Silver-copper composite conductive paste capable of being sintered at low temperature, method for preparing same and use thereof

By using a combination of multi-sized silver and copper particles and low melting point organic solvents in low-temperature sintering silver-copper composite conductive paste, the problems of high cost and insufficient conductive performance are solved, and low-temperature sintering and high-performance conductive effects are achieved, which is suitable for high temperature applications. Power device packaging under high irradiation conditions.

WO2024217073A1PCT designated stage expired Publication Date: 2024-10-24FOSHAN UNIVERSITY

Patent Information

Application Number
PCT/CN2024/070668
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-01-04
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

In the existing technology, low-temperature sintering silver-copper composite conductive paste has high cost, volatile organic solvents, and insufficient conductive properties, making it difficult to meet the packaging needs of power devices under high-temperature and high-irradiation conditions.

Method used

Using a variety of silver and copper particles of different sizes and shapes, through the combination of nano-silver flakes and micron copper particles, combined with low-melting point organic solvents, low-temperature sintering can be achieved, reducing costs, and improving thermal and electrical conductivity.

Benefits of technology

While achieving low-temperature sintering, it significantly reduces costs, improves electrical and thermal conductivity, ensures that organic solvents are completely decomposed at low temperatures, reduces the impact on performance, and is suitable for power device packaging under high-temperature and high-irradiation conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024070668_24102024_PF_FP_ABST
    Figure CN2024070668_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a silver-copper composite conductive paste capable of being sintered at a low temperature, a method for preparing the same, and use thereof. The first objective is to provide a silver-copper composite conductive paste capable of being sintered at a low temperature, which comprises the following components in percentage by weight: 20-80% of copper micron particles, 10-60% of silver nanoflakes, 1-20% of silver nanoparticles, and 1-10% of an organic carrier. According to the silver-copper composite conductive paste capable of being sintered at a low temperature, silver and copper with different sizes and different forms are adopted; large-size silver flakes and copper micron particles are used as a framework, and small-size silver nanoparticles are used as a filling material, thereby reducing gaps and improving the performance. A large number of copper micron particles are used in the silver-copper composite conductive paste capable of being sintered at a low temperature, so that the heat conduction performance and the electric conduction performance of the paste are improved, and also the cost can be effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

A silver-copper composite conductive paste capable of being sintered at low temperature, and its preparation method and application Technical Field

[0001] The present invention relates to the technical field of electronic power device packaging interface materials, in particular to a silver-copper composite conductive paste capable of being sintered at a low temperature, and a preparation method and application thereof. Background Art

[0002] Driven by demand from new energy (electric vehicles, wind power, photovoltaics), industry, power supplies, frequency conversion, and IoT devices, third-generation semiconductors such as silicon carbide and gallium nitride will dominate the future power device market. Silicon carbide and gallium nitride are typically used in harsh, high-temperature or high-irradiation conditions, placing higher demands on packaging materials than traditional semiconductor devices or integrated circuits. Power device packaging materials must possess excellent thermal conductivity.

[0003] Currently, traditional packaging materials are sintered at high temperatures, which inevitably causes some physical damage to the substrate device. The use of nanosilver particles can not only achieve low-temperature sintering, but also avoid the problem of intermetallic compound growth caused by excessively high temperatures, and has great application prospects. The use of nanosilver to achieve low-temperature sintering has been reported before, but the problem with previous research is that the cost of using all nanosilver is too high, and the water-based solvents used are too volatile, which is not conducive to large-scale industrial applications. After adding metallic copper, the cost can be effectively reduced and the performance of the slurry can also be improved.

[0004] For example, Chinese patent application number CN202110494206.4 discloses a glass material, a conductive paste, and its application in the preparation of ceramic dielectric filter electrodes. The conductive paste mainly includes glass material, an organic carrier, and conductive particles; the conductive particles include silver powder and copper powder; the silver powder includes flaky silver powder, nano-silver powder, and spherical silver powder with a particle size of 0.8-1.6μm, wherein the flaky silver powder accounts for 7-15% of the total mass of the silver powder, and the nano-silver powder accounts for 3-7% of the total mass of the silver powder; during the curing process, the conductive paste will form a layer structure with good density, Q value, and smooth surface. Although this conductive paste also uses nano-silver powder, micron silver flakes, and micron silver particles with a small amount of copper powder to prepare the conductive paste, the proportion of copper powder to the metal particles is small, the cost is high, and the paste composition contains high-melting-point materials such as glass powder, which greatly increases the sintering temperature.

[0005] For example, a silver-coated copper-silver paste and its preparation method disclosed in Chinese patent application number CN202210779926.X, a silver-coated copper-silver paste includes the following components in parts by weight: 22-25 parts of micron silver powder, 40-50 parts of nano silver powder, 20-22 parts of silver-coated copper powder, 2.5-9 parts of epoxy resin, 0.1-0.5 parts of epoxy curing accelerator, 2-4 parts of organic solvent and 0.5-1 part of silane coupling agent; its preparation method includes: accurately weighing each component, mixing and stirring each component in order to obtain a silver-carbon mixed slurry. The silver-coated copper-silver paste of the present application can reduce the production cost of silver paste, and at the same time can improve the conductive properties of silver paste, thereby expanding the application range of HJT heterojunction solar cells. Although the silver-coated copper-silver paste can also be cured at low temperatures, its resistivity is relatively high, and the resistivity is on the order of 1×10 -5 Ωcm, and the preparation of silver-coated copper powder is complicated, which makes the process difficult.

[0006] Summary of the Invention

[0007] In order to solve the above technical problems, the present invention provides a silver-copper composite conductive paste that can be sintered at low temperature, and a preparation method and application thereof.

[0008] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0009] The first object of the present invention is to provide a silver-copper composite conductive paste that can be sintered at low temperature, comprising the following components in weight percentage:

[0010] Furthermore, the micron copper particles are spherical in shape and have an average particle size of 1-10 μm.

[0011] Furthermore, the nano-silver flakes are in the shape of flakes, with an average plane diameter of 100-2000 nm and an average thickness of 5-500 nm, and a ratio of the plane diameter to the thickness of the flakes being greater than 2.

[0012] Furthermore, the nano silver particles are spherical in shape and have an average particle size of 1-100 nm.

[0013] Furthermore, the organic carrier may include one organic solvent selected from the group consisting of 1,2-propylene glycol, ethylene glycol, terpineol, and DBE, or a mixed organic solvent of multiple combinations thereof.

[0014] Furthermore, the organic vehicle may further comprise one or more combinations of organic resin, rheological agent, and surfactant, and the weight percentage of the one or more combinations of organic resin, rheological agent, and surfactant in the organic vehicle is 0-3%.

[0015] Preferably, the average particle size of the nanosilver particles is 3-8 nm.

[0016] A second object of the present invention is to provide a method for preparing a silver-copper composite conductive paste that can be sintered at low temperature, comprising the following steps:

[0017] Micron copper particles, nano silver flakes, nano silver particles, and an organic carrier are weighed according to weight percentage, the micron copper particles, nano silver flakes, and nano silver particles are added to the organic carrier, and then ground evenly with a mortar or a three-roll mill to obtain a silver-copper composite conductive slurry that can be sintered at a low temperature.

[0018] The third object of the present invention is to provide an application of a low-temperature sinterable silver-copper composite conductive paste as a chip packaging and connection material for power semiconductor devices. Specifically, the low-temperature sinterable silver-copper composite conductive paste is encapsulated on the chip of the semiconductor device using a hot pressing process. The process conditions are: pressure 0.1MPa-1MPa, sintering temperature 180-250°C, sintering time 15-30 minutes, and holding time 10 minutes.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The low-temperature sinterable silver-copper composite conductive paste provided by the present invention adopts silver and copper of various sizes and morphologies, uses large-sized silver flakes and micron copper particles as the skeleton, and small-sized nano-silver particles as filler, thereby reducing gaps and improving performance.

[0021] The silver-copper composite conductive paste capable of being sintered at low temperature of the present invention adopts a large number of micron copper particles, thereby improving the thermal conductivity and electrical conductivity of the paste and effectively reducing the cost.

[0022] The silver-copper composite conductive paste capable of low-temperature sintering of the present invention realizes low-temperature sintering due to the addition of small-sized nano-silver particles. The sintering temperature is 180-250° C., which is lower than the sintering temperature of traditional device packaging materials.

[0023] The low-temperature sinterable silver-copper composite conductive paste of the present invention is added with an organic solvent with a boiling point below 250° C., and can ensure that the organic solvent is completely decomposed and volatilized at a sintering temperature of 180-250° C., thereby reducing the influence of organic matter on performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] FIG1 is a TEM image of nanosilver particles added in Examples 1-4 and Comparative Example 1;

[0025] FIG2 is an SEM image of the nanosilver flakes added in Examples 1-4 and Comparative Example 1;

[0026] FIG3 is an SEM image of micron copper particles added in Examples 1-4;

[0027] FIG4 is a SEM image of the microstructure of the sintered body of Example 5;

[0028] FIG5 is a SEM image of the microstructure of the sintered body of Example 6;

[0029] FIG6 is a SEM image of the microstructure of the sintered body of Example 7;

[0030] FIG7 is a SEM image of the microstructure of the sintered body of Example 8. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. The specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0032] In the following examples, the reagents used are shown in Table 1. All experimental instruments used were commercially available unless otherwise stated. The morphology and size of the silver nanoparticles are shown in Figure 1 , the morphology and size of the silver nanoflakes are shown in Figure 2 , and the morphology and size of the micronized copper particles are shown in Figure 3 .

[0033] Table 1

[0034] Example 1

[0035] 10 g of terpineol is weighed, and then 10 g of nano-silver particles with a size of 3-8 nm are added to the terpineol (i.e., the main component of the organic carrier is terpineol, and of course 0-3% of an organic resin, a rheological agent, a surfactant, etc. can also be added as needed to adjust the physical properties of the slurry required under the use process conditions); 20 g of nano-silver flakes with a side length of 300-800 nm and a thickness of 30-80 nm are added; and 60 g of micron copper powder with a size of 2-8 μm is added, and then the mixture is evenly ground in a mortar to obtain a silver-copper composite conductive slurry that can be sintered at a low temperature.

[0036] Example 2

[0037] 10 g of DBE (i.e., the main component of the organic vehicle is DBE, and of course 0-3% of an organic resin, a rheological agent, a surfactant, etc. can also be added as needed to adjust the physical properties of the slurry required under the use process conditions) is weighed, and then 10 g of nanosilver particles with a size of 3-8 nm is added to the DBE; 20 g of nanosilver flakes with a side length of 300-800 nm and a thickness of 30-80 nm are added; and 60 g of micron copper powder with a size of 2-8 μm is added, and then the mixture is evenly ground in a mortar to obtain a silver-copper composite conductive slurry that can be sintered at a low temperature.

[0038] Example 3

[0039] 10 g of ethylene glycol (i.e., the main component of the organic vehicle is ethylene glycol, and of course 0-3% of an organic resin, a rheological agent, a surfactant, etc. can also be added as needed to adjust the physical properties of the slurry required under the use process conditions) is weighed, and then 10 g of nano-silver particles with a size of 3-8 nm are added to the ethylene glycol; 20 g of nano-silver flakes with a side length of 300-800 nm and a thickness of 30-80 nm are added; and 60 g of micron copper powder with a size of 2-8 μm is added, and then ground evenly in a mortar to obtain a silver-copper composite conductive slurry that can be sintered at a low temperature.

[0040] Example 4

[0041] 10 g of 1,2-propylene glycol (i.e., the main component of the organic vehicle is 1,2-propylene glycol, and of course 0-3% of an organic resin, a rheological agent, a surfactant, etc. can also be added as needed to adjust the physical properties of the slurry required under the use process conditions) is weighed, and then 10 g of nano silver particles with a size of 3-8 nm is added to the 1,2-propylene glycol; 20 g of nano silver flakes with a side length of 300-800 nm and a thickness of 30-80 nm are added; and 60 g of micron copper powder with a size of 2-8 μm is added, and then ground evenly in a mortar to obtain a silver-copper composite conductive slurry that can be sintered at a low temperature.

[0042] Comparative Example 1

[0043] 10 g of 1,2-propylene glycol (i.e., the main component of the organic vehicle is 1,2-propylene glycol, and of course, 0-3% of an organic resin, a rheological agent, a surfactant, etc. can also be added as needed to adjust the physical properties required for the slurry under the use process conditions) is weighed, and then 30 g of nano silver particles with a size of 3-8 nm are added to the 1,2-propylene glycol; 60 g of nano silver flakes with a side length of 300-800 nm and a thickness of 30-80 nm are added, and then ground evenly in a mortar to obtain a silver-copper composite conductive slurry that can be sintered at a low temperature.

[0044] Furthermore, in order to verify whether the low-temperature sinterable silver-copper composite conductive pastes prepared in the above embodiments and comparative examples can be used as chip packaging and connection materials for power semiconductor devices, the following hot pressing process was used to prepare samples of the low-temperature sinterable silver-copper composite conductive pastes prepared in the above embodiments 1-4 and comparative example 1, as follows.

[0045] Example 5

[0046] The low-temperature sinterable silver-copper composite conductive paste prepared in Example 1 was sintered using a mold and a hot press at a pressure of 0.5 MPa and a sintering temperature of 200° C. for 20 minutes. After the sintering was completed, the pressure was removed and the paste was kept warm for 10 minutes to obtain sample A. The microstructure of the sintered sample of sample A is shown in FIG4 .

[0047] Example 6

[0048] The low-temperature sinterable silver-copper composite conductive paste prepared in step Example 2 was sintered using a mold and a hot press at a pressure of 0.5 MPa and a sintering temperature of 200° C. for 20 minutes. After the sintering was completed, the pressure was removed and the paste was kept warm for 10 minutes to obtain sample B. The microstructure of the sintered sample of sample B is shown in Figure 5.

[0049] Example 7

[0050] The low-temperature sinterable silver-copper composite conductive paste prepared in step Example 3 was sintered using a mold and a hot press at a pressure of 0.5 MPa and a sintering temperature of 200° C. for 20 minutes. After the sintering was completed, the pressure was removed and the paste was kept warm for 10 minutes to obtain sample C. The microstructure of the sintered sample of sample C is shown in FIG6 .

[0051] Example 8

[0052] The low-temperature sinterable silver-copper composite conductive paste prepared in step Example 4 was sintered using a mold and a hot press at a pressure of 0.5 MPa and a sintering temperature of 200° C. for 20 minutes. After the sintering was completed, the pressure was removed and the paste was kept warm for 10 minutes to obtain sample D. The microstructure of the sintered sample of sample D is shown in FIG7 .

[0053] Comparative Example 2

[0054] The low-temperature sinterable silver-copper composite conductive paste prepared in Comparative Example 1 was sintered using a mold and a hot press at a pressure of 0.5 MPa and a sintering temperature of 200° C. for 20 minutes. After the sintering was completed, the pressure was removed and the paste was kept warm for 10 minutes to obtain Sample E.

[0055] As can be seen from Figures 4 to 7, the nanosilver flakes have undergone varying degrees of melting. This is because the addition of small-sized nanosilver particles, which have a very high specific surface area and surface activity, significantly lowers the melting point through the size effect, forming a eutectic with the nanosilver flakes and driving their melting. Simultaneously, the nanoscale effect synergizes with the micron-sized copper, forming connected heat conduction channels with the micron-sized copper particles. The more these connected structures, the stronger the sample's thermal and electrical conductivity.

[0056] The samples obtained in Examples 5 to 8 and Comparative Example 2 were sent to Shanghai Microspectra Testing Technology Group Co., Ltd. and tested for thermal conductivity according to the reference standard ASTM E1461-2013. The resistivity was obtained by testing using the electrical transport property measurement system of this unit, and then the conductivity was obtained by calculation. The resistivity and conductivity are reciprocals of each other, and the results are shown in Table 2.

[0057] Table 2

[0058] The data in Table 2 demonstrate that the low-temperature sinterable silver-copper composite conductive paste prepared by the present invention exhibits excellent thermal and electrical conductivity after sintering. This paste has promising applications in power electronic devices and provides a promising approach for packaging materials. Furthermore, the properties of the sintered bodies of the low-temperature sinterable silver-copper composite conductive paste vary depending on the addition of different organic solvents, with the thermal and electrical conductivity of the sintered bodies produced when 1,2-propylene glycol is used as the organic solvent being optimal.

[0059] In summary, the low-temperature sinterable silver-copper composite conductive paste prepared by the present invention has excellent thermal conductivity and electrical conductivity after low-temperature sintering, and therefore can be used as a chip packaging and connection material for high-speed semiconductor devices.

[0060] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. Any technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.

Claims

1. A silver-copper composite conductive paste capable of being sintered at low temperature, characterized in that: The composition includes the following weight percentages:

2. The low temperature sinterable silver-copper composite conductive paste according to claim 1, characterized in that: The micron copper particles are spherical in shape and have an average particle size of 1-10 μm.

3. The low temperature sinterable silver-copper composite conductive paste according to claim 1, characterized in that: The nano silver flakes are in the shape of flakes, with an average plane diameter of 100-2000nm, an average thickness of 5-500nm, and a ratio of the plane diameter to the thickness of the flakes being greater than 2.

4. The low temperature sinterable silver-copper composite conductive paste according to claim 1, characterized in that: The nano silver particles are spherical in shape and have an average particle size of 1-100 nm.

5. The low temperature sinterable silver-copper composite conductive paste according to claim 1, characterized in that: The organic carrier comprises an organic solvent selected from the group consisting of 1,2-propylene glycol, ethylene glycol, terpineol, and DBE, or a mixed organic solvent of a plurality of combinations thereof.

6. The low temperature sinterable silver-copper composite conductive paste according to claim 1, characterized in that: The organic carrier further comprises one or more combinations of organic resin, rheological agent and surfactant, and the weight percentage of the one or more combinations of organic resin, rheological agent and surfactant in the organic carrier is 0-3%.

7. The low temperature sinterable silver-copper composite conductive paste according to claim 4, characterized in that: The average particle size of the nano silver particles is 3-8 nm.

8. A method for preparing a silver-copper composite conductive paste capable of low temperature sintering according to any one of claims 1 to 7, characterized in that: The following steps are involved: Micron copper particles, nano silver flakes, nano silver particles, and an organic carrier are weighed according to weight percentage, the micron copper particles, nano silver flakes, and nano silver particles are added to the organic carrier, and then ground evenly with a mortar or a three-roll mill to obtain a silver-copper composite conductive slurry that can be sintered at a low temperature.

9. Use of the low-temperature sinterable silver-copper composite conductive paste according to any one of claims 1 to 7 as a chip packaging and connection material for power semiconductor devices.

10. Use of the low-temperature sinterable silver-copper composite conductive paste according to claim 9 as a chip packaging and connection material for power semiconductor devices, characterized in that: The low-temperature sinterable silver-copper composite conductive paste is packaged on the chip of the semiconductor device by a hot pressing process, and the process conditions are: pressure 0.1MPa-1MPa, sintering temperature 180-250°C, sintering time 15-30 minutes, and heat preservation time 10 minutes.

Citation Information

Patent Citations

  • Low-temperature sintered hybrid conductive silver paste for chip package and preparation method thereof

    CN107221373A

  • Composite nano silver paste and rapid sintering packaging method

    CN107833651A

  • Silver-based conductive paste and preparation method thereof and application of silver-based conductive paste in packaging chip interconnection

    CN110033877A

  • Micro-nano compound silver-copper alloy welding paste used for low-temperature sintering and interconnection and production method

    CN112756841A

  • Copper-silver composite slurry suitable for 3D printing and preparation method thereof

    CN115188522A

Cited By

  • Copper paste, preparation method of copper paste and N-type crystalline silicon solar cell

    CN119943469A

  • High-temperature-resistant working sealing silver copper paste for power chip and preparation method of high-temperature-resistant working sealing silver copper paste