Biaxially stretched polypropylene film
The biaxially oriented polypropylene film with controlled surface characteristics addresses the issues of uneven surface roughness and adhesion, enhancing voltage resistance and yield by ensuring uniform thermal history and adhesion, thus stabilizing film formation and improving high-temperature performance.
Patent Information
- Application Number
- PCT/JP2024/009622
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-03-12
- Publication Date
- 2024-10-24
AI Technical Summary
Biaxially oriented polypropylene films used in capacitors for electric vehicles and hybrid vehicles face issues with uneven surface roughness and adhesion during the stretching process, leading to local differences in thermal history, non-uniform plasticity, and reduced voltage resistance, which affects their stability and yield.
A biaxially oriented polypropylene film with specific surface characteristics, including an average maximum elliptical spot length of 3.0 mm or less, a difference in protruding peak height of 0.040 μm or less, and a controlled slow axis angle range, is developed to ensure uniform thermal history and adhesion, enhancing voltage resistance and yield.
The solution stabilizes film formation, improves voltage resistance, particularly at high temperatures, and increases the yield rate by ensuring uniform plasticity and adhesion, reducing the risk of film breakage and electric field concentration.
Smart Images

Figure JP2024009622_24102024_PF_FP_ABST
Abstract
Description
Biaxially oriented polypropylene film
[0001] The present invention relates to a biaxially oriented polypropylene film and the like.
[0002] Polypropylene films have excellent electrical properties, such as high voltage resistance and low dielectric loss, as well as high moisture resistance. Therefore, they are widely used in electronic and electrical devices. Specifically, they are used as films for filter capacitors and smoothing capacitors in power conversion circuits, such as high-voltage capacitors, converters, and inverters.
[0003] In particular, in recent years, polypropylene films have begun to be widely used as capacitors for inverter power supplies that control drive motors of electric vehicles, hybrid vehicles, etc. Capacitors for inverter power supplies used in automobiles, etc., are required to be small, lightweight, high-capacity, and highly reliable over a long period of time.
[0004] In Patent Document 1, the protrusion is 0.1 mm 2 Patent Document 1 discloses a biaxially oriented polypropylene film for capacitors, in which the number of particles per square meter and the 10-point average roughness satisfy a predetermined relationship. Patent Document 1 describes the effects of the biaxially oriented polypropylene film for capacitors having the above-mentioned configuration, such as excellent processability even for a thin film, and high voltage resistance even under a wide range of ambient temperature conditions from low (-40°C) to high (150°C).
[0005] International Publication No. 2013 / 146367
[0006] Polypropylene films used as resin films for capacitors in electric vehicles, hybrid vehicles, etc., are required to have thinner film thicknesses and larger electrode areas due to the recent trend toward smaller capacitor sizes and higher capacities. Furthermore, in recent years, there has been a strong demand for further cost reductions, and methods for producing films using high-speed stretch molding of resin sheets have been investigated. Furthermore, there is a demand for capacitor elements that have high voltage resistance (particularly high voltage resistance at high temperatures) with high yields.
[0007] Therefore, an object of the present invention is to provide a polypropylene film that can be stably produced for a longer period of time and has a higher voltage resistance (particularly voltage resistance at high temperatures) and a higher yield rate.
[0008] The present inventors have discovered the following in the course of their research.
[0009] Since the polypropylene film used in the above applications is thin and flexible, its stretched precursor cast sheet is also thin and flexible. When such a cast sheet is continuously transported, air bubbles are easily trapped between the sheet and the transport roll. In such cases, the sheet adheres unevenly to the roll, and the non-adhered portions appear as oval depressions on the surface of the sheet.
[0010] The conveying rolls are heated to induce β-crystals on the surface of the cast sheet and to impart plasticity to the sheet before stretching. If the above-mentioned elliptical depressions are scattered on the surface of the sheet, the adhesion state of these areas to the conveying rolls differs from that of other areas, resulting in differences in the formation of β-crystals and the roughening state during stretching. In such cases, elliptical spots appear scattered on the film surface.
[0011] If the difference in surface roughness between the "spots" and other areas becomes large, the film tends to break during transverse stretching. This is thought to be because if there are areas within the sheet that have been formed with different thermal histories, the plasticity of the resin during transverse stretching becomes locally uneven, inducing stretching breakage of the film.
[0012] Furthermore, in practical use, the spots tend to reduce the voltage resistance of the capacitor element and significantly reduce the yield. It is thought that if there are local differences in surface roughness within the sheet surface, local differences in interlayer adhesion will occur within the wound metallized polypropylene film, and the film will be damaged by electric field concentration.
[0013] Based on the above findings, the present inventors have conducted further research and have found that the above-mentioned problems can be solved by a biaxially oriented polypropylene film having a first surface and a second surface, in which the average maximum length of the approximately elliptical spots on the first surface is 3.0 mm or less, and the difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk within the spots is 0.040 μm or less.
[0014] Item 1. A biaxially oriented polypropylene film having a first surface and a second surface, wherein the average maximum length of substantially elliptical spots on the first surface is 3.0 mm or less, and the difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk within the spots is 0.040 μm or less.
[0015] Item 2. The biaxially oriented polypropylene film according to Item 1, wherein the difference between the average protruding valley depth Rvk outside the spots and the average protruding valley depth Rvk within the spots is 0.020 μm or less.
[0016] Item 3. The biaxially stretched polypropylene film according to Item 1, wherein the change range of the slow axis angle is in the range of 0.3° to 2.8°.
[0017] Item 4. The biaxially oriented polypropylene film according to Item 1, wherein the average number of approximately elliptical spots per 11.5 mm x 8.6 mm area on the first surface is 0.6 or less.
[0018] Item 5. The biaxially oriented polypropylene film according to Item 1, wherein the polypropylene resin constituting the biaxially oriented polypropylene film has a weight average molecular weight Mw of 250,000 or more and 450,000 or less, a ratio of the weight average molecular weight Mw to the number average molecular weight Mn (Mw / Mn) of 5.0 or more and 12.0 or less, a melt flow rate at 230°C under a load of 2.16 kg of 7.0 g / 10 min or less, and a heptane insoluble content of 96.0% or more and 99.5% or less.
[0019] Item 6. The biaxially oriented polypropylene film according to Item 1, having a thickness of 1.7 μm or more and 6.5 μm or less.
[0020] Item 7. The biaxially oriented polypropylene film according to Item 1, which is a monolayer film.
[0021] Item 8. The biaxially oriented polypropylene film according to any one of Items 1 to 7, which is for use in a capacitor.
[0022] Item 9. A metal layer-integrated polypropylene film comprising the biaxially oriented polypropylene film according to any one of items 1 to 7 and a metal layer disposed on one or both sides of the biaxially oriented polypropylene film.
[0023] Item 10. A capacitor comprising the metal layer-integrated polypropylene film according to Item 9.
[0024] Item 11. A method for producing the biaxially oriented polypropylene film according to any one of Items 1 to 7, comprising obtaining a cast sheet using a casting drum having a microcracked surface in which, when an imaginary line 0.1 mm long is formed at any position on the surface in the width direction, 1 to 15 grooves intersect with the imaginary line and the groove width is 1 μm to 10 μm, and biaxially stretching the cast sheet.
[0025] According to the present invention, it is possible to provide a polypropylene film which can be stably produced for a longer period of time and has a higher voltage resistance (particularly voltage resistance at high temperatures) and a higher yield rate.
[0026] A photograph of a typical approximately elliptical spot is shown. The major and minor axes of the typical spot are indicated. For the typical spot, the measurement points of the protruding peak height Rpk and the protruding valley depth Rvk within the spot are indicated by circles.
[0027] In this specification, the expressions "contain" and "comprise" include the concepts of "contain," "comprise," "consist essentially of," and "consist only of."
[0028] In this specification, ranges in which the upper and / or lower limits are arbitrarily interchanged between multiple ranges based on the ranges consisting of the upper and / or lower limits described for each parameter are also exemplified.
[0029] 1. Biaxially oriented polypropylene film In one aspect, the present invention relates to a biaxially oriented polypropylene film having a first surface and a second surface, wherein the average maximum length of substantially elliptical spots on the first surface is 3.0 mm or less, and the difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk within the spots is 0.040 μm or less (sometimes referred to as the "polypropylene film of the present invention" in this specification). This is described below.
[0030] The polypropylene film of the present invention has two main surfaces, one of which is a first surface and the other of which is a second surface. The first surface is the surface onto which a metal layer is laminated when a capacitor is fabricated.
[0031] The average maximum length of the approximately elliptical spots on the first surface of the polypropylene film of the present invention is 3.0 mm or less (property 1).
[0032] The "speckles" in relation to characteristic 1 are visible on an image obtained by the measurement method described below, and are regions whose roughening degree and / or roughened surface shape differ from those of the surrounding area. The maximum length (major axis) of the speckles can be, for example, 10 mm or less, 8 mm or less, 7 mm or less, 6 mm or less, or 5 mm or less.
[0033] Furthermore, in a preferred embodiment of the present invention, from the viewpoint of further improving the film formation stability and / or the yield rate of products with higher voltage resistance, it is preferable that the average number of approximately elliptical spots per 11.5 mm x 8.6 mm area of the first surface is 0.6 or less.
[0034] The method for measuring the average number of spots and the average maximum length of spots is as follows.
[0035] From the center position in the width direction of each biaxially stretched polypropylene film to be measured, 50 mm x 50 mm measurement samples were cut out at a total of 10 locations, 10 m apart in the longitudinal direction. Next, using a digital microscope (Keyence Corporation Digital Microscope VHX-2000), a lens magnification of 30x, light intensity of 50% of the full range, measurement method: reflection measurement, field of view: 11.5 mm x 8.6 mm, one side of each measurement sample (the side on which the metal layer will be laminated during capacitor fabrication) was observed in "halation removal + sharpening mode (a process that enhances the color and emphasizes the contours and removes glare)" and the number of approximately elliptical "spots" observed within the field of view (a representative example is shown in Figure 1) was counted. Note that if some of the spots do not fit within the field of view, the spots were not counted. The number of spots in the field of view of each measurement sample (10 in total) is added up, and the resulting total is divided by 10 (= the number of measurement samples) to determine the average number of elliptical spots per field of view (11.5 mm x 8.6 mm area). For each spot measured above, the longitudinal and lateral diameters of the biaxially oriented polypropylene film are measured, and the longer diameter (the major diameter of the spot) is taken as the maximum length of the spot (in the representative example shown in Figure 2, the lateral diameter is the major diameter). The maximum lengths of each spot are added up, and the resulting total is divided by the number of spots to determine the average maximum length of the spots.
[0036] The average number of spots is preferably 0 or more and 0.3 or less, more preferably 0 or more and 0.1 or less, and particularly preferably 0, from the viewpoints of film formation stability, yield rate, etc.
[0037] From the viewpoint of film formation stability, yield rate, etc., the average maximum length of the spots is preferably 0 mm or more and 1.0 mm or less, more preferably 0 mm or more and 0.5 mm or less, and particularly preferably 0 mm (= the average number of spots is 0).
[0038] The difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk inside the spots of the polypropylene film of the present invention is 0.040 μm or less (characteristic 2).
[0039] The method for measuring the difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk inside the spots is as follows.
[0040] The peak height Rpk of one side of the biaxially oriented polypropylene film (the side on which the metal layer is laminated during capacitor fabrication) is measured using a non-contact optical interference surface profiler, VertScan 2.0 (model: R5500GML) manufactured by Ryoka Systems Co., Ltd. First, using WAVE mode, a 530 white filter and a 1×BODY lens barrel are applied, and a ×10 objective lens is used to measure 470.92 μm × 353.16 μm per field of view.
[0041] Within the spots, for each of the spots counted using the method for measuring the number of spots described above, measurements are taken at five locations shown in Figure 3 (the intersection of the long axis and the short axis, the center of the line connecting one end of the long axis to the intersection, the center of the line connecting the other end of the long axis to the intersection, the center of the line connecting one end of the short axis to the intersection, and the center of the line connecting the other end of the short axis to the intersection).
[0042] For the areas outside the spots, measurements are taken at the center of each measurement sample cut out using the method for measuring the number of spots described above.
[0043] The obtained data is subjected to noise removal processing using a median filter (3 x 3), and then subjected to Gaussian filter processing with a cutoff value of 30 μm to remove waviness components. This makes it possible to properly measure the condition of the measurement surface. Next, analysis is performed using the "VS-Viewer" analysis software of "VertScan 2.0", and the average value of the peak height Rpk, a lubricity evaluation parameter, obtained at the above locations is calculated. Specifically, this is as follows.
[0044] The measured values of the protruding peak height Rpk within the spots are summed up, and the resulting sum is divided by X (= number of measured spots × 5 (measurement points within one spot)) to determine the average protruding peak height Rpk within the spots.
[0045] The measured values of the protruding peak height Rpk outside the spots of each measurement sample are summed up, and the resulting sum is divided by 10 (=number of measurement samples) to determine the average protruding peak height Rpk outside the spots.
[0046] The average protruding peak height Rpk within the spots is subtracted from the average protruding peak height Rpk outside the spots to obtain the difference between them.
[0047] The difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk inside the spots is preferably 0 μm or more and 0.030 μm or less, more preferably 0 μm or more and 0.010 μm or less, and particularly preferably 0 μm, from the viewpoints of film formation stability, yield rate, etc. Note that when the average number of spots is 0, the difference is 0 μm.
[0048] The average height Rpk of the protruding peaks outside the spots (= the average height Rpk of the protruding peaks of the film when the average number of spots is 0) is preferably 0.010 μm or more and 0.095 μm or less, more preferably 0.015 μm or more and 0.090 μm or less, and even more preferably 0.020 μm or more and 0.085 μm or less, from the viewpoint of the high temperature durability of the capacitor element, etc.
[0049] When the average number of spots exceeds 0, the average protruding peak height Rpk within the spots is preferably 0.003 μm or more and 0.095 μm or less, more preferably 0.005 μm or more and 0.090 μm or less, and even more preferably 0.010 μm or more and 0.085 μm or less, from the viewpoints of film formation stability, yield rate, etc.
[0050] The combination of Property 1 and Property 2 described below can further improve film formation stability and the yield rate of films with higher voltage resistance. While not limiting, the reasons for this are believed to be as follows. If Property 1 and Property 2 are satisfied, the thermal history of the cast sheet, which is the stretching precursor, is thought to be appropriately uniform during the film production process. As a result, the plasticity during transverse stretching is also thought to be uniform, and film breakage is thought to be suppressed. Furthermore, when capacitors are produced using such films, capacitors with high voltage resistance can be efficiently obtained with a high yield. Capacitors produced using such films are thought to have appropriately uniform voids between film layers within the capacitor, making it less likely for electric field concentration to occur due to localized interlayer adhesion. This is thought to suppress film damage due to localized heat generation within the capacitor, thereby achieving the effects described above.
[0051] From the viewpoint of further improving the film-forming stability and / or the yield rate of films having a higher voltage resistance, it is preferable that the difference between the average protruding valley depth Rvk outside the spots and the average protruding valley depth Rvk within the spots of the polypropylene film of the present invention is 0.020 μm or less. The difference is more preferably 0 μm or more and 0.015 μm or less, even more preferably 0 μm or more and 0.010 μm or less, and particularly preferably 0 μm. Note that the difference is 0 μm when the average number of spots is 0. Although a restrictive interpretation is not desired, by setting the difference within the above range, leakage current is less likely to occur from locally thin portions, and plasticity during transverse stretching is also uniformed, which is thought to result in further improvement of the film-forming stability and / or the yield rate of films having a higher voltage resistance.
[0052] The method for measuring the difference between the average protruding valley depth Rvk outside the spots and the average protruding valley depth Rvk inside the spots is similar to the method for measuring the difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk inside the spots described above.
[0053] The measured values of the protruding valley depth Rvk within the spots are summed up, and the resulting sum is divided by X (= number of measured spots × 5 (measurement points within one spot)) to determine the average protruding valley depth Rvk within the spots.
[0054] The measured values of the protruding valley depth Rvk outside the spots of each measurement sample are summed up, and the resulting sum is divided by 10 (= number of measurement samples) to determine the average protruding valley depth Rvk outside the spots.
[0055] The average protruding valley depth Rvk within the spots is subtracted from the average protruding valley depth Rvk outside the spots to obtain the difference between them.
[0056] The average protruding valley depth Rvk outside the spots (= the average protruding valley depth Rvk of the film when the average number of spots is 0) is preferably 0.005 μm or more and 0.060 μm or less, more preferably 0.010 μm or more and 0.050 μm or less, and even more preferably 0.015 μm or more and 0.040 μm or less, from the viewpoint of high temperature durability of the capacitor element, etc.
[0057] When the average number of spots exceeds 0, the average protruding valley depth Rvk within the spots is preferably 0.001 μm or more and 0.045 μm or less, more preferably 0.002 μm or more and 0.040 μm or less, and even more preferably 0.003 μm or more and 0.035 μm or less, from the viewpoints of film formation stability and reducing the number of insulation defects.
[0058] From the viewpoint of further improving the film formation stability and / or the yield rate of films with higher voltage resistance, the polypropylene film of the present invention has a 10 m insulation defect test when a DC voltage of 600 V per 1 μm of thickness is applied using an insulation defect inspection device having an unwinding-winding mechanism. 2 It is preferable that the number of insulation defects per 10 m is 1.0 or less. More preferably, the number is 0 / 10 m. 2 More than 0.5 pieces / 10m 2 Less than or equal to 0 pieces / 10m, more preferably 2 More than 0.1 piece / 10m 2 Below, particularly preferably 0 pieces / 10 m 2Although we do not wish to limit the interpretation, capacitors made using such films are unlikely to suffer damage to the film due to short circuiting even when used for long periods of time in high-temperature environments, and can achieve high reliability.
[0059] The method for measuring the number of insulation defects is as follows.
[0060] Using an insulation defect inspection device with an unwinding-winding mechanism, the number of insulation defects (number / 10 m) of the biaxially oriented polypropylene film to be measured was measured. 2 The polypropylene film to be measured is passed through a high-voltage electrode and a grounded metal roller, and a DC voltage is applied while the film is running. The number of discharges that occur at insulation defects is counted with a counter attached to the device. The number of measured defects is divided by the measurement area to determine the number of insulation defects (numbers / 10m) in the film. 2 The measurement conditions are as follows: Distance between the high-voltage electrode and the earthed metal roller: 50 μm Contact angle between the film and the earthed metal roller: 120° Shape of the high-voltage electrode: metal plate with a thickness of 4 mm and the same width as the metal roller Unwinding speed: 20 m / min DC voltage: 600 V / μm Measurement area: 472 m 2 -Test environment temperature: 20°C.
[0061] From the viewpoint of further improving film formation stability and / or the yield rate of films with higher voltage resistance, the polypropylene film of the present invention preferably has a change range of the slow axis angle of 0.3° to 2.8°, more preferably 0.3° to 2.0°, even more preferably 0.3° to 1.5°, and still more preferably 0.3° to 1.0°.
[0062] The slow axis angle of a biaxially stretched polypropylene film refers to the acute angle formed between the width direction of the biaxially stretched polypropylene film and the slow axis. The polypropylene film of the present invention is stretched in two axes, a first direction and a second direction perpendicular to the first direction. The biaxial stretching orients the polymer in-plane, resulting in the biaxially stretched film having birefringence. The direction in the film plane where the refractive index is maximum is called the slow axis because it is the direction in which light travels slowly (the phase is delayed).
[0063] In the sequential biaxial stretching method, a cast raw sheet is first stretched in the machine direction (MD), and then the sheet is stretched in the transverse direction (TD). In this case, the refractive index of the slow axis of the biaxially stretched polypropylene film in the transverse direction of the second direction tends to be larger than the refractive index of the slow axis of the first direction. In this case, the transverse direction of the second direction becomes the slow axis.
[0064] In the case of transverse direction (TD) stretching, when the film is completely stretched in the transverse direction (when the film is completely stretched in the direction perpendicular to the machine direction), the slow axis angle defined in this specification is 0°. However, in reality, shrinkage stress, external mechanical force, thermoplasticity of the film, etc. act during stretching, making it impossible to completely stretch the film in the transverse direction (TD), and the slow axis angle tends to be larger than 0°.
[0065] In areas where the change in the slow axis angle in the longitudinal direction is large, stretching is non-uniform, making the film prone to distortion. In practice, this non-uniformity in stretching tends to reduce the voltage resistance performance of the capacitor and significantly reduce yield. This is thought to be because, when stretching in the longitudinal direction is non-uniform, dimensional changes within the capacitor exposed to high temperatures become non-uniform, causing localized interlayer adhesion and electric field concentration, which results in film damage. It is thought that controlling the change in the slow axis angle in the longitudinal direction to a range of 0.3° to 2.8° can suppress the above-mentioned problems in the longitudinal direction.
[0066] The method for measuring the variation range of the slow axis angle and the average slow axis angle is as follows.
[0067] From the center of the biaxially stretched polypropylene film to be measured, 50 mm x 50 mm measurement samples are cut out at 10 m intervals in the longitudinal direction, at a total of 10 locations (0 m, 10 m, 20 m, 30 m, 40 m, 50 m, 60 m, 70 m, 80 m, and 90 m positions). Next, the width direction of the measurement sample is set to 0°, and the acute angle formed by the width direction of the measurement sample and the slow axis is measured as the slow axis angle. Among the 10 measurement samples, the difference between the maximum and minimum values of the slow axis angle is defined as the "variation range," and the average value is calculated as the "average slow axis angle." The measurement device and measurement conditions are as follows.
[0068] Measuring device: Retardation measuring device RE-100 manufactured by Otsuka Electronics Co., Ltd. Light source: laser light emitting diode (LED) Band pass filter: 550 nm (measurement wavelength) Measurement interval: 0.1 sec Number of integrations: 10 times Number of measurement points: 15 points Gain: 10 dB Measurement environment: temperature 23°C, humidity 60%.
[0069] From the viewpoint of the yield rate in film production, the average slow axis angle is preferably 0° or more and 20° or less, more preferably 0° or more and 15° or less, and even more preferably 0° or more and 13° or less.
[0070] The thickness of the polypropylene film of the present invention is preferably 6.5 μm or less, more preferably 5.5 μm or less, even more preferably 3.5 μm or less, particularly preferably 3.0 μm or less, and most preferably 2.8 μm or less, from the viewpoint of further improving the miniaturization and high capacity of the capacitor when used in a capacitor. Furthermore, from the viewpoint of production, the lower limit is preferably 0.8 μm or more, more preferably 1.0 μm or more, even more preferably 1.7 μm or more, and particularly preferably 2.0 μm or more. Furthermore, keeping the thickness within the above range is also preferable from the viewpoint of film formation stability and / or the yield rate of products with higher voltage resistance. The method for measuring the thickness of the biaxially oriented polypropylene film in this specification is the same as that described in the Examples.
[0071] The layer structure of the polypropylene film of the present invention is not particularly limited. The polypropylene film of the present invention may be a single layer consisting of one layer, or may be a multi-layer film having the same or different compositions. The polypropylene film of the present invention is preferably a film consisting of one or more film-like molded layers, and more preferably a single-layer film (a film consisting of one film-like molded layer).
[0072] The polypropylene film of the present invention is not particularly limited in terms of its constituent material, as long as it contains a polypropylene resin. Examples of polypropylene resins include propylene homopolymers such as isotactic polypropylene, propylene-ethylene copolymers, long-chain branched polypropylenes, and ultra-high molecular weight polypropylenes. Among these, isotactic polypropylene is preferred from the viewpoint of heat resistance.
[0073] The content of the polypropylene resin is preferably 90% by mass or more, more preferably 95% by mass or more, based on the total mass of the polypropylene film of the present invention (when the total mass of the polypropylene film is 100% by mass). The upper limit of the content of the polypropylene resin is, for example, 100% by mass, 98% by mass, etc., based on the total mass of the polypropylene film of the present invention.
[0074] The polypropylene resin may be one type alone or a combination of two or more types.
[0075] When the polypropylene film of the present invention contains two or more polypropylene resins, the polypropylene resin with the greater content is referred to herein as the "main polypropylene resin." When the polypropylene film of the present invention contains only one polypropylene resin, the polypropylene resin is referred to herein as the "main polypropylene resin."
[0076] Hereinafter, in this specification, when the term "polypropylene resin" is used without specifying whether it is the main component or not, it refers to both the polypropylene resin as the main component and polypropylene resins other than the main component unless otherwise specified. For example, when it is stated that "the weight average molecular weight Mw of the polypropylene resin is preferably 250,000 or more and 450,000 or less," it means both that the weight average molecular weight Mw of the polypropylene resin as the main component is preferably 250,000 or more and 450,000 or less, and that the weight average molecular weight Mw of the polypropylene resin other than the main component is preferably 250,000 or more and 450,000 or less.
[0077] The weight-average molecular weight (Mw) of the polypropylene resin is preferably 250,000 or more and 450,000 or less, more preferably 250,000 or more and 420,000 or less, even more preferably 250,000 or more and 400,000 or less, and even more preferably 260,000 or more and 390,000 or less, from the viewpoint of thickness uniformity, mechanical properties, and thermo-mechanical properties of the biaxially oriented polypropylene film. By using such a polypropylene resin, dielectric breakdown of the film is suppressed, making it easier to obtain an extremely thin biaxially oriented polypropylene film suitable for small, high-capacity capacitors. When two or more polypropylene resins are used, it is preferable to use a polypropylene resin (preferably a polypropylene resin as the main component) having an Mw of 250,000 or more and less than 330,000 (preferably 250,000 or more and 300,000 or less, more preferably 260,000 or more and 290,000 or less) in combination with a polypropylene resin (preferably a polypropylene resin other than the main component) having an Mw of 330,000 or more and 450,000 or less (preferably 350,000 or more and 420,000 or less, more preferably 370,000 or more and 400,000 or less, even more preferably 370,000 or more and 390,000 or less).
[0078] The ratio of the weight average molecular weight Mw to the number average molecular weight Mn (Mw / Mn) of the polypropylene resin is preferably 5.0 or more and 12.0 or less, more preferably 5.0 or more and 10.0 or less, and even more preferably 5.0 or more and 9.0 or less, from the viewpoint of obtaining appropriate resin fluidity during biaxial stretching and facilitating the production of an extremely thin biaxially stretched propylene film without thickness unevenness. When two or more polypropylene resins are used, it is preferable to use a polypropylene resin (preferably a polypropylene resin as the main component) having the above ratio of 5.0 or more and less than 7.0 (preferably 5.0 or more and 6.5 or less) in combination with a polypropylene resin (preferably a polypropylene resin other than the main component) having the above ratio of 7.0 or more and 12.0 or less (preferably 7.5 or more and 10.0 or less, more preferably 7.5 or more and 9.0 or less).
[0079] The weight average molecular weight Mw and number average molecular weight Mn of the polypropylene resin are measured by the method described in the examples.
[0080] The melt flow rate (MFR) of the polypropylene resin at 230°C and a load of 2.16 kg is not particularly limited, but is preferably 7.0 g / 10 min or less from the viewpoint of stretchability, etc., and more preferably 0.5 g / 10 min to 6.0 g / 10 min from the viewpoint of improving the thickness precision of the polypropylene film of the present invention. When two or more polypropylene resins are used, it is preferable to use a polypropylene resin (preferably a polypropylene resin as a main component) having an MFR of 4.0 g / 10 min to less than 7.0 g / 10 min (preferably 4.5 g / 10 min to 6.5 g / 10 min, more preferably 5.0 g / 10 min to 6.0 g / 10 min) in combination with a polypropylene resin (preferably a polypropylene resin other than the main component) having an MFR of 0.5 g / 10 min to less than 4.0 g / 10 min (preferably 1.0 g / 10 min to 3.5 g / 10 min, more preferably 1.5 g / 10 min to 3.0 g / 10 min). The melt flow rate of the polypropylene resin is measured by the method described in the Examples.
[0081] The heptane insoluble fraction (HI) of the polypropylene resin is preferably 96.0% or more and 99.5% or less, and more preferably 97.0% or more and 99.0% or less. Here, the higher the heptane insoluble fraction, the higher the stereoregularity of the resin. By using such a polypropylene resin, the crystallinity is appropriately improved, and the initial voltage resistance and long-term voltage resistance are improved. The heptane insoluble fraction (HI) is measured by the method described in the Examples.
[0082] The content of the polypropylene resin as the main component is preferably more than 50% by mass and 100% by mass or less, more preferably 55% by mass or more and 85% by mass or less, even more preferably 60% by mass or more and 75% by mass or less, and still more preferably 60% by mass or more and 70% by mass or less, relative to 100% by mass of the polypropylene resin.
[0083] The polypropylene resin can be produced by a generally known polymerization method, such as a gas phase polymerization method, a bulk polymerization method, or a slurry polymerization method.
[0084] The polymerization may be a single-stage polymerization using one polymerization reactor or a multi-stage polymerization using two or more polymerization reactors. The polymerization may be carried out by adding hydrogen or a comonomer as a molecular weight modifier to the reactor.
[0085] The catalyst used in the polymerization can be a commonly known Ziegler-Natta catalyst, and is not particularly limited as long as it can produce the polypropylene resin. The catalyst may contain a co-catalyst component or a donor. By adjusting the catalyst and polymerization conditions, it is possible to control the molecular weight, molecular weight distribution, stereoregularity, etc.
[0086] The molecular weight distribution of the polypropylene resin can be adjusted by resin blending. For example, two or more resins having different molecular weights or molecular weight distributions can be mixed. Generally, a two-polypropylene blend in which the main resin accounts for 55% by mass to 90% by mass of a resin having a higher or lower average molecular weight than the main resin, assuming the total resin content to be 100% by mass, is preferred because it is easy to adjust the amount of low molecular weight components.
[0087] When the above-mentioned mixing and adjusting method is adopted, the melt flow rate (MFR) may be used as a measure of the average molecular weight. In this case, it is preferable that the difference in MFR between the main resin and the additive resin is about 1 to 30 g / 10 min from the viewpoint of convenience during adjustment.
[0088] The method for mixing the resins is not particularly limited, and examples thereof include a method in which polymer powders or pellets of the main resin and the additive resin are dry-blended using a mixer or the like, and a method in which polymer powders or pellets of the main resin and the additive resin are fed to a kneader and melt-kneaded to obtain a blended resin.
[0089] The mixer and the kneader are not particularly limited. The kneader may be a single-screw type, a twin-screw type, or a multi-screw type having two or more screws. In the case of a twin or more screw type, the kneader may be either a co-rotating or counter-rotating type.
[0090] In the case of blending by melt kneading, the kneading temperature is not particularly limited as long as a good kneaded product is obtained. Generally, the temperature is in the range of 200°C to 300°C, and from the viewpoint of suppressing resin deterioration, 230°C to 270°C is preferred. To suppress deterioration during resin kneading and mixing, an inert gas such as nitrogen may be purged into the kneader. The melt-kneaded resin may be pelletized to an appropriate size using a commonly known granulator. This allows mixed polypropylene raw material resin pellets to be obtained.
[0091] Use of the above polypropylene resin makes it easier to adjust the film properties as described above, and is also preferable from the viewpoint of film formation stability and / or yield rate of films with higher voltage resistance.
[0092] The polypropylene film of the present invention may contain an additive. The "additive" is not particularly limited as long as it is an additive generally used in polypropylene resins.
[0093] Examples of the additives include antioxidants, light stabilizers, UV absorbers, plasticizers, lubricants, crosslinking agents, flame retardants, antistatic agents, heat resistance improvers, antiblocking agents, inorganic particles, resin particles, etc. The polypropylene resin may contain the additives in an amount that does not adversely affect the polypropylene film of the present invention (for example, 10% by mass or less, 5% by mass or less, 1% by mass or less, or 0.1% by mass or less, relative to 100% by mass of the polypropylene film of the present invention).
[0094] 2. Method for Producing Biaxially Stretched Polypropylene Film Biaxially oriented polypropylene films can be produced by obtaining a cast sheet, which corresponds to a stretched precursor, from resin pellets and then biaxially stretching the cast sheet. As will be apparent from the results of the examples described later, the biaxially oriented polypropylene film of the present invention can be obtained by controlling the microcracks on the casting drum surface, the air knife blowing air speed, the distance between the air knife outlet and the cast sheet, the stretching nip roll temperature, the stretching nip roll hardness, etc., specifically by producing the film according to the following method.
[0095] Among the above-mentioned production conditions, microcracks on the casting drum surface are an important condition. From this viewpoint, in one aspect, the present invention relates to a method for producing the biaxially oriented polypropylene film of the present invention, which comprises obtaining a cast sheet using a casting drum having a microcracked surface, in which, when an imaginary line 0.1 mm long is formed at any position on the surface in the width direction, 1 to 15 grooves intersect with the imaginary line, and the groove width is 1 μm to 10 μm, and subjecting the cast sheet to a biaxial stretching treatment.
[0096] The method for producing the biaxially oriented polypropylene film of the present invention will be described in detail below.
[0097] 2-1. Production of Cast Sheets Cast sheets can be molded using known methods. For example, polypropylene resin pellets, dry-mixed polypropylene resin pellets, or mixed polypropylene resin pellets prepared in advance by melt-kneading are fed into an extruder, heated and melted, passed through a filter to remove foreign matter and modified polymers, extruded into a sheet form from a T-die, and cooled and solidified on at least one metal drum (casting drum), thereby forming a cast sheet.
[0098] In the extruder, polypropylene resin is degraded to some extent by thermal degradation and oxidative degradation. To prevent such polymer degradation, the resin temperature during melt extrusion is 170°C or higher and 320°C or lower, preferably 200°C or higher and 300°C or lower. Degradation can also be prevented by nitrogen substitution in the extruder, screw shape, internal shape of the T-die during casting, amount of antioxidant added, etc.
[0099] The temperature of the casting drum is preferably maintained at 80° C. or higher and 140° C. or lower, and more preferably at 90° C. or higher and 105° C. or lower. The β-crystal fraction of the cast sheet obtained in this temperature range is approximately 5% or higher and 20% or lower as measured by X-ray analysis. Within this β-crystal fraction range, the roughness of the film surface is appropriately improved, and both capacitor characteristics and element winding processability can be satisfied.
[0100] The surface of the casting drum is not particularly limited, but rolls with an uneven surface, such as a sandblast roll or a ceramic roll, or a microcrack roll with an entrained air exhaust channel are preferred, as they can easily achieve the desired physical properties of the present invention. Methods for manufacturing these rolls are known, and for example, microcrack rolls can be manufactured according to or in accordance with the method described in Japanese Patent No. 6,974,939. Microcracks are generated by stress in the metal plating layer, and their shape and number can be controlled by the thickness of the metal plating layer, plating conditions, heat treatment, chemical treatment, multilayering, etc. For example, in the case of chrome plating, the plating thickness is preferably 100 μm to 400 μm, more preferably 120 μm to 350 μm, and even more preferably 150 μm to 300 μm. This range makes it easier to control the shape and number of grooves and makes it less likely for cracks to occur when the roll is heated.
[0101] With regard to the microcrack roll, when a virtual line 0.1 mm long is formed in the width direction at any position on the roll surface, it is preferable that 1 to 15 grooves intersect with the virtual line, more preferably 2 to 10 grooves, and even more preferably 3 to 8 grooves. Furthermore, the groove width is preferably 1 μm to 10 μm, more preferably 2 μm to 9 μm, and even more preferably 3 μm to 8 μm. By using a roll with the above-mentioned number of grooves and groove width ranges, air that infiltrates between the casting drum and the cast sheet is appropriately discharged, facilitating close transport even with a thinned cast sheet, making it easy to obtain an extremely thin biaxially oriented polypropylene film. Furthermore, even when the forming speed of the thinned cast sheet is increased, the phenomenon of wavy cast sheet thickness, known as draw resonance (surging), is less likely to occur, and an extremely thin biaxially oriented polypropylene film with a uniform thickness in the longitudinal direction can be easily obtained.
[0102] The method for adhering the sheet to the casting drum may be any of the air knife method, touch roll method, electrostatic application method, water-cooled casting method, etc., but the air knife method is preferred because it is easy to adjust the sheet adhesion and can be handled simply.
[0103] When an air knife is used, the wind speed of the blown air is preferably 70 m / s or more and 130 m / s or less, more preferably 80 m / s or more and 120 m / s or less, and even more preferably 90 m / s or more and 110 m / s or less. The distance between the air knife outlet and the cast sheet is preferably 2 mm or more and 5 mm or less, more preferably 2 mm or more and 4 mm or less. Using an air knife within this range allows the thin-film resin extruded into a sheet form from the T-die to be adequately adhered to the casting drum, and suppresses film vibration of the molten resin from the T-die outlet until it adheres to the casting drum. As a result, the above-mentioned film properties can be easily obtained.
[0104] The biaxially stretched polypropylene film of the present invention can be obtained by biaxially stretching the cast sheet in the longitudinal and transverse directions. Examples of the stretching method include simultaneous and sequential biaxial stretching methods, but sequential biaxial stretching is preferred from the viewpoint of stably uniforming the thickness and increasing the mechanical strength of the film.
[0105] In the sequential biaxial stretching method, it is preferable to first preheat the cast sheet by passing it through a conveying roll maintained at 70° C. or higher and 135° C. or lower, preferably 80° C. or higher and 130° C. or lower, and then, immediately before stretching in the longitudinal direction, to heat it to 130° C. or higher and 155° C. or lower, preferably 140° C. or higher and 150° C. or lower. By heating the cast sheet in this manner, excessive thermal expansion of the cast sheet is suppressed, the flatness of the sheet is easily maintained before stretching in the longitudinal direction described below, and the sheet is easily brought into uniform contact with the conveying roll.
[0106] From the viewpoint of easily obtaining the biaxially stretched polypropylene film of the present invention, a method of simultaneously heating both the front and back sides of the cast sheet immediately before longitudinal stretching is preferred. The method is not particularly limited, but from the viewpoint of suppressing the difference in thermal history within the surface of the cast sheet, a method of heating the stretching nip rolls or a method of heating by electromagnetic radiation is preferred. From the viewpoint of simultaneously fixing the cast sheet immediately before stretching and adjusting the temperature of the sheet, a method of heating the stretching nip rolls is more preferred.
[0107] When the stretching nip rolls are heated, the temperature of the stretching nip rolls is preferably 95°C or higher and 170°C or lower, more preferably 100°C or higher and 150°C or lower, from the viewpoint of suppressing the difference in thermal history between the front and back surfaces of the cast sheet.
[0108] When the stretching nip roll is heated, the rubber hardness of the roll is preferably 40° or more and 80° or less, more preferably 50° or more and 70° or less, so that the shape of the roll surface follows the shape of the cast sheet surface.
[0109] Thereafter, the film is stretched in the longitudinal direction by 3 to 7 times, preferably 4 to 6 times, and immediately cooled to room temperature.
[0110] After stretching in the longitudinal direction, the stretched film is introduced into a tenter, where both ends are held with clips heated to 80°C or higher and 140°C or lower, and the film is preheated to a temperature of 140°C or higher and 185°C or lower, preferably 150°C or higher and 175°C or lower, and then stretched in the width direction at a temperature of 140°C or higher and 170°C or lower, preferably 150°C or higher and 160°C or lower, by a magnification of 6 to 12 times, preferably 8 to 11 times.
[0111] The film is then relaxed, heat-set, and wound up. The wound up film is then aged in an atmosphere of 20° C. to 45° C., and can then be cut to a desired product width.
[0112] 3. Metal Layer-Integrated Polypropylene Film In one aspect, the present invention also provides a metal layer-integrated polypropylene film (sometimes referred to herein as the "metal layer-integrated polypropylene film of the present invention") comprising the biaxially oriented polypropylene film of the present invention and a metal layer disposed on one or both sides of the biaxially oriented polypropylene film. The metal layer-integrated polypropylene film of the present invention will be described in detail below. A capacitor obtained by winding the metal layer-integrated polypropylene film of the present invention has excellent initial voltage resistance and long-term durability under high temperature and high voltage conditions.
[0113] The polypropylene film of the present invention can be provided with an electrode on one or both sides for processing into a capacitor. The type of electrode is not particularly limited as long as the capacitor intended by this embodiment can be obtained, and any electrode typically used for manufacturing capacitors can be used. Examples of electrodes include metal foil, paper with at least one side metallized, and plastic film.
[0114] Since capacitors are increasingly required to be small and lightweight, it is preferable to form electrodes by directly metallizing one or both sides of the polypropylene film of the present invention. The metal to be used may be, for example, a single metal such as zinc, lead, silver, chromium, aluminum, copper, or nickel, or a mixture or alloy of two or more of these metals. However, taking into consideration the environment, economy, and capacitor performance, zinc and aluminum are preferred.
[0115] Examples of methods for directly metallizing the surface of a polypropylene film include vacuum deposition and sputtering, and are not particularly limited as long as the capacitor intended by this embodiment can be obtained. From the viewpoints of productivity and economy, vacuum deposition is preferred. Examples of vacuum deposition methods include the crucible method and the wire method, but are not particularly limited as long as the capacitor intended by this embodiment can be obtained, and the most appropriate method can be selected as appropriate.
[0116] From the viewpoint of the electrical characteristics of the capacitor, the film resistance of the metal vapor deposition film is preferably 1 Ω / □ or more and 100 Ω / □ or less. A higher value within this range is desirable from the viewpoint of self-healing characteristics, and from the viewpoint of safety, the film resistance is more preferably 5 Ω / □ or more and 50 Ω / □ or less, and even more preferably 10 Ω / □ or more and 30 Ω / □ or less. The film resistance of the metal vapor deposition film can be measured during metal vapor deposition, for example, by a four-terminal method known to those skilled in the art. The film resistance of the metal vapor deposition film can be adjusted, for example, by adjusting the output of the evaporation source to adjust the amount of evaporation.
[0117] When forming a metal vapor-deposited film on one side of the film, a certain width from one end of the film is left undeposited, forming an insulating margin, so that the film will become a capacitor when wound. Furthermore, to strengthen the bond between the metal layer-integrated polypropylene film of the present invention and the metallikon electrode, it is preferable to form a heavy edge structure on the end opposite the insulating margin, and the film resistance of the heavy edge is usually 1 Ω / □ to 8 Ω / □, preferably 1 Ω / □ to 5 Ω / □. The thickness of the metal film is not particularly limited, but is preferably 1 nm to 200 nm.
[0118] There are no particular restrictions on the margin pattern of the metal vapor deposition film to be formed, but from the viewpoint of improving the characteristics of the capacitor, such as safety, it is preferable to use a pattern including a so-called special margin, such as a fishnet pattern, a T-margin pattern, etc. Forming a metal vapor deposition film on one side of a polypropylene film in a pattern including a special margin improves the safety of the resulting capacitor and is also effective in preventing breakdown and short circuits of the capacitor, and is therefore preferable.
[0119] The margin can be formed by any known method without any limitation, such as a tape method in which masking is performed with tape during vapor deposition, or an oil method in which masking is performed by applying oil.
[0120] The metal layer-integrated polypropylene film of the present invention can be processed into the capacitor of the present invention described below by wrapping the film along its longitudinal direction. That is, two metal layer-integrated polypropylene films of the present invention are stacked and wound together so that the metal layer and the polypropylene film are alternately laminated. Then, a pair of metallikon electrodes is formed on both end surfaces by metal spraying to produce a film capacitor, thereby obtaining the capacitor.
[0121] 4. Capacitor In one aspect, the present invention provides a capacitor including the metal layer-integrated polypropylene film of the present invention (sometimes referred to as the "capacitor of the present invention" in this specification). The capacitor of the present invention will be described in detail below.
[0122] In the process of producing a capacitor, a film winding process is performed. For example, two pairs of metal layer-integrated polypropylene films of the present invention are overlapped and wound so that the metal layers and polypropylene films in the metal layer-integrated polypropylene film of the present invention are alternately stacked and the insulating margins are on opposite sides. In this case, it is preferable to stack the two pairs of metal layer-integrated polypropylene films of the present invention with a 1 to 2 mm offset. The winding machine used is not particularly limited, and for example, an automatic winding machine 3KAW-N2 manufactured by Kaito Seisakusho Co., Ltd. can be used.
[0123] When manufacturing flat capacitors, the resulting roll is usually pressed after winding. This press tightens the capacitor and forms the element. To control and stabilize the interlayer gap, the optimum pressure to be applied varies depending on the thickness of the polypropylene film, but is typically 2 to 20 kg / cm.
[0124] Next, a metal is sprayed onto both end surfaces of the wound body to form metallikon electrodes, completing the capacitor. The capacitor is then subjected to a predetermined heat treatment. In this embodiment, this process includes a step of heat treating the capacitor in a vacuum at a temperature of 80 to 125°C for at least one hour (hereinafter referred to as "thermal aging").
[0125] In the above-mentioned process of subjecting the capacitor to heat treatment, the heat treatment temperature is 80°C or higher and 130°C or lower, preferably 90°C or higher and 125°C or lower. Heat treatment at this temperature provides the effect of thermal aging. Specifically, the gaps between the films constituting the capacitor based on the metal layer-integrated polypropylene film of the present invention are reduced, corona discharge is suppressed, and the internal structure of the metal layer-integrated polypropylene film of the present invention changes, promoting crystallization. This is thought to result in improved voltage resistance. If the heat treatment temperature is lower than the specified temperature, the above-mentioned effects of thermal aging cannot be fully achieved. On the other hand, if the heat treatment temperature is higher than the specified temperature, the polypropylene film may experience thermal decomposition, oxidative degradation, or the like.
[0126] The method for subjecting the capacitor to heat treatment may be appropriately selected from known methods including, for example, a method using a thermostatic bath under a vacuum atmosphere, a method using high-frequency induction heating, etc. Specifically, it is preferable to employ a method using a thermostatic bath.
[0127] The heat treatment time is preferably 1 hour or more, more preferably 10 hours or more, from the viewpoint of achieving mechanical and thermal stability, but more preferably 20 hours or less, from the viewpoint of preventing molding defects such as heat wrinkles and molding. Lead wires are usually welded to the metallikon electrodes of the capacitor that has been subjected to heat aging. Furthermore, to impart weather resistance, particularly to prevent humidity degradation, the capacitor is preferably encapsulated in a case and potted with epoxy resin. The capacitor of the present invention is a small, large-capacity capacitor based on the metal layer-integrated polypropylene film of the present invention, and has initial voltage resistance and long-term durability under high temperature and high voltage.
[0128] The capacitor of the present invention, which utilizes the polypropylene film of the present invention, can be suitably used in high-temperature environments and can be small and have a high capacity (for example, a capacitance of 5 μF or more, preferably 10 μF or more, more preferably 20 μF or more, even more preferably 30 μF or more, and particularly preferably 40 μF or more. The upper limit of the capacitance is not particularly limited, and can be, for example, 100 μF, 80 μF, 70 μF, or 60 μF). Therefore, the capacitor of the present invention can be used as a high-voltage capacitor, a filter capacitor, a smoothing capacitor, etc., used in electronic devices and electrical equipment, etc., for various switching power supplies, converters, inverters, etc. Furthermore, the capacitor of the present invention can also be suitably used as an inverter capacitor, a converter capacitor, etc., which control the drive motor of electric vehicles and hybrid vehicles, etc., which have seen increasing demand in recent years.
[0129] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples.
[0130] (1) Measurement of Resin Properties (1-1) Measurement of Weight Average Molecular Weight (Mw), Number Average Molecular Weight (Mn), and Molecular Weight Distribution (Mw / Mn) of Polypropylene Resin Using GPC (gel permeation chromatography) under the following conditions, the weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) of the polypropylene resin used as a raw material in the examples and comparative examples were measured.
[0131] Specifically, a high-temperature GPC system with a built-in differential refractometer (RI), model HLC-8121GPC-HT, manufactured by Tosoh Corporation, was used. Three TSKgel GMHHR-H (20) HT columns manufactured by Tosoh Corporation were connected together and used. Measurements were performed at a column temperature of 140°C, with trichlorobenzene as the eluent at a flow rate of 1.0 ml / min. A calibration curve was prepared using standard polystyrene manufactured by Tosoh Corporation, and the measured molecular weight values were converted to polystyrene values to obtain the weight-average molecular weight (Mw) and number-average molecular weight (Mn). The molecular weight distribution (Mw / Mn) was obtained using these Mw and Mn values.
[0132] (1-2) Measurement of heptane insoluble matter (HI) The polypropylene resin used as a raw material in the examples and comparative examples was press-molded to a size of 10 mm x 35 mm x 0.3 mm to prepare a measurement sample of approximately 3 g. Next, approximately 150 mL of heptane was added, and Soxhlet extraction was performed for 8 hours. The heptane insoluble matter was calculated from the sample mass before and after extraction.
[0133] (1-3) Measurement of Melt Flow Rate (MFR) The melt flow rate (MFR) of the polypropylene resin used as a raw material in the Examples and Comparative Examples in the form of raw material resin pellets was measured using a melt indexer manufactured by Toyo Seiki Co., Ltd. in accordance with JIS K 7210, Condition M. Specifically, a 4 g sample was first inserted into a cylinder at a test temperature of 230°C and preheated for 3.5 minutes under a load of 2.16 kg. The weight of the sample extruded from the bottom hole over 30 seconds was then measured, and the MFR (g / 10 min) was calculated. The above measurement was repeated three times, and the average value was used as the measured MFR.
[0134] (2) Preparation of Casting Drums Casting drums A to E were prepared as metal drums (casting drums) used when producing sheets (cast sheets) to be subjected to biaxial stretching treatment in the manufacturing process of biaxially stretched polypropylene films.
[0135] At any position on the surface of the casting drum, a virtual line 0.1 mm long was drawn in the width direction, and the number of grooves intersecting the virtual line and the average groove width were measured. Specifically, the measurements were performed as follows. A total of 12 locations were observed: four locations in the circumferential direction of the casting drum (at 0, 90, 180, and 270 degrees clockwise) and three locations in the width direction (at 10 (one end), 50 (center), and 90 (one end) of a face length of 100). A virtual line 0.1 mm long was drawn in the width direction at the center of the image, and the number of grooves intersecting the virtual line and the average groove width were measured and calculated.
[0136] The number of grooves and groove width are shown in Table 1.
[0137]
[0138] (3) Production of Biaxially Stretched Polypropylene Film Biaxially oriented polypropylene films were produced according to the production conditions in Table 2. The thickness of the biaxially oriented polypropylene films was measured using a micrometer (JIS-B7502) in accordance with JIS-C2330.
[0139] Example 1 Polypropylene resin A (Mw = 270,000, Mw / Mn = 5.7, heptane insolubles = 97.8%, MFR = 5.6 g / 10 min, manufactured by Prime Polymer) and polypropylene resin B (Mw = 380,000, Mw / Mn = 8.3, heptane insolubles = 98.8%, MFR = 2.3 g / 10 min, manufactured by Daehan Oil & Chemical) were fed to an extruder in a mass ratio of A:B = 65:35 and melted at a resin temperature of 230 ° C. After that, foreign matter and modified polymers were removed using a filter installed in the middle of the polymer tube, and the extruded material was extruded using a T-die and solidified by wrapping around a casting drum maintained at a surface temperature of 92 ° C. A cast sheet having a thickness of 0.1 mm was produced at a speed of 60 m / min. The casting drum used was A in Table 1.
[0140] To adhere the sheet to the casting drum, an air knife was used, the blown air speed was 110 m / s, and the distance between the air knife outlet and the cast sheet was 3 mm.
[0141] The obtained cast sheet was preheated to a temperature of 130°C, sandwiched between a conveying roll heated to 145°C and a stretching nip roll with a rubber hardness of 70° heated to 110°C, stretched 5 times in the longitudinal direction, and immediately returned to room temperature.
[0142] The stretched film was then introduced into a tenter, held at both ends with clips at 110°C, preheated to 170°C, stretched 10 times in the width direction at a temperature of 155°C, and then relaxed and heat-set, and a biaxially stretched polypropylene film with a thickness of 2.3 μm was taken up in a roll.
[0143] Example 2 A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that in the production of the cast sheet, the distance between the air knife outlet and the sheet was set to 5 mm.
[0144] Example 3 A biaxially oriented polypropylene film was obtained in the same manner as in Example 2, except that in the production of the cast sheet, the air velocity of the air blown out of the air knife was set to 70 m / sec.
[0145] Example 4 A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that in the production of the cast sheet, the casting drum was changed to B in Table 1.
[0146] Example 5 A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that in the production of the cast sheet, the casting drum was changed to C in Table 1.
[0147] Example 6 A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that in the production of the cast sheet, the casting drum was E in Table 1, the wind speed of the air blown out of the air knife was 130 m / s, the distance between the air knife outlet and the sheet was 2 mm, and in the longitudinal stretching treatment, the temperature of the stretching nip rolls was 130°C.
[0148] Example 7 A biaxially oriented polypropylene film was obtained in the same manner as in Example 6, except that the rubber hardness of the stretching nip rolls was set to 50° in the longitudinal stretching treatment.
[0149] <Example 8> A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that in the production of the cast sheet, the casting drum was D in Table 1, the air knife blowing speed was 70 m / sec, and the distance between the air knife outlet and the sheet was 5 mm.
[0150] Example 9 A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that the thickness of the finally wound biaxially oriented polypropylene film was 1.8 μm.
[0151] Example 10 A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that the thickness of the finally wound biaxially oriented polypropylene film was set to 6 μm.
[0152] Example 11 A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that in the production of the cast sheet, the resin supplied to the extruder was changed to A.
[0153] Comparative Example 1 The procedure for producing a cast sheet was the same as in Example 1, except that the air velocity of the air blown from the air knife was set to 140 m / s. In this case, the air from the air knife entered between the resin extruded into a sheet form from the T-die and the casting drum, and film vibration of the molten resin from the T-die outlet until it came into close contact with the casting drum became significant, making it impossible to produce a biaxially stretched film.
[0154] <Comparative Example 2> A biaxially oriented polypropylene film was obtained in the same manner as in Example 4, except that in the production of the cast sheet, the air blown from the air knife was at a speed of 70 m / s and the distance between the air knife outlet and the sheet was 5 mm.
[0155] <Comparative Example 3> A biaxially oriented polypropylene film was obtained in the same manner as in Example 5, except that in the production of the cast sheet, the air blown out from the air knife was at a speed of 70 m / s and the distance between the air knife outlet and the sheet was 5 mm.
[0156] Comparative Example 4 A biaxially oriented polypropylene film was obtained in the same manner as in Example 6, except that the temperature of the stretching nip rolls was set to 90° C. in the longitudinal stretching treatment.
[0157] Comparative Example 5 A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that the thickness of the finally wound biaxially oriented polypropylene film was 1.6 μm.
[0158] <Comparative Example 6> A biaxially stretched polypropylene film was obtained in the same manner as in Example 12, except that in the longitudinal stretching treatment, the temperature of the stretching nip rolls was 90°C and the hardness of the stretching nip rolls was 50°.
[0159]
[0160] (4) Measurement of biaxially stretched polypropylene film characteristics (4-1) Measurement of spots From the center position in the width direction of each biaxially stretched polypropylene film of the examples and comparative examples, 50 mm x 50 mm measurement samples were cut out at a total of 10 locations every 10 m in the longitudinal direction. Next, using a digital scope (Keyence Corporation Digital Microscope VHX-2000), lens magnification: 30x, light intensity: 50% of full range, measurement method: reflection measurement, field of view: 11.5 mm x 8.6 mm, one side of each measurement sample (the side on which the metal layer is laminated during capacitor production) was observed in "halation removal + sharp mode (a process that enhances the color and emphasizes the contours and removes glare)," and the number of approximately elliptical "spots" observed within the field of view (a representative example is shown in Figure 1) was counted. Note that if some of the spots did not fit within the field of view, the spots were not counted. The number of spots in the field of view of each measurement sample (10 in total) was totaled, and the total value obtained was divided by 10 (= number of measurement samples) to determine the average number of oval spots per field of view (11.5 mm x 8.6 mm area).
[0161] For each of the spots measured above, the longitudinal and lateral diameters of the biaxially oriented polypropylene film were measured, and the longer diameter (the major diameter of the spot) was taken as the maximum length of the spot (in the representative example shown in Figure 2, the major diameter is the lateral diameter). The maximum lengths of each spot were summed, and the resulting sum was divided by the number of spots to determine the average maximum length of the spots.
[0162] (4-2) Measurement of protruding peak height Rpk and protruding valley depth Rvk Using a non-contact optical interference surface profiler manufactured by Ryoka Systems Co., Ltd., "VertScan 2.0 (model: R5500GML)", the protruding peak height Rpk and protruding valley depth Rvk of one side (the surface on which the metal layer is laminated during capacitor production) of the biaxially oriented polypropylene film of the examples and comparative examples were measured. First, using WAVE mode, a 530 white filter and a 1x BODY lens barrel were applied, and a x10 objective lens was used to measure 470.92 μm x 353.16 μm per field of view.
[0163] Within the spots, for each of the spots measured in (4-1) above, measurements were taken at five locations shown in Figure 3 (the intersection of the long axis and the short axis, the center of the line connecting one end of the long axis and the intersection, the center of the line connecting the other end of the long axis and the intersection, the center of the line connecting one end of the short axis and the intersection, and the center of the line connecting the other end of the short axis and the intersection).
[0164] Outside the spots, measurements were taken at the center of each measurement sample.
[0165] The obtained data was subjected to noise removal processing using a median filter (3 x 3), and then subjected to Gaussian filter processing with a cutoff value of 30 μm to remove waviness components. This made it possible to properly measure the state of the measurement surface. Next, analysis was performed using the "VS-Viewer" analysis software of "VertScan 2.0," and the average values of the protruding peak height Rpk and protruding valley depth Rvk obtained at the above locations were calculated for the lubricity evaluation parameters. Specifically, this is as follows.
[0166] The measured values of the protruding peak height Rpk within the spots were summed up, and the resulting sum was divided by X (= number of measured spots × 5 (measurement points within one spot)) to determine the average protruding peak height Rpk within the spots.
[0167] The measured values of the protruding peak height Rpk outside the spots of each measurement sample were summed up, and the obtained total value was divided by 10 (= number of measurement samples) to determine the average protruding peak height Rpk outside the spots.
[0168] The difference between the average protruding peak height Rpk within the spots and the average protruding peak height Rpk outside the spots was calculated by subtracting them.
[0169] The average protruding peak height Rpk of the film was determined by adding the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk inside the spots and dividing the resulting value by 2. When the average number of spots was 0, the average value measured at the center of each measurement sample was determined as the average protruding peak height Rpk of the film.
[0170] The measured values of the protruding valley depth Rvk within the spots were summed up, and the obtained sum was divided by X (= number of measured spots × 5 (measurement points within one spot)) to determine the average protruding valley depth Rvk within the spots.
[0171] The measured values of the protruding valley depth Rvk outside the spots of each measurement sample were summed up, and the resulting sum was divided by 10 (= number of measurement samples) to determine the average protruding valley depth Rvk outside the spots.
[0172] The average protruding valley depth Rvk within the spots was subtracted from the average protruding valley depth Rvk outside the spots to determine the difference between them.
[0173] The average protruding valley depth Rvk of the film was determined by adding the average protruding valley depth Rvk outside the spots and the average protruding valley depth Rvk inside the spots and dividing the resulting value by 2. When the average number of spots was 0, the average value measured at the center of each measurement sample was determined as the average protruding valley depth Rvk of the film.
[0174] (4-3) Measurement of the number of insulation defects Using an insulation defect inspection device with an unwinding-winding mechanism, the number of insulation defects (number / 10 m) of the biaxially oriented polypropylene films of the examples and comparative examples was measured. 2 The polypropylene film to be tested was passed between a high-voltage electrode and a grounded metal roller, and the film was run while a DC voltage was applied. The number of discharges occurring at the insulation defects was counted using a counter attached to the device. The number of measured defects was divided by the measured area to determine the number of insulation defects (numbers / 10 m 2 The measurement conditions were as follows: Distance between the high-voltage electrode and the earthed metal roller: 50 μm; Angle of contact between the film and the earthed metal roller: 120°; Shape of the high-voltage electrode: Metal plate with a thickness of 4 mm and the same width as the metal roller; Unwinding speed: 20 m / min; DC voltage: 600 V / μm; Measurement area: 472 m 2 -Test environment temperature: 20°C.
[0175] (4-4) Measurement of Slow Axis Angle and Slow Axis Angle Change Range 50 mm x 50 mm measurement samples were cut out from the center of each biaxially stretched polypropylene film of the Examples and Comparative Examples at 10 m intervals in the longitudinal direction, for a total of 10 locations (0 m, 10 m, 20 m, 30 m, 40 m, 50 m, 60 m, 70 m, 80 m, and 90 m positions). Next, the width direction of the measurement sample was set to 0°, and the acute angle formed between the width direction of the measurement sample and the slow axis was measured as the slow axis angle. The difference between the maximum and minimum values of the slow axis angle among the 10 measurement samples was calculated as the "change range." The measurement apparatus and measurement conditions were as follows:
[0176] Measuring device: Retardation measuring device RE-100 manufactured by Otsuka Electronics Co., Ltd. Light source: laser light emitting diode (LED) Band pass filter: 550 nm (measurement wavelength) Measurement interval: 0.1 sec Number of integrations: 10 times Number of measurement points: 15 points Gain: 10 dB Measurement environment: temperature 23°C, humidity 60%.
[0177] (4-5) Measurement Results The measurement results of the properties of the biaxially oriented polypropylene film are shown in Table 3.
[0178]
[0179] (5) Evaluation of processability Production of the biaxially stretched films of the Examples and Comparative Examples was started, and the time until the film broke due to stretching (the time during which film production was possible continuously) was measured from the time when the resulting film thickness reached the target thickness (Table 2) ±2%. The time when the thickness reached the target thickness ±2% was measured and confirmed using the thickness measurement method described in (3) above. Based on the obtained time, the processability was evaluated according to the following evaluation criteria. The results are shown in Table 4 below. A++: Film production was possible even after 48 hours without stretching fracture. A+: Film production was possible after more than 32 hours but less than 48 hours without stretching fracture. A: Film production was possible after more than 24 hours but less than 32 hours without stretching fracture. B: Film production was possible after more than 16 hours but less than 24 hours without stretching fracture. C: Stretching fracture occurred after more than 8 hours but less than 16 hours. D: Stretching fracture occurred in less than 8 hours. E: Film production was not possible.
[0180] (6) Evaluation of Voltage Resistance Capacitors were produced using the biaxially stretched films of the Examples and Comparative Examples, and the voltage resistance of the capacitors was evaluated.
[0181] (6-1) Preparation of Capacitor Using a vacuum deposition machine manufactured by ULVAC Corporation, the measurement sample obtained in (4-1) above was subjected to aluminum deposition in a T-margin deposition pattern at a deposition resistance of 20 Ω / □, thereby obtaining a metallized film containing a metal film on one side of a biaxially stretched polypropylene film.
[0182] After slitting to a width of 50 mm, two sheets of metallized film were placed together and wound 840 turns using an automatic winder, Model 3KAW-N2, manufactured by Kaito Manufacturing Co., Ltd., at a winding tension of 210 g. The wound element was then heat-treated at 120°C for 15 hours while being pressed, after which zinc metal was sprayed onto the element end faces to obtain a flat capacitor. Lead wires were soldered to the end faces of the flat capacitor, which was then sealed with epoxy resin. The resulting capacitor had a capacitance of 50 μF.
[0183] (6-2) Evaluation of initial voltage resistance The initial capacitance (C 0 ) was measured using an LCR HiTester 3522-50 manufactured by Hioki E.E. Corporation. Next, a DC voltage of 450 V / μm was applied to the capacitor for 10 seconds. The capacitance (C 1 ) was measured in the same manner, and the rate of change in capacity before and after voltage application was calculated using the following formula.
[0184]
[0185] The capacitance change rate ΔC was measured for 100 elements and evaluated according to the following criteria. The number of capacitors rated A+ to C was calculated, and the ratio of A+ and A capacitors (initial voltage yield) was determined. An initial voltage yield of 95% or more was considered to be acceptable. A+: ΔC is less than -0.2%. A: ΔC is -0.5% or less and less than -1%. B: ΔC is -1% or less and less than -2%. C: ΔC is -2% or less.
[0186] (6-3) Evaluation of long-term voltage resistance The initial capacitance (C 0) was measured using a Hioki E.E. Corporation LCR HiTester 3522-50. Next, a DC voltage of 320 V / μm was continuously applied to the capacitor for 1000 hours in a high temperature bath at 115°C. The capacitance (C 1000 ) was measured in the same manner, and the rate of change in capacity (ΔC 1000 ) was calculated using the following formula:
[0187]
[0188] The above-mentioned capacity change rate ΔC 1000 The long-term voltage yield was measured for 100 elements and evaluated according to the following criteria. The number of capacitors rated A+ to C was calculated, and the ratio of A+ to A capacitors (long-term voltage yield) was calculated. A long-term voltage yield of 90% or more was considered to be acceptable. A+: ΔC 1000 is less than 0.5%. A: ΔC 1000 is less than -0.5% and less than -5%. B: ΔC 1000 is less than -5% and less than -10%. C: ΔC 1000 But it's less than -10%.
[0189] (7) Evaluation Results The evaluation results of process passability and voltage resistance are shown in Table 4.
[0190]
Claims
1. A biaxially oriented polypropylene film having a first surface and a second surface, wherein the average maximum length of approximately elliptical spots on the first surface is 3.0 mm or less, and the difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk within the spots is 0.040 μm or less.
2. The biaxially oriented polypropylene film according to claim 1, wherein the difference between the average protruding valley depth Rvk outside the spots and the average protruding valley depth Rvk within the spots is 0.020 μm or less.
3. The biaxially oriented polypropylene film according to claim 1, wherein the variation range of the slow axis angle is in the range of 0.3° to 2.8°.
4. The biaxially oriented polypropylene film according to claim 1, wherein the average number of approximately elliptical spots per 11.5 mm x 8.6 mm area of said first surface is 0.6 or less.
5. The biaxially oriented polypropylene film according to claim 1, wherein the polypropylene resin constituting the biaxially oriented polypropylene film has a weight average molecular weight Mw of 250,000 or more and 450,000 or less, a ratio of the weight average molecular weight Mw to the number average molecular weight Mn (Mw / Mn) of 5.0 or more and 12.0 or less, a melt flow rate at 230°C and a load of 2.16 kg of 7.0 g / 10 min or less, and a heptane insoluble content of 96.0% or more and 99.5% or less.
6. The biaxially oriented polypropylene film according to claim 1, having a thickness of 1.7 μm or more and 6.5 μm or less.
7. The biaxially oriented polypropylene film according to claim 1, which is a monolayer film.
8. The biaxially oriented polypropylene film according to any one of claims 1 to 7, which is used for a capacitor.
9. A metal layer-integrated polypropylene film comprising the biaxially oriented polypropylene film according to any one of claims 1 to 7 and a metal layer disposed on one or both sides of the biaxially oriented polypropylene film.
10. A capacitor comprising the metal layer-integrated polypropylene film according to claim 9.
11. A method for producing a biaxially oriented polypropylene film according to any one of claims 1 to 7, comprising obtaining a cast sheet using a casting drum having a microcracked surface in which, when a virtual line of 0.1 mm in length is placed at any position on the surface in the width direction, 1 to 15 grooves intersect with the virtual line and the groove width is 1 μm to 10 μm, and subjecting the cast sheet to a biaxial stretching treatment.
Citation Information
Patent Citations
Polyvinyl alcohol film, method for producing polyvinyl alcohol film, and polarizing film
JP6974939B2
Biaxially stretched polypropylene film for capacitors, metallized film, and film capacitor
WO2013146367A1
Polypropylene film, metal layer-integrated polypropylene film, film capacitor and film roll
JP2020100800A
Polypropylene film roll and metalized polypropylene film roll
JP2020200188A
Film capacitor, film for film capacitor, method for manufacturing film for film capacitor, and method for manufacturing film capacitor
WO2019069540A1
Cited By
Dicing tape for semiconductor manufacturing processes, its composition, and method for manufacturing the same.