Sputtering target and process for producing the same
Patent Information
- Application Number
- PCT/CN2024/088901
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-24
Smart Images

Figure CN2024088901_24102024_PF_FP_ABST
Abstract
Description
SPUTTERING TARGET AND PROCESS FOR PRODUCING THE SAMEFIELD
[0001] The present disclosure relates to a sputtering target and a process for producing the sputtering target.BACKGROUND
[0002] W-Ni alloy is an alloy with high melting point, high hardness and high corrosion resistance, and is widely applied to machinery, electronics, medical instruments, automobile parts, aerospace military industry, daily hardware parts, industrial processing dies and the like.
[0003] Electrochromic layers composed of W-Ni mixed oxides have been known for many years. A particularly advantageous atomic ratio of W / Ni in the NiOx alloyed with W (W-Ni mixed oxide) is about 0.33. At this ratio, the charge transfer resistance is optimal so as to ensure very fast optical switching behaviour of the electrochromic layer. Electrochromic layers produced in this way are made using, for example, sputtering targets composed of W-Ni alloys which are ablated by reactive magnetron sputtering under oxygen to form W-Ni mixed oxide layers. Oxidic targets are also known from the prior art.
[0004] In addition, W-Ni alloys can be used as a barrier layer for Cu / Sn bonding applications, wherein a submicron Cu / Sn bonding with a transient Ni diffusion buffer layer at 225 ℃overcomes 5μm Cu / Sn physical limitation. The 10-nm Ni layer suppresses immense Cu / Cn interdiffusion during step prior to major bonding process. When the temperature is close to the Sn melting point, The Ni laver dissolves, and molten Sn gives submicrometric Cu / Sn bonding. The excellent mechanical strength and electrical performance of this scheme show the great potential for high dense 3D interconnects. From the same principle, W-Ni alloys also can be used for bonding layer between TFT and LED cell.
[0005] For a sputtering target consisting of W-Ni alloys, conventional application used powder hot spraying process, which could cause high chemical impurity and lower density. High levels of chemical impurities lead to different coating rates, and therefore have a negative effect on the homogeneity of the deposited layer. Low densities of the sputtering target material likewise have an adverse effect on the coating rates. Furthermore, only limited material thicknesses can be produced by means of thermal spraying, which limits the materials utilization and useful life of the target.
[0006] If sputtering targets composed of W-Ni alloys as used at present are produced by thermal spraying, the use of Ni and W powders as starting material for making the targets has the consequence that pure nickel, which displays ferromagnetic properties, is sometimes present in the target material. These ferromagnetic regions are disadvantageous for magnetron sputtering since they result in different coating rates and thus have a disadvantageous influence on the homogeneity of the deposited layer.
[0007] In addition, only limited material densities can be produced in thermal spraying processes. Low densities of the sputtering target material likewise have an adverse effect on the coating rates. Furthermore, only limited material thicknesses can be produced by means of thermal spraying, which limits the materials utilization and useful life of the target.
[0008] The metallic impurities present in the spray powder as a result of the method of production, which are transferred directly into the target material produced, are a further disadvantage. Impurities in the sputtered layers can have an adverse effect on the optical layer properties.
[0009] Additional non-metallic, in particular oxidic or dielectric inclusions or phases which can be incorporated into the target material during thermal spraying, lead to an increased number of particles during sputtering which in turn can have a disadvantageous effect on the properties of the sputtered layer (adhesion, specific electrical resistance, layer homogeneity) and the coating process (high arcing rate) .
[0010] In order to overcome the defects brought about by thermal spraying as described above, WO2015089533A1 describes a sputtering target with low Ni content and high W content. With the defined sintering process, the oxygen content can be controlled within 100μg / g and density can reach above 90 wt. %. However, this process has the following drawbacks: W phase as a second phase which can lead the un-even distribution of the sputtered surface; high pure W phase, and the sputtering target includes pure Ni phase, which will reduce the uniformity of the material and impact the sputtering effect.SUMMARY
[0011] The present disclosure aims to overcome, at least in part, the defects of the prior art by providing an improved sputtering target and a process for producing the sputtering target.
[0012] A first aspect of the present disclosure relates to a sputtering target, comprising from 55%to 80%by weight of Ni, a balance of W and normal impurities,
[0013] the sputtering target contains a W phase, a Ni (W) solid solution phase, no pure Ni phase and no or less than 5%by area on average of intermetallic phases measured at a cross section of the target material.
[0014] Alternatively, the sputtering target comprises 60%to 70%by weight of Ni.
[0015] Alternatively, the sputtering target comprises 60%to 65%by weight of Ni.
[0016] Alternatively, the sputtering target comprises an oxygen content of less than 50μg / g.
[0017] Alternatively, the sputtering target comprises an oxygen content of less than 40μg / g.
[0018] Alternatively, the sputtering target has a hardness of less than 500 HV10.
[0019] Alternatively, the intermetallic phase is one or more selected from the group consisting of Ni4W, WNi or W2Ni.
[0020] Alternatively, the sputtering target has an average grain size of the W phase of less than 40 μm.
[0021] Alternatively, the sputtering target has a relative density of more than 90%.
[0022] Alternatively, the sputtering target has a relative density of more than 99.5%.
[0023] A second aspect of the present disclosure relates to a process for producing a sputtering target as described in the first aspect of the present disclosure using a powder-metallurgical route comprising the following steps:
[0024] carrying out a compacting step in which a powder mixture of W powder and Ni powder is compacted by application of pressure, heat or pressure and heat to get a compacted blank; and
[0025] carrying out a cooling step in which the compacted blank is cooled at a cooling rate of greater than 3 K / min to a temperature range of from 750℃ to 1000℃.
[0026] If the compacting step is effected by sintering temperatures of from 1100℃ to 1450℃, and the sintering atmosphere is combined with a first gas and / or a vacuum. Preferably the sintering atmosphere is changed from vacuum to a first gas, i.e. sintering is carried out successively with vacuum and the first gas.
[0027] Alternatively, the process further comprises performing a thermomechanical or thermal treatment of the blank between the compacting step and the cooling step. However, if such a thermomechanical or thermal treatment is performed after the sintering step, the cooling rate in the cooling step is changed to greater than 30K / min at least in a temperature range from 900 to 750℃.
[0028] Alternatively, the process further comprises performing the thermomechanical or thermal treatment at temperatures in a range of from 970℃ to 1450℃.
[0029] Alternatively, the thermomechanical or thermal treatment includes at least one forging step or rolling step.
[0030] BRIEF DESCRIPTION OF THE DRAWING
[0031] Fig. 1 shows a phase diagram of the Ni-W system, wherein the composition range according to a sputtering target of a first aspect of the present disclosure is marked.
[0032] Fig. 2 shows a microscopic view of a sputtering target manufactured in Examples 1 to 3 of the process for producing a sputtering target of a second aspect of the present disclosure.
[0033] Fig. 3A shows a microscopic view of a sputtering target manufactured in Example 4 of the process for producing a sputtering target of a second aspect of the present disclosure.
[0034] Fig. 3B shows a microscopic view of a sputtering target manufactured in Example 4 of the process for producing a sputtering target of a second aspect of the present disclosure.DETAILED DESCRIPTION
[0035] Hereinafter, first, the sputtering target involved in the first aspect of the present disclosure is described in detail.
[0036] As shown in Fig. 1 (cf. ASM Handbook Vol. III, Alloy Phase Diagrams 1992) , the sputtering target contains a W phase, a Ni (W) solid solution phase, no Ni phase, wherein the Ni(W) solid solution phase has W-alloyed Ni mixed crystals, preferably a Ni mixed crystal saturated with W.
[0037] A sputtering target according to the present disclosure preferably contains less than 5%by area on average of intermetallic phases measured at a cross section of the target material. Preferably, the sputtering target according to the present disclosure contains less than 5%by area on average of pure W phase.
[0038] To determine the proportion of intermetallic phases present in a sputtering target according to the present disclosure, the average proportion by area is analysed at a cross section. For this purpose, a metallographic polished section is produced and examined by optical or electron microscopy. A metallographic polished section is a two-dimensional section of the three-dimensional target material. Areal analyses can be carried out by means of commercially available image analysis software on micrographs produced in this way. This is carried out by image analysis in order to determine proportions of individual phases in the abovementioned microstructure, typically by contrasting of the phases to be distinguished. Difficult-to-distinguish phases can be contrasted further by means of suitable etching processes. In the present case, the intermetallic phase can be made distinguishable from the Ni mixed crystal (Ni (W) phase, W-saturated Ni mixed crystal) by etching with a suitable etching solution (e.g. 85 ml of ammonia solution and 5 ml of 30%solution hydrogen peroxide) and the proportion by area can be determined. However, depending on the state of the microstructure, alternative etching solutions and processes are conceivable. The average proportion by area is calculated as arithmetic mean of 5 measurements of the proportion by area measured on 5 image regions having a size of 100×100μm of a metallographic polished section, recorded with 1000×magnification. An intermetallic phase of less than 5%results in a uniform elemental distribution on the sputtered surface. The maximum deviation of Ni-content of the sputtering target manufactured is much lower than those produced by the process of WO2015089533A1, resulting in a very high uniformity of Ni at different positions of the sputtering target. As an alternative, the occurrence of intermetallic phases in a sputtering target can very easily be confirmed or ruled out by means of X-ray diffraction (XRD) (taking into account the respective X-ray detection limit) using the relevant JCPDS cards.
[0039] The intermetallic phase may be, for example, selected from any one of the following: Ni4W, WNi, W2Ni.
[0040] As can be seen from the phase diagram in Fig. 1, the brittle Ni4W phase occurs preferentially at a Ni content of more than 55%by weight in a sputtering target. At even higher contents of Ni, ferromagnetic Ni phase can occur.
[0041] The sputtering target of the present disclosure contains from 55%to 80%by weight of Ni, a balance of W and normal impurities. The term “normal impurities” refers to production-related contamination with gases or accompanying elements which originate from the raw materials used. The proportion of such impurities in a sputtering target according to the present disclosure is preferably in the range below 100μg / g (corresponding to ppm) for gases (C, H, N, O) and below 500μg / g for other elements. Suitable methods of chemical elementary analysis are known to be dependent on the chemical element to be analysed. The sputtering target of the present disclosure has high Ni content and low W content. In a Ni-W layer produced by the claimed sputtering target, Ni can be used as buffer layer to dissolve molten Sn, and successfully achieves submicron Cu / Sn bonding, whereby excellent mechanical strength and electrical properties can be achieved. The Ni-W layers produced from the target can be used for TFT electrode bonding and semiconductor 3D integration. It effectively solves the technical problems of reducing material uniformity and impacting the sputtering effect in the existing sputtering targets, and has high purity, high density and good application performance. The sputtering target of the present disclosure is further preferred to contain from 60%to 70%by weight of Ni, and even further preferred to contain from 60%to 65%by weight of Ni, a content that further yields better material uniformity and application properties.
[0042] The sputtering targets of the present disclosure preferably have an oxygen content of less than 50μg / g, and particularly preferably less than 40μg / g.
[0043] The oxygen content can be determined in a simple way by ICP-OES.
[0044] The sputtering targets of the present disclosure preferably have a Vickers hardness of less than 500 HV10.
[0045] It has been found that satisfactory toughness of the target material can optimally be ensured at hardnesses of less than 500 HV10. This simplifies handling during the production process, for example during an optional mechanical shaping step. During use, especially as single-piece tubular target in one embodiment, a hardness of less than 500 HV10 significantly simplifies handling.
[0046] The hardness in HV10 (Vickers hardness) is for the present purposes an arithmetic mean determined from 5 hardness measurements.
[0047] The sputtering target of the present disclosure preferably has a relative density of more than 90%, more preferably more than 92%and most preferably more than 99.5%. The higher the density of the target, the more advantageous are its properties. Targets having a low relative density have a relatively high proportion of pores which can be a virtual leak and / or a source of impurities and particles during the sputtering process. In addition, targets having a low density tend to absorb water or other impurities, which can lead to difficult-to-control process parameters. In addition, the ablation rate of material which is densified to only a low extent is lower during the sputtering process than that of material having a higher relative density.
[0048] It is well known that, relative density can be easily measured using Archimedes' principle by means of buoyancy methods.
[0049] The installation of a sputtering target according to the present disclosure in various coating plants and also for the coating of substrates having different geometries places various geometric demands on a sputtering target according to the present disclosure. Thus, a target of this type can be in the form of a flat target, for example as plate or disc, as rod, as tubular target or as body having another complex shape.
[0050] A sputtering target according to the present disclosure preferably has an average grain size of the W phase of less than 40μm, more preferably less than 20μm.
[0051] An average grain size of the W phase of less than 40μm, more preferably less than 20μm, leads to a particularly uniform sputtering behaviour and thus to deposition of particularly homogeneous layers having a particularly uniform thickness. In addition, the notch effect of the W phase is kept low in this way and satisfactory toughness of the target material is optimally ensured as a result.
[0052] Agglomerates of a plurality of grains of the W phase can exceed dimensions of 40μm in diameter, but such agglomerates are not considered to be individual grains of the W phase in a sputtering target according to the present disclosure.
[0053] The average grain size of the W phase can be determined in a simple way by a line section method on a metallographic polished section.
[0054] As described above, the sputtering target according to the first aspect of the present disclosure effectively solves the technical problem of reducing the homogeneity of the material and impacting the sputtering effect, thus it has a high density and good application performance.
[0055] Such sputtering target of the present disclosure is applicable in the following fields:
[0056] -Bonding solution in display applications for example of LED chips on TFT backplane;
[0057] -As thin layer in electrochromic devices or in solar control coating stacks;
[0058] -As cover-layer to protect underlying metal lines, e.g. copper-or aluminum-based layers, from ambient exposure and oxidation;
[0059] -As Bufer layer to control difusion of elements between different layers by applying a specific thickness, e.g 5nm<t<50nm;
[0060] -As Ni source for application in packaging and soldering;
[0061] -To deposit oxides or nitrides with a reactive sputtering process;
[0062] -As Barrier layer in a thin film stack to prevent cross diffusion of elements e.g. into semiconducting material or into copper metal lines for example in thin film transistor metallization, which would decrease electrical performance.
[0063] The process for producing the sputtering target of the second aspect of the present disclosure is described below.
[0064] The process for producing the sputtering target described in the first aspect of the present disclosure using a powder-metallurgical route of the second aspect of the present disclosure is characterized in that, the method comprises at least the following steps:
[0065] carrying out a compacting step in which a powder mixture of W powder and Ni powder is compacted by application of pressure, heat, or pressure and heat to get a compacted blank; and
[0066] carrying out a cooling step in which the compacted blank is cooled at a cooling rate of greater than 3 K / min to a temperature range of from 750℃ to 1000℃.
[0067] The compaction step as part of the process according to the invention for producing the W-Ni sputtering target leads to an appropriate powder mixture being compacted and densified by application of pressure, heat, or pressure and heat to form a blank. This can occur by means of various processing steps, for example by pressing and sintering, cold isostatic pressing, hot isostatic pressing, hot pressing, or spark plasma sintering (SPS) or a combination of these methods or further methods of compacting powder mixtures.
[0068] The production of a powder mixture which can be used for a process according to the present disclosure is preferably effected by weighing the appropriate amounts of W powder and Ni powder into a suitable mixing apparatus and mixing until homogeneous distribution of the components in the powder mixture is ensured. For the purposes of the present disclosure, the expression powder mixture includes pre-alloyed or partially alloyed powders containing the components W and Ni.
[0069] A powder mixture produced in this way is preferably introduced into a mould in order to implement the compacting step. Suitable moulds here are the die or flexible tube in cold isostatic pressing, the die of a hot press or a spark plasma sintering plant and also the can in the case of hot isostatic pressing.
[0070] A cooling step in which the blank is cooled at a cooling rate of greater than 3 K / min to a temperature range of from 750℃ to 1000℃ as part of a process according to the present disclosure for producing a W-Ni sputtering target avoids the occurrence of undesirable intermetallic phases. In a preferred embodiment, the blank is held at this temperature range for 15 minutes to 3 hours, more preferably 45 minutes to 2 hours, and further preferably 45 minutes to 90 minutes. An excessively high proportion of intermetallic phases in a W-Ni sputtering target produced by means of a process according to the present disclosure can, firstly, lead to a sputtering rate different from that of the remaining target and thus to nonuniform ablation over the target material and consequently to fluctuations in the thickness of the deposited layer. Furthermore, brittle intermetallic phases in the microstructure of the target material can lead to arcing or increased particle formation. Secondly, handling of such a sputtering target is made more difficult by the low toughness of intermetallic phases.
[0071] As already outlined above if a thermomechanical or thermal treatment is performed after the compacting step, e.g. the sintering step, the cooling rate is changed to greater than 30K / min to a temperature in the range from 900-750℃. Preference is also given to the blank obtained being cooled at a cooling rate of greater than 50 K / min to a temperature range of from 750℃ to 900 ℃, in such a cooling step since the materials properties described and the microstructure of the target can be set in a particularly optimized manner. A cooling step of this type can, for example, be realized by cooling in air, water or oil. Such a cooling step ensures that the formation of intermetallic phases is optimally avoided and that the sputtering target produced by the process has the best possible combination of microstructural and mechanical properties.
[0072] Preferably, the compacting step is effected by sintering at temperatures of from 1100℃ to 1450℃, and the sintering atmosphere is combined with a first gas and / or a vacuum. In a preferred embodiment, both a first gas and vacuum are used in the sintering process. It has been found to be particularly advantageous for the compacting step to be effected by sintering at temperatures of from 1100℃ to 1450℃ in a process according to the present disclosure for producing a W-Ni sputtering target. Here, sintering is a sintering process referred to as pressureless sintering at pressures of less than 2 MPa, preferably at pressures below atmospheric pressure.
[0073] Compaction at these temperatures optimally ensures that solid-phase sintering to very high relative densities takes place in the powder mixture present. At compaction at below 1100℃, the achievable density can be too low, while at temperatures above 1450℃ reductions in the mechanical stability of the target material can occur. In the case of compaction in the temperature range indicated, an optimal combination of high achieved density and optimal mechanical properties is ensured. Due to high Ni content in the produced sputtering target, conventional process is hard to control the O content in low value and to achieve the density under closed-hole condition. The oxygen content can be substantially reduced if the sintering is carried out at a temperature of 1100℃ to 1450℃, and the sintering atmosphere is combined with a first gas and / or a vacuum. The first gas is preferably a mixture of gases predominantly hydrogen, the mixture of gases may, for example, also include argon, but is not limited to this, and may include other suitable gases.
[0074] In a process according to the present disclosure for producing a W-Ni sputtering target, a thermomechanical or thermal treatment of the ingot obtained preferably takes place between the compacting step and the cooling step. Such a thermomechanical or thermal treatment can produce advantageous properties such as a further increase in the density and / or further homogenization of the microstructure.
[0075] Any small proportions of intermetallic phases still present can preferably be distributed homogeneously in the microstructure of the target material and adverse effects of these phases can thus be minimized by means of such a thermomechanical or thermal treatment. This fine distribution ensures uniform ablation without relief formation during sputtering.
[0076] In the process for producing a W / Ni sputtering target, it has been found to be particularly advantageous for a thermomechanical or thermal treatment employed to take place at temperatures in the range from 970℃ to 1450℃.
[0077] A thermomechanical or thermal treatment in the temperature range indicated takes place in the two-phase region W (Ni) +Ni (W) and in the preferred case leads to no or essentially no formation of further undesirable brittle intermetallic phases occurring. In the optimal case, intermetallic phases which can be present after compaction can largely be dissolved by such a thermomechanical or thermal treatment.
[0078] As a result of such substantial avoidance of undesirable brittle intermetallic phases, a W-Ni sputtering target produced by means of a process according to the present disclosure can be shaped particularly well by forming. This in turn simplifies the production of large-format sputtering targets and in particular long and preferably one-piece tubular targets and also has an advantageous effect on the nearness to the final geometry which can be achieved.
[0079] Preferably, the thermomechanical or thermal treatment includes at least one forging step or rolling step.
[0080] A thermomechanical or thermal treatment for the purposes of the present disclosure can be carried out as a single-stage or multistage process. A combination of a plurality of suitable processes is also possible. Thus, a thermomechanical or thermal treatment can contain one or more substeps which comprise no or essentially no deformation of the target material.
[0081] It has been found to be particularly advantageous for a thermomechanical or thermal treatment in a process according to the present disclosure for producing a W-Ni sputtering target to contain at least one rolling step or forging step.
[0082] Defined degrees of deformation can be introduced into the target material in a particularly targeted way by a thermomechanical or thermal treatment containing at least one rolling step or forging step. In this way, excessive strengthening, for example, and consequently exceeding of the deformation forces which can be applied can be avoided thereby.
[0083] Textures can be introduced into the target material in a targeted way by means of a thermomechanical or thermal treatment containing at least one rolling step or forging step and these can in turn exert a positive influence both on the mechanical properties and on the sputtering properties of the target material.
[0084] Furthermore, one or more rolling step (s) or forging step (s) make (s) it possible to vary the thickness of the formed material over its length and set this thickness in a targeted manner.
[0085] In addition, a uniform surface quality which is favourable for further mechanical processing or a further thermomechanical or thermal treatment of the target material, high straightness and good roundness can be achieved by means of rolling or forging.
[0086] Preferably, a sputtering target containing from 55 to 80%by weight of W, a balance of Ni and normal impurities is produced by means of a process according to the present disclosure for producing a sputtering target. In this case, the resulting W-Ni sputtering target by the process of the present disclosure contains a W phase, a Ni (W) solid solution phase, no Ni phase and no or less than 5%by area on average of intermetallic phases measured at a cross section of the target material. Here, the proportion by area is the average proportion by area calculated as arithmetic mean of 5 measurements of the proportion by area measured on 5 image parts having a size of 100×100μm of a metallographic polished section, recorded at 1000×enlargement.
[0087] A process according to the present disclosure for producing a W-Ni sputtering target makes it possible to ensure relative densities of more than 90%, preferably more than 92%, most preferably more than 99.5%in a W-Ni sputtering target produced by this process. The purity and the mechanical properties of the resulting target material are also optimized by a process according to the present disclosure for producing a W-Ni sputtering target.
[0088] Thus, a process according to the present disclosure leads to very low contents of impurities in sputtering targets produced thereby, for example a preferred oxygen content of less than 50 μg / g, particularly preferably less than 40μg / g. The substantial avoidance of formation of brittle intermetallic phases also preferably leads to an optimized hardness of a W-Ni sputtering target produced by means of a process according to the present disclosure.
[0089] Preferably, hardnesses of less than 500 HV10 are achieved by means of a process according to the present disclosure.
[0090] Preferably, an average grain size of the W phase of less than 40μm, more preferably less than 20μm, is achieved by means of a process according to the present disclosure.
[0091] The present disclosure is described below by reference to embodiments.
[0092] Examples
[0093] Example 1:
[0094] W metal powders having a particle size determined by the Fisher method of 4μm and Ni metal powders having a particle size measured by the Fisher method of 4.2μm were used as raw materials. 40 wt. %of Tungsten powder mixed with 60 wt. %Nickel powder in blending machine, mixed for 1 h with 12 rpm rotation speed.
[0095] The powder mixture was introduced into a rubber and the rubber was closed at its open end by means of a rubber cap. The closed rubber was positioned in a cold isostatic press and pressed at a pressure of 200 MPa, 1 min holding time, to give a green block having a relative density of 67%, a thickness of 23 mm, a width of 158 mm and a length of 748 mm.
[0096] The green block then sintered in vacuum with ramp of 3℃ / min to 1350℃, hold at 1350 ℃ for 1 hour, then the sintering atmosphere changed to first gas continue hold for 3 hours, then with cooling with speed of 8℃ / min to 980℃, the sintering atmosphere again changed to H2 gas atmosphere hold for 1 hours, then with cooling speed of 10℃ / min to room temperature. After sintering, the sintered block has a thickness of 20 mm, a width of 144 mm and a length of 665 mm, a relative density of 90.6%and an oxygen content of 23.6μg / g.
[0097] After sintering, the sintered block is machined to the dimension of a thickness of 15 mm, a width of 128 mm and a length of 620 mm. The uniformity of the sputtering target after sintering in Example 1 is very high, wherein its maximum deviation in the percentage of Ni content at different length positions of the sputtering target is only 0.1%-0.3%.
[0098] X-ray fluorescence spectroscopy (XRF) is performed to measure the percentage of Ni content at different lengths of the sintered sputtering target (1 / 4 length, 1 / 2 length and 3 / 4 length, respectively) , and the maximum deviation is calculated. A sputtering target (Comparative Example 5) having 40 wt. %W and 60 wt. %Ni manufactured by the process of WO2015089533A1 is also inspected at the same position for comparison. Validation is based on test results.
[0099] As can be seen, the maximum deviation of Ni-content of the sputtering target manufactured in Example 1 is much lower than the control group, with a very low maximum deviation of only 0.28%, resulting in a very high uniformity of Ni at different positions. In addition, XRD measurement is performed on both Example 1 and Comparative Example 5 separately, and no pure Ni phase is found in the sputtering target manufactured in Example 1, while a localized pure Ni phase is found in the sputtering target manufactured in the control group.
[0100] Fig. 2 left column show the microstructure of Example 1 in an optical light microscope image and in a SEM (scanning electron microscope) image. In the light microscope the Ni (W) solid solution phase appears in light grey color. The pure W-phase appears in patterned dark grey color. The pores (resulting from the powder metallurgical production method) and / or other artefacts (resulting from the preparation) appear in black. In the SEM image the light grey color shows the Ni (W) solid solution phase, pores and / or artefacts appear in black and pure W-phase appears in white color.
[0101] Comparative Example 5 (example prepared by the process of WO2015089533A1-see also Table 1, example 4 of WO2015089533A1) :
[0102] W metal powder having particle size determined by the Fisher method of 4μm and Ni metal powders sieved to a particle size less than 160μm were used as raw materials. 43 wt. %of Tungsten powder was mixed with 57 wt. %Nickel powder in a blending machine. Cold isostatic pressing was carried out at a pressure of 200 MPa to achieve a green block having a diameter of 25 mm and a thickness of 13.5 mm. The green block was then sintered by heating up to 1350℃in 2 hours then holding at that temperature for 4 hours and cooling down in 2 hours. The relative density of the sintered block was 73.7%and the oxygen content was 268μg / g. By XRD measurement intermetallic phases could be detected.
[0103] Example 2:
[0104] W metal powders having a particle size determined by the Fisher method of 4μm and Ni metal powders having a particle size measured by the Fisher method of 4.2μm were used as raw materials. 35 wt. %of Tungsten powder mixed with 65 wt. %Nickel powder in blending machine, mixed for 1h with 12 rpm rotation speed.
[0105] The powder mixture was introduced into a rubber and the rubber was closed at its open end by means of a rubber cap. The closed rubber was positioned in a cold isostatic press and pressed at a pressure of 200 MPa, 1 min holding time, to give a green block having a relative density of 66%, a thickness of 25 mm, a width of 160 mm and a length of 750 mm.
[0106] The green block then sintered in vacuum with ramp of 3℃ / min to 1350℃, hold at 1350 ℃ for 1 hour, then the sintering atmosphere changed to first gas continue hold for 3 hours, then with cooling with speed of 8℃ / min to 980℃, the sintering atmosphere again changed to H2 gas atmosphere hold for 1 hours, then with cooling speed of 10℃ / min to room temperature. After sintering, the sintered block has a thickness of 22 mm, a width of 142 mm and a length of 667 mm, a relative density of 90.8%and an oxygen content of 29.8μg / g. The uniformity of the sputtering target after sintering in Example 2 is very high, wherein its maximum deviation in the percentage of Ni content at different length positions of the sputtering target is only 0.1%-0.3%.
[0107] X-ray fluorescence spectroscopy (XRF) is performed to measure the percentage of Ni content at different lengths of the sintered sputtering target (1 / 4 length, 1 / 2 length and 3 / 4 length, respectively) , and the maximum deviation is calculated. A sputtering target (Comparative Example 6) having 35 wt. %W and 65 wt. %Ni manufactured by the process of WO2015089533A1 is also inspected at the same position for comparison. Validation is based on test results.
[0108] As can be seen, the maximum deviation of Ni-content of the sputtering target manufactured in Example 2 is much lower than the control group, with a very low maximum deviation of only 0.15%, resulting in a very high uniformity of Ni at different positions. In addition, XRD measurement is performed on both Example 2 and Comparative Example 6 separately, and no pure Ni phase is found in the sputtering target manufactured in Example 2, while a localized pure Ni phase is found in the sputtering target manufactured in the control group. In Example 2 no intermetallic phase or pure W could be detected by XRD measurement.
[0109] Fig. 2 middle column show the microstructure of Example 2 in an optical light microscope image and in a SEM (scanning electron microscope) image. In the light microscope the Ni (W) solid solution phase appears in light grey color. The pores (resulting from the powder metallurgical production method) and / or other artefacts (resulting from the preparation) appear in black. No pure W-phase is shown in this image. In the SEM image the light grey color shows the Ni (W) solid solution phase, pores and / or artefacts appear in black. Although a pure W-phase in white color is shown in this image, no W-phase could be detected in an XRD of this Example, i.e., W-phase is below the detection limit.
[0110] Comparative Example 6 (example prepared by the process of WO2015089533A1) :
[0111] W metal powder having particle size determined by the Fisher method of 4μm and Ni metal powders sieved to a particle size of less than 160μm were used as raw materials. 35 wt. %of Tungsten powder was mixed with 65 wt. %Nickel powder in a blending machine. Cold isostatic pressing was carried out at a pressure of 200 MPa to achieve a green block having a diameter of 25 mm and a thickness of 14.1 mm. The green block was then sintered by heating up to 1350℃for 2 hours then holding at that temperature for 4 hours and cooling down in 2 hours. The relative density of the sintered block was 85.2%and the oxygen content was 82μg / g.
[0112] Example 3:
[0113] W metal powders having a particle size determined by the Fisher method of 4μm and Ni metal powders having a particle size measured by the Fisher method of 4.2μm were used as raw materials. 30 wt. %of Tungsten powder mixed with 70 wt. %Nickel powder in blending machine, mixed for 1 h with 12 rpm rotation speed.
[0114] The powder mixture was introduced a rubber and the rubber was closed at its open end by means of a rubber cap. The closed rubber was positioned in a cold isostatic press and pressed at a pressure of 200 MPa, 1 min holding time, to give a green block having a relative density of 67%, and a dimension of
[0115] The green block was then sintered in vacuum with a ramp of 3℃ / min to 1350℃, held at 1350℃ for 1 hour, then the sintering atmosphere changed to first gas continued hold for 3 hours, then with cooling with a speed of 8℃ / min to 980℃, the sintering atmosphere again changed to H2 gas atmosphere hold for 1 hours, then with cooling speed of 10℃ / min to room temperature. The size of the green block after sintering has a length of a relative density of 92%and an oxygen content of 32μg / g. The uniformity of the sputtering target after sintering in Example 3 is very high, wherein its maximum deviation in the percentage of Ni content at different length positions of the sputtering target is only 0.1%-0.3%.
[0116] X-ray fluorescence spectroscopy (XRF) is performed to measure the percentage of Ni content at different lengths of the sintered sputtering target (1 / 4 length, 1 / 2 length and 3 / 4 length, respectively) , and the maximum deviation is calculated. A sputtering target (Comparative Example 7) having 30 wt. %W and 70 wt. %Ni manufactured by the process of WO2015089533A1 is also inspected at the same position for comparison. Validation is based on test results.
[0117] As can be seen, the maximum deviation of Ni-content of the sputtering target manufactured in Example 3 is much lower than the control group, with a very low maximum deviation of only 0.15%, resulting in a very high uniformity of Ni at different positions. In addition, XRD measurement is performed on both Example 3 and Comparative Example 7 separately, and no pure Ni phase is found in the sputtering target manufactured in Example 3, while a localized pure Ni phase is found to in the sputtering target manufactured in the control group. In Example 3 no intermetallic phase or pure W could be detected by XRD measurement.
[0118] Fig. 2 right column shows the microstructure of Example 3 in an optical light microscope image and in a SEM (scanning electron microscope) image. In the light microscope the Ni (W) solid solution phase appears in light grey color. The pores (resulting from the powder metallurgical production method) and / or other artefacts (resulting from the preparation) appear in black. No pure W-phase is detectable in this image. In the SEM image the light grey color shows the Ni (W) solid solution phase, pores and / or artefacts appear in black. Although a small pure W-phase in white color is shown in this image, no W-phase could be detected in an XRD of this Example, i.e., W-phase is below the detection limit.
[0119] Comparative Example 7 (example prepared by the process of WO2015089533A1) :
[0120] W metal powder having particle size determined by the Fisher method of 4μm and Ni metal powders sieved to a particle size of less than 160μm were used as raw materials. 30 wt. %of Tungsten powder was mixed with 70 wt. %Nickel powder in a blending machine. Cold isostatic pressing was carried out at a pressure of 200 MPa to achieve a green block having a diameter of 25 mm and a thickness of 14.6 mm. The green block was then sintered by heating up to 1350℃for 2 hours then holding at that temperature for 4 hours and cooling down in 2 hours. The relative density of the sintered block was 85.7%and the oxygen content was 120μg / g.
[0121] Example 4
[0122] W metal powders having a particle size determined by the Fisher method of 4μm and Ni metal powders having a particle size measured by the Fisher method of 4.2μm were used as raw materials. 35 wt. %of Tungsten powder mixed with 65 wt. %Nickel powder in blending machine, mixed for 1h with 12 rpm rotation speed.
[0123] The powder mixture was introduced into a rubber and the rubber was closed at its open end by means of a rubber cap. The closed rubber was positioned in a cold isostatic press and pressed at a pressure of 200 MPa, 1 min holding time, to give a green block having a thickness of 22 mm. The green block was then sintered in vacuum with a ramp of 3℃ / min to 1350℃, held at 1350 ℃ for 1 hour, then the sintering atmosphere changed to first gas continued hold for 3 hours, then with cooling with a speed of 8℃ / min to 980℃, the sintering atmosphere again changed to H2 gas atmosphere hold for 1 hours, then with cooling speed of 10℃ / min to room temperature. After sintering, the sintered block has a thickness of 22 mm, a width of 142 mm and a length of 667 mm. After sintering, a 2-pass rolling is carried out to obtain a thickness of 15mm. The rolled block is then annealed at 1300℃ for half an hour, and again 2-pass rolled to obtain a thickness of 10mm. Then processed with a flattening machine, and finally annealed at 1200℃for half an hour. After annealing, a cooling rate of at least 34 K / min was achieved in the temperature range from 900 to 750℃. The relative density of the green block after this process is 99.8%and the oxygen content is 15.9μg / g.
[0124] The process for producing a sputtering target according to the second aspect of the present disclosure, effectively solves the technical problem of reducing the homogeneity of the material and affecting the sputtering effect, thus the sputtering target has a high density and good application performance.
[0125] Fig. 3A shows the microstructure of Example 4 in an optical microscope image wherein the orientation of the grains as well as the high density of the material is shown.
[0126] Fig. 3B shows the microstructure of Example 4 in an optical light microscope image and in a SEM (scanning electron microscope) image. In the light microscope, the Ni (W) solid solution phase appears in light grey color. Almost no pores are shown in this image due to the high density of this material. No pure W-phase is detectable in this image. The SEM image shows the orientation of the grains in the longitudinal direction. One single pure W-grain can still be found in this image–however this is below the detection level of XRD.
[0127] Also in this Example 4, no pure Ni, no pure W and no intermetallic phases can be detected.
[0128] Pure Ni can interfere with the proper operation of magnetron sputtering due to its ferromagnetic nature, that is the reason why the technical solution recited in WO2015089533A1 utilizes a W-Ni ratio with a lower Ni content. At the same time, it is generally recognized in the art that, if there is a necessity to increase the homogeneity of the elemental distribution of the material, the content of the desired alloying element needs to be reduced, i.e., to increase the homogeneity of the distribution of Ni requires a further reduction in the content of Ni.
[0129] However, the inventors of the present disclosure have found that, in their research, if the content of Ni is further reduced in accordance with the existing understanding, the following problem arises, that is, the W-Ni phase, which acts as the second phase, leads to an uneven distribution of Ni element content in various parts of the target material due to the low Ni phase region.
[0130] The present disclosure adopts a technical solution contrary to WO2015089533A1 by using a higher Ni content, but such solution leads to the following problems: 1) the high Ni content may lead to the generation of magnetism due to the production of pure Ni phase of the material, which is unfavorable to magnetron sputtering, and 2) due to the stronger oxygen affinity of the Ni element, it may lead to an increase of the oxygen content in the material. In other words, it is difficult to achieve the result of pure Ni phase-free material for W-Ni targets with high Ni content, and how to control the generation of pure Ni phase becomes a technical challenge to be overcome. The inventors of the present disclosure are able to effectively solve the technical problem of reducing the uniformity of the material and affecting the sputtering effect, thus the sputtering effect has a high density and good application performance, precisely overcoming the above technical difficulties by the improved technology documented in the above mentioned first embodiment and second embodiment.
[0131] The sputtering target and the process for producing the sputtering target according to the present disclosure effectively solve the technical problem of reducing the homogeneity of the material and affecting the sputtering effect, and have a high density and good application performance.
[0132] Although the present disclosure has been illustrated and described by reference to specific preferred embodiments of the present disclosure, it should be appreciated by those of ordinary skill in the art that various modifications can be made thereto in form and detail without departing from the spirit and scope of the present disclosure.
Claims
1.A sputtering target, containing from 55%to 80%by weight of Ni, a balance of W and normal impurities, characterized in that the sputtering target contains a W phase, a Ni (W) solid solution phase, no pure Ni phase and no or less than 5%by area on average of intermetallic phases measured at a cross section of the target material.2.The sputtering target according to claim 1, characterized in that, the sputtering target comprises 60%to 70%by weight of Ni.3.The sputtering target according to claim 2, characterized in that, the sputtering target comprises 60%to 65%by weight of Ni.4.The sputtering target according to any one of claims 1 to 3, characterized in that, the sputtering target comprises an oxygen content of less than 50μg / g.5.The sputtering target according to claim 4, characterized in that, the sputtering target comprises an oxygen content of less than 40μg / g.6.The sputtering target according to any one of claims 1 to 5, characterized in that, the sputtering target has a hardness of less than 500 HV10.7.The sputtering target according to any one of claims 1 to 6, characterized in that, the intermetallic phase is one or more selected from the group consisting of Ni4W, WNi or W2Ni.8.The sputtering target according to any one of claims 1 to 7, characterized in that, the sputtering target has an average grain size of the W phase of less than 40μm.9.The sputtering target according to any one of claims 1 to 8, characterized in that, the sputtering target has a relative density of more than 90%.10.The sputtering target according to claim 9, characterized in that, the sputtering target has a relative density of more than 99.5%.11.A process for producing a sputtering target according to any of claims 1 to 10 using a powder-metallurgical route, characterized in that the process comprises the following steps:carrying out a compacting step in which a powder mixture of W powder and Ni powder is compacted by application of pressure, heat, or pressure and heat to get a compacted blank; andcarrying out a cooling step in which the compacted blank is cooled at a cooling rate of greater than 3 K / min to a temperature range of from 750℃ to 1000℃.12.The process for producing a sputtering target according to claim 11, characterized in that, the compacting step is effected by sintering at temperatures of from 1100℃ to 1450℃, and the sintering atmosphere is combined with a first gas and / or a vacuum.13.A process for producing a sputtering target according to any of claims 1 to 10 using a powder-metallurgical route, characterized in that the process comprises the following steps:carrying out a compacting step in which a powder mixture of W powder and Ni powder is compacted by application of pressure, heat, or pressure and heat to get a compacted blank;performing a thermomechanical or thermal treatment of the compacted blank after the compacting step andcarrying out a cooling step in which the compacted blank is cooled at a cooling rate of greater than 30 K / min to at least in a temperature range from 900℃ to 750℃.14.The process for producing a sputtering target according to claim 13, characterized in that, the compacting step is effected by sintering at temperatures of from 1100℃ to 1450℃, and the sintering atmosphere is combined with a first gas and / or a vacuum.15.The process for producing a sputtering target according to claim 13 or 14, characterized in that, the process further comprises:performing the thermomechanical or thermal treatment at temperatures in a range of from 970℃ to 1450℃.16.The process for producing a sputtering target according to claim 14, characterized in that,the thermomechanical or thermal treatment includes at least one forging step or rolling step.
Citation Information
Patent Citations
W-ni sputter target
WO2015089533A1
Ni-W BASED SINTERED TARGET MATERIAL
JP2009155722A
Method for Producing Sputtering Target Material for Ni-W Based Interlayer
US20090022614A1
Process for producing and using a w-ni sputtering target
US20210246544A1
Cited By
Method for detecting number of inclusions in alloy powder
CN120253388A