Polyacrylonitrile carbon fiber, polyacrylonitrile precursor, and preparation methods therefor
By controlling the penetration gradient and content of silicon in carbon fibers and employing a two-stage oiling process with a specific Si/C ratio, the problem of high ash content and low performance in wet spinning carbon fibers was solved, enabling the preparation of low-ash, high-performance carbon fibers and long-term operation of the equipment.
Patent Information
- Application Number
- PCT/CN2023/143018
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2023-12-29
- Publication Date
- 2024-10-24
AI Technical Summary
In the existing technology for preparing carbon fibers by wet spinning, the mechanical properties of carbon fibers decrease due to the effort to reduce ash content, especially the high content of silicon impurities, which affects fiber quality and equipment lifespan.
By controlling the penetration gradient and content of silicon in carbon fibers, and employing a two-stage oiling process, the first stage uses a silicon-free or low-silicone oil, while the second stage uses a silicone-containing oil. The drying and densification treatment is avoided between the two stages, thus preparing polyacrylonitrile precursor fibers with a specific Si/C ratio, ensuring the uniform distribution and penetration control of silicon on the fiber surface.
This approach achieves low ash content while improving the mechanical properties of carbon fiber, extending equipment operating cycles, reducing equipment cleaning frequency, and ensuring high strength and high modulus of carbon fiber.
Smart Images

Figure CN2023143018_24102024_PF_FP_ABST
Abstract
Description
Polyacrylonitrile carbon fiber and precursor and method for producing the same Technical Field
[0001] The present invention relates to polyacrylonitrile carbon fibers and a method for producing the same. The present invention also relates to polyacrylonitrile carbon fiber precursor yarn used for producing the carbon fibers and a method for producing the same. Background Art
[0002] Carbon fiber is an inorganic polymer fiber material with a carbon content of over 90%. Its chemical structure is stable, and it exhibits high strength, high modulus, and low mass. It also possesses numerous excellent properties, including high-temperature resistance, corrosion resistance, low thermal expansion coefficient, excellent heat transfer, chemical stability, and electrical conductivity. Carbon fiber is used as a reinforcement for high-performance composite materials and is widely used in aerospace, building reinforcement, sporting goods, automotive structures, wind turbine blades, the photovoltaic industry, and medical devices. However, the continuous development of aerospace and high-end equipment has also placed new performance requirements on carbon fiber materials, which are no longer limited to basic indicators such as strength and modulus. In particular, aerospace applications have imposed new requirements on the ash content of carbon fiber.
[0003] The performance of carbon fiber is primarily affected by defects. High-quality oils and a well-defined oiling process are effective means of preventing these defects. After PAN precursor is treated with a specialized oil, a heat-resistant protective film forms on the fiber surface, separating the individual filaments and preventing them from sticking and doubling during the pre-oxidation process. Currently, silicone oils are primarily used in the production of high-performance carbon fiber precursor. However, some silicon components in silicone oils decompose poorly at high temperatures, resulting in incomplete decomposition during the pre-oxidation and carbonization processes. The resulting impurities, such as silicon carbide and silicon nitride, remain within the carbon fiber, creating weak spots during stretching or bending, severely impacting its quality. Furthermore, silicon oxides generated during the pre-oxidation and carbonization processes are the primary source of ash. Ash not only contaminates equipment, shortening its production cycle and service life, but also reduces operating time, requiring frequent equipment shutdowns for cleaning.
[0004] There are many types of precursor fibers that can be used to produce carbon fibers. Currently, over 90% of carbon fibers on the market are made from PAN fibers. PAN-based carbon fibers, characterized by high carbon yield, excellent mechanical properties, and mature processing, have become the primary carbon fiber product. Currently, PAN fibers are primarily produced by wet spinning and dry-jet-wet spinning. In the dry-jet-wet spinning process, the solution, after being extruded from the spinneret, passes through an air section before entering a coagulation bath for solidification. This operation results in significant differences between dry-jet-wet spinning and wet spinning, from the solution system, spinning process, to spinning equipment, and the resulting precursor and carbon fibers have different morphologies and structures. Dry-jet-wet-spun carbon fibers have a smooth surface and a denser structure, while wet-spun carbon fibers have a distinct grooved surface structure, where the height difference between the top of the protrusion and the bottom of the groove can reach tens of nanometers. This concave-convex groove structure acts as a defect, causing the carbon fibers to break. Therefore, the key structural features that influence fracture in wet-spun and dry-jet-wet-spun carbon fibers are also different. In the preparation process of PAN fibers, compared with dry-jet wet spinning, the wet spinning process is more mature, the spinning process is stable and easy to control, the residual solvent in the fiber is easy to remove, and the obtained carbon fiber is easier to combine with composite materials. It is an important method for preparing high-performance carbon fiber precursors.
[0005] High-quality carbon fiber precursors must exhibit characteristics such as few surface defects, minimal porosity, a dense structure, good stretchability, and high heat resistance. To produce high-quality carbon fibers with excellent performance and controllable silicon content and silicon permeability, the precursors must have low silicon content, low silicon permeability, and a uniform oil film coating on the fiber surface. During carbon fiber precursor production, the solidification process is a double diffusion process, resulting in numerous pores in the nascent fibers. During the subsequent stretching and washing processes, some of these pores gradually decrease in size or even close. Unclosed pores can be infiltrated with silicone oil during the oiling process. During the subsequent drying and densification process, these pores may close, making it difficult to completely remove the silicone oil from the pores, leaving it inside the fiber. This, in turn, results in a high ash content during the carbonization process, making it difficult to completely remove the infiltrated Si, which remains in the carbon fibers and affects the final performance of the carbon fibers.
[0006] Therefore, selecting a high-quality oil and a reasonable oiling process are important operations for preparing low-ash, high-performance polyacrylonitrile carbon fibers and the carbon fiber precursors.
[0007] CN113597484A discloses a method for manufacturing carbon fibers that inhibits the intrusion of oils into the fiber surface and suppresses surface pores, wherein SIMS (secondary ion mass spectrometry) is used to calculate the Si / C ratio at a certain depth from the fiber surface. The application clearly states that this invention cannot be used to improve the strength of wet-spun carbon fibers. In addition, wet spinning generally uses a multi-stage coagulation process, and the coagulation bath concentration, temperature, and immersion time are completely different from those of dry-jet wet spinning. Therefore, the dry-jet wet spinning coagulation conditions and air residence time of the invention of CN113597484A cannot be used for the preparation of wet-spun carbon fiber precursors, and it is also impossible to inhibit the intrusion of oils into the fiber surface during the wet spinning process, and it is impossible to inhibit inter-fiber bonding and the pores of the carbon fiber surface. Moreover, compared to dry-jet wet spinning, wet-spun nascent fibers have a looser structure and larger pores in the fibers, making it easier for oils to invade the fiber interior during the oiling process. Therefore, a new method is needed to achieve the purpose of inhibiting Si infiltration and improving carbon fiber performance.
[0008] CN111088559A discloses a method in which the first oiling step uses an ultra-low silicone oil agent or a silicone-free oil agent. After the first drying and densification step, the second oiling step uses a general silicone oil agent. This method is used to solve the problems of excessive carbon fiber filaments, poor mechanical properties and large coke discharge in low-carbon furnaces.
[0009] CN114622417A discloses a carbon fiber silicone oiling agent that can reduce friction damage between the raw yarn and the roller, ensures homogeneous pre-oxidation of the fibers, and inhibits carbonized filament adhesion and doubling, but does not address the issues of carbonized ash and carbon fiber impurities.
[0010] CN112424418A discloses a carbon fiber silicone oil. This application solves the problem of fuzzing during the spinning process of the raw yarn and can effectively protect the carbon fibers. However, the resulting carbon fibers have low strength and the problem of carbonized ash and carbon fiber impurities is not mentioned.
[0011] CN112726207A discloses a silicone-free oil agent for the manufacture of carbon fiber precursor, which produces very little ash and greatly reduces damage to equipment such as carbonization furnaces. However, the resulting carbon fiber has a low strength modulus and is not suitable for the preparation of high-strength and high-modulus carbon fibers.
[0012] CN110863270A discloses a method for reducing the ash content of high-strength polyacrylonitrile-based carbon fibers, comprising the steps of impregnating the polyacrylonitrile-based carbon fibers with an organic solvent and treating them with hydrofluoric acid. However, this method has an adverse effect on the properties of the carbon fibers, such as tensile modulus.
[0013] CN103290527A discloses a method for reducing the ash content of polyacrylonitrile-based carbon fibers. Based on a quaternary ammonium-modified copolymer system, this application prepares a highly hydrophilic PAN spinning solution. The oil content of the filaments is then controlled by controlling the swelling of the precursor before application of an oil and by introducing a low-silicone oil. However, the modified copolymer system described in this application is not suitable for producing high-performance carbon fibers.
[0014] In the prior art, in the wet spinning preparation of high-performance carbon fibers, reducing the ash content of the carbon fibers often leads to reduced carbon fiber performance.
[0015] Summary of the Invention
[0016] The present inventors have found through in-depth research that a large amount of penetration and distribution of oil in the fiber is the main reason for the high ash content in the subsequent pre-oxidation and carbonization processes, and it will also lead to a high impurity content in the final carbon fiber, affecting the performance of the carbon fiber. On the other hand, if the Si content of the raw silk cortex is too low, problems such as paralleling, adhesion and hairiness will easily occur during the pre-oxidation process, and the performance of the carbon fiber will eventually be reduced. The present inventors have further found that controlling the penetration depth and gradient of silicon in the carbon fiber can well balance the high performance and low ash content of the carbon fiber, thereby obtaining a carbon fiber with low ash content and high performance, thereby completing the present invention.
[0017] One of the technical problems addressed by the present invention is the problem that reducing the ash content of carbon fibers in prior wet spinning methods results in lower mechanical properties of the resulting carbon fibers. The present invention therefore provides a low-ash, high-performance polyacrylonitrile carbon fiber in which silicon has a specific surface silicon permeation gradient and silicon content, thereby improving the mechanical properties of the carbon fibers while reducing their ash content.
[0018] The second technical problem addressed by the present invention is to provide a method for preparing low-ash, high-performance carbon fibers, corresponding to one of the aforementioned technical problems. This method features low ash content during the carbonization process (requiring only shutdowns for ash cleaning every six months or longer), and produces carbon fibers with low silicon impurities and excellent strength, modulus, and elongation.
[0019] The third technical problem solved by the present invention is to provide a polyacrylonitrile precursor for preparing the low-ash high-performance carbon fiber corresponding to solving one of the above technical problems.
[0020] The fourth technical problem solved by the present invention is to provide a method for preparing polyacrylonitrile precursor corresponding to the solution to the third technical problem mentioned above.
[0021] The present invention provides a polyacrylonitrile carbon fiber having a groove structure on its surface, characterized in that the Si / C ratio of the carbon fiber in an area X between the top of the protrusion on the fiber surface and the bottom of the groove is in the range of 1% to 10%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100 nm is in the range of 0.1% to 1%, and the Si / C ratio of the area Z greater than 100 nm is not higher than 0.06%.
[0022] The present invention also provides a method for manufacturing polyacrylonitrile carbon fiber, preferably the polyacrylonitrile carbon fiber according to the present invention, which includes the step of carbonizing polyacrylonitrile precursor to obtain the polyacrylonitrile carbon fiber; characterized in that the Si / C ratio of the polyacrylonitrile precursor from the top of the fiber surface protrusion to the inner 2μm area is in the range of 1.0% to 20%, and the Si / C ratio of the area greater than 2μm is not higher than 0.15%.
[0023] The present invention provides a polyacrylonitrile precursor, characterized in that the Si / C ratio of the polyacrylonitrile precursor from the top of the fiber surface protrusion to the inner 2μm area is in the range of 1.0% to 20%, and the Si / C ratio of the area larger than 2μm is not higher than 0.15%.
[0024] The present invention also provides a method for preparing polyacrylonitrile precursor, preferably the polyacrylonitrile precursor according to the present invention, which includes wet spinning and an oiling step, wherein the oiling step includes two consecutive oiling processes, and there is no drying and densification stage between the two oiling processes, wherein the first oiling process uses a silicone-free oil agent, a low-silicone oil agent or a combination thereof and the second oiling process uses a silicone-containing oil agent. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solution of the present invention, accompanying drawings are provided.
[0026] FIG1 is a schematic diagram of a cross-section of a single carbon fiber of the present invention.
[0027] In Figure 1, 1 is the convex structure on the surface of the carbon fiber; 2 is the groove structure on the surface of the carbon fiber; a and b are the scanning lines of the adjacent convex structure and groove structure from the center of the fiber to the surface of the fiber, respectively; X represents the area from the top of the convexity on the surface of the carbon fiber to the bottom of the groove; Y represents the area from the bottom of the groove to 100 nm inside the carbon fiber (i.e., the depth of this area is 100 nm); and Z represents the area greater than 100 nm inside the carbon fiber.
[0028] In the present invention, the top of a protrusion refers to the highest point of the protrusion structure; the bottom of a groove refers to the lowest point of the groove structure. DETAILED DESCRIPTION
[0029] In one aspect, the present invention provides a polyacrylonitrile carbon fiber having a groove structure on its surface, wherein the Si / C ratio of the carbon fiber in a region X between the top of the protrusion on the fiber surface and the bottom of the groove is in the range of 1% to 10%, the Si / C ratio of the region Y between the bottom of the groove and the inner 100 nm is in the range of 0.1% to 1%, and the Si / C ratio of the region Z greater than 100 nm (from the bottom of the groove on the surface) is not higher than 0.06%.
[0030] In the present invention, the Si / C ratio of the carbon fiber in the region X between the top of the protrusion on the fiber surface and the bottom of the groove is in the range of 1% to 10%. For example, the Si / C ratio can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 9.5%, 10%, or a range consisting of any two of the above values. In some embodiments, the Si / C ratio can be in the range of 2% to 10%, in the range of 3% to 10%, in the range of 4% to 10%, or in the range of 4% to 9.5%.
[0031] In the present invention, the Si / C ratio of the carbon fiber in the region Y between the bottom of the groove and the inner 100 nm is in the range of 0.1% to 1%. For example, the Si / C ratio can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 0.95%, 1.0%, or a range consisting of any two of the above values. In some embodiments, the Si / C ratio can be in the range of 0.2% to 1%, in the range of 0.3% to 1%, in the range of 0.4% to 1%, or in the range of 0.4% to 0.95%.
[0032] In the present invention, the Si / C ratio of the carbon fibers in a region Z greater than 100 nm (from the bottom of the surface grooves) is not higher than 0.06%. For example, the Si / C ratio may be 0%, 0.005%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, or a range consisting of any two of the aforementioned values, such as 0% to 0.06%. In some embodiments, the Si / C ratio may be in the range of 0.005% to 0.06%, or in the range of 0.01% to 0.06%.
[0033] In the present invention, the Si / C ratio is the ratio of the number of Si atoms to the number of C atoms. In the present invention, the Si / C ratio is determined by TEM-EDS; see below for details.
[0034] In the present invention, the total silicon content in the carbon fiber may be 500 to 1500 ppm by weight. For example, by weight, the total silicon content in the carbon fiber may be 500 ppm, 600 ppm, 700 ppm, 800 ppm, 900 ppm, 1000 ppm, 1100 ppm, 1200 ppm, 1300 ppm, 1400 ppm, 1500 ppm, or a range consisting of any two of the foregoing values.
[0035] In some embodiments of the present invention, in the carbon fiber, the Si / C ratio of region X between the top of the protrusion on the fiber surface and the bottom of the groove is not less than 8.5 times the Si / C ratio of region Y between the bottom of the groove and the inner 100 nm. In some embodiments of the present invention, in the carbon fiber, the Si / C ratio of region X between the top of the protrusion on the fiber surface and the bottom of the groove is 8.5 to 12 times the Si / C ratio of region Y between the bottom of the groove and the inner 100 nm.
[0036] In some embodiments of the present invention, the carbon fibers of the present invention have fewer than 20 pores, preferably fewer than 16, within regions X and Y extending from the top of the protrusions on the fiber surface to within 100 nm of the fiber surface; wherein the average length of the pores is 10 to 50 nm and the average width is 5 to 25 nm. In the present invention, the number of pores, average length of the pores, and average width of the pores are average values of 10 carbon fibers observed by gallium focused ion beam sectioning and transmission electron microscopy.
[0037] In some embodiments of the present invention, the orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is less than or equal to 4°, preferably less than or equal to 3°.
[0038] The carbon fibers may have a tensile strength of 5.6-5.8 GPa, a tensile modulus of 360-390 GPa, and an elongation at break of 1.45%-1.6%.
[0039] In the present invention, the polyacrylonitrile carbon fiber is prepared from polyacrylonitrile precursor obtained by wet spinning.
[0040] In another aspect, the present invention provides a method for manufacturing the polyacrylonitrile carbon fiber of the present invention, which includes the step of carbonizing a polyacrylonitrile precursor to obtain the polyacrylonitrile carbon fiber; wherein the Si / C ratio of the polyacrylonitrile precursor from the top of the protrusion on the fiber surface to the inner 2μm area is in the range of 1.0% to 20%, and the Si / C ratio of the area greater than 2μm is not higher than 0.15%.
[0041] In some embodiments, the Si / C ratio of the polyacrylonitrile precursor from the top of the protrusion on the fiber surface to the inner 2 μm region may be in the range of 2.0% to 20%, in the range of 3.0% to 20%, in the range of 4.0% to 20%, or in the range of 5.0% to 19%. In some embodiments, the Si / C ratio of the polyacrylonitrile precursor from the top of the protrusion on the fiber surface to the inner region greater than 2 μm may be in the range of 0.01% to 0.15%, in the range of 0.02% to 0.15%, in the range of 0.03% to 0.15%, in the range of 0.04% to 0.15%, or in the range of 0.05% to 0.15%.
[0042] In some embodiments, the oil content of the precursor can be 0.5% to 2.5%, preferably 0.8% to 2.5%, preferably 0.8% to 2.4%, and more preferably 0.9% to 2.0%. For example, the oil content of the precursor can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, or a range consisting of any two of the above values.
[0043] In some embodiments, the silicon content of the precursor can be 0.01% to 0.5%, preferably 0.05% to 0.5%. For example, the silicon content of the precursor can be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, or a range consisting of any two of the above values. In some embodiments, the single yarn linear density of the polyacrylonitrile precursor is 0.7 to 1.0 dtex. For example, the single yarn linear density of the polyacrylonitrile precursor can be 0.7 dtex, 0.8 dtex, 0.9 dtex, 1.0 dtex, or a range consisting of any two of the above values.
[0044] In the present invention, the polyacrylonitrile precursor is prepared by wet spinning.
[0045] In the present invention, the polyacrylonitrile precursor is prepared by wet spinning and includes an oiling step, wherein the oiling step includes two consecutive oiling processes, wherein there is no drying and densification stage between the two oiling processes, wherein the first oiling process uses a silicone-free oil agent, a low-silicone oil agent or a combination thereof, and the second oiling process uses a silicone-containing oil agent.
[0046] In the present invention, the absence of a drying and densification stage between the two oiling processes means that after the first oiling process is completed, the fibers treated by the first oiling process are not subjected to drying and densification treatment, but continue to undergo the second oiling process.
[0047] In the preparation process of polycarbon fiber precursor, it is known in the art to apply oil to the fiber through an oiling step. As known in the art, the oil used in the oiling step can include silicone-free oil, low silicone oil and silicone-containing oil.
[0048] The present invention has no particular limitation on the silicone-free oil agent, and various silicone-free oil agents commonly used in the preparation of polyacrylonitrile precursor in the art can be used.
[0049] In some embodiments, the silicone-free oil comprises a non-silicone component as the primary component of the oil. For example, one or more of the following substances can be used as the primary component of the silicone-free oil: polyesters of long-chain fatty acids and polyols, ethylene oxide adducts of long-chain fatty amides, polybutene, polyoxyethylene ether, neopentyl alcohol derivatives, fatty acid esters, amide compounds, ammonium salts of fatty acid esters, aromatic esters, and amide compounds.
[0050] The present invention does not particularly limit the silicone-containing oil, and various silicone-containing oils used in the preparation of polyacrylonitrile precursors in the art can be used. In some embodiments, the silicone-containing oil contains an organopolysiloxane and / or its derivatives. Examples include polydimethylsiloxane, polyphenylmethylsiloxane, polymethylhydrogensiloxane, alkyl-aralkyl-modified polysiloxane, amino-modified polysiloxane, polyether-modified polysiloxane, epoxy-modified polysiloxane, and amide-modified polysiloxane.
[0051] The present invention has no particular limitation on the low-silicone oil agent, and various low-silicone oil agents used for preparing polyacrylonitrile precursor in the art can be used.
[0052] In the present invention, the silicon content of the silicone-containing oil can be 0.01% to 0.9% by weight, while the silicon content of the low-silicone oil can be 0.001% to less than 0.01% by weight. In some embodiments, the silicon-containing component of the low-silicone oil accounts for less than or equal to 1% by weight of the total oil components.
[0053] In the present invention, there is no particular limitation on the form of the oil. In the present invention, the oil used is preferably an oil-in-water emulsion.
[0054] In some embodiments, the silicone-free oil agent can be an oil-in-water emulsion comprising an oil component and water, wherein the mass percentage of the oil component is 1% to 40%; the oil component comprises one or more of aromatic ester compounds, aromatic polyoxyethylene ethers, amine compounds, alcohol compounds, and acid compounds, as well as non-ionic surfactants, emulsifiers, antioxidants, and antistatic agents; wherein, based on the mass sum of the oil components being 100%, the content of the aromatic ester compounds is 40% to 90%, the content of the aromatic polyoxyethylene ether is 10% to 30%, the content of the amine compounds is 0% to 7%, the content of the alcohol compounds is 0% to 7%, the content of the acid compounds is 0% to 7%, the content of the non-ionic surfactant is 10% to 65%, the content of the emulsifier is 10% to 30%, the content of the antioxidant is 1% to 10%, and the content of the antistatic agent is 1% to 10%.
[0055] In some embodiments, the silicone-containing oil agent can be an oil-in-water emulsion comprising an oil component and water, wherein the mass percentage of the oil component is 1% to 40%; the oil component comprises dimethylsiloxane, modified silicone, a nonionic surfactant, an emulsifier, an antioxidant, and an antistatic agent; wherein, based on the mass sum of the oil components being 100%, the content of the dimethylsiloxane is 10% to 50%, the content of the modified silicone is 10% to 75%, the content of the nonionic surfactant is 10% to 65%, the content of the emulsifier is 10% to 30%, the content of the antioxidant is 1% to 10%, and the content of the antistatic agent is 1% to 10%.
[0056] In some embodiments, the low-silicone oil agent is an oil-in-water emulsion comprising an oil component and water, and the mass percentage of the oil component is 1% to 40%; the oil component comprises a heat-resistant ester compound, a modified silicone, a nonionic surfactant, an emulsifier, an antioxidant, and an antistatic agent; wherein, based on the mass sum of the oil components being 100%, the content of the heat-resistant ester compound is 10% to 70%, the content of the modified silicone is 0.1% to 1%, the content of the nonionic surfactant is 10% to 65%, the content of the emulsifier is 10% to 30%, the content of the antioxidant is 1% to 10%, and the content of the antistatic agent is 1% to 10%.
[0057] In the present invention, the oil component includes all substances in the oil except water.
[0058] There are no particular limitations on the concentration of the oil in the present invention. In the present invention, the first oiling process uses a silicone-free oil, a low-silicone oil, or a combination thereof, and the weight concentration thereof may be 0.1% to 5.0%. For example, the weight concentration of the silicone-free oil, low-silicone oil, or a combination thereof used in the first oiling process may be 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, or a range consisting of any two of the aforementioned values. In the present invention, the second oiling process uses a silicone-containing oil, and the weight concentration thereof may be 0.1% to 5.0%. For example, the weight concentration of the silicone-containing oil used in the second oiling process may be 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, or a range consisting of any two of the aforementioned values. In the present invention, the weight concentration of the oil refers to the ratio of the weight of all oil components in the oil to the weight of the oil.
[0059] In some embodiments, preferably, the average particle size of the silicone-free oil agent, the low-silicone oil agent, and the silicone-containing oil agent can each independently be 50 nm to 500 nm. For example, the average particle size of the silicone-free oil agent, the low-silicone oil agent, and the silicone-containing oil agent can be 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, or a range consisting of any two of the above values, such as 100 nm to 400 nm, etc.
[0060] In the present invention, the silicon content of the silicone oil used in the second oiling process can be 0.01% to 0.9% by weight. For example, the silicon content of the silicone oil can be 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or a range consisting of any two of the above values.
[0061] In the present invention, there is no particular limitation on the method of applying the oil to the fiber, and various methods generally known in the art can be used, such as dipping, roll dipping, spraying, and the like.
[0062] In the present invention, the pH values of the silicone-free, low-silicone, and silicone-containing agents are not particularly limited, and those skilled in the art can appropriately determine and select the pH values of the silicone-free, low-silicone, and silicone-containing agents. In some embodiments, the pH difference between the silicone-free or low-silicone agent and the silicone-containing agent may be no greater than 1. In some embodiments, the pH difference between the silicone-free or low-silicone agent and the silicone-containing agent may be greater than or equal to 0 and less than or equal to 1.
[0063] In the present invention, in some embodiments, the silicone-free oil agent, low-silicone oil agent and silicone-containing oil agent each contain a surfactant, wherein the polarity of the surfactant in the silicone-free oil agent or low-silicone oil agent is not opposite to that of the surfactant in the silicone-containing oil agent. In the present invention, the surfactants that can be used in the oil agent include cationic surfactants, anionic surfactants, amphoteric surfactants and nonionic surfactants. In the present invention, opposite polarity means that the surfactant in the silicone-free oil agent or low-silicone oil agent contains a cationic surfactant and the surfactant in the silicone-containing oil agent contains an anionic surfactant, or the surfactant in the silicone-free oil agent or low-silicone oil agent contains an anionic surfactant and the surfactant in the silicone-containing oil agent contains a cationic surfactant; any case other than the above two cases is considered to be a case of non-opposite polarity. Various surfactants known in the art can be used as long as the above requirements for polarity are met. In some embodiments, the silicone-containing oil agent preferably contains a nonionic surfactant.
[0064] In the present invention, there is no particular limitation on the temperature of the oil during oiling, and the oil temperature commonly used in the art can be used. In some embodiments, the temperature of the oil during oiling can be 20-30°C.
[0065] In the present invention, there is no particular limitation on the time required for oiling, and the time commonly used in the art can be used. In some embodiments, the time for the first oiling pass, such as the residence time in the oiling tank, can be 0.05 to 0.5 seconds, preferably 0.06 to 0.4 seconds, and more preferably 0.07 to 0.3 seconds. In some embodiments, the time for the second oiling pass, such as the residence time in the oiling tank, can be 0.03 to 0.3 seconds, preferably 0.04 to 0.3 seconds, and more preferably 0.04 to 0.2 seconds.
[0066] In some embodiments, the residence time of the second oiling pass is less than the residence time of the first oiling pass.
[0067] As is known in the art, a drying and densification process is performed after oiling. In the present invention, there is no particular limitation on the drying and densification process, and any drying and densification process known in the art can be used. In some embodiments, the drying and densification process can include multiple stages of drying and densification. In some embodiments, the drying and densification process can include four stages of drying and densification, with temperatures of 90° C., 100° C., 115° C., and 130° C., respectively.
[0068] In some embodiments, the swelling degree of the polyacrylonitrile precursor fibers after washing before oiling can be 80% to 150%. For example, the swelling degree of the polyacrylonitrile precursor fibers after washing before oiling can be 80%, 90%, 100%, 110%, 120%, 130%, 140%, or a range consisting of any two of the above values, for example, the swelling degree can be 90% to 140%.
[0069] In some embodiments, the manufacturing method may include the steps of wet coagulation molding of polyacrylonitrile stock solution, coagulation drawing, hot water drawing, water washing, oiling, drying and densification, steam drawing, and steam heat setting to obtain the polyacrylonitrile precursor.
[0070] The preparation of precursor from polyacrylonitrile solution is generally known in the art. In the present invention, the preparation of the precursor adopts a wet spinning process, which is known in the art.
[0071] For preparing polyacrylonitrile precursor from polyacrylonitrile stock solution, the preparation process may include coagulation molding, coagulation drawing, drawing such as hot water drawing, washing such as water washing, oiling, drying and densification, drawing such as steam drawing, and heat setting such as steam heat setting. These steps are known in the art, and those skilled in the art can appropriately select and implement these steps. As described above, in the method of the present invention, the oiling step includes two consecutive oiling processes, wherein there is no drying and densification stage between the two oiling processes; wherein the first oiling process uses a silicone-free oil agent, a low-silicone oil agent, or a combination thereof, and the second oiling process uses a silicone-containing oil agent.
[0072] In some embodiments, in the method of the present invention, for the coagulation and forming step, after the spun fibers leave the spinneret, they enter the first coagulation bath to coagulate the spun fibers. Those skilled in the art can easily select the composition and temperature of the first coagulation bath. In some embodiments, the temperature of the first coagulation bath is 28°C and the first coagulation bath is a 51.5% dimethyl sulfoxide aqueous solution. After leaving the first coagulation bath, the filaments can further pass through one or more subsequent coagulation baths for further coagulation and drawing. In some embodiments, after leaving the first coagulation bath, the filaments are further subjected to three-stage coagulation and drawing, with concentrations of 30%, 20%, and 10%, respectively, temperatures of 30°C, 40°C, and 50°C, respectively, and draw ratios of 1.0, 1.1, and 1.2, respectively. In some embodiments, after leaving the last coagulation bath, the coagulated filaments can be drawn. The drawing is performed, for example, in steam or hot water. Those skilled in the art can appropriately select the draw ratio. In some embodiments, four-stage hot water drawing can be implemented, with temperatures of 95°C, 96°C, 97°C and 99°C and draw ratios of 1.35, 1.50, 1.70 and 2.00, respectively. After drawing, the filaments can be washed, for example, with water, to remove residual solvent. In some embodiments, a six-step water washing process can be used, with temperatures of 70°C, 70°C, 80°C, 80°C, 90°C and 90°C, respectively. The swelling degree of the fiber after washing can be 80% to 140%. In the method of the present invention, after washing, the filaments can be oiled and dried and densified. In the present invention, as described above, the oiling includes two consecutive oiling processes, wherein there is no drying and densification stage between the two oiling processes; wherein the first oiling process uses a silicone-free oil agent, a low-silicone oil agent or a combination thereof, and the second oiling process uses a silicone-containing oil agent. Oiling can be performed using an oiling agent commonly used in the art and drying and densification can be performed using a drying and densification operation commonly used in the art. In some embodiments, the drying and densification treatment includes four stages of drying and densification treatment at temperatures of 90°C, 100°C, 115°C, and 130°C, respectively. In some embodiments, after drying and densification, the obtained filaments can be further stretched, such as steam stretched. Those skilled in the art can appropriately select the stretching ratio and stretching conditions. In some embodiments, steam stretching is used, wherein the stretching ratio is 3.0 times and the steam pressure is 0.35MPa. In some embodiments, after stretching, the obtained filaments can be heat-set. For example, heat setting can be performed by passing the filaments through multiple stages of hot rollers, or steam heat setting can be used. After heat setting, the raw silk is obtained and can be wound up for subsequent use.
[0073] As known to those skilled in the art, one or more of the above steps may be omitted or added, or the order of the steps may be adjusted.
[0074] In the present invention, the linear density of the polyacrylonitrile precursor is not particularly limited, and those skilled in the art can appropriately select and determine the linear density. In some embodiments, the linear density of the polyacrylonitrile precursor can be 0.7 to 1.0 dtex. For example, the linear density of the polyacrylonitrile precursor can be 0.7 dtex, 0.8 dtex, 0.9 dtex, 1.0 dtex, or a range consisting of any two of the foregoing values.
[0075] After obtaining the precursor, the precursor can be prepared into polyacrylonitrile carbon fibers. The process of preparing polyacrylonitrile carbon fibers from polyacrylonitrile precursor is known in the art. The present invention can use processes known in the art to prepare polyacrylonitrile carbon fibers from the precursor.
[0076] In the present invention, the polyacrylonitrile precursor can be subjected to pre-oxidation treatment and carbonization treatment to obtain the polyacrylonitrile carbon fiber.
[0077] In some embodiments, the pre-oxidation treatment is performed in an air atmosphere at a temperature of 170 to 300° C. and a total draft of no more than 5%.
[0078] In some embodiments, the pre-oxidation treatment can be performed in an air atmosphere using a gradient temperature ramp method in multiple temperature zones, for example, 2 to 6 zones. The starting temperature for the pre-oxidation treatment can be 170°C to 200°C, and the ending temperature can be 260°C to 300°C. During the pre-oxidation treatment, a certain draft can be applied to the fiber, for example, the draft rate can be 0-5%. The pre-oxidation treatment time can be 30 to 120 minutes.
[0079] In some embodiments, the carbonization treatment includes a low-temperature carbonization treatment at a temperature of 300-750° C. in an inert atmosphere with a total draw ratio of 0-4%, and a high-temperature carbonization treatment at a temperature of 800-1500° C. in an inert atmosphere with a total draw ratio of -4--2%. The inert atmosphere can be achieved, for example, by using nitrogen, helium, argon, or xenon.
[0080] After the carbonization treatment, optionally, a graphitization treatment may be performed. In the present invention, the graphitization treatment is not particularly limited, and graphitization treatments known in the art may be used. In some embodiments, the graphitization treatment may be performed at 2800°C.
[0081] In some embodiments, the preparation method may further include a surface treatment step, a water washing step, and a sizing step.
[0082] As known to those skilled in the art, the carbon fibers of the present invention may be surface treated before sizing, for example, by oxidation to improve the affinity and adhesion between the carbon fibers and the matrix resin in the composite material.
[0083] The sizing treatment can be carried out using various sizing methods known in the art. The present invention does not particularly limit the sizing method, sizing agent, or sizing conditions, as long as the desired sizing agent can be imparted to the carbon fibers. After the sizing treatment, a drying process can be performed to remove the solvent or dispersion medium used in the sizing process. For example, drying can be performed at 120°C. Finally, the fibers can be collected to obtain the carbon fibers.
[0084] In another aspect, the present invention provides a polyacrylonitrile precursor, wherein the Si / C ratio of the polyacrylonitrile precursor from the top of the protrusion on the fiber surface to the inner 2μm area is in the range of 1.0% to 20%, and the Si / C ratio of the area larger than 2μm is not higher than 0.15%.
[0085] In some embodiments, the Si / C ratio of the polyacrylonitrile precursor from the top of the fiber surface protrusion to the inner 2 μm area can be in the range of 2.0% to 20%, in the range of 3.0% to 20%, in the range of 4.0% to 20%, or in the range of 5.0% to 19%. In some embodiments, the Si / C ratio of the polyacrylonitrile precursor from the top of the fiber surface protrusion to the inner area greater than 2 μm can be in the range of 0.01% to 0.15%, in the range of 0.02% to 0.15%, in the range of 0.03% to 0.15%, in the range of 0.04% to 0.15%, or in the range of 0.05% to 0.15%.
[0086] In some embodiments, the oil content of the precursor can be 0.5% to 2.5%, preferably 0.8% to 2.5%, preferably 0.8% to 2.4%, and more preferably 0.9% to 2.0%. For example, the oil content of the precursor can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, or a range consisting of any two of the above values.
[0087] In some embodiments, the silicon content of the precursor can be 0.01% to 0.5%, preferably 0.05% to 0.5%. For example, the silicon content of the precursor can be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, or a range consisting of any two of the above values.
[0088] In some embodiments, the linear density of the polyacrylonitrile precursor is 0.7 to 1.0 dtex. For example, the linear density of the polyacrylonitrile precursor can be 0.7 dtex, 0.8 dtex, 0.9 dtex, 1.0 dtex, or a range consisting of any two of the above values.
[0089] In the present invention, the polyacrylonitrile precursor is prepared by wet spinning.
[0090] In one aspect, the present invention provides a method for preparing polyacrylonitrile precursor of the present invention, comprising wet spinning and two consecutive oiling steps, with no drying and densification stage between the two oiling steps, wherein the first oiling step uses a silicone-free oil, a low-silicone oil, or a combination thereof, and the second oiling step uses a silicone-containing oil. In the present invention, "no drying and densification stage between the two oiling steps" means that after the first oiling step is completed, the precursor treated with the first oiling step is not subjected to drying and densification, but is instead subjected to the second oiling step.
[0091] The various aspects and features of the method for preparing the polyacrylonitrile precursor of the present invention are the same as the various aspects and features related to the preparation of the precursor in the above section on the method for producing polyacrylonitrile carbon fibers, and therefore will not be repeated here.
[0092] In the present invention, the polyacrylonitrile precursor is prepared from a polyacrylonitrile stock solution. In the present invention, the polyacrylonitrile stock solution comprises a polyacrylonitrile polymer and a solvent. There is no particular limitation on the concentration of the polyacrylonitrile polymer in the polyacrylonitrile stock solution, and any suitable concentration commonly known in the art for polyacrylonitrile spinning stock solutions can be used. In the present invention, for example, the concentration of the polyacrylonitrile polymer in the polyacrylonitrile spinning stock solution can be 15 to 30% by weight. In the present invention, various solvents for polyacrylonitrile stock solutions can be used. For example, the solvent can be at least one of dimethyl sulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMAC), and mixtures thereof.
[0093] In the present invention, the polyacrylonitrile stock solution can be obtained by dissolving a polyacrylonitrile polymer in a solvent, or by polymerizing monomers in a solvent.
[0094] The polyacrylonitrile precursor of the present invention or the polyacrylonitrile precursor prepared by the precursor preparation method of the present invention can be used to prepare the low-ash high-performance polyacrylonitrile carbon fiber of the present invention.
[0095] In the present invention, except for the limitations on oiling and densification given above in this application, there are no special limitations on other aspects of the preparation of the polyacrylonitrile-based precursor. It can be prepared using a polyacrylonitrile spinning solution commonly used or known in the art through a spinning process commonly used or known in the art, and there are no special requirements for the polyacrylonitrile spinning solution and the spinning process. In the present invention, except for the limitations on oiling and densification given above in this application, the precursor can be prepared from the polyacrylonitrile spinning solution using commonly known methods and process parameters. Compared with the prior art for preparing polyacrylonitrile carbon fibers, the present invention can achieve the purpose of improving the mechanical properties of the fiber and reducing the ash content.
[0096] In the present invention, the polyacrylonitrile polymer in the polyacrylonitrile stock solution may comprise a polyacrylonitrile homopolymer, a polyacrylonitrile copolymer or a mixture thereof. In the present invention, various polyacrylonitrile homopolymers, polyacrylonitrile copolymers or mixtures thereof used to prepare carbon fibers may be used. For example, when a polyacrylonitrile copolymer is used, the comonomer may be a vinyl-containing monomer. In some embodiments, the comonomer is preferably one or more of acrylates, vinyl esters, acrylamides, sulfonates, and ammonium salts. In some embodiments, the polyacrylonitrile polymer may contain 90 to 100% by mass of monomer units derived from acrylonitrile and 0 to 10% by mass of structural units derived from monomers copolymerizable with acrylonitrile. Various comonomers commonly known in the art may be used as monomers copolymerizable with acrylonitrile, including, for example, acrylic acid, methacrylic acid, itaconic acid and their alkali metal salts, ammonium salts and lower alkyl esters; acrylamide and its derivatives; allyl sulfonic acid, methallyl sulfonic acid and their salts or alkyl esters; and the like.
[0097] The inventors unexpectedly discovered that by controlling the silicon penetration gradient and silicon content on the fiber surface, the ash content of carbon fibers can be reduced and the mechanical properties of carbon fibers can be improved. In the present invention, the problems existing in the prior art can be solved by controlling the Si / C ratio of the carbon fibers in the region X between the top of the protrusion and the bottom of the groove on the fiber surface to be within the range of 1% to 10%, the Si / C ratio of the region Y between the bottom of the groove and the inner 100nm to be within the range of 0.1% to 1%, and the Si / C ratio of the region Z greater than 100nm to be no higher than 0.06%.
[0098] On the other hand, the method of the present invention includes two consecutive oiling steps, wherein there is no drying and densification stage between the two oiling steps, wherein the first oiling step uses a silicone-free oil, a low-silicone oil, or a combination thereof, and the second oiling step uses a silicone-containing oil. This can achieve control of the silicon penetration gradient and silicon content on the fiber surface, thereby producing carbon fiber precursor and carbon fiber with low silicon content and a good silicon penetration gradient. The present invention can achieve a long operating cycle and can produce carbon fiber with extremely low ash content and excellent properties such as strength and modulus.
[0099] In the present invention, the swelling degree is measured by the following method:
[0100] Take about 10g of wet washed fiber and wash it in flowing deionized water for 30 minutes. Place the fiber evenly in a 50ml centrifuge tube, and then place the centrifuge tube in a centrifugal dehydrator (3000r / min, 15min) for dehydration to remove the water attached to the fiber surface and the water trapped between the fibers. After centrifugation, the dehydrated fiber is obtained and its mass is weighed and calculated as W. The dehydrated fiber is then dried in a hot air drying oven at 110℃ for 2h, then placed in a desiccator to cool to room temperature, and then its mass is weighed and calculated as W0. Swelling degree (wt%) = (W-W0) / W0×100%.
[0101] In the present invention, the silicon content of the precursor and carbon fiber is determined by the following method:
[0102] 5 g of sample was placed in a quartz crucible, which was placed in a muffle furnace and heated to 400 ° C for 2 hours, and then heated to 960 ° C for 3 hours; the ash in the crucible was transferred to a polytetrafluoroethylene test tube, and hydrochloric acid, nitric acid and hydrofluoric acid with concentrations of 37%, 68% and 50% were added, with volumes of 3 ml, 1 ml and 1 ml respectively, and heated at 120 ° C for 5 hours. After that, ICP-OES inductively coupled plasma emission spectrometry was used for quantitative determination to determine the Si content in the sample.
[0103] In the present invention, the silicon content in the oil is determined by the following method:
[0104] 0.5 g of oil was added to a quartz crucible, which was placed in a muffle furnace and heated to 90°C for 2 h, then heated to 150°C for 0.5 h, continued to heat to 300°C for 0.5 h, and finally heated to 400°C for 2 h; the ash in the crucible was transferred to a polytetrafluoroethylene test tube, and hydrochloric acid, nitric acid, and hydrofluoric acid with concentrations of 37%, 68%, and 50%, respectively, were added in volumes of 3 ml, 1 ml, and 1 ml, respectively, and heated at 120°C for 5 h. The sample was then diluted to 100 times with water and quantitatively determined using ICP-OES inductively coupled plasma emission spectrometry to determine the Si content in the sample.
[0105] In the present invention, linear density is measured in the following manner:
[0106] Use a hand-cranked yarn linear density tester to wind the raw silk with a K number of N straightly onto a hand-cranked roller with a circumference of 1 meter. Wrap it 10 times and weigh the fiber weight (in g) as W. The linear density (dtex) = W / N. Measure 10 times and take the average value.
[0107] In the present invention, the mechanical properties of the carbon fiber precursor including tensile strength, initial modulus and elongation at break are measured according to GB / T 14337-2008; the mechanical properties of the carbon fiber including tensile strength, tensile modulus and elongation at break are measured according to GB / T 3362-2017.
[0108] In the present invention, the particle size of the oil (emulsion) is measured by laser particle size analysis, using a laser particle size analyzer, Mastersizer 2000 (Malvern, UK).
[0109] In the present invention, the Si / C ratio and the number and size of pores in the fiber are determined by:
[0110] The fiber was cut into 100nm thick slices using a low-temperature FIB (gallium ion focused ion beam) microscope. Transmission electron microscopy (TEM) was used to observe the colorless, transparent pores in regions X and Y extending from the top of a protrusion on the fiber surface to within 100nm of the fiber. The length was defined as the longer side, and the width as the shorter side. Using a TEM-EDS module, 50 scan lines were taken circumferentially from the fiber center to the outer surface. Of these, 25 lines were taken from the fiber center to the top of an adjacent protrusion and the bottom of a groove on the fiber surface, with each scan taken every 20nm. The Si / C atomic ratio at various depths from the fiber center to the surface was determined. The average Si / C atomic ratio of the region X between the top of the fiber surface protrusion and the bottom of the groove was calculated using data from the X region of the scan line from the fiber center to the top of the fiber surface protrusion (as shown by the scan line a in Figure 1). The average Si / C atomic ratio of the region Y between the bottom of the groove and the inner 100 nm and the region Z greater than 100 nm were calculated using data from the Y and Z regions from the fiber center to the bottom of the fiber surface groove (as shown by the scan line b in Figure 1). A total of 10 carbon fibers were measured. The Si / C ratio, number of pores, average pore length, and average width in the present invention are average values obtained from 10 carbon fibers.
[0111] In the present invention, the oil content of the raw silk is measured by the following method:
[0112] Take a 3g sample of raw silk and dry it at 105°C in air for 2 hours. The mass is then measured and recorded as W1. The sample is then placed in a Soxhlet extractor, cyclohexane is added, and the temperature is raised to 100°C for extraction for 4 hours. Remove the sample and dry it at 105°C in air for 2 hours. The mass is then measured and recorded as W2. Oil content (wt%) = (W1-W2) / W1 × 100%.
[0113] In the present invention, the orientation deviation angle of the pores in the carbon fiber along the fiber axis is measured according to the following document [1] by the following method:
[0114] Take a carbon fiber bundle and use tape to fix the carbon fiber bundle on a metal frame with a size of 4cm×3cm×0.2cm and a central opening size of 3cm×2cm. Spread it evenly into the same width and measure the sample by the small-angle X-ray scattering (SAXS) device of the Shanghai Light Source (SSRF, BL16B) beam station. The distance from the sample to the detector is calibrated with a standard tendon, which is 1980mm; an incident X-ray with a wavelength of 0.12398nm is used. SAXS data are collected using a Mar CCD 165 imaging plate. The obtained data are processed using xPolar (Precision works NY, Inc., USA) software, and the average length of the micropores along the fiber axis (L f ) and orientation deviation angle Calculated according to the Cauchy-Cauchy formula:
[0115] Where s (s = 2sinθ / λ) is the scattering vector corresponding to the azimuth scanning curve, B obs is the angular width of the half-height width of the azimuth scanning curve. The azimuth scanning curve is obtained by processing the SAXS image, in which the air scattering is reasonably deducted, scanning along the tangent parallel to the meridian direction is performed, and then the azimuth scanning curve is obtained by integration. The data is fitted using Gaussian distribution, and then the Perform linear fitting on the scattering vector s corresponding to each azimuth angle, and then calculate L based on the intercept and slope data after linear fitting. f and The value of .
[0116] Literature [1] Andreas F. Thünemann et al. Microvoids in Polyacrylonitrile Fibers: A Small-Angle X-ray Scattering Study [J]. Macromolecules, 2000, 33(5): 1848-1852.
[0117] During the carbon fiber production process, the equipment needs to be stopped for cleaning and maintenance due to the decrease in carbon fiber strength or problems with the equipment. The method of the present invention can continue production for a longer time without stopping the equipment for cleaning and maintenance.
[0118] In the present invention, the precursor has a good silicon infiltration gradient, resulting in significantly less ash during the carbonization process. The resulting carbon fiber has a low silicon content and effectively suppressed silicon penetration depth. Even after six months of continuous production or longer, the prepared carbon fiber can still have a tensile strength greater than or equal to 5.6 GPa, a tensile modulus greater than or equal to 360 GPa, and an elongation at break greater than or equal to 1.5%.
[0119] DETAILED DESCRIPTION
[0120] The present invention will be further described below by way of examples.
[0121] The raw materials and reagents used in the Examples and Comparative Examples can be purchased directly or prepared according to methods disclosed in the prior art. If necessary, the raw materials or reagents can be treated before use using methods known in the art to meet the requirements of the reaction. For example, acrylonitrile can be distilled to remove polymerization inhibitors before use.
[0122] In the test of silicon content in raw silk, carbon fiber and oil, ICP-OES inductively coupled plasma emission spectrometry was performed using Varian 725-ES from Varian, and the samples were dissolved using Digiblock ST36 electrothermal digester from Labtech.
[0123] During the Si / C ratio test, low-temperature FIB (gallium ion focused ion beam) cutting was performed using a ZEISS Crossbeam Laser, and TEM and EDS tests were performed using a FEI Titan Cubed Themis G2 300 and an Aztec X-Max 100TLE Oxford Instruments.
[0124] In the examples and comparative examples, the silicone-free oil agent used is TFA-1208 from Tianjin Gongda Textile Auxiliary Co., Ltd.; the silicone-containing oil agent used is JH88 from Matsumoto Oil. The silicone-free oil agents of different particle sizes in Examples 7, 8 and 12 and Comparative Examples 10 and 11 are the TFA-1208 series synthesized by Tianjin Gongda Textile Auxiliary Co., Ltd., and the silicone-containing oil agents of different particle sizes are the JSYJ series from Sinopec (Shanghai) Petrochemical Research Institute. The anionic silicone-free oil agent in Comparative Example 4 is TFA-1208 and the cationic silicone-containing oil agent is the JLQR oil agent from Jilin Qianren New Materials Co., Ltd. The pH of the oil agent in Example 16 is adjusted by adding an appropriate amount of dilute ammonia water. The pH of the silicone-free oil agent in Comparative Example 3 is adjusted by adding an appropriate amount of dilute ammonia water, and the acidic silicone-containing oil agent is Wacker Chemical (China) Co., Ltd. CF 3295.
[0125] In the embodiments and comparative examples, in the preparation of the spinning solution, the molar ratio of acrylonitrile to itaconic acid is 99:1, the monomer concentration is 20% by weight, and the polymerization is carried out at 60°C in a nitrogen atmosphere for 20 hours, with a conversion rate of 91.5%; then, the spinning solution is obtained through de-monomerization and degassing.
[0126] In the examples and comparative examples, the spinning solution was accurately metered by a metering pump and then filtered using a 10 μm candle wick filter before being extruded through a spinneret.
[0127] [Example 1]
[0128] 1. Preparation of raw yarn: A wet spinning method was adopted. The spinning solution used was prepared by copolymerizing acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity was 2.5 dL / g and the solid content was 18%. The spinning solution is precisely measured and filtered by a metering pump, extruded through a spinneret with 6000 holes and a pore size of 60μm, and enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing with concentrations of 30%, 20%, and 10% respectively, temperatures of 30°C, 40°C, and 50°C respectively, and draw ratios of 1.0, 1.1, and 1.2 respectively; four-stage hot water drawing with temperatures of 95°C, 96°C, 97°C, and 99°C respectively, and draw ratios of 1.35, 1.50, 1.70, and 2.00 respectively; six water washing processes with temperatures of 70°C, 70°C, 80°C, 80°C, 90°C, and 90°C respectively. The swelling degree of the fiber after washing is 110%.
[0129] After washing, the fiber first passes through the first oiling tank, which contains a non-ionic, silicone-free oil with a pH of 7.2, a concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oiling tank, which contains a non-ionic, silicone-containing oil with a pH of 7.8, a concentration of 1.2%, an oil particle size of 300nm, a silicon content of 0.15%, and a residence time of 0.1s.
[0130] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, followed by steam drawing with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, heat setting with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then winding, to obtain polyacrylonitrile carbon fiber precursor.
[0131] The raw yarn has a linear density of 0.85 dtex, an oil content of 1.2%, and a silicon content of 0.15%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 10%, and the Si / C ratio in the region greater than 2μm is 0.11%. The tensile strength, initial modulus, and elongation at break are 7.5 cN / dtex, 125 cN / dtex, and 12.0%, respectively.
[0132] 2. Preparation of carbon fiber: The precursor obtained in step 1 is pre-oxidized in air at 180-260°C, with a total pre-oxidation draw ratio of 0.95 times, to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are performed at 300-750°C and 800-1500°C, with a draw ratio of 0.96 times; then graphitization is performed at 2800°C, and finally, surface treatment, water washing, sizing, drying at 120°C and collecting are performed to obtain carbon fiber.
[0133] The total silicon content in the carbon fiber is 800ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 5.8%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.5%, and the Si / C ratio of the area Z greater than 100nm is 0.04%. The number of pores present in the surface layer of the carbon fiber (areas X and Y from the top of the protrusion on the fiber surface to the inner 100nm) is 10, the average length of the pores is 20nm, and the average width is 15nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 2.3°. The tensile strength of the carbon fiber is 5.74GPa, the tensile modulus is 370GPa, and the elongation at break is 1.52%. After 7 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0134] [Example 2]
[0135] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump. It is extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0136] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 3.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 3%, an oil particle size of 300nm, an oil silicon content of 0.35%, and a residence time of 0.1s.
[0137] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0138] The raw yarn has a linear density of 0.85 dtex, an oil content of 2.2%, and a silicon content of 0.47%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 19%, and the Si / C ratio in the region greater than 2μm is 0.14%. The tensile strength, initial modulus, and elongation at break are 7.2 cN / dtex, 120 cN / dtex, and 12.3%, respectively.
[0139] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0140] The total silicon content in the carbon fiber is 1400ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 9%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.9%, and the Si / C ratio of the area Z greater than 100nm is 0.05%. There are 15 pores in the surface of the carbon fiber, the average length of the pores is 42nm, and the average width is 22nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 3.5°. The tensile strength of the carbon fiber is 5.63GPa, the tensile modulus is 360GPa, and the elongation at break is 1.56%. After 6 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0141] [Example 3]
[0142] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump. It is extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0143] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.1%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 0.8%, an oil particle size of 300nm, an oil silicon content of 0.1%, and a residence time of 0.1s.
[0144] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, followed by steam drawing with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat-set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0145] The raw yarn has a linear density of 0.85 dtex, an oil content of 0.85%, and a silicon content of 0.09%. The Si / C ratio in the region from the top of the protrusion on the fiber surface to the inner 2μm is 6%, and the Si / C ratio in the region greater than 2μm is 0.07%. The tensile strength, initial modulus, and elongation at break are 8.1 cN / dtex, 137 cN / dtex, and 11.8%, respectively.
[0146] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0147] The total silicon content in the carbon fiber is 620ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 4.5%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.47%, and the Si / C ratio of the area Z greater than 100nm is 0.03%. There are 7 pores in the surface of the carbon fiber, the average length of the pores is 15nm, and the average width is 10nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 2.2°. The tensile strength of the carbon fiber is 5.75GPa, the tensile modulus is 374GPa, and the elongation at break is 1.51%. After 8 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0148] [Example 4]
[0149] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump. It is extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0150] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.1%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 1.5%, an oil particle size of 300nm, an oil silicon content of 0.2%, and a residence time of 0.05s.
[0151] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0152] The raw yarn has a linear density of 0.85 dtex, an oil content of 0.9%, and a silicon content of 0.13%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 9%, and the Si / C ratio in the region greater than 2μm is 0.1%. The tensile strength, initial modulus, and elongation at break are 7.8 cN / dtex, 121 cN / dtex, and 11.8%, respectively.
[0153] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0154] The total silicon content in the carbon fiber is 690ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 4.8%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.54%, and the Si / C ratio of the area Z greater than 100nm is 0.04%. There are 8 pores on the surface of the carbon fiber, the average length of the pores is 17nm, and the average width is 13nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 2.2°. The tensile strength of the carbon fiber is 5.75GPa, the tensile modulus is 374GPa, and the elongation at break is 1.55%. After 8 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0155] [Example 5]
[0156] 1. Preparation of the raw yarn: wet spinning method is adopted. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide, with an intrinsic viscosity of 2.5 dL / g and a solid content of 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing with concentrations of 30%, 20%, and 10% respectively, at temperatures of 30°C, 40°C, and 50°C respectively, and with draw ratios of 1.0, 1.1, and 1.2 respectively; four-stage hot water drawing with temperatures of 95°C, 96°C, 97°C, and 99°C respectively, and with draw ratios of 1.35, 1.50, 1.70, and 2.00 respectively; six water washing processes with temperatures of 70°C, At 70℃, 80℃, 80℃, 90℃, and 90℃, the swelling degree of the fiber after washing is 110%.
[0157] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.25s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.13s.
[0158] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0159] The raw yarn has a linear density of 0.85 dtex, an oil content of 1.8%, and a silicon content of 0.39%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 14%, and the Si / C ratio in the region greater than 2μm is 0.12%. The tensile strength, initial modulus, and elongation at break are 7.2 cN / dtex, 127 cN / dtex, and 11.8%, respectively.
[0160] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0161] The total silicon content in the carbon fiber is 1340ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 8%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.85%, and the Si / C ratio of the area Z greater than 100nm is 0.04%. There are 15 pores in the surface of the carbon fiber, the average length of the pores is 35nm, and the average width is 20nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 3.0°. The tensile strength of the carbon fiber is 5.66GPa, the tensile modulus is 361GPa, and the elongation at break is 1.58%. After 6 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0162] [Example 6]
[0163] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0164] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.08s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.05s.
[0165] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0166] The raw yarn has a linear density of 0.85 dtex, an oil content of 0.9%, and a silicon content of 0.08%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 5%, and the Si / C ratio in the region greater than 2μm is 0.05%. The tensile strength, initial modulus, and elongation at break are 7.4 cN / dtex, 126 cN / dtex, and 11.5%, respectively.
[0167] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0168] The total silicon content in the carbon fiber is 560ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 4.3%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.41%, and the Si / C ratio of the area Z greater than 100nm is 0.02%. There are 10 pores in the surface of the carbon fiber, the average length of the pores is 23nm, and the average width is 18nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 2.8°. The tensile strength of the carbon fiber is 5.68GPa, the tensile modulus is 364GPa, and the elongation at break is 1.55%. After 8 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0169] [Example 7]
[0170] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0171] The washed fiber first passes through the first oiling tank, which contains the TFA-1208-10 non-ionic silicone-free oil synthesized by Tianjin Gongda Textile Auxiliary Co., Ltd., with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 100nm, and a residence time of 0.15s. It then passes through the second oiling tank, which contains the JSYJ-20 non-ionic silicone-containing oil synthesized by Sinopec (Shanghai) Petrochemical Research Institute, with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 200nm, an oil silicon content of 0.15%, and a residence time of 0.1s.
[0172] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0173] The raw yarn has a linear density of 0.85 dtex, an oil content of 1.4%, and a silicon content of 0.14%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 9%, and the Si / C ratio in the region greater than 2μm is 0.1%. The tensile strength, initial modulus, and elongation at break are 7.7 cN / dtex, 130 cN / dtex, and 11.5%, respectively.
[0174] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0175] The total silicon content in the carbon fiber is 700ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 5%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.55%, and the Si / C ratio of the area Z greater than 100nm is 0.04%. There are 8 pores in the surface of the carbon fiber, the average length of the pores is 17nm, and the average width is 13nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 2.2°. The tensile strength of the carbon fiber is 5.75GPa, the tensile modulus is 374GPa, and the elongation at break is 1.51%. After 8 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0176] [Example 8]
[0177] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0178] The washed fiber first passes through the first oiling tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oiling tank, which contains the JSYJ-20 non-ionic silicone-containing oil synthesized by Sinopec (Shanghai) Petrochemical Research Institute with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 200nm, an oil silicon content of 0.15%, and a residence time of 0.04s.
[0179] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0180] The raw yarn has a linear density of 0.85 dtex, an oil content of 1.1%, and a silicon content of 0.07%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 5%, and the Si / C ratio in the region greater than 2μm is 0.06%. The tensile strength, initial modulus, and elongation at break are 8.4 cN / dtex, 130 cN / dtex, and 12.0%, respectively.
[0181] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0182] The total silicon content in the carbon fiber is 550ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 4.3%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.4%, and the Si / C ratio of the area Z greater than 100nm is 0.02%. There are 7 pores on the surface of the carbon fiber, the average length of the pores is 15nm, and the average width is 9nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 2.1°. The tensile strength of the carbon fiber is 5.8GPa, the tensile modulus is 390GPa, and the elongation at break is 1.45%. After 8 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0183] [Example 9]
[0184] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0185] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 2%, an oil particle size of 300nm, an oil silicon content of 0.3%, and a residence time of 0.1s.
[0186] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0187] The raw yarn has a linear density of 0.85 dtex, an oil content of 1.3%, and a silicon content of 0.34%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 13%, and the Si / C ratio in the region greater than 2μm is 0.12%. The tensile strength, initial modulus, and elongation at break are 7.5 cN / dtex, 126 cN / dtex, and 11.7%, respectively.
[0188] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0189] The total silicon content in the carbon fiber is 1200ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 6.7%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.7%, and the Si / C ratio of the area Z greater than 100nm is 0.04%. There are 14 pores on the surface of the carbon fiber, the average length of the pores is 30nm, and the average width is 19nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 2.8°. The tensile strength of the carbon fiber is 5.69GPa, the tensile modulus is 365GPa, and the elongation at break is 1.54%. After 6 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0190] [Example 10]
[0191] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0192] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 1.5%, an oil particle size of 300nm, an oil silicon content of 0.2%, and a residence time of 0.1s.
[0193] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0194] The raw yarn has a linear density of 0.85 dtex, an oil content of 1.1%, and a silicon content of 0.08%. The Si / C ratio in the region from the top of the protrusion on the fiber surface to the inner 2μm is 7%, and the Si / C ratio in the region greater than 2μm is 0.07%. The tensile strength, initial modulus, and elongation at break are 8.1 cN / dtex, 137 cN / dtex, and 11.8%, respectively.
[0195] 2. Preparation of carbon fiber: The precursor obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then, low-temperature carbonization and high-temperature carbonization are performed at 300-750°C and 800-1500°C with a draw ratio of 0.96; then, graphitization is performed at 2800°C, and finally, surface treatment, water washing, sizing, drying at 120°C and collecting are performed to obtain carbon fiber.
[0196] The total silicon content in the carbon fiber is 600ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 4.5%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.45%, and the Si / C ratio of the area Z greater than 100nm is 0.03%. There are 7 pores in the surface of the carbon fiber, the average length of the pores is 15nm, and the average width is 10nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 2.2°. The tensile strength of the carbon fiber is 5.76GPa, the tensile modulus is 379GPa, and the elongation at break is 1.5%. After 8 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0197] [Example 11]
[0198] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the drawing ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the drawing ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 140%.
[0199] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 1%, an oil particle size of 300nm, an oil silicon content of 0.11%, and a residence time of 0.1s.
[0200] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0201] The raw yarn has a linear density of 0.85 dtex, an oil content of 2.3%, and a silicon content of 0.4%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 16%, and the Si / C ratio in the region greater than 2μm is 0.14%. The tensile strength, initial modulus, and elongation at break are 7.2 cN / dtex, 119 cN / dtex, and 12.5%, respectively.
[0202] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0203] The total silicon content in the carbon fiber is 1350ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 8%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.85%, and the Si / C ratio of the area Z greater than 100nm is 0.04%. There are 15 pores on the surface of the carbon fiber, the average length of the pores is 38nm, and the average width is 20nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 3.2°. The tensile strength of the carbon fiber is 5.66GPa, the tensile modulus is 362GPa, and the elongation at break is 1.55%. After 6 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0204] [Example 12]
[0205] 1. Preparation of the raw yarn: wet spinning method is adopted. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28℃ and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20% and 10% respectively; the temperatures are 30℃, 40℃ and 50℃ respectively; the drawing ratios are 1.0, 1.1 and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃ and 99℃ respectively; the drawing ratios are 1.35, 1.50, 1.70 and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃ and 90℃ respectively; the swelling degree of the fiber after washing is 90%.
[0206] The washed fiber first passes through the first oiling tank, which contains the TFA-1208-10 non-ionic silicone-free oil synthesized by Tianjin Gongda Textile Auxiliary Co., Ltd., with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 100nm, and a residence time of 0.15s. It then passes through the second oiling tank, which contains the JSYJ-10 non-ionic silicone-containing oil synthesized by Sinopec (Shanghai) Petrochemical Research Institute, with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 100nm, an oil silicon content of 0.15%, and a residence time of 0.1s.
[0207] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, followed by steam drawing with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat-set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0208] The raw yarn has a linear density of 0.85 dtex, an oil content of 1.4%, and a silicon content of 0.16%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 12%, and the Si / C ratio in the region greater than 2μm is 0.12%. The tensile strength, initial modulus, and elongation at break are 7.5 cN / dtex, 134 cN / dtex, and 11.7%, respectively.
[0209] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0210] The total silicon content in the carbon fiber is 900ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 6%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.63%, and the Si / C ratio of the area Z greater than 100nm is 0.04%. There are 12 pores in the surface of the carbon fiber, the average length of the pores is 26nm, and the average width is 16nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 2.5°. The tensile strength of the carbon fiber is 5.7GPa, the tensile modulus is 377GPa, and the elongation at break is 1.52%. After 7 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0211] [Example 13]
[0212] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0213] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 8, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 9, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.1s.
[0214] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0215] The raw yarn has a linear density of 0.85 dtex, an oil content of 1.2%, and a silicon content of 0.14%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 9%, and the Si / C ratio in the region greater than 2μm is 0.11%. The tensile strength, initial modulus, and elongation at break are 7.7 cN / dtex, 135 cN / dtex, and 11.5%, respectively.
[0216] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0217] The total silicon content in the carbon fiber is 700ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 5%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.55%, and the Si / C ratio of the area Z greater than 100nm is 0.04%. There are 8 pores on the surface of the carbon fiber, the average length of the pores is 17nm, and the average width is 13nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 2.2°. The tensile strength of the carbon fiber is 5.75GPa, the tensile modulus is 375GPa, and the elongation at break is 1.51%. After 8 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0218] [Comparative Example 1]
[0219] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0220] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone oil with a pH of 7.8, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone oil with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.1s.
[0221] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0222] The raw yarn has a linear density of 0.85 dtex, an oil content of 3%, and a silicon content of 0.67%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 34%, and the Si / C ratio in the region greater than 2μm is 0.5%. The tensile strength, initial modulus, and elongation at break are 8.1 cN / dtex, 131 cN / dtex, and 11.9%, respectively.
[0223] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0224] The total silicon content in the carbon fiber is 3000ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 77%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 20%, and the Si / C ratio of the area Z greater than 100nm is 2%. There are 40 pores on the surface of the carbon fiber, the average length of the pores is 70nm, and the average width is 45nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 4.1°. The tensile strength of the carbon fiber is 5.23GPa, the tensile modulus is 355GPa, and the elongation at break is 1.46%. After 2.5 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0225] [Comparative Example 2]
[0226] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0227] The washed fiber first passes through the first oil tank, which contains water, a pH of 7, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone oil with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.1s.
[0228] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0229] The raw yarn has a linear density of 0.85 dtex, an oil content of 2.8%, and a silicon content of 0.55%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 24%, and the Si / C ratio in the region greater than 2μm is 0.19%. The tensile strength, initial modulus, and elongation at break are 7.9 cN / dtex, 131 cN / dtex, and 11.5%, respectively.
[0230] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0231] The total silicon content in the carbon fiber is 2600ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 72%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 18%, and the Si / C ratio of the area Z greater than 100nm is 1.8%. There are 39 pores in the surface of the carbon fiber, the average length of the pores is 66nm, and the average width is 45nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 3.8°. The tensile strength of the carbon fiber is 5.35GPa, the tensile modulus is 357GPa, and the elongation at break is 1.48%. After three months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0232] [Comparative Example 3]
[0233] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0234] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 8, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 6, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.1s.
[0235] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0236] The raw yarn has a linear density of 0.85 dtex, an oil content of 3.1%, and a silicon content of 0.68%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 35%, and the Si / C ratio in the region greater than 2μm is 0.5%. The tensile strength, initial modulus, and elongation at break are 7.5 cN / dtex, 128 cN / dtex, and 11.3%, respectively.
[0237] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0238] The total silicon content in the carbon fiber is 3200ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 80%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 13%, and the Si / C ratio of the area Z greater than 100nm is 1.5%. There are 50 pores in the surface of the carbon fiber, the average length of the pores is 77nm, and the average width is 52nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 4.3°. The tensile strength of the carbon fiber is 5.05GPa, the tensile modulus is 361GPa, and the elongation at break is 1.39%. After three months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0239] [Comparative Example 4]
[0240] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0241] The washed fiber first passes through the first oil tank, which contains the TFA-1208-Y anionic silicone-free oil agent synthesized by Tianjin Gongda Textile Additives Co., Ltd., with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains the JLQR-Y cationic silicone-containing oil agent synthesized by Jilin Qianren New Materials Co., Ltd., with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.1s.
[0242] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0243] The raw yarn has a linear density of 0.85 dtex, an oil content of 3.1%, and a silicon content of 0.69%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 35%, and the Si / C ratio in the region greater than 2μm is 0.5%. The tensile strength, initial modulus, and elongation at break are 7.5 cN / dtex, 129 cN / dtex, and 11.3%, respectively.
[0244] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0245] The total silicon content in the carbon fiber is 3300ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 82%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 15%, and the Si / C ratio of the area Z greater than 100nm is 2%. There are 56 pores in the surface of the carbon fiber, the average length of the pores is 80nm, and the average width is 60nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 4.3°. The tensile strength of the carbon fiber is 5GPa, the tensile modulus is 358GPa, and the elongation at break is 1.37%. After three months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0246] [Comparative Example 5]
[0247] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0248] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.1s.
[0249] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0250] The raw yarn has a linear density of 0.85 dtex, an oil content of 2.6%, and a silicon content of 0%. The Si / C ratio is 0% from the top of the protrusion to the inner 2μm of the fiber surface, and 0% in areas greater than 2μm. The tensile strength, initial modulus, and elongation at break are 7.2 cN / dtex, 120 cN / dtex, and 11.6%, respectively.
[0251] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0252] The total silicon content in the carbon fiber is 0 ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 0%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100 nm is 0%, and the Si / C ratio of the area Z greater than 100 nm is 0%. There are 64 pores on the surface of the carbon fiber, the average length of the pores is 89 nm, and the average width is 71 nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 4.8°. The tensile strength of the carbon fiber is 4.6 GPa, the tensile modulus is 340 GPa, and the elongation at break is 1.35%. After 7 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0253] [Comparative Example 6]
[0254] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0255] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 6%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 2%, an oil particle size of 300nm, an oil silicon content of 0.3%, and a residence time of 0.1s.
[0256] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0257] The raw yarn has a linear density of 0.85 dtex, an oil content of 2.6%, and a silicon content of 0.01%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 0.8%, and the Si / C ratio in the region greater than 2μm is 0.09%. The tensile strength, initial modulus, and elongation at break are 7.4 cN / dtex, 127 cN / dtex, and 11.6%, respectively.
[0258] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0259] The total silicon content in the carbon fiber is 400ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 0.8%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.07%, and the Si / C ratio of the area Z greater than 100nm is 0.01%. There are 58 pores in the surface of the carbon fiber, the average length of the pores is 75nm, and the average width is 50nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 4.5°. The tensile strength of the carbon fiber is 4.92GPa, the tensile modulus is 367GPa, and the elongation at break is 1.32%. After 6 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0260] [Comparative Example 7]
[0261] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0262] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 3.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 6%, an oil particle size of 300nm, an oil silicon content of 1%, and a residence time of 0.1s.
[0263] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0264] The raw yarn has a linear density of 0.85 dtex, an oil content of 2.7%, and a silicon content of 0.53%. The Si / C ratio in the region from the top of the protrusion on the fiber surface to the inner 2μm is 23%, and the Si / C ratio in the region greater than 2μm is 0.19%. The tensile strength, initial modulus, and elongation at break are 7.7 cN / dtex, 136 cN / dtex, and 11.3%, respectively.
[0265] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0266] The total silicon content in the carbon fiber is 2400ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 48%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 15%, and the Si / C ratio of the area Z greater than 100nm is 1%. There are 38 pores in the surface of the carbon fiber, the average length of the pores is 65nm, and the average width is 44nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 3.9°. The tensile strength of the carbon fiber is 5.3GPa, the tensile modulus is 354GPa, and the elongation at break is 1.47%. After three months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0267] [Comparative Example 8]
[0268] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0269] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.25s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.3s.
[0270] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0271] The raw yarn has a linear density of 0.85 dtex, an oil content of 2.7%, and a silicon content of 0.55%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 26%, and the Si / C ratio in the region greater than 2μm is 0.25%. The tensile strength, initial modulus, and elongation at break are 7.6 cN / dtex, 132 cN / dtex, and 11.5%, respectively.
[0272] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0273] The total silicon content in the carbon fiber is 2100ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 48%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 9%, and the Si / C ratio of the area Z greater than 100nm is 1%. There are 39 pores in the surface of the carbon fiber, the average length of the pores is 66nm, and the average width is 44nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 4.1°. The tensile strength of the carbon fiber is 5.28GPa, the tensile modulus is 360GPa, and the elongation at break is 1.41%. After three months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0274] [Comparative Example 9]
[0275] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0276] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.02s.
[0277] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, followed by steam drawing with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat-set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0278] The raw yarn has a linear density of 0.85 dtex, an oil content of 1%, and a silicon content of 0.01%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 0.8%, and the Si / C ratio in the region greater than 2μm is 0.05%. The tensile strength, initial modulus, and elongation at break are 7.4 cN / dtex, 130 cN / dtex, and 11.4%, respectively.
[0279] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0280] The total silicon content in the carbon fiber is 400ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 0.9%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.07%, and the Si / C ratio of the area Z greater than 100nm is 0.01%. There are 60 pores in the surface of the carbon fiber, the average length of the pores is 87nm, and the average width is 69nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 4.6°. The tensile strength of the carbon fiber is 4.9GPa, the tensile modulus is 366GPa, and the elongation at break is 1.31%. After 7 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0281] [Comparative Example 10]
[0282] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0283] The washed fiber first passes through the first oil tank, which contains TFA-1208-80 non-ionic silicone-free oil synthesized by Tianjin Gongda Textile Auxiliary Co., Ltd., with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 800nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains non-ionic silicone-containing oil, with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.1s.
[0284] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0285] The raw yarn has a linear density of 0.85 dtex, an oil content of 2.6%, and a silicon content of 0.52%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 22%, and the Si / C ratio in the region greater than 2μm is 0.16%. The tensile strength, initial modulus, and elongation at break are 7.3 cN / dtex, 128 cN / dtex, and 11.5%, respectively.
[0286] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0287] The total silicon content in the carbon fiber is 2000ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 45%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 13%, and the Si / C ratio of the area Z greater than 100nm is 0.08%. There are 45 pores on the surface of the carbon fiber, the average length of the pores is 60nm, and the average width is 40nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 5°. The tensile strength of the carbon fiber is 4.8GPa, the tensile modulus is 350GPa, and the elongation at break is 1.3%. After 4 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0288] [Comparative Example 11]
[0289] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0290] The washed fiber first passes through the first oiling tank, which contains the TFA-1208-04 non-ionic silicone-free oil synthesized by Tianjin Gongda Textile Auxiliary Co., Ltd., with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 40nm, and a residence time of 0.15s. It then passes through the second oiling tank, which contains the JSYJ-04 non-ionic silicone-containing oil synthesized by Sinopec (Shanghai) Petrochemical Research Institute, with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 40nm, an oil silicon content of 0.15%, and a residence time of 0.1s.
[0291] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0292] The raw yarn has a linear density of 0.85 dtex, an oil content of 2.7%, and a silicon content of 0.63%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 31%, and the Si / C ratio in the region greater than 2μm is 0.28%. The tensile strength, initial modulus, and elongation at break are 7.5 cN / dtex, 129 cN / dtex, and 11.3%, respectively.
[0293] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0294] The total silicon content in the carbon fiber is 2500ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 50%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 17%, and the Si / C ratio of the area Z greater than 100nm is 1.3%. There are 48 pores in the surface of the carbon fiber, the average length of the pores is 69nm, and the average width is 50nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 4.2°. The tensile strength of the carbon fiber is 5.1GPa, the tensile modulus is 351GPa, and the elongation at break is 1.4%. After three months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0295] [Comparative Example 12]
[0296] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0297] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 6%, an oil particle size of 300nm, an oil silicon content of 1%, and a residence time of 0.1s.
[0298] After that, four stages of drying and densification treatment are carried out at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam drawing is carried out with a drawing ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it is heat set with a drawing ratio of 0.95 and a steam pressure of 120MPa, and then it is collected to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0299] The raw yarn has a linear density of 0.85 dtex, an oil content of 2.7%, and a silicon content of 0.16%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 12%, and the Si / C ratio in the region greater than 2μm is 0.12%. The tensile strength, initial modulus, and elongation at break are 7.8 cN / dtex, 130 cN / dtex, and 11.5%, respectively.
[0300] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0301] The total silicon content in the carbon fiber is 1750ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 30%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 2.8%, and the Si / C ratio of the area Z greater than 100nm is 0.07%. There are 36 pores in the surface of the carbon fiber, the average length of the pores is 64nm, and the average width is 30nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 3.6°. The tensile strength of the carbon fiber is 5.35GPa, the tensile modulus is 356GPa, and the elongation at break is 1.47%. After three months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0302] [Comparative Example 13]
[0303] 1. The raw yarn is prepared by wet spinning. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5 dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60 μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28°C and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations are 30%, 20%, and 10% respectively; the temperatures are 30℃, 40℃, and 50℃ respectively; the draw ratios are 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing has temperatures of 95℃, 96℃, 97℃, and 99℃ respectively; the draw ratios are 1.35, 1.50, 1.70, and 2.00 respectively; the six-step water washing process has temperatures of 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing is 110%.
[0304] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then undergoes four stages of drying and densification treatment at temperatures of 90°C, 100°C, 115°C, and 130°C. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.1s.
[0305] After that, it undergoes four stages of drying and densification treatment at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam stretching with a stretching ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it undergoes heat setting with a stretching ratio of 0.95 and a steam pressure of 120MPa, and then yarn collection to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0306] The raw yarn has a linear density of 0.85 dtex, an oil content of 2%, and a silicon content of 0.15%. The Si / C ratio in the region from the top of the protrusion to the inner 2μm of the fiber surface is 0.5%, and the Si / C ratio in the region greater than 2μm is 0.05%. The tensile strength, initial modulus, and elongation at break are 7.6 cN / dtex, 132 cN / dtex, and 11.5%, respectively.
[0307] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0308] The total silicon content in the carbon fiber is 450ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 0.9%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 0.03%, and the Si / C ratio of the area Z greater than 100nm is 0.01%. There are 43 pores in the surface of the carbon fiber, the average length of the pores is 67nm, and the average width is 41nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 4.1°. The tensile strength of the carbon fiber is 5.16GPa, the tensile modulus is 359GPa, and the elongation at break is 1.42%. After 6 months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0309] [Comparative Example 14]
[0310] 1. Preparation of the raw yarn: wet spinning method is adopted. The spinning solution is prepared by copolymerization of acrylonitrile and itaconic acid in dimethyl sulfoxide. The intrinsic viscosity is 2.5dL / g and the solid content is 18%. The spinning solution is accurately measured and filtered by a metering pump, and then extruded through a spinneret with 6000 holes and a pore size of 60μm. It enters the first coagulation bath of dimethyl sulfoxide aqueous solution for coagulation at a coagulation temperature of 28℃ and a concentration of 51.5%. It then undergoes three-stage coagulation and drawing. The concentrations were 30%, 20%, and 10% respectively; the temperatures were 30℃, 40℃, and 50℃ respectively; the drawing ratios were 1.0, 1.1, and 1.2 respectively; the four-level hot water drawing, the temperatures were 95℃, 96℃, 97℃, and 99℃ respectively; the drawing ratios were 1.10, 1.15, 1.15, and 1.2 respectively; the six-step water washing process, the temperatures were 70℃, 70℃, 80℃, 80℃, 90℃, and 90℃ respectively; the swelling degree of the fiber after washing was 170%.
[0311] The washed fiber first passes through the first oil tank, which contains a non-ionic silicone-free oil with a pH of 7.2, an oil concentration of 1.5%, an oil particle size of 300nm, and a residence time of 0.15s. It then passes through the second oil tank, which contains a non-ionic silicone-containing oil with a pH of 7.8, an oil concentration of 1.2%, an oil particle size of 300nm, an oil silicon content of 0.15%, and a residence time of 0.1s.
[0312] After that, it undergoes four stages of drying and densification treatment at temperatures of 90°C, 100°C, 115°C and 130°C respectively, and then steam stretching with a stretching ratio of 3.0 times and a steam pressure of 0.35MPa; finally, it undergoes heat setting with a stretching ratio of 0.95 and a steam pressure of 120MPa, and then yarn collection to obtain high-performance polyacrylonitrile carbon fiber precursor.
[0313] The raw yarn has a linear density of 0.9 dtex, an oil content of 3.3%, and a silicon content of 0.74%. The Si / C ratio in the region from the top of the protrusion on the fiber surface to the inner 2μm is 46%, and the Si / C ratio in the region greater than 2μm is 0.69%. The tensile strength, initial modulus, and elongation at break are 7.0 cN / dtex, 117 cN / dtex, and 12.7%, respectively.
[0314] 2. Preparation of carbon fiber: The raw silk obtained in step 1 is pre-oxidized at 180-260°C with a total pre-oxidation draw ratio of 0.95 to obtain pre-oxidized fiber; then low-temperature carbonization and high-temperature carbonization are carried out at 300-750°C and 800-1500°C with a draw ratio of 0.96 times; then graphitization is carried out at 2800°C, and finally, carbon fiber is obtained after surface treatment, water washing, sizing, drying at 120°C and collecting.
[0315] The total silicon content in the carbon fiber is 3500ppm, the Si / C ratio of the carbon fiber in the area X between the top of the protrusion on the fiber surface and the bottom of the groove is 81%, the Si / C ratio of the area Y between the bottom of the groove and the inner 100nm is 20%, and the Si / C ratio of the area Z greater than 100nm is 3.7%. There are 70 pores in the surface of the carbon fiber, the average length of the pores is 84nm, and the average width is 77nm. The orientation deviation angle of the pores along the fiber axis obtained by small-angle X-ray scattering is 5.5°. The tensile strength of the carbon fiber is 4.58GPa, the tensile modulus is 339GPa, and the elongation at break is 1.34%. After two months of continuous production, the strength of the carbon fiber began to decline, and the equipment was stopped to clean the ash.
[0316] Table 1
[0317] Table 2
[0318] Table 3
[0319] Table 4
Claims
1. A polyacrylonitrile carbon fiber having a groove structure on the surface, characterized in that The Si / C ratio of the carbon fiber in the region X between the top of the protrusion on the fiber surface and the bottom of the groove is in the range of 1% to 10%, the Si / C ratio of the region Y between the bottom of the groove and the inner 100nm is in the range of 0.1% to 1%, and the Si / C ratio of the region Z greater than 100nm is not higher than 0.06%.
2. The polyacrylonitrile carbon fiber according to claim 1, characterized in that The polyacrylonitrile carbon fiber is obtained from polyacrylonitrile precursor fibers obtained by wet spinning.
3. The polyacrylonitrile carbon fiber according to claim 1 or 2, characterized in that The total silicon content in the carbon fiber is 500-1500 ppm, and / or the Si / C ratio of the region X between the top of the protrusion and the bottom of the groove on the fiber surface is not less than 8.5 times the Si / C ratio of the region Y between the bottom of the groove and the inner 100 nm.
4. The polyacrylonitrile carbon fiber according to any one of claims 1 to 3, characterized in that The number of pores present in the regions X and Y from the top of the protrusions on the fiber surface to the inner 100 nm is less than 20, preferably less than 16; wherein the average length of the pores is 10-50 nm and the average width is 5-25 nm.
5. The polyacrylonitrile carbon fiber according to any one of claims 1 to 4, characterized in that The pore orientation deviation angle along the fiber axis obtained by small angle X-ray scattering is less than or equal to 4°; and / or The carbon fiber has a tensile strength of 5.6-5.8 GPa, a tensile modulus of 360-390 GPa, and an elongation at break of 1.45%-1.6%.
6. A method for producing polyacrylonitrile carbon fiber, preferably the polyacrylonitrile carbon fiber according to any one of claims 1 to 5, comprising the step of carbonizing polyacrylonitrile precursor to obtain the polyacrylonitrile carbon fiber; characterized in that The Si / C ratio of the polyacrylonitrile precursor from the top of the fiber surface protrusion to the inner 2μm area is in the range of 1.0% to 20%, and the Si / C ratio of the area larger than 2μm is not higher than 0.15%.
7. The method for producing polyacrylonitrile carbon fiber according to claim 6, characterized in that The oil content of the raw silk is 0.5% to 2.5%, preferably 0.8% to 2.5%, preferably 0.8% to 2.4%, more preferably 0.9% to 2.0%; and / or The silicon content of the precursor is 0.01% to 0.5%; and / or The single-filament linear density of the polyacrylonitrile precursor is 0.7 to 1.0 dtex; and / or The polyacrylonitrile precursor is prepared by wet spinning.
8. The method for producing polyacrylonitrile carbon fiber according to claim 6 or 7, characterized in that The polyacrylonitrile precursor is prepared by wet spinning and includes an oiling step, wherein the oiling step includes two consecutive oiling processes without a drying and densification stage between the two oiling processes; wherein the first oiling process uses a silicone-free oil agent, a low-silicone oil agent or a combination thereof, and the second oiling process uses a silicone-containing oil agent.
9. The method for producing polyacrylonitrile carbon fiber according to claim 8, characterized in that The first oiling process uses a silicone-free oil, a low-silicone oil or a combination thereof, with a weight concentration of 0.1% to 5.0%; and the second oiling process uses a silicone-containing oil, with a weight concentration of 0.1% to 5.0%; and / or The average particle size of the silicone-free agent, the low-silicone agent and the silicone-containing agent is independently 50 nm to 500 nm; and / or The silicon content of the silicone oil used in the second oiling process is 0.01 wt% to 0.9 wt%; and / or The residence time of the second oiling is shorter than that of the first oiling.
10. The method for producing polyacrylonitrile carbon fiber according to any one of claims 6 to 9, characterized in that The pH difference between the silicone-free or low-silicone agent and the silicone-containing agent is not greater than 1; and / or The surfactant in the silicone-free oil agent or the low-silicone oil agent has a polarity different from that of the surfactant in the silicone-containing oil agent. Preferably, the silicone-containing oil agent is an oil agent containing a nonionic surfactant.
11. The method for producing polyacrylonitrile carbon fiber according to any one of claims 6 to 10, characterized in that Before oiling, the swelling degree of the polyacrylonitrile fiber after washing is 80-150%.
12. The method for producing polyacrylonitrile carbon fiber according to any one of claims 6 to 11, characterized in that The manufacturing method comprises the steps of wet coagulation molding of polyacrylonitrile stock solution, coagulation drawing, hot water drawing, water washing, oiling, drying and densification, steam drawing and steam heat setting to obtain the polyacrylonitrile raw yarn.
13. The method for producing polyacrylonitrile carbon fiber according to any one of claims 6 to 12, characterized in that The polyacrylonitrile precursor is subjected to pre-oxidation treatment and carbonization to obtain the polyacrylonitrile carbon fiber.
14. The method for producing polyacrylonitrile carbon fiber according to claim 13, characterized in that The pre-oxidation treatment is carried out in an air atmosphere at a temperature of 170-300° C. and a total draft of no more than 5%; and / or The carbonization includes low temperature carbonization treatment at 300-750°C in an inert atmosphere with a total draw ratio of 0-4% and high temperature carbonization treatment at 800-1500°C in an inert atmosphere with a total draw ratio of -4--2%.
15. A polyacrylonitrile precursor, characterized in that The Si / C ratio of the polyacrylonitrile precursor from the top of the fiber surface protrusion to the inner 2μm area is in the range of 1.0% to 20%, and the Si / C ratio of the area larger than 2μm is not higher than 0.15%.
16. The polyacrylonitrile carbon fiber precursor according to claim 15, characterized in that The oil content of the raw silk is 0.5% to 2.5%, preferably 0.8% to 2.5%, preferably 0.8% to 2.4%, more preferably 0.9% to 2.0%; and / or The silicon content of the precursor is 0.01% to 0.5%; and / or The single-filament linear density of the polyacrylonitrile precursor is 0.7 to 1.0 dtex; and / or The polyacrylonitrile precursor is prepared by wet spinning.
17. A method for preparing polyacrylonitrile precursor, preferably the polyacrylonitrile precursor according to claim 15 or 16, which comprises wet spinning and an oiling step, wherein the oiling step comprises two consecutive oiling processes, and there is no drying and densification stage between the two oiling processes, wherein the first oiling process uses a silicone-free oil agent, a low-silicone oil agent or a combination thereof and the second oiling process uses a silicone-containing oil agent.
18. The method according to claim 17, characterized in that The first oiling process uses a silicone-free oil, a low-silicone oil or a combination thereof, with a weight concentration of 0.1% to 5.0%; and the second oiling process uses a silicone-containing oil, with a weight concentration of 0.1% to 5.0%; and / or The second oiling residence time is less than the first oiling residence time; and / or The average particle size of the silicone-free agent, the low-silicone agent and the silicone-containing agent is independently 50 nm to 500 nm; and / or The silicon content of the silicone oil used in the second oiling process is 0.01 wt% to 0.9 wt%; and / or The pH difference between the silicone-free or low-silicone oil agent and the silicone-containing agent is no more than 1; and / or The surfactant in the silicone-free oil agent or the low-silicone oil agent has a polarity different from that of the surfactant in the silicone-containing oil agent, and preferably the silicone-containing oil agent is an oil agent containing a nonionic surfactant; and / or The swelling degree of the polyacrylonitrile raw silk after washing before oiling is 80-150%; and / or The preparation method comprises the steps of wet coagulation molding of polyacrylonitrile stock solution, coagulation drawing, hot water drawing, water washing, oiling, drying and densification, steam drawing and steam heat setting to obtain the polyacrylonitrile precursor.
Citation Information
Patent Citations
Method for reducing ash content of high-strength polyacrylonitrile-based carbon fibers and application thereof
CN110863270A
Treatment agent for carbon fiber precursor and carbon fiber precursor
CN112424418A
Oiling agent for manufacturing carbon fiber precursors, carbon fiber manufacturing method and carbon fiber
CN112726207A
Carbon fiber bundle and production method thereof
CN113597484A
Carbon fiber oiling agent capable of rapidly cross-linking to form film
CN114622417A
Cited By
3k polyacrylonitrile precursor, high-strength 3k carbon fiber and preparation method of 3k polyacrylonitrile precursor and high-strength 3k carbon fiber
CN119465429A
Ammoniation method of polyacrylonitrile powder
CN119841990A