Sintered graphite bearing

The sintered graphite bearing, made with spherical graphite and amorphous carbon, addresses inefficiencies in existing methods by eliminating resin impregnation and backing metals, enhancing radial crushing strength and wear resistance, and maintaining a stable liquid film for improved performance in liquid environments.

WO2024219225A1PCT designated stage expired Publication Date: 2024-10-24TRIS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013713
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-03
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing sintered graphite bearing manufacturing methods require resin impregnation, cutting, and backing metals, which are inefficient and result in insufficient radial crushing strength, wear, and contamination issues, especially when used in liquids.

Method used

A sintered graphite bearing composed of a cylindrical graphite sintered body with 60-84% spherical graphite, 5-22% amorphous carbon, and resin carbide, where amorphous carbon protrudes to support sliding with point contact, reducing wear and maintaining a liquid film for lubrication, without resin impregnation or backing metals.

Benefits of technology

The solution enhances radial crushing strength, wear resistance, and sliding performance in liquids, maintaining a stable liquid film and reducing frictional heat, while preventing amorphous carbon from falling off, thus improving durability and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013713_24102024_PF_FP_ABST
    Figure JP2024013713_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This sintered graphite bearing is cylindrical and comprises 60-84 mass% of spherical graphite, 5-22 mass% of amorphous carbon having an average particle diameter larger than that of the spherical graphite, and a resin carbide. When a sliding surface of the graphite sintered body is observed through an electron microscope, the occupied area ratio of the amorphous carbon is 3-20%. The amorphous carbon is larger in size than the spherical graphite, protrudes from the sliding surface of the bearing, and comes into point contact with a sliding counterpart to support sliding. The hardness of the bearing is high due to containing the spherical graphite as a main component, which makes it difficult for the amorphous carbon to fall off.
Need to check novelty before this filing date? Find Prior Art

Description

sintered graphite bearings

[0001] The present invention relates to a sintered graphite bearing, and more particularly to a bearing for use in a liquid. The sintered graphite bearing of the present invention can be used in the presence of lubricating oil or in the absence of liquid or lubricating oil.

[0002] The typical manufacturing method for graphite bearings involves impregnating a graphite molded body with resin under reduced pressure for a long period of time, then cutting the graphite into the required shape and machining it into the bearing shape. Resin impregnation is performed to increase the strength of the graphite bearing; without resin impregnation, for example, the bearing may not be able to support radial loads due to insufficient radial crushing strength. This method is inefficient because it requires time and effort: 1) it takes a long time to impregnate the resin, 2) there is a large amount of material loss because the resin is not evenly impregnated into the molded body, and 3) the bearing must be cut out from the molded body and then machined into the bearing shape.

[0003] Related prior art: Patent Document 1 (Patent No. 5905699) describes a graphite-added bearing for a fuel injection pump, in which a sliding layer of polyimide or polyimide amide resin and graphite is provided on a backing metal. Because it is a graphite-based sliding layer provided on a backing metal, the bearing is not made up of graphite and resin only.

[0004] In the sliding member of Patent Document 2 (Patent No. 6030465), spherical carbides are dispersed in a substrate made of graphite and a binder. The spherical carbides support the sliding motion with the sliding counterpart, and the sliding counterpart surface must be highly smooth.

[0005] In the sliding material of Patent Document 3 (Patent 3607778), spherical carbon is blended into a mixture of graphite and a resin binder. When this sliding material is used in a liquid, the liquid penetrates into the protrusions of the spherical carbon and the depressions created when the spherical carbon falls off, providing lubrication by the liquid. The sliding material of Patent Document 3 is based on the premise that the spherical carbon will fall off, and contamination by the fallen spherical carbon becomes a problem.

[0006] Patent 5905699 Patent 6030465 Patent 3607778

[0007] An object of the present invention is to provide a sintered graphite bearing that does not require resin impregnation, cutting from a graphite molded body, or support by a backing metal.A further object of the present invention is to provide a sintered graphite bearing that is less affected by the smoothness and roughness of the surface of the sliding mating material and experiences less wear.A further object of the present invention is to provide a sintered graphite bearing that is suitable for use while immersed in a liquid.

[0008] This invention is a sintered graphite bearing made of a cylindrical graphite sintered body, characterized in that the graphite sintered body is made of 60 mass% to 84 mass% spherical graphite, 5 mass% to 22 mass% amorphous carbon having an average particle size larger than that of the spherical graphite, and resin carbide, and when the sliding surface of the graphite sintered body is observed with an electron microscope, the area occupied by the amorphous carbon is 3% to 20%.

[0009] Irregular carbon, such as coke or coal, is larger in size than spherical graphite; for example, the ratio of the average particle diameter is between 2 and 10, preferably between 3 and 6. Irregular carbon, also known as amorphous carbon or amorphous carbon, is a carbon material that does not have a graphite structure and has low crystallinity overall. Examples include coke, carbon black, and activated carbon. Irregular carbon is characterized by a large average particle size, hardness, and resistance to peeling into thin layers. Irregular carbon protrudes from the sliding surface of the bearing and supports the sliding motion by making point contact with the sliding counterpart. Since the bearing is primarily composed of spherical graphite, it is highly hard, and therefore the amorphous carbon is less likely to fall off. This results in improved wear resistance of the bearing. When sintered graphite bearings are used in liquid, the area ratio of the amorphous carbon on the sliding surface is set to between 3% and 20%, which facilitates the formation of a continuous liquid film between the irregular carbon protrusions. This allows the liquid film to support the shaft and cool the shaft and bearing, improving sliding performance in the liquid.

[0010] The graphite sintered body preferably has a high hardness, and in this invention, the Rockwell hardness is preferably 90 HRR to 130 HRR (110 HRM or less). In this invention, the graphite bearing preferably does not contain a solid lubricant such as molybdenum disulfide, so the graphite bearing preferably consists of only three components: spherical graphite, amorphous carbon, and resin carbide. The resin carbide content is, for example, 5 mass% to 20 mass%. The resin is, for example, a thermosetting resin, particularly a phenolic resin.

[0011] The spherical graphite has, for example, an average particle size of 3 μm to 20 μm and an aspect ratio (ratio of the major axis diameter to the minor axis diameter of the graphite particle) of 2 or less. Bearings made from sintered spherical graphite have high isotropy, which allows for increased radial crushing strength (strength against loads in the diameter direction of the bearing), which is necessary for bearings. Preferably, the ratio of the compressive strength (compressive strength in the axial direction of the bearing) to the radial crushing strength of the sintered graphite bearing is 1 to 2. The amorphous carbon used has an average particle size larger than that of the spherical graphite, and preferably the average particle size of the amorphous carbon is, for example, 2 to 10 times the average particle size of the spherical graphite and is 10 to 200 μm, and more preferably 3 to 6 times the average particle size of the spherical graphite and is 30 to 150 μm.

[0012] The sintered graphite bearing of this invention can be used without liquid or lubricating oil, or in the presence of a lubricant, but is preferably used immersed in liquid, such as in dishwasher pumps, slurry pumps, and drainage pumps. In this case, a liquid film is retained between the protrusions of the amorphous carbon, supporting sliding. The bearing contains a large amount of spherical graphite, making it hard, and the amorphous carbon is less likely to fall off. This results in high wear resistance. Furthermore, with an amorphous carbon content of 5% to 22% by mass, the area occupied by the amorphous carbon on the sliding surface is 3% to 20%, allowing for the retention of a liquid film.

[0013] Preferably, the graphite sintered body contains 60 to 75 mass% of spherical graphite, 5 to 10 mass% of amorphous carbon, and the remainder being a carbide of resin (see the best example). If the contents of spherical graphite and amorphous carbon are slightly reduced within the ranges of this invention and the content of resin is increased, the Rockwell hardness, bending strength, and wear resistance will increase.

[0014] More preferably, the spherical graphite has an average particle size of 3 μm or more and 10 μm or less, and an aspect ratio of 2 or less. When the average particle size of the spherical graphite is within this range, the Rockwell hardness, bending strength, and wear resistance are increased.

[0015] It is particularly preferable that the amorphous carbon has an average particle size of 10 μm or more and 50 μm or less, and that the average particle size is two to five times that of spherical graphite. Under these conditions, the Rockwell hardness and bending strength are significantly increased, and the wear resistance is also improved. When amorphous carbon having an average particle size of 10 μm or more and 50 μm or less, and that the average particle size is two to five times that of spherical graphite, the Rockwell hardness, bending strength, and wear resistance are increased.

[0016] Most preferably, the Rockwell hardness of the graphite sintered body is 100 HRR or more and 130 HRR or less (110 HRM or less for HRM). In the range obtained through experiments, the maximum Rockwell hardness was 112.5 HRR, so the Rockwell hardness is, for example, 100 HRR or more and 130 HRR or less, and more preferably 100 HRR or more and 115 HRR or less. At 130 HRR or less (110 HRM or less for HRM), the higher the Rockwell hardness, the less amorphous carbon falls off the bearing.

[0017] This is an electron microscope photograph of the spherical graphite used in the cross-section of the sintered graphite bearing of the example, showing an average particle size of 15 μm and an aspect ratio of 1.23. This is an electron microscope photograph of the amorphous carbon used, showing an average particle size of 70 μm. This is an electron microscope photograph of the flake graphite used in the comparative example, showing an average particle size of 26 μm. In this electron microscope photograph of the sliding surface of the sintered graphite bearing of the example, the slightly whitish areas are amorphous carbon, and the area ratio of amorphous carbon is 5.7%. In this high-magnification electron microscope photograph of the sliding surface of the sintered graphite bearing of the example, the large gray particle in the center is amorphous carbon, and the small, slightly dark, cornerless particles around it are spherical graphite. 12A is a schematic cross-sectional view of a sintered graphite bearing of an example; 12B is a schematic cross-sectional view of a sintered graphite bearing of a comparative example; 12C is a characteristic diagram showing the bearing temperature change during a high thrust load test at a PV value of 3140 and a rotation speed of 10,000 rpm for Example 1 and Comparative Example 1; 12D is a characteristic diagram showing the rotation speed and bearing temperature of Example 1 during a high thrust load test; 12E is a characteristic diagram showing the rotation speed and bearing temperature of Comparative Example 1 during a high thrust load test; 12F is a high-magnification electron microscope photograph of the sliding surface of the sintered graphite bearings of Example 1 and the optimal example, where the large gray particles are amorphous carbon and the surrounding small, slightly dark particles are spherical graphite. 12A is the same photograph as FIG. 6, and 12B is a photograph of the optimal example (Example 4), with (A) and (B) at the same magnification. 12D is a characteristic diagram showing the wear resistance of the sintered graphite bearings of Examples 1 and 4 and Comparative Example 3; 12E is a schematic diagram showing the wear test method.

[0018] The best mode for carrying out the present invention will be described below. The present invention is not limited to the mode, but is defined by the claims, and can be modified by adding matters known to those skilled in the art to the mode.

[0019] Figure 1 shows a sintered graphite bearing 1 of an embodiment. The bearing 1 is cylindrical, with an outer diameter D of 9.0 mm, an inner diameter r (diameter of hole 2) of 2.0 mm, and a length L of 5.0 mm, but the size is arbitrary. The bearing 1 is press-fitted into a housing (not shown), and a shaft (not shown) is press-fitted into hole 2. The edges of the bearing are chamfered to prevent chipping when pressed into the housing. The inner surface of the bearing 1 is the sliding surface with the shaft, and the outer surface is the sliding surface with the housing. The axial direction of the bearing 1 is the direction of pressure applied during molding.

[0020] Sintered graphite bearings of Examples 1 to 3 were prepared using the blending ratios shown in Table 1. Sintered graphite bearings of Comparative Examples 1 to 3 were prepared using the blending ratios shown in Table 2. The "parts" in the blending ratios are parts by weight, and the phenolic resin binder may be replaced with a furan-based resin, a xylene-based resin, or a thermosetting polyimide resin. The phenolic resin remains in the form of a charcoal resin after sintering. Although the phenolic resin contains oxygen and hydrogen atoms, weight loss due to carbonization is minimal, and the blended phenolic resin may be present in the bearing as a charcoal resin at the blending concentration (13 mass% in the examples). The preferred resin content (concentration of the charcoal resin) is 5 mass% or more and 20 mass% or less.

[0021] When the carbon content of the sintered bearing was measured using "JIS K 7120-1987 Thermogravimetric Measurement Method for Plastics," components other than carbon (mainly ash) were found to be less than 1.0 mass%. This is because the sintering temperature was set at 900°C, and almost the entire amount of resin was measured as resin carbide. The ash content in the bearing is thought to be mainly derived from amorphous carbon.

[0022] In addition to spherical graphite, amorphous carbon, and resin carbide, the bearing may contain solid lubricants such as molybdenum disulfide and tungsten disulfide, or abrasives such as alumina, at a concentration of, for example, 3 mass % or less.

[0023]

[0024]

[0025] The spherical graphite used is shown in Figure 2, and has an average particle size of 15 µm as measured using a laser diffraction / scattering particle size distribution analyzer MT3300EXII manufactured by Microtrac Bell Co., Ltd., and an average value of the ratio of the major axis diameter to the minor axis diameter (aspect ratio) of the particles as observed under an electron microscope is 1.23. The spherical graphite preferably has an average particle size of 3 µm or more and 20 µm or less, and an aspect ratio of 2 or less and 1 or more.

[0026] 3 shows the amorphous carbon (coke) used, which has an average particle size of 70 μm as measured by the laser diffraction / scattering particle size distribution analyzer. Preferably, the average particle size of the amorphous carbon is, for example, two to ten times the average particle size of the spherical graphite and is 10 μm to 200 μm, more preferably three to six times the average particle size of the spherical graphite and is 30 μm to 150 μm.

[0027] Figure 4 shows the flake graphite used in Comparative Example 3. It has an average particle size of 26 μm and is characterized by its angular shape. When flake graphite with an angular shape slides against a mating shaft, the thin graphite layer is likely to peel off. In contrast, with amorphous carbon, the thin carbon layer is less likely to peel off. In other words, increasing the hardness of the bearing and preventing carbon from falling off can increase the durability of the bearing.

[0028] Figure 5 is an electron microscope photograph of the sliding surface of bearing 1, and the slightly white (bright) areas are amorphous carbon. To determine the area ratio of amorphous carbon, for example, use image analysis software Image J to select 30 of the largest amorphous carbon particles in the image and calculate the area of ​​each individual amorphous carbon particle. The area ratio is calculated by adding up the areas of the 30 particles and comparing this with the image area. The area ratio in Figure 5 was 5.7%.

[0029] Figure 6 is a high-magnification electron microscope photograph of the sliding surface of bearing 1. The large gray particles extending from the lower center to the upper left are amorphous carbon, and the numerous small, slightly dark, cornerless particles around them are spherical graphite. The spherical graphite particles are smaller than the amorphous carbon particles, and black gaps can be seen between them. The black and white areas within the amorphous carbon particles are grooves and corners on the particle surface.

[0030] The materials were mixed according to the ratios shown in Tables 1 and 2, filled into a mold, press-molded, and then sintered at 900°C in a non-oxidizing atmosphere. At this temperature, the phenolic resin binder was almost completely carbonized. The sintering temperature should be such that the resin is almost completely carbonized. In addition to the bearings, a 20mm x 10mm x 5mm rectangular sintered compact (thickness direction of pressure) was prepared under the same conditions as Bearing 1 to measure the bending strength in the pressure direction of the sintered compact. The three-point bending strength in the pressure direction was measured. The radial crushing strength (measured according to JIS Z 2507) and compressive strength (axial compressive strength) of Bearing 1 were also measured. The Rockwell hardness of a 30mm x 20mm x 7mm sintered compact was prepared under the same conditions as Bearing 1 and measured using a Mitutoyo Corporation ATK-F1000 Rockwell Hardness Tester in accordance with JIS Z 2245. Rockwell hardness was first measured using scale R, and since JIS recommends selecting a scale so that the Rockwell hardness is between 50 and 115, if the measured value exceeded 115 HRR it was measured using scale M. The Rockwell hardness of the bearing was 125 HRR, which was equivalent to 105 HRM. Observation of the bearing condition showed that a Rockwell hardness of over 110 HRM would damage the shaft, and below 90 HRR amorphous carbon was prone to falling off.

[0031] Tables 1 and 2 show that the presence of a sufficient amount of spherical graphite (60 to 84 mass%) increases Rockwell hardness and simultaneously improves bending strength. In addition, in Examples 1 to 3 and Comparative Example 1, the ratio of compressive strength to radial crushing strength was 1 or more and 2 or less, but in Comparative Examples 2 and 3, it exceeded 2.

[0032] Because amorphous carbon is larger in size than spherical graphite, it protrudes from the sliding surface and makes point contact. When used immersed in liquid, if the area ratio of the amorphous carbon is low (Comparative Example 1) and there are few protrusions of the amorphous carbon as shown in Figure 8, the liquid is pushed out onto the sliding shaft, making it easy for the liquid film to break. When the area ratio of the amorphous carbon is appropriate (3% to 20%: Examples 1 to 3), the liquid is retained between the protrusions of the amorphous carbon, and the liquid film remains stable. However, when the amorphous carbon content was excessive (Comparative Example 2), both the Rockwell hardness and bending strength decreased.

[0033] Figures 9 to 11 show the results of underwater high-thrust load tests (PV tests) for Example 1 and Comparative Example 1. In the tests, the shaft and bearing were placed underwater, and the shaft rotation speed was varied over a 90-minute cycle. The temperature of bearing 1 was measured using a temperature sensor attached to the axial end of bearing 1. In Comparative Example 1, the bearing temperature rose sharply to over 100°C after 240 minutes when the rotation speed was increased from 6,000 rpm to 10,000 rpm. The difference between Example 1 and Comparative Example 1 is the content of amorphous carbon. In Comparative Example 1, the amount of amorphous carbon protruding from the sliding surface was low, which resulted in the breakdown of the liquid film between the bearing and shaft, resulting in the accumulation of frictional heat. In Example 1, the bearing temperature remained stable at around 40°C even after 360 minutes, demonstrating stable lubrication with the shaft and heat dissipation by the liquid film.

[0034] In the embodiment, the spherical graphite provides a bearing with high hardness and bending strength, as well as high isotropy of strength in the axial and diametric directions. In this bearing, point contact between the amorphous carbon and the shaft results in low friction, and the bearing's high hardness reduces the amount of amorphous carbon falling off. This results in high bearing durability. Furthermore, when used immersed in liquid, a liquid film is retained in the gaps between the protrusions of the amorphous carbon, supporting the shaft and dissipating heat. This reduces damage caused by frictional heat with the shaft.

[0035] Best Example: A sintered graphite bearing was manufactured in which the average particle size of the spherical graphite and the average particle size of the amorphous carbon were reduced, their contents were reduced, and the carbide content of the resin was increased compared to Examples 1 to 3. This sintered graphite bearing had high bending strength, high Rockwell hardness, a strength ratio in the pressure direction to the interlayer direction close to 1, and high wear resistance. This sintered graphite bearing is called the best example (Example 4).

[0036] 12 shows the sliding surfaces of Example 1 (A) and the optimum example (B). In the optimum example, both the average particle size of the spherical graphite and the average particle size of the amorphous carbon are smaller than those of Example 1. In addition, the content of the spherical graphite and the content of the amorphous carbon are smaller than those of Example 1, and the content of the resin carbide is increased accordingly.

[0037] The composition, particle size of each material, bending strength (in the pressure direction), and Rockwell hardness HRR of the optimum example (Example 4) and Example 1 are shown in Table 3. The results of the wear resistance test of Examples 1 and 4 and Comparative Example 3 are shown in Figure 13. Except where otherwise noted, the optimum example is the same as Example 1, including the manufacturing conditions.

[0038] The test method for the wear resistance test is shown schematically in Figure 14. A sintered graphite shaft bearing 1 was placed in contact with a mating member 10 made of SUS304, and both bearing 1 and mating member 10 were immersed in cooling oil. With an axial load applied, bearing 1 was rotated at 6,000 revolutions per minute, and the amount of wear was measured after 200 hours. As shown in Figure 13, the amount of wear in the optimal example (Example 4) was reduced by approximately 20% from Example 1. Furthermore, the amount of wear in Examples 1 and 4 was significantly smaller than that in Comparative Example 3, which did not contain spherical graphite.

[0039]

[0040] The optimum example, compared to Example 1, has: - reduced the content of spherical graphite and amorphous carbon and increased the content of resin carbide (derived from phenolic resin), - reduced the average particle size of spherical graphite and amorphous carbon while maintaining the same average particle size ratio. The resulting effects are increased Rockwell hardness, increased bending strength, and increased wear resistance, which significantly improve the overall durability of the sintered graphite bearing.

[0041] The data for the optimal example (Table 3, Figure 13) show that slightly decreasing the content of spherical graphite and amorphous carbon and increasing the content of resin increases Rockwell hardness, bending strength, and wear resistance. It also shows that slightly decreasing the average particle size of the spherical graphite (3 μm to 10 μm, with an aspect ratio of 2 or less) increases Rockwell hardness and bending strength. Furthermore, increasing the average particle size of the amorphous carbon (10 μm to 50 μm, i.e., two to five times that of the spherical graphite) significantly increases Rockwell hardness and bending strength. For Rockwell hardnesses of 130 HRR or less (110 HRM or less), the higher the Rockwell hardness, the less likely the amorphous carbon will fall off the bearing. Most preferably, the Rockwell hardness of the graphite sintered compact is 100 HRR to 130 HRR, for example, 100 HRR to 115 HRR.

[0042] 1 sintered graphite bearing 2 hole 3 spherical graphite 4 amorphous carbon 5 liquid 10 mating material

Claims

1. A sintered graphite bearing comprising a cylindrical graphite sintered body, the graphite sintered body comprising 60 mass% or more and 84 mass% or less of spheroidal graphite, amorphous carbon with an average particle size larger than that of the spheroidal graphite and a content of 5 mass% or more and 22 mass% or less, and resin carbide, wherein when the sliding surface of the graphite sintered body is observed under an electron microscope, the area occupied by the amorphous carbon is 3% or more and 20% or less.

2. The sintered graphite bearing of claim 1, wherein the graphite sintered body has a Rockwell hardness of 90 HRR or more and 130 HRR or less.

3. A sintered graphite bearing according to claim 1 or 2, characterized in that the spherical graphite has an average particle size of 3 μm or more and 20 μm or less and an aspect ratio of 2 or less.

4. A sintered graphite bearing as claimed in claim 1, characterized in that it is made up of only said cylindrical graphite sintered body, said cylindrical graphite sintered body being made up of only spheroidal graphite, amorphous carbon and carbide of resin.

5. A sintered graphite bearing as claimed in claim 1, characterized in that it is a bearing used while immersed in a liquid.

6. A sintered graphite bearing as claimed in claim 1, characterized in that the graphite sintered body contains 60 mass% to 75 mass% of spheroidal graphite, 5 mass% to 10 mass% of amorphous carbon, and the remainder being resin carbide.

7. The sintered graphite bearing according to claim 6, wherein said spherical graphite has an average particle size of 3 μm or more and 10 μm or less and an aspect ratio of 2 or less.

8. A sintered graphite bearing as claimed in claim 7, characterized in that the amorphous carbon has an average particle size of 10 µm or more and 50 µm or less, and an average particle size of at least two times and at most five times that of spheroidal graphite.

9. The sintered graphite bearing according to claim 6, wherein the Rockwell hardness of said graphite sintered body is not less than 100 HRR and not more than 130 HRR.

Citation Information

Patent Citations

  • Polyphenylene sulfide resin composition

    JP1998077407A

  • Slide bearing made of graphite added resin-based material, for automatic transmission

    JP2013083302A

  • Sliding material, molded body thereof, and sliding member

    JP6657740B2