the monomer conversion rate of the third stage may be 0.5-5%, for example 1-5%.
[0089] The solution polymerization in the present invention is preferably carried out in the presence of an inert gas, such as nitrogen, helium, argon, xenon, and the like.
[0090] In the present invention, the use of inert gas is such that the oxygen content (by volume) in the inert atmosphere is reduced to less than 3000 ppm, less than 2500 ppm, less than 2000 ppm, or less than 1000 ppm.
[0091] In some embodiments, preferably, the solution polymerization is carried out under inert gas protection, wherein the oxygen content is less than 1000 ppm.
[0092] In the present invention, the solution polymerization can be carried out in any suitable polymerization reactor. In some embodiments, the solution polymerization is carried out in a polymerization kettle.
[0093] As is known in the art, after the polymerization is completed, the obtained crude stock solution can be processed, for example, the crude stock solution can be subjected to single-layer and degassing treatments to obtain polyacrylonitrile spinning stock solution.
[0094] In some advantageous embodiments, the method for preparing the polyacrylonitrile spinning solution of the present invention prepares the polyacrylonitrile spinning solution of the present invention.
[0095] In order to achieve the fourth purpose of the above invention, the present invention provides a method for preparing polyacrylonitrile-based carbon fiber as described in one of the above invention purposes, comprising the following steps: a step of preparing polyacrylonitrile spinning stock solution into precursor, and a step of pre-oxidizing and carbonizing the precursor to obtain the polyacrylonitrile-based carbon fiber; wherein the polyacrylonitrile spinning stock solution is the polyacrylonitrile spinning stock solution described in the second purpose of the above invention or the polyacrylonitrile spinning stock solution prepared by the preparation method described in the third purpose of the above invention.
[0096] The preparation of precursors from polyacrylonitrile spinning dopes and the preparation of polyacrylonitrile-based carbon fibers from the precursors are generally known in the art.
[0097] The precursor can be prepared by wet spinning or dry-jet wet spinning, both of which are known in the art. In the present invention, the precursor is preferably prepared by wet spinning.
[0098] For preparing precursor by polyacrylonitrile spinning solution, preparation process can comprise coagulation, drawing, washing, oiling, drying densification, steam drawing, heat setting and winding step.These steps are all known in the art and those skilled in the art can suitably select and use these steps.
[0099] For the coagulation step, after the spun fibers leave the spinneret, they enter the first coagulation bath to coagulate the spun fibers. Those skilled in the art can easily select the composition and temperature of the first coagulation bath. In some embodiments, the temperature of the first coagulation bath is 35°C and the first coagulation bath is an 80% dimethyl sulfoxide aqueous solution. After leaving the first coagulation bath, the filaments can optionally be further passed through one or more subsequent coagulation baths, for example, second and third coagulation baths. After leaving the last coagulation bath, the coagulated filaments can be drawn. The drawing is performed, for example, in steam or hot water. Those skilled in the art can appropriately select the drawing ratio. After drawing, the filaments can be washed, for example, with water, to remove residual solvent. After washing, the filaments can be oiled and dried and densified. Oiling can be performed using an oiling agent commonly used in the art and drying and densification operations commonly used in the art can be used to implement drying and densification. The oiling and drying densification can be performed once or multiple times, and the same or different oiling agents and drying densification conditions can be used. After drying and densification, the resulting filaments can be further stretched, for example, by steam stretching. Those skilled in the art can appropriately select the stretch ratio and stretching conditions. After stretching, the resulting filaments can be heat-set. For example, heat setting can be performed by passing the filaments through multiple stages of heated rollers. After heat setting, the raw yarn is obtained and can be wound for subsequent use.
[0100] As known to those skilled in the art, one or more of the above steps may be omitted or added, or the order of the steps may be adjusted.
[0101] In some embodiments, preferably, the raw silk is prepared by a wet spinning process, wherein the wet spinning process includes the following steps: (1) coagulation of the nascent fiber, (2) hot water drawing, (3) hot water washing, (4) oiling, (5) drying and densification, (6) steam drawing, and (7) winding.
[0102] After obtaining the precursor, the precursor can be prepared into polyacrylonitrile-based carbon fibers. The process of preparing polyacrylonitrile-based carbon fibers from polyacrylonitrile-based precursor is known in the art. The method of the present invention can use processes known in the art to prepare polyacrylonitrile-based carbon fibers.
[0103] The preparation of the precursor into polyacrylonitrile-based carbon fibers may include a pre-oxidation step and a carbonization step. The pre-oxidation step may be performed in an air atmosphere using a gradient temperature ramp method in multiple temperature zones, for example, 2 to 6 temperature zones. The pre-oxidation starting temperature may be 170°C to 200°C, and the pre-oxidation ending temperature may be 260°C to 300°C. During the pre-oxidation, a certain amount of drafting may be applied to the fibers, for example, a drafting rate of 1-5%. The pre-oxidation time may be 30 to 120 minutes.
[0104] The obtained pre-oxidized fiber is carbonized to obtain polyacrylonitrile-based carbon fiber. The carbonization treatment may include low-temperature carbonization and high-temperature carbonization. The temperature of the low-temperature carbonization treatment may be 300°C to 900°C and the treatment time may be 1 to 8 minutes. The temperature of the high-temperature carbonization treatment may be 1000 to 1500°C and the treatment time may be 1 to 8 minutes. In some embodiments, the temperature of the low-temperature carbonization treatment is 300 to 700°C, and the temperature of the high-temperature carbonization treatment is 1000 to 1500°C. As known in the art, the carbonization treatment is carried out in the presence of an inert gas. The inert gas may be, for example, nitrogen, helium, argon, xenon, and the like.
[0105] In some embodiments, preferably, the pre-oxidation temperature is 180-300°C, more preferably divided into 4-6 temperature zones. In some embodiments, preferably, the carbonization includes low-temperature carbonization and high-temperature carbonization, the low-temperature carbonization temperature is 300-700°C, and the high-temperature carbonization temperature is 1000-1500°C.
[0106] In some embodiments, optionally, after carbonization, a graphitization process may be performed. Graphitization processes are known in the art, and graphitization processes generally known in the art may be used.
[0107] In some embodiments, the preparation method may further include a surface treatment step and a gluing step.
[0108] As known to those skilled in the art, the carbon fibers (bundles) of the present invention may be surface treated before sizing, for example, by oxidation to improve the affinity and adhesion between the carbon fibers and the matrix resin in the composite material.
[0109] The sizing treatment can be carried out using various sizing methods known in the art. The present invention does not particularly limit the sizing method, sizing agent, or sizing conditions, as long as the desired sizing agent can be imparted to the carbon fibers. Following the sizing treatment, a drying process can be performed to remove the solvent or dispersion medium used during the sizing process.
[0110] The present invention uses an acrylonitrile solution polymerization process to prepare a polyacrylonitrile spinning solution, wherein the polymerization process adopts three-stage temperature control and optionally, but preferably, controls the oxygen content of the polymerization kettle, so that the gel particles present in the obtained polyacrylonitrile spinning solution meet the requirements of this application and have a high equilibrium swelling degree as defined in this application. In subsequent processing, the gel particles will follow the fiber body to undergo axial tensile deformation and produce axially narrow micropores in the final carbon fiber, which can reduce the negative impact on the mechanical properties of the carbon fiber and ensure that the carbon fiber has good mechanical properties. Therefore, a high-performance carbon fiber containing micropores of the present invention can be obtained.
[0111] In the present invention, the obtained carbon fiber has micropores, and the average radial size L of the micropores is P Less than or equal to 2.0nm, the aspect ratio of the micropore is L / L P The ratio of the volume of micropores with a diameter greater than or equal to 50 and a radial dimension greater than 15 nm to the total micropore volume is less than 10%. When the micropores meet the requirements of this application, the negative impact of the presence of micropores on the mechanical properties of the carbon fiber can be reduced, so that the carbon fiber has good mechanical properties.
[0112] The testing method of the present invention
[0113] Zero shear viscosity of polyacrylonitrile polymer solution
[0114] The test was performed using a rotational rheometer at a temperature of 50 ± 0.01°C, a rotor diameter of 25 mm, and a pitch of 1 mm. To prevent water absorption and solvent evaporation from affecting the results, a uniform layer of methyl silicone oil was applied to the free surface of the sample exposed to air. The change in sample viscosity with shear rate was measured, and the zero-shear viscosity of the polyacrylonitrile polymer solution was obtained by extrapolation.
[0115] Conversion rate
[0116] The monomer conversion rate during polymerization was determined gravimetrically. The initial monomer concentration was A. During or after polymerization, 2.0000 g of the polymer solution was placed on a glass plate. The polymer solution was flattened with the glass plate and washed with water to form a film. The polymer film was then washed with boiling water for 1 hour to remove residual solvent. The polymer film was then dried in a vacuum oven (pressure 2 kPa A, drying temperature 80°C, drying time 8 hours) to constant weight. The mass was recorded as m (in grams). The conversion rate was [m / (A × 2)] × 100%.
[0117] Gel Particle Counting and Sizing Analysis
[0118] The number and size of gel particles in polyacrylonitrile polymer solutions were determined using an AccuSizer A7000 SIS counting particle size analyzer. The test environment maintained a temperature of 25±1°C and a humidity range of 20-80%. The counting particle size analyzer was housed in a cleanroom to minimize the impact of dust and impurities on the test results. The AccuSizer A7000 SIS utilizes single-particle optical sensing technology to count and analyze particles. When a single particle passes through a narrow photosensitive zone, it blocks a portion of the incident light, causing a momentary decrease in the intensity of the incident light reaching the detector. The attenuation of the intensity signal is theoretically proportional to the particle cross-section, or the square of the particle diameter. A calibration curve was established using standard particles to determine the relationship between particle size and intensity signal magnitude. The particle size was then calculated based on the calibration curve and the number of particles counted. The detector used was the LE400-05, with a particle size detection range of 0.15-400 μm and a maximum detectable concentration of 10,000 particles per milliliter. The sample volume was 5 mL, and the flow rate was 30.0 mL / min. Before testing, dilute the polyacrylonitrile polymer solution 20-fold with clean solvent to ensure that the particle count per milliliter of the diluted solution is less than 10,000. Clean solvent is obtained by filtering the solvent through a 0.45-micron PTFE filter to a particle count of less than 100 particles per milliliter.
[0119] Equilibrium swelling
[0120] In the present invention, the equilibrium swelling degree of gel particles is measured in the following manner.
[0121] Take an appropriate amount of gel sample and extract it using a Soxhlet extractor (solvent: DMF, extraction temperature: 145°C, pressure: normal pressure). Remove the soluble polymer adhering to the surface of the gel sample by extraction. At the same time, fully swell to equilibrium in the Soxhlet extractor. The entire extraction process lasts for at least 24 hours. Then take out the swollen equilibrium gel sample, absorb the residual solvent on the surface with absorbent paper, and accurately weigh its mass, which is recorded as m eq Finally, the gel sample that has reached equilibrium swelling is washed with water and then vacuum-dried (pressure 2 kPa A, temperature 80°C, time 8 hours). After complete drying, it is placed in a desiccator and allowed to cool naturally to room temperature to obtain a dry gel sample. The cooled, dried gel sample is removed and its mass is accurately weighed, recorded as m0. The equilibrium swelling degree is calculated using the following formula:
[0122] The gel sample is taken from the insoluble polymer attached to the outer surface of the filter element of the filter. The filter is a 316L stainless steel metal fiber sintered felt filter with a filtration accuracy of 1 μm. The polyacrylonitrile solution (spinning solution) flows from the outer surface of the filter element to the core of the filter element, and the filtered polyacrylonitrile solution flows out of the core. The gel particles are intercepted on the outer surface of the filter element and in the internal pore structure of the stainless steel metal fiber sintered felt. When the pressure difference before and after the filter exceeds 4 MPa, switch to the spare filter, remove the old filter element, and take the insoluble polymer attached to the outer surface of the filter element for the gel particle equilibrium swelling test.
[0123] Number and diameter of polyacrylonitrile precursor and carbon fiber
[0124] Determination is performed using a microscope in accordance with GB / T3364-2008. A randomly cut, approximately 200 mm long segment of the polyacrylonitrile precursor or carbon fiber multifilament sample is sampled. A small fiber bundle, 0.2-0.3 mm in length, is cut from the multifilament using a sharp knife. This fiber bundle is placed on a microscope slide, and a small drop of optical adhesive diluted with xylene is added. The fibers are dispersed with a clean, sharp needle, and then covered with a microscope cover slip. The transmission microscope has a stage mechanism that allows the observation slide to move in two perpendicular directions. The minimum resolution of the transmission microscope should be 2 μm, provided the observation magnification is at least 500x.
[0125] Carbon fiber tensile strength and tensile modulus
[0126] The mechanical tensile method, in accordance with GB / T3362-2005, measures tensile strength by tensile loading until failure after resin impregnation and curing of the fiber. The tensile strength is calculated by dividing the load to failure by the cross-sectional area of the carbon fiber multifilament, and the tensile modulus is determined by the specified strain limit. Ten specimens are tested in each test, with at least six valid specimens. The multifilaments are prepared by manual impregnation with a solution consisting of TDE-85 epoxy resin, diaminodiphenylmethane (DDM), and acetone in a weight ratio of 100:45:150. After impregnation, the specimens should be free of liquid beads and free of adhesion between the multifilaments. A three-stage curing process is employed, with temperatures ranging from 60°C to 90°C and then to 150°C, each stage lasting 45 minutes. After curing, the specimens are attached with reinforcement sheets and placed in an oven at 80°C for one hour to obtain the final test specimens.
[0127] Coefficient of dispersion
[0128] According to GB / T 1446-2005, the arithmetic mean of the test performance is calculated by the following formula: And the standard deviation S, the dispersion coefficient C of the performance can be calculated V .
[0129] Arithmetic mean
[0130] Standard deviation
[0131] Characterization of micropores in precursor and carbon fibers
[0132] The small-angle X-ray scattering (SAXS) method was used for characterization with reference to the following literature [1]. The test was carried out at the BL16B1 small-angle scattering beamline of the Shanghai Synchrotron Radiation Facility. The wavelength of the incident X-ray was 0.124 nm, and a Pilatus 2M detector was used. The detector had 1475*1679 pixels and a pixel size of 172*172 μm. The distance from the bundle sample to the detector was 2092 mm. The test data was processed by determining the center of the scattering signal, converting the scattering data, normalizing the light intensity, and subtracting the background, eliminating the influence of external conditions such as the sample, light intensity, and background during the test.
[0133] For the two-size micropore system, the following dual-model Debye-Bueche analysis method is used:
[0134] Where q is the scattering vector, I(q) is the scattering intensity, I0 is the intensity scaling factor, and L c is the Debye correlation length, and I f It is the background of electron density fluctuation. f It is obtained by: 4 -I(q)*q 4 The slope of the curve after linear fitting is the background of the electron density fluctuation at this location. I0 and Lc can be obtained by linear fitting. On this basis, the relevant distance L can be obtained by fitting the above formula. c1 and L c2 For sparse microporous systems, the size of the correlation distance is close to the size of the micropores. Therefore, Debye-Bueche analysis of the SAXS signals in the meridian and equatorial directions can be performed to obtain the axial size L and radial size L of the micropores along the fiber. P , and according to the axial size L and radial size L of the micropore P The micropore aspect ratio L / L can be calculated P .
[0135] For the scattering of micropores, there is an invariant
[0136] V is the volume of the micropores. Based on the scattering curves of the two micropores fitted by the Debye-Bueche method, the relative volumes of the two micropores can be calculated using this formula.
[0137] Literature [1]: Analyzing the nanoporous structure of aramid fibers, Brian R.Pauw et al., J.Appl.Cryst.(2010).43,837–849
[0138] Evaluation of the amount of fuzz in nascent fibers
[0139] During the normal spinning process, the amount of filaments accumulated at the bath roller of the first coagulation bath was collected every 24 hours. After thorough drying (pressure of 2 kPa A, temperature of 80°C, and time of 8 hours), the weight of the filaments was weighed and used as the amount of nascent fiber filaments.
[0140] Primary fiber breakage
[0141] The frequency of shutdowns due to yarn breakage is used to determine the yarn breakage situation. For example, if a shutdown occurs due to yarn breakage after 20 days of continuous spinning, the shutdown frequency due to yarn breakage is 20 days / time.
[0142] The present invention will be further described below by way of examples.
[0143] The raw materials and reagents used in the Examples and Comparative Examples can be purchased directly or prepared according to methods disclosed in the prior art. If necessary, the raw materials or reagents can be treated before use using methods known in the art to meet the requirements of the reaction. For example, acrylonitrile can be distilled to remove polymerization inhibitors before use.
[0144] In the examples and comparative examples, the oil used was from Wacker Chemicals (China) Co., Ltd. CF 3295.
[0145] [Example 1]
[0146] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, DMSO was used as solvent, and azobisisobutyronitrile was used as initiator. The total monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, and the comonomer was itaconic acid, which accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization kettle was 980 ppm. The initial initiation temperature was 40°C, the duration was 60 min, the middle constant temperature polymerization temperature was 80°C, the duration was 600 min, and the final cooling polymerization temperature was 45°C, the duration was 120 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 KPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 KPa A, the degassing feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 19.0 wt%, and a zero-shear viscosity of 86 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 96,579 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.12%, and the equilibrium swelling degree of the gel particles was 300%.
[0147] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 12,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0 respectively, followed by 9 water washings with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. Afterwards, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation process of primary fiber, there are few hairy and broken fibers, and the frequency of downtime caused by hairy and broken fibers is 37 days / time. V The average radial size of the micropores was L P is 1.85nm, and the micropore aspect ratio is L / L P It is 62.
[0148] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 1.65nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 5 μm, and the diameter dispersion coefficient (C V value) is 2.5%, the tensile strength is 5.5GPa, the tensile strength C V The value is 4.5%, the tensile modulus is 303GPa, and the tensile modulus C V The value is 4.0%.
[0149] [Example 2]
[0150] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, using DMF as solvent and azobisisobutyronitrile as initiator. The total monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization kettle was 760 ppm. The initial initiation temperature was 55°C, the duration was 80 min, the middle constant temperature polymerization temperature was 65°C, the duration was 500 min, and the final cooling polymerization temperature was 40°C, the duration was 200 min. The crude stock solution obtained after the polymerization was subjected to de-monomerization and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the de-monomerization pressure was 1.0 KPa A, the de-monomerization feed temperature was 72°C, and the de-monomerization residence time was 60 min; the degassing pressure was 2.0 KPa A, the degassing feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 18.0 wt%, and a zero-shear viscosity of 50 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 75,744 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.11%, and the equilibrium swelling degree of the gel particles was 500%.
[0151] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 24,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0 respectively, followed by 9 water washings with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. Afterwards, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation process of primary fiber, there are few hairy and broken fibers, and the frequency of downtime caused by hairy and broken fibers is 35 days / time. V The original silk was characterized by small angle X-ray scattering (SAXS), and the average radial size of the micropores was L P is 1.85nm, and the micropore aspect ratio is L / L P It is 58.
[0152] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 1.76nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 7 μm, and the diameter dispersion coefficient (C V value) is 2.6%, the tensile strength is 4.9GPa, the tensile strength C V The value is 4.5%, the tensile modulus is 282GPa, and the tensile modulus C V The value is 4.9%.
[0153] [Example 3]
[0154] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, using DMAC as solvent and azobisisobutyronitrile as initiator. The total monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization reactor was 340 ppm. The initial initiation temperature was 70°C, the duration was 30 min, the middle constant temperature polymerization temperature was 50°C, the duration was 600 min, and the final cooling polymerization temperature was 30°C, the duration was 150 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 KPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 KPa A, the degassing feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 22.0 wt%, and a zero-shear viscosity of 150 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 67,738 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.10%, and the equilibrium swelling degree of the gel particles was 1000%.
[0155] (2) Preparation of raw fibers: The polyacrylonitrile solution prepared in (1) was metered by a metering pump and filtered through a sintered metal filter (filter accuracy 5 μm). It was then extruded through a spinneret and entered the first coagulation bath. The spinneret aperture was 55 μm and the number of spinneret holes was 3000. The temperature of the first coagulation bath was 35°C, the first coagulation bath was an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the raw fibers passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. The fibers were then drawn through three hot water draws at temperatures of 90°C, 92°C, and 95°C, respectively, with draft ratios of 1.20, 1.41, and 2.0, respectively. Then, 9 water washings are carried out, using a step-by-step heating method, with the 1-3 water washing temperatures at 50°C, the 4-6 water washing temperatures at 60°C, and the 7-9 water washing temperatures at 70°C. No stretching is performed during the water washing stage. Afterwards, the first oiling is carried out with an oil concentration of 1.2%, and the first drying and densification is carried out with a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is carried out with a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretching ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. There are fewer hairs and broken fibers during the coagulation process of the primary fiber, and the frequency of downtime due to hairs and broken fibers is 48 days / time. The diameter dispersion coefficient of the precursor (C V The original silk was characterized by small angle X-ray scattering (SAXS), and the average radial size of the micropores was L P is 1.62nm, and the micropore aspect ratio is L / L P It is 62.
[0156] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 1.57nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 6 μm, and the diameter dispersion coefficient (C V value) is 2.4%, the tensile strength is 5.8GPa, the tensile strength C V The value is 3.5%, the tensile modulus is 323GPa, and the tensile modulus C V The value is 4.3%.
[0157] [Example 4]
[0158] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, DMSO was used as the solvent, and azobisisobutyronitrile was used as the initiator. The monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, and the comonomer was itaconic acid, which accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization reactor was 600 ppm. The initial initiation temperature was 40°C, the duration was 60 min, the middle constant temperature polymerization temperature was 80°C, the duration was 600 min, and the final cooling polymerization temperature was 45°C, the duration was 120 min. The crude stock solution obtained after the polymerization was subjected to de-monomerization and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the de-monomerization pressure was 1.0 KPa A, the de-monomerization feed temperature was 72°C, and the de-monomerization residence time was 60 min; the degassing pressure was 2.0 KPa A, the de-monomerization feed temperature was 65°C, and the de-gassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 19.8 wt%, and a zero-shear viscosity of 88 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 91,456 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.11%, and the equilibrium swelling degree of the gel particles was 800%.
[0159] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 12,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0 respectively, followed by 9 water washings with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. Afterwards, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation process of primary fiber, there are few hairy and broken fibers, and the frequency of downtime caused by hairy and broken fibers is 37 days / time. V The original silk was characterized by small angle X-ray scattering (SAXS), and the average radial size of the micropores was L P is 1.65nm, and the micropore aspect ratio is L / L P It is 61.
[0160] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 1.45nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 5 μm, and the diameter dispersion coefficient (C V value) is 2.5%, the tensile strength is 5.7GPa, the tensile strength C V The value is 4.4%, the tensile modulus is 312GPa, and the tensile modulus C V The value is 4.0%.
[0161] [Example 5]
[0162] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, using DMF as solvent and azobisisobutyronitrile as initiator. The total monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization reactor was 500 ppm. The initial initiation temperature was 55°C, the duration was 80 min, the middle constant temperature polymerization temperature was 65°C, the duration was 500 min, and the final cooling polymerization temperature was 40°C, the duration was 200 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 KPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 KPa A, the degassing feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 18.0 wt%, and a zero-shear viscosity of 55 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 72,324 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.10%, and the equilibrium swelling degree of the gel particles was 900%.
[0163] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 24,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0, respectively. Then it is washed in water for 9 times, with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. After that, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation process of primary fiber, there are few hairy and broken fibers, and the frequency of downtime caused by hairy and broken fibers is 35 days / time. V The original silk was characterized by small angle X-ray scattering (SAXS), and the average radial size of the micropores was L P is 1.55nm, and the micropore aspect ratio is L / L P is 60.
[0164] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 1.46nm, and the micropore aspect ratio is L / L PThe average diameter of carbon fiber is 7 μm, and the diameter dispersion coefficient (C V value) is 2.6%, the tensile strength is 5.2GPa, the tensile strength C V The value is 4.7%, the tensile modulus is 289GPa, and the tensile modulus C V The value is 4.6%.
[0165] [Example 6]
[0166] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, using DMAC as solvent and azobisisobutyronitrile as initiator. The total monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization reactor was 100 ppm. The initial initiation temperature was 70°C, the duration was 30 min, the middle constant temperature polymerization temperature was 50°C, the duration was 600 min, and the final cooling polymerization temperature was 30°C, the duration was 150 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 KPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 KPa A, the degassing feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 22.0 wt%, and a zero-shear viscosity of 162 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 60,128 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.08%, and the equilibrium swelling degree of the gel particles was 2000%.
[0167] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 3000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0, respectively. Then it is washed in water for 9 times, with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. After that, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation process of primary fiber, there are few hairy and broken fibers, and the frequency of downtime caused by hairy and broken fibers is 48 days / time. V The average radial size of the micropores was L P is 1.42nm, and the micropore aspect ratio is L / L P It is 65.
[0168] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 1.37nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 6 μm, and the diameter dispersion coefficient (C V value) is 2.4%, the tensile strength is 5.8GPa, the tensile strength C V The value is 2.5%, the tensile modulus is 323GPa, and the tensile modulus C V The value is 2.3%.
[0169] [Example 7]
[0170] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, using DMF as solvent and azobisisobutyronitrile as initiator. The total monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization reactor was 1500 ppm. The initial initiation temperature was 55°C, the duration was 80 min, the middle constant temperature polymerization temperature was 65°C, the duration was 500 min, and the final cooling polymerization temperature was 30°C, the duration was 200 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 KPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 KPa A, the deaeration feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 18.0 wt%, and a zero-shear viscosity of 48 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 78,630 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.13%, and the equilibrium swelling degree of the gel particles was 480%.
[0171] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 24,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0, respectively. Then it is washed in water for 9 times, with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. After that, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation process of primary fiber, there are few hairy and broken fibers, and the frequency of downtime caused by hairy and broken fibers is 35 days / time. V The average radial size of the micropores was L P is 1.98nm, and the micropore aspect ratio is L / L P It is 48.
[0172] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 1.83 nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 7 μm, and the diameter dispersion coefficient (C V value) is 2.8%, the tensile strength is 4.98GPa, the tensile strength C V The value is 4.9%, the tensile modulus is 292GPa, and the tensile modulus C V The value is 4.7%.
[0173] [Example 8]
[0174] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, using DMSO as solvent and azobisisobutyronitrile as initiator. The total monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization reactor was 2500 ppm. The initial initiation temperature was 55°C, the duration was 120 min, the middle constant temperature polymerization temperature was 65°C, the duration was 550 min, and the final cooling polymerization temperature was 45°C, the duration was 100 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 KPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 KPa A, the degassing feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 19.8 wt %, and a zero-shear viscosity of 96 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 87,339 particles / mL. The proportion of gel particles with a particle size greater than 5 μm was 0.21% of the total number of gel particles. The equilibrium swelling ratio of the gel particles was 390%.
[0175] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 24,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0, respectively. Then it is washed in water for 9 times, with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. After that, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation process of primary fiber, there are few hairy and broken fibers, and the frequency of downtime caused by hairy and broken fibers is 33 days / time. V The average radial size of the micropores was L P is 1.99 nm, and the micropore aspect ratio is L / L P It is 46.
[0176] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 1.96nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 7 μm, and the coefficient of diameter dispersion (C V value) is 2.8%, the tensile strength is 4.93GPa, the tensile strength C V The value is 4.9%, the tensile modulus is 289GPa, and the tensile modulus C V The value is 4.8%.
[0177] [Comparative Example 1]
[0178] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, using DMF as solvent and azobisisobutyronitrile as initiator. The total monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a two-stage method. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization reactor was 1500 ppm. The initial initiation temperature was 30°C, the duration was 30 min, and the constant temperature polymerization temperature was 65°C, the duration was 750 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 kPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 kPa A, the deaeration feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 18.2 wt%, and a zero-shear viscosity of 65 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 112,822 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.65%, and the equilibrium swelling degree of the gel particles was 180%.
[0179] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 24,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0, respectively. Then it is washed in water for 9 times, with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. After that, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation of primary fibers, hairy fibers and broken fibers appeared, and the frequency of downtime caused by hairy fibers and broken fibers was 20 days / time. V The average radial size of the micropores was L P is 3.29nm, and the micropore aspect ratio is L / L P It is 43.
[0180] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 3.18 nm, and the micropore aspect ratio is L / L PThe average diameter of carbon fiber is 7 μm, and the coefficient of diameter dispersion (C V value) is 3.6%, the tensile strength is 4.2GPa, the tensile strength C V The value is 6.5%, the tensile modulus is 257GPa, and the tensile modulus C V The value is 7.2%.
[0181] [Comparative Example 2]
[0182] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, using DMSO as solvent and azobisisobutyronitrile as initiator. The total monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a two-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization kettle was 680 ppm. The initial initiation temperature was 20°C, the duration was 60 min, and the constant temperature polymerization temperature was 80°C, the duration was 720 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 KPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 KPa A, the degassing feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 19.0 wt%, and a zero-shear viscosity of 92 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 134,925 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.87%, and the equilibrium swelling degree of the gel particles was 120%.
[0183] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 12,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0 respectively. Then it is washed in water for 9 times, with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. After that, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation of primary fibers, hairy fibers and broken fibers appeared, and the frequency of downtime caused by hairy fibers and broken fibers was 23 days / time. V The original silk was characterized by small angle X-ray scattering (SAXS), and the average radial size of the micropores was L P is 3.92nm, and the micropore aspect ratio is L / L P It is 38.
[0184] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 3.73nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 5 μm, and the diameter dispersion coefficient (C V value) is 7.5%, the tensile strength is 3.8GPa, the tensile strength C V The value is 6.5%, the tensile modulus is 233GPa, and the tensile modulus C V The value is 7.0%.
[0185] [Comparative Example 3]
[0186] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, using DMAC as solvent and azobisisobutyronitrile as initiator. The total monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a two-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization reactor was 340 ppm. The initial initiation temperature was 20°C, the duration was 100 min, and the constant temperature polymerization temperature was 85°C, the duration was 680 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 KPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 KPa A, the degassing feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 22.0 wt%, and a zero-shear viscosity of 146 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 170,738 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 1.2%, and the equilibrium swelling degree of the gel particles was 100%.
[0187] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 3000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0, respectively. Then it is washed in water for 9 times, with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. After that, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation process of primary fiber, hairy and broken fibers appeared, and the frequency of downtime caused by hairy and broken fibers was 18 days / time. V The original silk was characterized by small angle X-ray scattering (SAXS), and the average radial size of the micropores was L P is 4.62nm, and the micropore aspect ratio is L / L P is 35.
[0188] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 3.92nm, and the micropore aspect ratio is L / L PThe average diameter of carbon fiber is 6 μm, and the diameter dispersion coefficient (C V value) is 6.4%, the tensile strength is 3.8GPa, the tensile strength C V The value is 6.5%, the tensile modulus is 256GPa, and the tensile modulus C V The value is 6.3%.
[0189] [Comparative Example 4]
[0190] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, DMSO was used as the solvent, and azobisisobutyronitrile was used as the initiator. The monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization kettle was 2500 ppm. The initial initiation temperature was 25°C, the duration was 120 min, the middle constant temperature polymerization temperature was 80°C, the duration was 640 min, and the final polymerization temperature was 65°C, the duration was 120 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 KPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 KPa A, the degassing feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 18.6 wt%, and a zero-shear viscosity of 78 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 125,990 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.96%, and the equilibrium swelling degree of the gel particles was 150%.
[0191] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 12,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0, respectively. Then it is washed in water for 9 times, with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. After that, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation of primary fibers, hairy fibers and broken fibers appeared, and the frequency of downtime caused by hairy fibers and broken fibers was 19 times per day. V The average radial size of the micropores was L P is 3.35nm, and the micropore aspect ratio is L / L P It is 38.
[0192] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 3.65nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 5 μm, and the diameter dispersion coefficient (C V value) is 6.5%, the tensile strength is 4.06GPa, and the tensile strength C V The value is 7.5%, the tensile modulus is 233GPa, and the tensile modulus C V The value is 6.0%.
[0193] [Comparative Example 5]
[0194] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, DMSO was used as the solvent, and azobisisobutyronitrile was used as the initiator. The monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization reactor was 600 ppm. The initial initiation temperature was 40°C, the duration was 60 min, the middle constant temperature polymerization temperature was 75°C, the duration was 600 min, and the final polymerization temperature was 65°C, the duration was 120 min. The crude stock solution obtained after the polymerization was subjected to de-monomerization and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the de-monomerization pressure was 1.0 KPa A, the de-monomerization feed temperature was 72°C, and the de-monomerization residence time was 60 min; the degassing pressure was 2.0 KPa A, the degassing feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 19.8 wt%, and a zero-shear viscosity of 97 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 121,440 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.85%, and the equilibrium swelling degree of the gel particles was 200%.
[0195] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 12,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0, respectively. Then it is washed in water for 9 times, with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. After that, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation of primary fibers, hairy fibers and broken fibers appeared, and the frequency of downtime caused by hairy fibers and broken fibers was 23 days / time. V The original silk was characterized by small angle X-ray scattering (SAXS), and the average radial size of the micropores was L P is 3.25nm, and the micropore aspect ratio is L / L P It is 41.
[0196] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (1) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fibers. The obtained pre-oxidized fibers were subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fibers. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fibers were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0.05. P is 2.79nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 5 μm, and the coefficient of diameter dispersion (C V value) is 6.9%, the tensile strength is 4.10GPa, the tensile strength C V The value is 7.3%, the tensile modulus is 238GPa, and the tensile modulus C V The value is 6.0%.
[0197] [Comparative Example 6]
[0198] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, DMSO was used as the solvent, and azobisisobutyronitrile was used as the initiator. The monomer concentration was 21.5 wt%, the initiator dosage was 0.45 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization kettle was 340 ppm. The initial initiation temperature was 20°C, the duration was 100 min, the middle constant temperature polymerization temperature was 85°C, the duration was 550 min, and the final polymerization temperature was 45°C, the duration was 120 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 KPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 KPa A, the degassing feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 22.0 wt%, and a zero-shear viscosity of 146 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 119,380 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.83%, and the equilibrium swelling degree of the gel particles was 260%.
[0199] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 12,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0, respectively. Then it is washed in water for 9 times, with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. After that, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation of primary fibers, hairy fibers and broken fibers appeared, and the frequency of downtime caused by hairy fibers and broken fibers was 21 times per day. V The average radial size of the micropores was L P is 3.16nm, and the micropore aspect ratio is L / L P It is 44.
[0200] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 2.56nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 5 μm, and the diameter dispersion coefficient (C V value) is 6.9%, the tensile strength is 4.32GPa, the tensile strength C V The value is 6.8%, the tensile modulus is 248GPa, and the tensile modulus C V The value is 5.5%.
[0201] [Comparative Example 7]
[0202] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, DMSO was used as the solvent, and azobisisobutyronitrile was used as the initiator. The monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, and the comonomer was itaconic acid, which accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization reactor was 600 ppm. The initial initiation temperature was 50°C, the duration was 60 min, the middle constant temperature polymerization temperature was 45°C, the duration was 200 min, and the final polymerization temperature was 75°C, the duration was 550 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 KPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 KPa A, the degassing feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 19.8 wt%, and a zero-shear viscosity of 112 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 123,650 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.89%, and the equilibrium swelling degree of the gel particles was 190%.
[0203] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 12,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0, respectively. Then it is washed in water for 9 times, with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. After that, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation of primary fibers, hairy fibers and broken fibers appeared, and the frequency of downtime caused by hairy fibers and broken fibers was 21 times per day. V The average radial size of the micropores was L P is 3.35nm, and the micropore aspect ratio is L / L P It is 39.
[0204] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 3.26nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 5 μm, and the coefficient of diameter dispersion (C V value) is 7.0%, the tensile strength is 4.12GPa, the tensile strength C V The value is 6.6%, the tensile modulus is 237GPa, and the tensile modulus C V The value is 6.5%.
[0205] [Comparative Example 8]
[0206] (1) Preparation of stock solution: Acrylonitrile was subjected to solution polymerization, DMSO was used as solvent, and azobisisobutyronitrile was used as initiator. The monomer concentration was 20.5 wt%, the initiator dosage was 0.34 wt% of the total monomer mass, the comonomer was itaconic acid, and itaconic acid accounted for 1 mol% of the total monomer mass. The polymerization temperature was controlled by a three-stage temperature control. Nitrogen was purged before the polymerization temperature was raised, and the oxygen content in the polymerization kettle was 600 ppm. The initial initiation temperature was 40°C, the duration was 60 min, the middle constant temperature polymerization temperature was 65°C, the duration was 450 min, and the final polymerization temperature was 75°C, the duration was 250 min. The crude stock solution obtained after the polymerization was subjected to deaeration and degassing treatment to obtain a polyacrylonitrile solution (stock solution), wherein the deaeration pressure was 1.0 KPa A, the deaeration feed temperature was 72°C, and the deaeration residence time was 60 min; the degassing pressure was 2.0 KPa A, the deaeration feed temperature was 65°C, and the degassing residence time was 120 min. The polyacrylonitrile solution had a solid content of 19.8 wt%, and a zero-shear viscosity of 134 Pa·s at 50°C. The total number (Np) of gel particles with a particle size greater than 0.15 μm in the polyacrylonitrile solution was 123,920 particles / mL, the proportion of gel particles with a particle size greater than 5 μm to the total number of gel particles was 0.92%, and the equilibrium swelling degree of the gel particles was 180%.
[0207] (2) Preparation of Precursor Fiber: The polyacrylonitrile solution prepared in (1) above was metered by a metering pump, filtered through a sintered metal filter (filter precision 5 μm), and extruded through a spinneret. The spinneret had an aperture of 55 μm and 12,000 holes. The first coagulation bath temperature was 35°C, the first coagulation bath consisted of an 80% dimethyl sulfoxide aqueous solution, and the draft ratio was -30%. After coagulation, the nascent fiber passed through a godet roller and entered the second and third coagulation baths. The coagulation bath concentrations were 60% and 30%, respectively, and the temperatures were 40°C and 60°C, respectively, with draft ratios of 1.0 and 1.05, respectively. Then it is stretched in hot water for 3 times at temperatures of 90°C, 92°C and 95°C, with stretch ratios of 1.20, 1.41 and 2.0, respectively. Then it is washed in water for 9 times, with a step-by-step heating method, with the 1-3 washing temperatures at 50°C, the 4-6 washing temperatures at 60°C and the 7-9 washing temperatures at 70°C. No stretching is performed during the washing stage. After that, the first oiling is performed with an oil concentration of 1.2%, and the first drying and densification is performed at a drying temperature of 95°C; followed by a second oiling with an oil concentration of 2.0%, and a second drying and densification is performed at a drying temperature of 130°C. The fiber is then steam stretched with a steam pressure of 0.35MPa and a steam stretch ratio of 3.2. The fiber is then heat-set with a heat-setting steam pressure of 0.1MPa. Finally, the fiber is wound up to obtain carbon fiber precursor. During the coagulation of primary fibers, hairy fibers and broken fibers appeared, and the frequency of downtime caused by hairy fibers and broken fibers was 20 days / time. V The original silk was characterized by small angle X-ray scattering (SAXS), and the average radial size of the micropores was L P is 3.25nm, and the micropore aspect ratio is L / L P It is 38.
[0208] (3) Preparation of carbon fiber: The polyacrylonitrile precursor prepared in the above (2) was subjected to heat stabilization treatment in the range of 180-280°C through 5 air atmosphere heating furnaces, and the temperatures were 181°C, 222°C, 234°C, 252°C, and 273°C respectively; the total heating time was 62 minutes, and the total draft was 2.2% to obtain pre-oxidized fiber. The obtained pre-oxidized fiber was subjected to low-temperature carbonization and high-temperature carbonization treatment in nitrogen to obtain carbon fiber. The low-temperature carbonization temperature was 300-700°C, the heat treatment time was 3.8 minutes, and the draft was 2.8%; the high-temperature carbonization temperature was 1000-1500°C, the heat treatment time was 1.8 minutes, and the draft was -2.8%. The micropores of the obtained carbon fiber were characterized by small-angle X-ray scattering (SAXS), and the average radial size L of the micropores perpendicular to the fiber axis was 0. P is 3.19 nm, and the micropore aspect ratio is L / L PThe average diameter of the carbon fiber is 5 μm, and the diameter dispersion coefficient (C V value) is 6.8%, the tensile strength is 4.16GPa, the tensile strength C V The value is 6.5%, the tensile modulus is 239GPa, and the tensile modulus C V The value is 6.3%.
[0209] The data in the above examples and comparative examples are summarized in the following table.
Claims
1. A polyacrylonitrile-based carbon fiber containing micropores, wherein the average radial size L of the micropores is P is less than or equal to 2.0 nm, and the aspect ratio of the micropore is L / L P is greater than or equal to 50 and less than or equal to 100, and the ratio of the volume of micropores having a radial dimension greater than 15 nm to the total micropore volume is greater than 0 and less than 10%.
2. The polyacrylonitrile-based carbon fiber according to claim 1, characterized in that The average radial dimension L of the micropores P is less than or equal to 1.5nm, and the micropore aspect ratio is L / L P is greater than or equal to 60 and less than or equal to 100, and the ratio of the volume of micropores having a radial dimension greater than 15 nm to the total micropore volume is greater than 0 and less than 5%.
3. The polyacrylonitrile-based carbon fiber according to any one of claims 1 to 2, characterized in that The diameter C of the carbon fiber V Value less than or equal to 3%.
4. The polyacrylonitrile-based carbon fiber according to any one of claims 1 to 3, characterized in that The fiber number of the polyacrylonitrile-based carbon fiber is 3,000 to 24,000.
5. The polyacrylonitrile-based carbon fiber according to any one of claims 1 to 4, characterized in that The diameter of the polyacrylonitrile-based carbon fiber is 5-7 μm; the tensile strength is 4.9-5.8 GPa, and the tensile strength C V value is less than 5%; and / or the tensile modulus is 282-323GPa, and the tensile modulus C V Value is less than 5%.
6. A polyacrylonitrile spinning stock solution containing gel particles, wherein the total number of gel particles with a particle size greater than 0.15 μm contained in the solution is less than or equal to 1×10 5 / mL, and the proportion of gel particles with a particle size greater than 5 μm to the total gel particles is less than or equal to 0.3%; wherein the equilibrium swelling degree of the gel particles is 250-5000%.
7. The polyacrylonitrile spinning solution according to claim 6, characterized in that: The polyacrylonitrile spinning stock solution comprises a polyacrylonitrile polymer and a solvent, and the weight ratio of the polyacrylonitrile polymer to the solvent is (15-30):(85-70), preferably (18-22):(82-78).
8. The polyacrylonitrile spinning solution according to claim 7, characterized in that: The solvent is at least one of dimethyl sulfoxide, dimethylformamide, dimethylacetamide, and a mixture thereof; and / or the polyacrylonitrile polymer is a polyacrylonitrile homopolymer, a polyacrylonitrile copolymer, or a mixture thereof.
9. The polyacrylonitrile spinning solution according to any one of claims 6 to 8, characterized in that: The zero shear viscosity of the polyacrylonitrile spinning solution is 30-200 Pa·s, preferably 50-150 Pa·s, wherein the viscosity test temperature is 50°C.
10. A method for preparing a polyacrylonitrile spinning solution, preferably the polyacrylonitrile spinning solution according to any one of claims 6 to 9, which includes solution polymerization, wherein the solution polymerization adopts three-stage temperature control, wherein the temperature of the first initial initiation section is T1°C, the temperature of the second constant temperature polymerization section is T2°C, and the temperature of the third cooling polymerization section is T3°C; wherein T1, T2, and T3 satisfy the following relationship: T1 = (0.5~1.4)*T2 and 35≤T1≤80; and T3 = T2-(5~50) and 50≥T3≥25.
11. The method for preparing polyacrylonitrile spinning solution according to claim 10, characterized in that: 35°C≤T1≤80°C, preferably 40°C≤T1≤70°C; 40°C≤T2≤90°C, preferably 50°C≤T2≤80°C; and 25°C≤T3≤50°C, preferably 25°C≤T3≤45°C, more preferably 30°C≤T3≤45°C.
12. The method for preparing polyacrylonitrile spinning solution according to claim 10 or 11, characterized in that: 50℃≤T2≤80℃, 40℃≤T1≤70℃, and 30℃≤T3≤45℃; and / or T3=T2-(15~50), preferably T3=T2-(15~40), more preferably T3=T2-(20~35).
13. The method for preparing polyacrylonitrile spinning solution according to any one of claims 10 to 12, characterized in that: The polymerization time of the first initial initiation stage is 20-150 minutes, preferably 30-120 minutes, more preferably 30-80 minutes; the polymerization time of the second constant temperature polymerization stage is 300-900 minutes, preferably 400-800 minutes, preferably 400-700 minutes, more preferably 500-600 minutes; and the polymerization time of the third temperature reduction polymerization stage is 80-300 minutes, preferably 80-250 minutes, preferably 100-250 minutes, more preferably 120-200 minutes; and / or The monomer conversion rate of the second constant temperature polymerization section is X, the monomer conversion rate of the first initial initiation section is (0.125-0.215)*X, and the monomer conversion rate of the third temperature reduction polymerization section is (0.007-0.0715)*X, wherein the monomer conversion rate X of the second constant temperature polymerization section is 60%-85%, preferably 65%-85%, more preferably 70%-80% or 70%-79%.
14. The method for preparing polyacrylonitrile spinning solution according to any one of claims 10 to 13, characterized in that: The solution polymerization is protected by an inert gas; preferably, the solution polymerization is protected by an inert gas and the oxygen content is less than 1000 ppm; and / or The solution polymerization is carried out in a polymerization vessel.
15. A method for preparing the polyacrylonitrile-based carbon fiber according to any one of claims 1 to 5, comprising the steps of preparing a polyacrylonitrile spinning solution into a precursor, and pre-oxidizing and carbonizing the precursor to obtain the polyacrylonitrile-based carbon fiber; wherein the polyacrylonitrile spinning solution is the polyacrylonitrile spinning solution according to any one of claims 6 to 9 or the polyacrylonitrile spinning solution obtained by the preparation method according to any one of claims 10 to 14.
16. The method for preparing polyacrylonitrile-based carbon fiber according to claim 15, characterized in that The raw silk preparation steps include: (1) coagulation of primary fibers, (2) hot water drawing, (3) hot water washing, (4) oiling, (5) drying and densification, (6) steam drawing, and (7) winding.
17. The method for preparing polyacrylonitrile-based carbon fiber according to claim 15, characterized in that: The pre-oxidation temperature is 180-300°C, preferably divided into 4-6 temperature zones; and / or the carbonization includes low-temperature carbonization and high-temperature carbonization, preferably, the low-temperature carbonization temperature is 300-700°C, and the high-temperature carbonization temperature is 1000-1500°C.
18. The method for preparing polyacrylonitrile-based carbon fiber according to claim 15, characterized in that: The preparation method also includes the steps of surface treatment and gluing.
Citation Information
Patent Citations
Carbon fiber bundle and method for manufacturing same
CN110832127A
Prepn of polyacrylonitrile-base high-performance raw carbon fiber
CN1417393A
Polyacrylonitrile-based polymer and method for producing the same, and method for producing carbon fiber precursor, and carbon fiber and method for producing the same
JP2008248219A
Method for producing carbon fiber precursor fiber bundle and carbon fiber bundle
JP2017128838A
Carbon fiber bundle and method for producing the same
JP2018141251A