Method for manufacturing printed wiring board, photosensitive resin composition, photosensitive resin film, printed wiring board, and semiconductor package

The described method for printed wiring boards uses a sulfuric acid-dissolvable photosensitive resin composition to form vias and improve adhesive strength, overcoming the inefficiencies of traditional laser processing and trade-offs in surface roughness and adhesion, enabling efficient and effective via formation.

WO2024219251A1PCT designated stage expired Publication Date: 2024-10-24RESONAC CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014028
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-04-05
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The challenge in manufacturing printed wiring boards is the inefficiency in forming small-diameter vias due to the limitations of laser processing, which requires forming each via individually, and the trade-off between reducing surface roughness of interlayer insulating layers and achieving high adhesive strength with copper plating.

Method used

A method involving a photosensitive resin composition with particles that dissolve in sulfuric acid, used for laminating a photosensitive resin film on a circuit board, exposing and developing to form vias, roughening the surfaces, dissolving particles with an acidic solution, and forming circuit patterns, achieving high adhesive strength while reducing surface roughness.

Benefits of technology

This method enables the efficient formation of multiple small-diameter vias simultaneously and maintains high adhesive strength with copper plating, addressing the inefficiencies of traditional laser processing and trade-offs in surface roughness and adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014028_24102024_PF_FP_ABST
    Figure JP2024014028_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: a method for manufacturing a printed wiring board that exhibits high adhesive strength to copper plating while achieving a reduction in surface roughness of an interlayer insulating layer; a photosensitive resin composition and a photosensitive resin film with which the printed wiring board can be provided; and a printed wiring board obtained by the manufacturing method, and a semiconductor package having the printed wiring board. This method for manufacturing the printed wiring board comprises the following (1) to (4). (1): Laminating, on one surface or both surfaces of a circuit board, a photosensitive resin film containing particles (X) 95 mass% or more of which are dissolved in a sulfuric acid aqueous solution with a concentration of 5-100 ml / L at 70°C for 20 minutes. (2): Forming an interlayer insulating layer having a via by exposing and developing the photosensitive resin film laminated in (1). (3-1): Performing roughening treatment on the surfaces of the via and the interlayer insulating layer. (3-2) Dissolving the particles (X) present on the surface of the interlayer insulating layer subjected to the roughening treatment by treating the interlayer insulating layer with an acid solution. (4): Forming a circuit pattern on the interlayer insulating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Printed wiring board manufacturing method, photosensitive resin composition, photosensitive resin film, printed wiring board, and semiconductor package

[0001] The present disclosure relates to a method for producing a printed wiring board, a photosensitive resin composition, a photosensitive resin film, a printed wiring board, and a semiconductor package.

[0002] In recent years, electronic devices have become smaller and more powerful, and printed wiring boards have become increasingly dense due to an increase in the number of circuit layers and finer wiring. In particular, the density of semiconductor package substrates, such as BGA (ball grid array) and CSP (chip size package), on which semiconductor chips are mounted, has increased significantly, and in addition to finer wiring, thinner insulating layers and smaller diameters of vias (also called via holes) for interlayer connection are required.

[0003] A conventional method for manufacturing printed wiring boards is the build-up method (see, for example, Patent Document 1), in which an interlayer insulating layer and a conductor circuit layer are sequentially laminated. As wiring becomes finer, semi-additive processes, in which circuits are formed by plating, have become mainstream for printed wiring boards. Conventional semi-additive processes include, for example, (1) laminating a thermosetting resin film on a conductor circuit, and then curing the thermosetting resin film by heating to form an "interlayer insulating layer." (2) Next, vias for interlayer connection are formed by laser processing, followed by desmearing and roughening treatments such as alkaline permanganate treatment. (3) Subsequently, electroless copper plating is performed on the substrate, followed by pattern formation using a resist, followed by electrolytic copper plating to form a copper circuit layer. (4) Next, the resist is stripped, and the electroless layer is flash-etched to form a copper circuit.

[0004] As mentioned above, laser processing is the mainstream method for forming vias in an interlayer insulating layer formed by curing a thermosetting resin film, but the reduction in the diameter of vias by laser irradiation using a laser processing machine is reaching its limit. Furthermore, when forming vias using a laser processing machine, each via hole must be formed one by one, and when a large number of vias are required for high density, forming the vias takes a long time, resulting in poor manufacturing efficiency.

[0005] Under these circumstances, a method capable of forming a large number of vias at once has been proposed, which involves forming a plurality of small vias at once by photolithography using a photosensitive resin composition containing an acid-modified vinyl group-containing epoxy resin, a photopolymerizable compound, a photopolymerization initiator, an inorganic filler, and a silane compound, with the inorganic filler content being 10 to 80 mass % (see, for example, Patent Document 2). Patent Document 2 addresses one of the problems to be solved, namely, suppressing the decrease in adhesion to copper plating that results from using a photosensitive resin composition instead of a conventional thermosetting resin composition as a material for an interlayer insulating layer or a surface protective layer, and further addresses the problems of via resolution and adhesion to silicon substrates and chip components, and claims to have solved these problems.

[0006] JP 7-304931 A JP 2017-116652 A

[0007] However, in recent years, the miniaturization of wiring has been progressing more and more. One of the means for achieving further miniaturization of wiring is to reduce the surface roughness of the interlayer insulating layer. However, reducing the surface roughness of the interlayer insulating layer reduces adhesion to copper plating, which is a trade-off. Therefore, it is difficult to achieve both a reduction in the surface roughness of the interlayer insulating layer and an improvement in adhesion to copper plating, and it is not easy to achieve further miniaturization of wiring.

[0008] Therefore, an object of the present disclosure is to provide a method for manufacturing a printed wiring board that exhibits high adhesive strength with copper plating while reducing the surface roughness of the interlayer insulating layer, to provide a photosensitive resin composition and a photosensitive resin film that can provide such a printed wiring board, and to provide a printed wiring board obtained by the manufacturing method and a semiconductor package having the printed wiring board.

[0009] As a result of extensive research, the present inventors have found that the above-mentioned object can be achieved by the present disclosure. The present disclosure includes the following embodiments [1] to

[16] . [1] A method for manufacturing a printed wiring board, including the following (1) to (4): (1): laminating a photosensitive resin film containing particles (X) that dissolve at 95% by mass or more in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L at 70°C for 20 minutes on one or both sides of a circuit board. (2): forming an interlayer insulating layer having vias by exposing and developing the photosensitive resin film laminated in (1). (3-1): roughening the vias and the surface of the interlayer insulating layer. (3-2): treating the roughened interlayer insulating layer with an acidic solution to dissolve the particles (X) present on the surface of the interlayer insulating layer. (4): forming a circuit pattern on the interlayer insulating layer. [2] The method for producing a printed wiring board according to [1] above, wherein the roughening treatment in (3-1) is carried out using a roughening solution. [3] The method for producing a printed wiring board according to [1] above, wherein the roughening treatment in (3-1) is carried out by dry etching. [4] The method for producing a printed wiring board according to any one of [1] to [3] above, wherein the surface roughness (Ra) of the interlayer insulating layer after the roughening treatment in (3-1) is 0.30 μm or less. [5] The method for producing a printed wiring board according to any one of [1] to [4] above, wherein the acidic solution used in (3-2) contains an aqueous sulfuric acid solution. [6] The method for producing a printed wiring board according to any one of [1] to [5] above, wherein the particle (X) has a volume average particle diameter of 0.1 to 3 μm. [7] The method for producing a printed wiring board according to any one of [1] to [6] above, wherein the photosensitive resin film contains the particle (X) in an amount of 10 to 70% by volume. [8] A photosensitive resin composition comprising particles (X) that are soluble in an aqueous sulfuric acid solution having a concentration of 5 to 100 ml / L at 70°C for 20 minutes at a rate of 95% by mass or more. [9] The photosensitive resin composition according to [8] above, further comprising (A) a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent, and (B) a thermosetting resin.

[10] The photosensitive resin composition according to [9] above, wherein the component (A) contains an alicyclic skeleton represented by the following general formula (A-1): (In the formula, R A1represents an alkyl group having 1 to 12 carbon atoms, and may be substituted anywhere in the alicyclic skeleton. 1 is an integer of 0 to 6. * is a bonding site to another structure.)

[11] The photosensitive resin composition according to any one of [8] to

[10] above, wherein the average particle size of the particles (X) is 0.1 to 3 μm.

[12] The photosensitive resin composition according to any one of [8] to

[11] above, wherein the content of the particles (X) is 10 to 70 volume % based on the total solid content.

[13] A photosensitive resin composition for forming photovia holes, comprising the photosensitive resin composition according to any one of [8] to

[12] above.

[14] A photosensitive resin film comprising the photosensitive resin composition according to any one of [8] to

[12] above.

[15] A printed wiring board comprising the photosensitive resin composition according to any one of [8] to

[12] above or the photosensitive resin film according to

[14] above.

[16] A semiconductor package comprising the printed wiring board according to

[15] above and a semiconductor element.

[0010] According to the present disclosure, it is possible to provide a method for manufacturing a printed wiring board that exhibits high adhesive strength with copper plating while reducing the surface roughness of the interlayer insulating layer, as well as to provide a photosensitive resin composition and a photosensitive resin film that can provide such a printed wiring board, and further to provide a printed wiring board obtained by the manufacturing method and a semiconductor package that includes the printed wiring board.

[0011] 1 is a schematic diagram showing a laminating step (1). 2 is a schematic diagram showing a photovia forming step (2). 3 is a schematic diagram showing a roughening treatment step (3-1). 4 is a schematic diagram showing a particle (X) dissolving step (3-2). 5 is a schematic diagram showing a circuit pattern forming step (4). 6 is a schematic diagram of a multilayered printed wiring board. 7 is an SEM image of a via formed in Example 2. 8 is an SEM image of a via formed in Example 11. 9 is an SEM image of an interlayer insulating layer surface after a particle (X) dissolving step (3-2) in Example 2. 10 is an SEM image of an interlayer insulating layer surface after a particle (X) dissolving step (3-2) in Example 5. 11 is an SEM image of an interlayer insulating layer surface after a particle (X) dissolving step (3-2) in Example 8. 12 is an SEM image of an interlayer insulating layer surface after a particle (X) dissolving step (3-2) in Example 11. 13 is an SEM image of an interlayer insulating layer surface after a particle (X) dissolving step (3-2) in Comparative Example 5. 10 is an SEM image of the surface of the interlayer insulating layer after the roughening treatment step (3-1) in Example 13. FIG. 11 is an SEM image of the surface of the interlayer insulating layer after the particle (X) dissolving step (3-2) in Example 13.

[0012] In the numerical ranges described in this disclosure, the upper or lower limit of the numerical range may be replaced with the values ​​shown in the examples. Furthermore, the lower and upper limits of a numerical range can be arbitrarily combined with the lower or upper limit of another numerical range. In the expression "AA to BB," the numerical values ​​AA and BB at both ends are included as the lower and upper limits, respectively, of the numerical range. In this disclosure, for example, the expression "10 or more" means 10 and a numerical value greater than 10, and this also applies when the numerical values ​​differ. Furthermore, for example, the expression "10 or less" means 10 and a numerical value less than 10, and this also applies when the numerical values ​​differ. In this disclosure, when multiple substances corresponding to each component are present, the content of each component in the photosensitive resin composition refers to the total content of the multiple substances present in the photosensitive resin composition, unless otherwise specified. In this disclosure, the "number of ring carbon atoms" refers to the number of carbon atoms required to form a ring and does not include the number of carbon atoms of substituents on the ring. For example, both the cyclohexane skeleton and the methylcyclohexane skeleton have six ring carbon atoms. The term "XX (meth)acrylate" refers to either or both of XX acrylate and XX methacrylate. Furthermore, the term "(meth)acryloyl group" refers to either or both of an acryloyl group and a methacryloyl group. In the present disclosure, the term "resin component" refers to the (A) and (B) components described below, as well as other components that may be contained as needed (e.g., components (C), (D), (F), (G), (H), (I), and (J)), but does not include inorganic compounds such as inorganic fillers and pigments. Furthermore, the term "solid content" refers to the non-volatile content excluding water and the diluent described below contained in the photosensitive resin composition, and includes liquid, starch syrup-like, and wax-like substances at room temperature around 25°C. In the present disclosure, the term "dielectric constant" refers to the dielectric constant in the 10 GHz band, unless otherwise specified. Furthermore, any combination of the descriptions in the present disclosure is also included in the present embodiment.

[0013] [Method for Manufacturing Printed Wiring Board] A method for manufacturing a printed wiring board according to one embodiment of the present disclosure (hereinafter, sometimes simply referred to as this embodiment) is a method for manufacturing a printed wiring board, including the following steps (1) to (4). (1): Laminating a photosensitive resin film containing particles (X) (hereinafter, sometimes simply referred to as "particles (X)") that dissolve at 95% by mass or more in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L at 70°C for 20 minutes onto one or both sides of a circuit board (hereinafter, referred to as "laminating step (1)"). (2): Forming an interlayer insulating layer having vias by exposing and developing the photosensitive resin film laminated in step (1) (hereinafter, referred to as "photovia forming step (2)"). (3-1): Roughening the surfaces of the vias and the interlayer insulating layer (hereinafter, referred to as "roughening treatment step (3-1)"). (3-2): Treating the roughened interlayer insulating layer with an acidic solution to dissolve the particles (X) present on the surface of the interlayer insulating layer (hereinafter referred to as "particle (X) dissolving step (3-2)"). (4): Forming a circuit pattern on the interlayer insulating layer (hereinafter referred to as "circuit pattern forming step (4)"). Herein, as described above, for convenience, in this disclosure, a predetermined operation may be referred to as "XX step," but the XX step is not limited to only the embodiments specifically described in this disclosure.

[0014] In this embodiment, by providing the particle (X) dissolving step (3-2) after the roughening treatment step (3-1), the particles (X) present on the surface of the interlayer insulating layer can be dissolved to form depressions on the surface of the interlayer insulating layer, thereby making it possible to obtain high adhesive strength with the copper plating while reducing the surface roughness of the interlayer insulating layer. Each step will be described in order below.

[0015] (Laminating Step (1)) The laminating step (1) is a step of laminating the photosensitive resin film of this embodiment onto one or both sides of a circuit board (a substrate 101 having a circuit pattern 102) using a vacuum laminator (see FIG. 1). Examples of the vacuum laminator include a vacuum applicator manufactured by Nikko Materials Co., Ltd. and a vacuum pressure laminator manufactured by The Japan Steel Works, Ltd.

[0016] When a protective film is provided on the photosensitive resin film, the protective film can be peeled off or removed, and then the photosensitive resin film can be laminated to the circuit board while being pressed and heated in contact with the circuit board. The lamination can be carried out, for example, by preheating the photosensitive resin film and circuit board as necessary, followed by a pressure bonding temperature of 70 to 130°C, a pressure bonding pressure of 0.1 to 1.0 MPa, and a reduced pressure of 20 mmHg (26.7 hPa) or less, but is not particularly limited to these conditions. The lamination method can be either a batch method or a continuous method using a roll. Finally, the photosensitive resin film laminated to the circuit board is cooled to around 25°C to form the interlayer insulating layer 103. If the photosensitive resin film has a carrier film, the carrier film may be peeled off at this stage, or, as described below, may be peeled off after exposure.

[0017] (Photovia Forming Step (2)) In the photovia forming step (2), at least a portion of the photosensitive resin film laminated to the circuit board is exposed to light, followed by development. The exposed portion is photocured to form a pattern. The exposure method is not particularly limited. For example, a method of irradiating the actinic rays imagewise through a negative or positive mask pattern known as artwork (mask exposure method) may be employed, or a method of irradiating the actinic rays imagewise by a direct imaging exposure method such as LDI (Laser Direct Imaging) exposure method or DLP (Digital Light Processing) exposure method may be employed. Known light sources can be used as the light source for the actinic rays. Specific examples of light sources include gas lasers such as carbon arc lamps, mercury vapor arc lamps, high-pressure mercury lamps, xenon lamps, and argon lasers; solid-state lasers such as YAG lasers; and semiconductor lasers that effectively emit ultraviolet or visible light. The exposure dose is appropriately selected depending on the light source used, the thickness of the photosensitive layer, etc. For example, in the case of ultraviolet irradiation from a high-pressure mercury lamp, when the photosensitive layer has a thickness of 1 to 100 μm, the exposure dose is usually 10 to 1,000 mJ / cm 2Preferably, the intensity is about 50 to 700 mJ / cm 2 More preferably, 150 to 550 mJ / cm 2 is more preferable.

[0018] During development, the uncured portions of the photosensitive layer are removed from the substrate, resulting in the photocured portions being formed on the substrate as an interlayer insulating layer. If a carrier film is present on the photosensitive layer, the carrier film is removed before the unexposed portions are removed (developed). Development methods include wet development and dry development, either of which may be employed. However, wet development is widely used, and wet development can also be employed in this embodiment. In wet development, development is carried out by a known development method using a developer suitable for the photosensitive resin composition. Examples of development methods include dipping, bathing, spraying, brushing, slapping, scraping, and swing immersion. Among these, the spray method is preferred from the viewpoint of improving via resolution, and among spray methods, the high-pressure spray method is more preferred. Development may be carried out by one method, or two or more methods may be combined. The composition of the developer is appropriately selected depending on the composition of the photosensitive resin composition. Examples include alkaline aqueous solutions, water-based developers, and organic solvent-based developers, with alkaline aqueous solutions being preferred.

[0019] In the photovia forming process (2), after exposure and development, 0.2 to 10 J / cm 2 (preferably 0.5 to 5 J / cm 2) and post-thermal cure at a temperature of about 60 to 250°C (preferably 120 to 200°C), as needed, to further harden the interlayer insulating layer, which is also preferred. The above method results in an interlayer insulating layer having vias 104 (see FIG. 2). The shape of the vias is not particularly limited, and examples of the cross-sectional shape include a rectangle and an inverted trapezoid (the upper side is longer than the lower side), and examples of the shape viewed from the front (the direction from which the via bottom is visible) include a circle and a rectangle. In the formation of vias by photolithography in this embodiment, vias having a cross-sectional shape of an inverted trapezoid (the upper side is longer than the lower side) can be formed, which is preferred because it enhances the adhesion of copper plating to the via wall surface.

[0020] The size (diameter) of the via 104 formed by this process can be less than 40 μm, and can even be 35 μm or less, 30 μm or less, 25 μm or less, or 20 μm or less, which is smaller than the size of vias formed by laser processing. There is no particular limit to the lower limit of the size (diameter) of the via formed by this process, but it may be 5 μm or more, 10 μm or more, or 15 μm or more. However, the size (diameter) of the via 104 formed by this process is not limited to less than 40 μm, and may be selected arbitrarily in the range of 5 to 300 μm, for example, 15 to 100 μm, or 20 to 80 μm.

[0021] (Roughening Treatment Step (3-1)) In the roughening treatment step (3-1), a roughening treatment is performed on the surfaces of the via and the interlayer insulating layer (see FIG. 3). The roughening treatment forms anchors of fine irregularities on the surfaces of the via and the interlayer insulating layer. From the viewpoint of finer wiring, the surface roughness (Ra) of the interlayer insulating layer after the roughening treatment is preferably 0.30 μm or less, more preferably 0.25 μm or less, even more preferably 0.01 to 0.12 μm, particularly preferably 0.02 to 0.10 μm, and most preferably 0.02 to 0.09 μm. Here, in the present disclosure, the surface roughness (Ra) is the result of measurement using a high-performance non-contact three-dimensional surface profile roughness measurement system (Wyko NT9100, manufactured by Bruker Japan Co., Ltd.), and more specifically, is a value measured by the method described in the examples.

[0022] The roughening treatment method is not particularly limited, and known roughening treatment methods for vias and interlayer insulating layers can be used. The roughening treatment method is not particularly limited, but includes a method using a roughening solution and a method using dry etching. Here, the method using a roughening solution is also called wet etching.

[0023] An oxidizing agent can be used as the roughening solution. Examples of the oxidizing agent include an alkaline permanganate solution obtained by dissolving potassium permanganate, sodium permanganate, or the like in an aqueous solution of sodium hydroxide, dichromate, ozone, hydrogen peroxide-sulfuric acid, and nitric acid. The permanganate concentration in the alkaline permanganate solution is preferably 5 to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as Concentrate Compact CP and Dosing Solution Securigance (registered trademark) P (both manufactured by Atotech Japan Co., Ltd.). Note that if smears occur in the photovia formation step (2), the smears may be removed using the roughening solution. The roughening treatment and smear removal (desmearing) can be performed simultaneously.

[0024] When the roughening liquid is used, preferably, the via surface and the interlayer insulating layer surface are subjected to a swelling treatment, followed by a roughening treatment of the via surface and the interlayer insulating layer surface. Here, a commercially available swelling liquid can be used for the swelling treatment. Examples of the swelling liquid include an alkaline solution and a surfactant solution, and alkaline solutions are preferred. Examples of the alkaline solution include a sodium hydroxide solution and a potassium hydroxide solution. Examples of commercially available swelling liquids include Swelling Dip Securigance (registered trademark) P and Swelling Dip Securigance (registered trademark) SBU (both manufactured by Atotech Japan Co., Ltd.). The swelling time and temperature are not particularly limited, but are preferably 50 to 90°C, more preferably 60 to 80°C, and are preferably 1 to 20 minutes, more preferably 3 to 15 minutes, and even more preferably 3 to 8 minutes.

[0025] After the swelling treatment and the roughening treatment, a water washing treatment may be carried out as necessary. The time and temperature of the water washing treatment are not particularly limited, but are preferably 5 to 40°C, more preferably 15 to 30°C, and are preferably 0.1 to 10 minutes, more preferably 0.5 to 7 minutes. The water washing treatment may be a combination of so-called "reservoir washing", in which water is simply stored, and so-called "running water washing", in which water is flowing, or only one of these may be carried out. However, it is preferable to carry out at least running water washing, and it is more preferable to carry out both retained water washing and running water washing.

[0026] Examples of the dry etching include reactive ion etching (RIE), and examples of the RIE include dry etching using a reactive gas and dry etching using plasma. Among these, dry etching using plasma is preferred. For dry etching using plasma, a commercially available plasma etching device may be used. The conditions for dry etching using plasma are not particularly limited, but preferably oxygen plasma is used, and the output is preferably 100 to 500 W, more preferably 200 to 400 W. The time and temperature of dry etching are not particularly limited, but are preferably 5 to 40°C, more preferably 15 to 30°C, and are preferably 0.1 to 10 minutes, more preferably 0.5 to 7 minutes.

[0027] 3, the roughening treatment step (3-1) causes some of the particles (X) to appear in a protruding form on the surface of the interlayer insulating layer 103. The particles (X) will be described later.

[0028] (Particle (X) Dissolving Step (3-2)) In the particle (X) dissolving step (3-2), the roughened interlayer insulating layer is treated with an acidic solution to dissolve the particles (X) present on the surface of the interlayer insulating layer (see FIG. 4). The acidic solution is not particularly limited, but examples thereof include an aqueous sulfuric acid solution, an aqueous hydrochloric acid solution, an aqueous sodium persulfate solution, an aqueous ammonium persulfate solution, and an aqueous potassium persulfate solution. The acidic solution preferably contains an aqueous sulfuric acid solution or an aqueous hydrochloric acid solution, more preferably contains an aqueous sulfuric acid solution, and even more preferably is an aqueous sulfuric acid solution. From the viewpoint of the solubility of the particles (X), the concentration of the aqueous sulfuric acid solution is preferably 5 to 100 ml / L, more preferably 10 to 80 ml / L, and even more preferably 15 to 50 ml / L, and may be 10 to 30 ml / L, 35 to 80 ml / L, or 35 to 60 ml / L. From the viewpoint of the solubility of the particles (X), the concentration of the hydrochloric acid aqueous solution is preferably 5 to 100 g / L, more preferably 10 to 80 g / L, and even more preferably 15 to 50 g / L, and may be 10 to 30 ml / L, 35 to 80 ml / L, or 35 to 60 ml / L. Although not particularly limited, it is preferable that the acidic solution is not toxic (for example, hydrofluoric acid).

[0029] The particle (X) dissolving step (3-2) may be performed before or during the circuit pattern forming step (4) described below. Furthermore, when a roughening solution is used in the roughening treatment step (3-1), the particle (X) dissolving step (3-2) can be regarded as a neutralization step after the roughening treatment. When a dry etching treatment is performed in the roughening treatment step (3-1), the particle (X) dissolving step (3-2) can also be regarded as a pretreatment for forming a seed layer when a semi-additive process is performed in the circuit pattern forming step (4) described below. In any case, it is important that the particle (X) dissolving step (3-2) dissolves the particles (X) present on the surface of the interlayer insulating layer, thereby forming depressions 2 as shown in FIG. 4 .

[0030] The temperature when treating the interlayer insulating layer with the acidic solution is preferably 15 to 80°C, more preferably 20 to 75°C, and even more preferably 25 to 70°C, from the viewpoint of the solubility of the particles (X), and may be 40 to 70°C, 50 to 70°C, or 60 to 70°C. The time for treatment with the acidic solution is not particularly limited, but from the viewpoint of the solubility of the particles (X), it is preferably 0.1 to 40 minutes, more preferably 0.3 to 35 minutes, even more preferably 3 to 30 minutes, particularly preferably 5 to 25 minutes, and most preferably 15 to 25 minutes. The method for treating the interlayer insulating layer with the acidic solution is not particularly limited, and examples thereof include (1) a method in which a substrate having an interlayer insulating layer is immersed in an acidic solution and, if necessary, agitating the substrate having the interlayer insulating layer, (2) a method in which a substrate having an interlayer insulating layer is immersed in an acidic solution and, if necessary, stirring the acidic solution, and (3) a method in which an acidic solution is sprayed onto the interlayer insulating layer. From the viewpoint of the solubility of the particles (X), the above method (1) or (2) is preferred.

[0031] After the treatment with the acidic solution, a water-washing treatment may be carried out, if necessary. The time and temperature of the water-washing treatment are not particularly limited, but are preferably 5 to 40°C, more preferably 15 to 30°C, and are preferably 0.1 to 10 minutes, more preferably 0.5 to 7 minutes. The water-washing treatment may involve both stored water washing and running water washing, or only one of them may be carried out, but it is preferable to carry out at least running water washing, and it is more preferable to carry out both stored water washing and running water washing.

[0032] (Circuit Pattern Forming Step (4)) The circuit pattern forming step (4) is a step of forming a circuit pattern on the interlayer insulating layer after the particle (X) dissolving step (3-2) (see FIG. 5). From the viewpoint of forming fine wiring, the circuit pattern is preferably formed by a semi-additive process. The semi-additive process forms the circuit pattern and also establishes via conductivity. In the semi-additive process, first, a seed layer 105 is formed by electroless copper plating using a palladium catalyst or the like on the via bottom, via wall surface, and the entire surface of the interlayer insulating layer after the particle (X) dissolving step (3-2). The seed layer 105 serves to form a power supply layer for electrolytic copper plating, and is preferably formed to a thickness of approximately 0.1 to 2.0 μm. If the thickness of the seed layer 105 is 0.1 μm or more, a decrease in connection reliability during electrolytic copper plating tends to be suppressed. If the thickness is 2.0 μm or less, there is no need to increase the amount of etching when flash etching the seed layer between wirings, and damage to the wiring during etching tends to be suppressed.

[0033] As pretreatments before the formation of the seed layer, a cleaner treatment (also referred to as a conditioner treatment) and a water rinsing treatment, as well as soft etching and a water rinsing treatment, may be performed as necessary. The cleaner treatment may be performed using a commercially available alkaline cleaner (conditioner solution) at preferably 40 to 80°C, more preferably 50 to 70°C, for preferably 0.1 to 10 minutes, more preferably 0.5 to 7 minutes. The water rinsing treatment after the cleaner treatment is similar to the water rinsing treatment described above, and preferred embodiments are also the same. Soft etching can be performed using sodium persulfate and sulfuric acid, or ammonium persulfate and sulfuric acid, at preferably 10 to 40°C, more preferably 20 to 35°C, for preferably 0.1 to 3 minutes, more preferably 0.3 to 1 minute. The water rinsing treatment after the soft etching is similar to the water rinsing treatment described above, and preferred embodiments are also the same. The soft etching can also be performed as the particle (X) dissolving step (3-2).

[0034] The electroless copper plating process is carried out by depositing metallic copper on the surface of the via and the interlayer insulating layer by a reaction between copper ions and a reducing agent. The electroless plating process and the electrolytic plating process may be performed by any known method and are not particularly limited. Commercially available electroless copper plating solutions can be used, such as "MSK-DK" manufactured by Atotech Japan K.K. and "ThruCup (registered trademark) PEA series" manufactured by Uemura Kogyo Co., Ltd.

[0035] After the electroless copper plating process, a dry film resist is thermocompressed onto the electroless copper plating using a roll laminator. The thickness of the dry film resist must be greater than the wiring height after electrolytic copper plating. From this perspective, a dry film resist with a thickness of 5 to 30 μm is preferred. Examples of dry film resists that can be used include the "Photec (registered trademark)" series manufactured by Resonac Corporation. After thermocompression bonding of the dry film resist, the dry film resist is exposed, for example, through a mask on which the desired wiring pattern is drawn. Exposure can be performed using the same equipment and light source as those used to form vias in the photosensitive resin film. After exposure, the dry film resist is developed using an alkaline aqueous solution, and the unexposed portions are removed to form a resist pattern 106. If necessary, a process of removing development residue from the dry film resist using plasma or the like may then be performed. After development, electrolytic copper plating is performed to form a copper circuit layer (circuit pattern) 107 and via filling.

[0036] After electrolytic copper plating, the dry film resist is stripped using an alkaline aqueous solution or an amine-based stripper. After stripping the dry film resist, the seed layer between the wirings is removed (flash etching). Flash etching is performed using an acidic solution such as sulfuric acid and hydrogen peroxide, and an oxidizing solution. After flash etching, palladium and other materials adhering to the portions between the wirings are removed as needed. Palladium removal is preferably performed using an acidic solution such as nitric acid or hydrochloric acid.

[0037] After the dry film resist is removed or after the flash etching step, a post-baking process is preferably performed. This post-baking process can sufficiently cure unreacted thermosetting components, thereby tending to improve insulation reliability, curing characteristics, and adhesive strength with copper plating. While the thermosetting conditions vary depending on the type of resin composition, a curing temperature of 150 to 240°C and a curing time of 15 to 100 minutes are preferred. The post-baking process completes the entire photovia process for manufacturing the printed wiring board 100A. This process can be repeated depending on the number of interlayer insulating layers required to manufacture a multilayer printed wiring board 100A (see Figure 6). A solder resist layer 108 is preferably formed as the outermost layer.

[0038] [Photosensitive Resin Composition] The photosensitive resin composition of this embodiment is a photosensitive resin composition containing particles (X) that dissolve at 95% by mass or more in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L under conditions of 70° C. and 20 minutes. By using this photosensitive resin composition as a material for an interlayer insulating layer of a printed wiring board, it becomes possible to dissolve the particles (X) in the particle (X) dissolving step (3-2).

[0039] The photosensitive resin composition of this embodiment is suitable for via formation by photolithography (also referred to as photovia formation), and is therefore suitable for forming one or more layers selected from the group consisting of photovias and interlayer insulating layers. Herein, when the term "layer" is used in the present disclosure, such as an interlayer insulating layer, it includes not only solid layers, but also layers that are not solid but have at least a portion in the shape of islands, have holes, and have unclear interfaces with adjacent layers. The solid layer refers to a sheet-like layer that has not been subjected to any particular processing. The photosensitive resin composition of this embodiment is suitable for use as a negative-type photosensitive resin composition. Below, the particles (X) will be described in detail, followed by a detailed description of other components that may be contained in the photosensitive resin composition of this embodiment.

[0040] <Particles (X)> As described above, particles (X) are particles that dissolve at 95% by mass or more in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L at 70°C for 20 minutes. The particles (X) are easily dissolved in the particle (X) dissolving step (3-2). From the viewpoint of the solubility of particles (X) in the particle (X) dissolving step (3-2), the concentration of the sulfuric acid aqueous solution is preferably 10 to 80 ml / L, more preferably 15 to 50 ml / L. The particles (X) are particles that dissolve at 97% by mass or more, more preferably 99% by mass or more, and may even be particles that dissolve 100% by mass in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L at 70°C for 20 minutes. Here, the dissolution amount is the amount of particles (X) that dissolves when the particles (X) are submerged in the sulfuric acid aqueous solution and stirred at 70°C for 1 hour. The amount of dissolved particles (X) can be calculated from the weight of particles (X) obtained by immersing particles (X) in a sulfuric acid aqueous solution of the predetermined concentration at 70° C. for 20 minutes and then filtering the solution. Note that if no solid content is obtained upon filtration, it can be said that particles (X) are 100% dissolved.

[0041] The particles (X) may be inorganic particles or organic particles. The inorganic particles are not particularly limited, but include magnesium-containing inorganic particles such as magnesium hydroxide, magnesium carbonate, magnesium oxide, magnesium peroxide, magnesium diboride, magnesium nitride, magnesium sulfide, calcium magnesium carbonate, magnesium nitrate, magnesium sulfate, magnesium sulfite, trimagnesium phosphate, magnesium phosphate, spinel, talc, and serpentine; calcium-containing inorganic particles such as calcium oxide, calcium hydroxide, calcium sulfide, calcium sulfate, calcium hydrogen sulfate, calcium thiosulfate, calcium sulfite, calcium selenide, calcium selenate, calcium nitrite, calcium phosphate, calcium carbonate, calcium hydrogen carbonate, calcium metasilicate, calcium tetraborate, calcium chromate, and calcium dichromate; and zinc-containing inorganic particles such as zinc oxide, zinc hydroxide, zinc sulfate, zinc nitrate, and zinc carbonate. Among these, magnesium-containing inorganic particles and zinc-containing inorganic particles are preferred from the viewpoint of solubility in the particle (X) dissolution step (3-2), with magnesium hydroxide, magnesium carbonate, and zinc oxide being more preferred, and magnesium hydroxide and magnesium carbonate being even more preferred. The organic particles are not particularly limited, but examples thereof include melamine resin, benzoguanamine, polyadamantyl(meth)acrylate, polyt-butyl(meth)acrylate, polyacrylic acid, etc. Among these, polyadamantyl(meth)acrylate and polyt-butyl(meth)acrylate are preferred from the viewpoint of solubility in the particle (X) dissolving step (3-2).

[0042] The volume average particle diameter of the particles (X) is not particularly limited, but from the viewpoint of peel strength with copper plating, it is preferably 0.1 to 3 μm, more preferably 0.2 to 2.0 μm, even more preferably 0.3 to 1.7 μm, and particularly preferably 0.3 to 1.5 μm, and may be 0.5 to 1.5 μm or 0.7 to 1.5 μm. Here, in the present disclosure, the volume average particle diameter is determined as the particle diameter corresponding to an integrated value of 50% (by volume) in the particle size distribution by measuring particles dispersed in a solvent at a refractive index of 1.38 using a submicron particle analyzer (manufactured by Beckman Coulter, Inc., product name: N5) in accordance with ISO 13321.

[0043] In the photosensitive resin composition of this embodiment, the content of particles (X) is not particularly limited, but is preferably 10 to 70 vol%, more preferably 15 to 60 vol%, and even more preferably 20 to 55 vol%, based on the total solid content. It may be 25 to 50 vol%, or may be 25 to 40 vol%. When the content of particles (X) is equal to or greater than the lower limit, high adhesive strength with copper plating tends to be exhibited while reducing the surface roughness of the interlayer insulating layer. When the content is equal to or less than the upper limit, good resolution tends to be maintained. Incidentally, when the content of particles (X) is 15 vol% or greater based on the total solid content, the effect of improving high adhesive strength with copper plating tends to be further enhanced.

[0044] The photosensitive resin composition of the present embodiment preferably further contains (A) a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent, and (B) a thermosetting resin. Hereinafter, the components (A) and (B) will be described in detail in this order, followed by detailed descriptions of the other components.

[0045] <(A) Photopolymerizable Compound Having an Ethylenically Unsaturated Group and an Acidic Substituent> The component (A) is a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent. As the component (A), one type may be used alone, or two or more types may be used in combination.

[0046] Component (A) is a compound that exhibits photopolymerizability, particularly radical polymerizability, due to the presence of an ethylenically unsaturated group. Examples of the ethylenically unsaturated group contained in component (A) include photopolymerizable functional groups such as vinyl, allyl, propargyl, butenyl, ethynyl, phenylethynyl, maleimide, nadimide, and (meth)acryloyl groups. Among these, (meth)acryloyl groups are preferred from the viewpoints of reactivity and via resolution.

[0047] Component (A) has an acidic substituent to enable alkaline development. Examples of the acidic substituent that component (A) has include a carboxy group, a sulfonic acid group, and a phenolic hydroxyl group. Of these, a carboxy group is preferred from the viewpoint of via resolution. The acid value of component (A) is preferably 20 to 200 mgKOH / g, more preferably 40 to 180 mgKOH / g, even more preferably 70 to 150 mgKOH / g, and particularly preferably 90 to 120 mgKOH / g. When the acid value of component (A) is equal to or greater than the lower limit, the solubility of the photosensitive resin film in dilute alkaline solutions tends to be excellent, while when the acid value is equal to or less than the upper limit, the dielectric constant tends to be excellent. The acid value of component (A) can be measured by the method described in the Examples. Two or more components (A) with different acid values ​​may be used in combination. In this case, it is preferable that the weighted average acid value of the acid values ​​of the two or more components (A) falls within one of the above-mentioned ranges.

[0048] The weight-average molecular weight (Mw) of component (A) is preferably 600 to 30,000, more preferably 800 to 25,000, even more preferably 1,000 to 18,000, still more preferably 1,000 to 8,000, particularly preferably 1,200 to 5,000, and most preferably 1,200 to 3,500. When the weight-average molecular weight (Mw) of component (A) is within this range, the adhesive strength to copper plating, heat resistance, and insulation reliability tend to be excellent. Herein, the weight-average molecular weight (Mw) is a value determined by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent, converted into standard polystyrene, and more specifically, a value measured according to the method described in the Examples.

[0049] From the viewpoint of via resolution, adhesive strength with copper plating, and electrical insulation reliability, component (A) preferably contains an alicyclic skeleton, but is not required to contain an alicyclic skeleton. The alicyclic skeleton contained in component (A) is preferably an alicyclic skeleton having 5 to 20 ring carbon atoms, more preferably an alicyclic skeleton having 5 to 18 ring carbon atoms, even more preferably an alicyclic skeleton having 6 to 18 ring carbon atoms, particularly preferably an alicyclic skeleton having 8 to 14 ring carbon atoms, and most preferably an alicyclic skeleton having 8 to 12 ring carbon atoms, from the viewpoint of via resolution, adhesive strength with copper plating, and electrical insulation reliability. Furthermore, from the viewpoint of via resolution, adhesive strength with copper plating, and electrical insulation reliability, the alicyclic skeleton preferably consists of two or more rings, more preferably two to four rings, and even more preferably three rings. Examples of alicyclic skeletons having two or more rings include a norbornane skeleton, a decalin skeleton, a bicycloundecane skeleton, and a saturated dicyclopentadiene skeleton. Among these, a saturated dicyclopentadiene skeleton is preferred from the viewpoints of via resolution, adhesive strength with copper plating, and electrical insulation reliability. From the same viewpoints, component (A) preferably contains an alicyclic skeleton represented by the following general formula (A-1):

[0050] (In the formula, R A1 represents an alkyl group having 1 to 12 carbon atoms, and may be substituted anywhere in the alicyclic skeleton. 1 is an integer from 0 to 6. * is a binding site to another structure.)

[0051] In the general formula (A-1), R A1 Examples of the alkyl group having 1 to 12 carbon atoms represented by m include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, etc. As the alkyl group, an alkyl group having 1 to 6 carbon atoms is preferred, an alkyl group having 1 to 3 carbon atoms is more preferred, and a methyl group is even more preferred. 1 is an integer of 0 to 6, preferably an integer of 0 to 2, and more preferably 0. 1 is an integer from 2 to 6, a plurality of R A1 may be the same or different. A1may be substituted on the same carbon atom or different carbon atoms, to the extent possible. * represents a bonding site to another structure, and may be bonded to any carbon atom on the alicyclic skeleton, but is preferably bonded to the carbon atom at the site represented by 1 or 2 and the carbon atom at the site represented by 3 or 4 in the following general formula (A-1'):

[0052] (In the formula, R A1 , m 1 and * are the same as those in general formula (A-1).

[0053] Furthermore, from the viewpoints of via resolution and adhesive strength with copper plating, component (A) is preferably an acid-modified vinyl group-containing resin obtained by reacting (a3) ​​a saturated or unsaturated group-containing polybasic acid anhydride with (a1) an epoxy resin modified with (a2) an ethylenically unsaturated group-containing organic acid [hereinafter, sometimes referred to as component (A')]. Here, the term "acid-modified" in the acid-modified vinyl group-containing resin refers to the presence of an acidic substituent, and the term "vinyl group" refers to an ethylenically unsaturated group. Preferred embodiments of component (A) obtained from (a1) an epoxy resin, (a2) an ethylenically unsaturated group-containing organic acid, and (a3) ​​a saturated or unsaturated group-containing polybasic acid anhydride are described below.

[0054] ((a1) Epoxy Resin) The (a1) epoxy resin is preferably an epoxy resin having two or more epoxy groups. The (a1) epoxy resin may be used alone or in combination of two or more types. The (a1) epoxy resin is classified into glycidyl ether type epoxy resin, glycidyl amine type epoxy resin, glycidyl ester type epoxy resin, etc. Among these, glycidyl ether type epoxy resin is preferred.

[0055] (a1) Epoxy resins can be classified into various epoxy resins depending on the main skeleton, such as epoxy resins having an alicyclic skeleton, novolac epoxy resins, bisphenol epoxy resins, aralkyl epoxy resins, and other epoxy resins. Among these, epoxy resins having an alicyclic skeleton and novolac epoxy resins are preferred. Although not particularly limited, it is preferred that novolac epoxy resins, bisphenol epoxy resins, aralkyl epoxy resins, and other epoxy resins have an alicyclic skeleton.

[0056] -Epoxy resin having an alicyclic skeleton- The alicyclic skeleton of the epoxy resin having an alicyclic skeleton is explained in the same manner as the alicyclic skeleton of the component (A) described above, and preferred embodiments are also the same. As the epoxy resin having an alicyclic skeleton, an epoxy resin represented by the following general formula (A-2) is preferred.

[0057] (In the formula, R A1 represents an alkyl group having 1 to 12 carbon atoms, and may be substituted anywhere in the alicyclic skeleton. A2 represents an alkyl group having 1 to 12 carbon atoms. 1 is an integer from 0 to 6, m 2 is an integer from 0 to 3. n is a number from 0 to 50.

[0058] In general formula (A-2), R A1 represents R in general formula (A-1). A1 The preferred embodiments are also the same as those of the general formula (A-2). A2 Examples of the alkyl group having 1 to 12 carbon atoms represented by m include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, etc. As the alkyl group, an alkyl group having 1 to 6 carbon atoms is preferred, an alkyl group having 1 to 3 carbon atoms is more preferred, and a methyl group is even more preferred. 1 is m in general formula (A-1) 1 The preferred embodiments are also the same as those of the general formula (A-2). 2is an integer of 0 to 3, preferably 0 or 1, and more preferably 0. In general formula (A-2), n represents the repeating number of the structural unit in the parentheses and is a number of 0 to 50. Usually, epoxy resins are mixtures of structural units in the parentheses with different repeating numbers, and in such cases, n represents the average value of the mixture. Preferably, n is a number of 0 to 30.

[0059] As the epoxy resin having an alicyclic skeleton, commercially available products may be used, and examples of commercially available products include XD-1000 (trade name, manufactured by Nippon Kayaku Co., Ltd.) and EPICLON (registered trademark) HP-7200 (trade name, manufactured by DIC Corporation).

[0060] -Novolac-type epoxy resin- Examples of novolac-type epoxy resins include bisphenol novolac-type epoxy resins such as bisphenol A novolac-type epoxy resin, bisphenol F novolac-type epoxy resin, and bisphenol S novolac-type epoxy resin; phenol novolac-type epoxy resin, cresol novolac-type epoxy resin, biphenyl novolac-type epoxy resin, and naphthol novolac-type epoxy resin. The novolac-type epoxy resin is not particularly limited, but cresol novolac-type epoxy resin is preferred. Furthermore, the novolac-type epoxy resin is preferably an epoxy resin having a structural unit represented by the following general formula (A-3):

[0061] (In the formula, R A3 represents a hydrogen atom or a methyl group, and Y A1 Each of R independently represents a hydrogen atom or a glycidyl group. A3 may be the same or different. A1 At least one of these represents a glycidyl group.

[0062] R A3 From the viewpoints of via resolution and adhesive strength with copper plating, it is preferable that Y be a hydrogen atom. A1are preferably glycidyl groups. The number of structural units in the (a1) epoxy resin having the structural unit represented by general formula (A-3) is 1 or more, preferably 10 to 100, more preferably 15 to 80, and even more preferably 15 to 70. When the number of structural units is within the above range, the adhesive strength with copper plating, heat resistance, and insulation reliability tend to be improved. In general formula (A-3), R A3 are all hydrogen atoms, and Y A1 In addition, those in which R is a glycidyl group are commercially available as EXA-7376 series (trade name, manufactured by DIC Corporation). A3 are all methyl groups, and Y A1 However, those having a glycidyl group are commercially available as EPON SU8 series (trade name, manufactured by Mitsubishi Chemical Corporation).

[0063] Examples of bisphenol-type epoxy resins include bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol S-type epoxy resins, and 3,3',5,5'-tetramethyl-4,4'-diglycidyloxydiphenylmethane. Examples of aralkyl-type epoxy resins include phenol aralkyl-type epoxy resins, biphenyl aralkyl-type epoxy resins, and naphthol aralkyl-type epoxy resins. Other examples of epoxy resins include stilbene-type epoxy resins, naphthalene skeleton-containing epoxy resins, biphenyl-type epoxy resins, dihydroanthracene-type epoxy resins, cyclohexanedimethanol-type epoxy resins, trimethylol-type epoxy resins, alicyclic epoxy resins, aliphatic linear epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, and rubber-modified epoxy resins.

[0064] ((a2) Ethylenically Unsaturated Group-Containing Organic Acid) The (a2) ethylenically unsaturated group-containing organic acid is preferably an ethylenically unsaturated group-containing monocarboxylic acid. Examples of the ethylenically unsaturated group contained in the component (a2) include the same ethylenically unsaturated groups as those contained in the component (A). Examples of the component (a2) include acrylic acid, acrylic acid dimer, methacrylic acid, β-furfurylacrylic acid, β-styrylacrylic acid, cinnamic acid, crotonic acid, α-cyanocinnamic acid and other acrylic acid derivatives; half-ester compounds which are reaction products of hydroxyl group-containing acrylates and dibasic acid anhydrides; and half-ester compounds which are reaction products of vinyl group-containing monoglycidyl ethers or vinyl group-containing monoglycidyl esters and dibasic acid anhydrides. One type of component (a2) may be used alone, or two or more types may be used in combination.

[0065] The half-ester compound can be obtained by reacting one or more ethylenically unsaturated group-containing compounds selected from the group consisting of hydroxyl group-containing acrylates, vinyl group-containing monoglycidyl ethers, and vinyl group-containing monoglycidyl esters with a dibasic acid anhydride. The reaction is preferably carried out by reacting the ethylenically unsaturated group-containing compound and the dibasic acid anhydride in equimolar amounts.

[0066] Examples of the hydroxyl group-containing acrylate used in the synthesis of the semi-ester compound include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, etc. Examples of the vinyl group-containing monoglycidyl ether include glycidyl (meth)acrylate, etc.

[0067] The dibasic acid anhydride used in the synthesis of the half-ester compound may contain either a saturated group or an unsaturated group, and examples of the dibasic acid anhydride include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride.

[0068] In the reaction between component (a1) and component (a2), the amount of component (a2) used relative to 1 equivalent of the epoxy group in component (a1) is preferably 0.6 to 1.05 equivalents, more preferably 0.7 to 1.02 equivalents, and even more preferably 0.8 to 1.0 equivalents. By reacting components (a1) and (a2) in this ratio, the photopolymerizability of component (A) is improved, and the resulting photosensitive resin composition tends to have improved via resolution.

[0069] It is preferable that the (a1) component and the (a2) component are dissolved in an organic solvent and reacted. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ether compounds such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl cellosolve acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha. The organic solvent may be used alone or in combination of two or more.

[0070] The reaction between component (a1) and component (a2) preferably uses a catalyst to promote the reaction. Examples of such catalysts include amine-based catalysts such as triethylamine and benzylmethylamine; quaternary ammonium salt catalysts such as methyltriethylammonium chloride, benzyltrimethylammonium chloride, benzyltrimethylammonium bromide and benzyltrimethylammonium iodide; and phosphine-based catalysts such as triphenylphosphine. Among these, phosphine-based catalysts are preferred, with triphenylphosphine being more preferred. One catalyst may be used alone, or two or more catalysts may be used in combination. When a catalyst is used, the amount used is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 2 parts by mass, per 100 parts by mass of the total of component (a1) and component (a2), from the viewpoint of obtaining an appropriate reaction rate.

[0071] In the reaction between component (a1) and component (a2), it is preferable to use a polymerization inhibitor to prevent polymerization during the reaction. Examples of polymerization inhibitors include hydroquinone, methylhydroquinone, hydroquinone monomethyl ether, catechol, and pyrogallol. One polymerization inhibitor may be used alone, or two or more polymerization inhibitors may be used in combination. When a polymerization inhibitor is used, the amount used is preferably 0.01 to 1 part by mass, more preferably 0.02 to 0.8 parts by mass, and even more preferably 0.1 to 0.5 parts by mass, per 100 parts by mass of the total of component (a1) and component (a2).

[0072] The reaction temperature between component (a1) and component (a2) is preferably 60 to 150°C, more preferably 80 to 120°C, and even more preferably 90 to 110°C, from the viewpoint of ensuring sufficient reactivity and allowing the reaction to proceed homogeneously.

[0073] As described above, when an ethylenically unsaturated group-containing monocarboxylic acid is used as component (a2), component (A') obtained by reacting component (a1) with component (a2) has hydroxyl groups formed by a ring-opening addition reaction between the epoxy groups of component (a1) and the carboxyl groups of component (a2). Next, by further reacting component (A') with component (a3), an acid-modified vinyl group-containing resin can be obtained in which the hydroxyl groups of component (A') (including the hydroxyl groups originally present in component (a1)) and the acid anhydride groups of component (a3) ​​are half-esterified.

[0074] ((a3) Polybasic Acid Anhydride) The component (a3) ​​may contain a saturated group or an unsaturated group. Examples of the component (a3) ​​include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride. Among these, tetrahydrophthalic anhydride is preferred from the viewpoint of via resolution. One type of component (a3) ​​may be used alone, or two or more types may be used in combination.

[0075] In the reaction between component (A') and component (a3), for example, the acid value of the acid-modified vinyl group-containing resin can be adjusted by reacting 0.1 to 1.0 equivalents of component (a3) ​​with 1 equivalent of hydroxyl groups in component (A').

[0076] The reaction temperature between component (A') and component (a3) ​​is preferably 50 to 150°C, more preferably 60 to 120°C, and even more preferably 70 to 100°C, from the viewpoint of ensuring sufficient reactivity and allowing the reaction to proceed homogeneously.

[0077] The content of the component (A) in the photosensitive resin composition of the present embodiment is not particularly limited, but from the viewpoints of heat resistance, dielectric constant, and chemical resistance, it is preferably 10 to 80 mass %, more preferably 15 to 75 mass %, even more preferably 25 to 70 mass %, particularly preferably 35 to 70 mass %, and most preferably 45 to 70 mass %, based on the total amount of resin components in the photosensitive resin composition.

[0078] <(B) Thermosetting Resin> Component (B) is a thermosetting resin. Component (B) does not include component (A). By including the thermosetting resin (B) in the photosensitive resin composition of this embodiment, the heat resistance tends to be improved in addition to the adhesive strength with copper plating and the insulating reliability. Examples of thermosetting resins include epoxy resins, phenolic resins, unsaturated imide resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins, and melamine resins. Furthermore, without being particularly limited thereto, known thermosetting resins can be used. Among these, epoxy resins are preferred from the viewpoints of adhesive strength with copper plating, insulating reliability, and heat resistance. Component (B) may be used alone or in combination of two or more.

[0079] The epoxy resin is preferably an epoxy resin having two or more epoxy groups. Epoxy resins are classified into glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, etc. Among these, glycidyl ether type epoxy resins are preferred.

[0080] Epoxy resins are also classified into various epoxy resins depending on the difference in the main skeleton, and each of the above types of epoxy resins is further classified as follows: Specifically, bisphenol-based epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, and bisphenol S-type epoxy resins; bisphenol-based novolac-type epoxy resins such as bisphenol A-type epoxy resins and bisphenol F-type novolac-type epoxy resins; novolac-type epoxy resins other than the above bisphenol-based novolac-type epoxy resins such as phenol novolac-type epoxy resins, cresol novolac-type epoxy resins, and biphenyl novolac-type epoxy resins; phenol aralkyl-type epoxy resins; stilbene-type epoxy resins; naphtha-type epoxy resins; They are classified into naphthalene skeleton-containing epoxy resins such as novolac-type epoxy resins, naphthol-type epoxy resins, naphthol aralkyl-type epoxy resins, and naphthylene ether-type epoxy resins; biphenyl-type epoxy resins; biphenyl aralkyl-type epoxy resins; xylylene-type epoxy resins; dihydroanthracene-type epoxy resins; alicyclic epoxy resins such as saturated dicyclopentadiene-type epoxy resins; heterocyclic epoxy resins; spiro ring-containing epoxy resins; cyclohexanedimethanol-type epoxy resins; trimethylol-type epoxy resins; aliphatic linear epoxy resins; and rubber-modified epoxy resins.

[0081] Among these, the epoxy resin preferably contains at least one selected from the group consisting of bisphenol-based epoxy resins, naphthalene skeleton-containing epoxy resins, and biphenylaralkyl-type epoxy resins, particularly from the viewpoints of heat resistance, electrical insulation reliability, developability, and adhesive strength with copper plating, and more preferably contains at least one selected from the group consisting of naphthalene skeleton-containing epoxy resins and biphenylaralkyl-type epoxy resins.

[0082] In the photosensitive resin composition of this embodiment, the equivalent ratio of the acidic substituent in component (A) to the epoxy group in component (B) [epoxy group / acidic substituent] is not particularly limited, but from the viewpoints of insulation reliability, dielectric constant, heat resistance, and adhesive strength with copper plating, it is preferably 0.5 to 6.0, more preferably 0.7 to 4.0, even more preferably 0.8 to 2.0, and particularly preferably 0.9 to 1.8.

[0083] The content of the component (B) in the photosensitive resin composition of the present embodiment is not particularly limited, but from the viewpoints of insulation reliability, relative dielectric constant, heat resistance, and adhesive strength with copper plating, it is preferably 1 to 50 mass %, more preferably 5 to 30 mass %, even more preferably 10 to 25 mass %, and most preferably 15 to 25 mass %, based on the total amount of resin components in the photosensitive resin composition.

[0084] <(C) Crosslinking Agent> The photosensitive resin composition of this embodiment preferably further contains a crosslinking agent as component (C). The crosslinking agent is preferably a crosslinking agent having two or more ethylenically unsaturated groups and no acidic substituent. The crosslinking agent reacts with the ethylenically unsaturated groups of component (A) to increase the crosslink density of the photosensitive resin film after curing. Therefore, by including a crosslinking agent, the photosensitive resin composition of this embodiment tends to further improve the heat resistance and relative dielectric constant. The component (C) may be used alone or in combination of two or more types.

[0085] Examples of component (C) include a bifunctional monomer having two ethylenically unsaturated groups and a polyfunctional monomer having three or more ethylenically unsaturated groups. Component (C) preferably contains the polyfunctional monomer. Examples of the ethylenically unsaturated groups contained in component (C) include the same ethylenically unsaturated groups as those contained in component (A), and preferred examples are also the same.

[0086] Examples of the bifunctional monomer include aliphatic di(meth)acrylates such as trimethylolpropane di(meth)acrylate, polypropylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate; di(meth)acrylates having an alicyclic skeleton such as dicyclopentadiene di(meth)acrylate and tricyclodecane dimethanol di(meth)acrylate; and aromatic di(meth)acrylates such as 2,2-bis(4-(meth)acryloxypolyethoxypolypropoxyphenyl)propane and bisphenol A diglycidyl ether di(meth)acrylate. Among these, from the viewpoint of obtaining a lower dielectric constant, di(meth)acrylates having an alicyclic skeleton are preferred, and tricyclodecane dimethanol diacrylate is more preferred.

[0087] Examples of the polyfunctional monomer include (meth)acrylate compounds having a skeleton derived from trimethylolpropane, such as trimethylolpropane tri(meth)acrylate; (meth)acrylate compounds having a skeleton derived from tetramethylolmethane, such as tetramethylolmethane tri(meth)acrylate and tetramethylolmethane tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from pentaerythritol, such as pentaerythritol tri(meth)acrylate and pentaerythritol tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from dipentaerythritol, such as dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate; (meth)acrylate compounds having a skeleton derived from ditrimethylolpropane, such as ditrimethylolpropane tetra(meth)acrylate; and (meth)acrylate compounds having a skeleton derived from diglycerin. Among these, from the viewpoints of via resolution and adhesive strength with copper plating, (meth)acrylate compounds having a skeleton derived from trimethylolpropane are preferred, and trimethylolpropane tri(meth)acrylate is more preferred. Here, the "(meth)acrylate compound having a skeleton derived from XXX" (where XXX is the name of the compound) refers to an esterification product of XXX and (meth)acrylic acid, and the esterification product also includes compounds modified with an alkyleneoxy group.

[0088] When the photosensitive resin composition of the present embodiment contains a (C) crosslinking agent, the content of the (C) crosslinking agent is not particularly limited, but from the viewpoints of heat resistance and relative dielectric constant, it is preferably 1 to 85 parts by mass, more preferably 5 to 70 parts by mass, even more preferably 10 to 50 parts by mass, and particularly preferably 10 to 40 parts by mass per 100 parts by mass of the component (A).

[0089] <(D) Elastomer> The photosensitive resin composition of this embodiment preferably further contains an elastomer as component (D). By containing the (D) elastomer, the photosensitive resin composition of this embodiment tends to further improve the adhesive strength with copper plating. Furthermore, by containing the (D) elastomer, the photosensitive resin composition of this embodiment tends to have the effect of suppressing "a decrease in flexibility and adhesive strength with copper plating" caused by distortion (internal stress) that may occur due to cure shrinkage of the (A) component. One type of (D) elastomer may be used alone, or two or more types may be used in combination.

[0090] The (D) elastomer may have a reactive functional group at the molecular end or in the molecular chain. Examples of the reactive functional group include an acid anhydride group, an epoxy group, a hydroxyl group, a carboxyl group, an amino group, an amide group, an isocyanato group, an acrylic group, a methacrylic group, and a vinyl group. Among these, from the viewpoints of via resolution and adhesive strength with copper plating, an acid anhydride group, an epoxy group, a hydroxyl group, a carboxyl group, an amino group, and an amide group are preferred, an acid anhydride group and an epoxy group are more preferred, and an acid anhydride group is even more preferred. The acid anhydride group is preferably an acid anhydride group derived from phthalic anhydride, maleic anhydride, trimellitic anhydride, pyromellitic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylnadic anhydride, nadic anhydride, glutaric anhydride, dimethylglutaric anhydride, diethylglutaric anhydride, succinic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, or the like, and more preferably an acid anhydride group derived from maleic anhydride. When the (D) elastomer has acid anhydride groups, the number of acid anhydride groups in one molecule is preferably 1 to 10, more preferably 3 to 10, and even more preferably 6 to 10, from the viewpoints of via resolution and dielectric constant.

[0091] The photosensitive resin composition of this embodiment preferably contains, as the elastomer (D), an elastomer having an ethylenically unsaturated group and an acidic substituent. Examples of the acidic substituent and the ethylenically unsaturated group include the same acidic substituent and ethylenically unsaturated group as those contained in the component (A). Among these, the elastomer (D) preferably has the aforementioned acid anhydride group as the acidic substituent and the ethylenically unsaturated group as the 1,2-vinyl group described below.

[0092] Examples of the (D) elastomer include polybutadiene-based elastomers, polyester-based elastomers, styrene-based elastomers, olefin-based elastomers, urethane-based elastomers, polyamide-based elastomers, acrylic-based elastomers, silicone-based elastomers, derivatives of these elastomers, etc. Among these, polybutadiene-based elastomers are preferred from the viewpoints of improving adhesive strength with copper plating and further improving compatibility and solubility with resin components.

[0093] Suitable examples of polybutadiene elastomers include those containing 1,2-vinyl groups and having 1,4-trans structural units and 1,4-cis structural units. As described above, from the viewpoint of via resolution, the polybutadiene elastomer is preferably a polybutadiene elastomer having an acid anhydride group that has been modified with an acid anhydride, and more preferably a polybutadiene elastomer having an acid anhydride group derived from maleic anhydride. Polybutadiene-based elastomers are commercially available, and specific examples thereof include "POLYVEST (registered trademark) MA75" and "POLYVEST (registered trademark) EP MA120" (all of which are product names manufactured by Evonik), "Ricon (registered trademark) 100," "Ricon (registered trademark) 130MA8," "Ricon (registered trademark) 131MA5," "Ricon (registered trademark) 131MA17," and "Ricon (registered trademark) 184MA6" (all of which are product names manufactured by Cray Valley).

[0094] From the viewpoint of adhesive strength with copper plating, the polybutadiene-based elastomer may be a polybutadiene having an epoxy group (hereinafter, may be referred to as an epoxidized polybutadiene). From the viewpoint of adhesive strength with copper plating and flexibility, the epoxidized polybutadiene is preferably an epoxidized polybutadiene represented by the following general formula (D-1):

[0095] (In the formula, a, b, and c each represent the ratio of the structural units in parentheses, where a is 0.05 to 0.40, b is 0.02 to 0.30, and c is 0.30 to 0.80, and further, a+b+c=1.00 and (a+c)>b are satisfied. y represents the number of structural units in square brackets and is an integer from 10 to 250.)

[0096] In the general formula (D-1), the structural units in the square brackets may be bonded in any order. In other words, the structural unit shown on the left, the structural unit shown in the center, and the structural unit shown on the right may be interchanged, and when they are represented as (a), (b), and (c), respectively, various bonding orders are possible, such as -[(a)-(b)-(c)]-[(a)-(b)-(c)-]-, -[(a)-(c)-(b)]-[(a)-(c)-(b)-]-, -[(b)-(a)-(c)]-[(b)-(a)-(c)-]-, -[(a)-(b)-(c)]-[(c)-(b)-(a)-]-, -[(a)-(b)-(a)]-[(c)-(b)-(c)-]-, -[(a)-(b)-(a)]-[(c)-(b)-(c)-]-, -[(c)-(b)-(c)]-[(b)-(a)-(a)-]-. From the viewpoints of adhesive strength with copper plating and flexibility, a is preferably 0.10 to 0.30, b is preferably 0.10 to 0.30, and c is preferably 0.40 to 0.80. From the same viewpoints, y is preferably an integer of 30 to 180.

[0097] Examples of polyester elastomers include those obtained by polycondensation of dicarboxylic acids or their derivatives with diol compounds or their derivatives. Examples of dicarboxylic acids include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, as well as aromatic dicarboxylic acids in which the hydrogen atoms of the aromatic nuclei are substituted with methyl groups, ethyl groups, phenyl groups, or the like; aliphatic dicarboxylic acids having 2 to 20 carbon atoms such as adipic acid, sebacic acid, and dodecanedicarboxylic acid; and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid. Examples of diol compounds include aliphatic diols such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, and 1,10-decanediol; alicyclic diols such as 1,4-cyclohexanediol; and aromatic diols such as bisphenol A, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-3-methylphenyl)propane, and resorcinol. Suitable polyester elastomers include multiblock copolymers in which an aromatic polyester (e.g., polybutylene terephthalate) portion serves as the hard segment component and an aliphatic polyester (e.g., polytetramethylene glycol) portion serves as the soft segment component. Multiblock copolymers are available in a variety of grades depending on the type, ratio, and molecular weight of the hard and soft segments.

[0098] The number average molecular weight of the (D) elastomer is not particularly limited, but is preferably 10,000 to 80,000, or may be 20,000 to 70,000, 30,000 to 65,000, or 40,000 to 60,000. The number average molecular weight of the (D) elastomer is determined by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent, in terms of standard polystyrene.

[0099] When the photosensitive resin composition of the present embodiment contains the elastomer (D), the content of the elastomer (D) is not particularly limited, but from the viewpoints of heat resistance and adhesive strength with copper plating, it is preferably 0.5 to 15 mass %, more preferably 1 to 10 mass %, even more preferably 1 to 8 mass %, and particularly preferably 3 to 8 mass %, based on the total amount of resin components in the photosensitive resin composition.

[0100] <(E) Inorganic Filler> The photosensitive resin composition of this embodiment may further contain an inorganic filler as component (E). This component (E) does not contain the particles (X). In other words, component (E) is an inorganic filler other than the particles (X). When the photosensitive resin composition of this embodiment contains the inorganic filler (E), the low thermal expansion coefficient, heat resistance, and flame retardancy tend to be further improved. Examples of component (E) include, but are not limited to, silica, alumina, titanium oxide, mica, beryllia, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, aluminum hydroxide, aluminum silicate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay (e.g., calcined clay), molybdenum compounds such as zinc molybdate, aluminum borate, and silicon carbide. One type of component (E) may be used alone, or two or more types may be used in combination. Among these, silica, alumina, and mica are preferred as inorganic fillers from the viewpoints of thermal expansion coefficient, heat resistance, and flame retardancy, silica and alumina are more preferred, and silica is even more preferred. Examples of silica include crushed silica, fumed silica, and fused silica (fused spherical silica).

[0101] There are no particular limitations on the volume average particle size of component (E), but it is preferably 0.01 to 20 μm, more preferably 0.1 to 10 μm, even more preferably 0.2 to 1 μm, and particularly preferably 0.3 to 0.8 μm.

[0102] (Content of Component (E)) When the photosensitive resin composition of this embodiment contains the component (E), the content of the component (E) is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less, based on the total solid content of the photosensitive resin composition, from the viewpoint of not impairing the effect of the particles (X). The photosensitive resin composition of this embodiment does not need to contain the component (E).

[0103] <(F) Organic Filler> The photosensitive resin composition of this embodiment may further contain an organic filler as component (F). The component (F) does not contain the particles (X). In other words, the component (F) is an organic filler other than the particles (X). By including the organic filler (F) in the photosensitive resin composition of this embodiment, the photosensitive resin composition and the photosensitive resin film tend to have a low specific gravity, and depending on the material, the dielectric constant tends to be further reduced. The component (F) preferably contains resin particles formed from at least one selected from the group consisting of a resin having fluorine atoms, polyethylene, polypropylene, polystyrene, polyphenylene ether, and silicone. Among these, from the viewpoint of the effect of reducing the dielectric constant, the component (F) preferably contains resin particles formed from a resin having fluorine atoms, and more preferably contains resin particles formed from a polytetrafluoroethylene (PTFE) resin. The volume average particle diameter of the resin particles is not particularly limited, but is preferably 20 to 1,000 nm, more preferably 30 to 800 nm, even more preferably 50 to 500 nm, and particularly preferably 100 to 300 nm. The method for measuring the volume average particle diameter is as described above.

[0104] When the photosensitive resin composition of this embodiment contains an organic filler (F), the content of the organic filler (F) is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on the total amount of the resin components of the photosensitive resin composition, from the viewpoint of not impairing the effect of the particles (X). The photosensitive resin composition of this embodiment does not need to contain the component (F).

[0105] <(G) Curing Agent> The photosensitive resin composition of this embodiment preferably further contains a curing agent as component (G). By containing the (G) curing agent, the photosensitive resin composition of this embodiment tends to be able to further improve heat resistance, relative dielectric constant, etc. One type of (G) curing agent may be used alone, or two or more types may be used in combination.

[0106] The (G) curing agent may be a curing agent for the (B) thermosetting resin. For example, when the (B) thermosetting resin is an epoxy resin, an epoxy resin curing agent is preferably used. Examples of the epoxy resin curing agent include guanamines such as acetoguanamine and benzoguanamine; polyamines such as diaminodiphenylmethane, m-phenylenediamine, m-xylenediamine, diaminodiphenylsulfone, dicyandiamide, urea, urea derivatives, melamine, and polybasic hydrazides; organic acid salts and / or epoxy adducts thereof; amine complexes of boron trifluoride; triazine derivatives such as ethyldiamino-S-triazine, 2,4-diamino-S-triazine, and 2,4-diamino-6-xylyl-S-triazine; and polyphenols such as polyvinylphenol, polyvinylphenol bromide, phenol novolac, alkylphenol novolac, and triazine ring-containing phenol novolac resin. The polyphenol may be a modified polyphenol modified with, for example, melamine or benzoguanamine. The hydroxyl equivalent of the polyphenol is not particularly limited, but is preferably 40 to 300 g / eq, or may be 40 to 250 g / eq, 60 to 200 g / eq, 80 to 160 g / eq, or 100 to 140 g / eq. Here, the hydroxyl equivalent (g / eq) can be determined by titration using an acetylation method with acetic anhydride.

[0107] When the photosensitive resin composition of the present embodiment contains a (G) curing agent, the content of the (G) curing agent is not particularly limited, but from the viewpoint of further improving the heat resistance and the relative dielectric constant, it is preferably 0.01 to 10 mass %, more preferably 0.05 to 5 mass %, and even more preferably 0.1 to 1 mass %, based on the total amount of the resin components of the photosensitive resin composition.

[0108] <(H) Curing Accelerator> The photosensitive resin composition of the present embodiment preferably further contains a curing accelerator as component (H). By containing the curing accelerator (H), the photosensitive resin composition of the present embodiment tends to be able to further improve heat resistance, relative dielectric constant, etc. One type of (H) curing accelerator may be used alone, or two or more types may be used in combination.

[0109] (H) Examples of the curing accelerator include imidazole compounds such as 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenylimidazole, 2-phenyl-1-benzyl-1H-imidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and isocyanate-masked imidazole (an addition reaction product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole); trimethylamine, N,N-dimethyloctylamine, N-benzyldimethylamine, pyridine, N-methylmorpholine, hexa(N-methyl)melamine, 2,4,6-tris(dimethylaminophenol), and tetramethylamine. Examples of suitable curing agents include tertiary amines such as methylguanidine and m-aminophenol; organic phosphines such as tributylphosphine, triphenylphosphine and tris-2-cyanoethylphosphine; phosphonium salts such as tri-n-butyl(2,5-dihydroxyphenyl)phosphonium bromide and hexadecyltributylphosphonium chloride; quaternary ammonium salts such as benzyltrimethylammonium chloride and phenyltributylammonium chloride; the aforementioned polybasic acid anhydrides; diphenyliodonium tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, and 2,4,6-triphenylthiopyrylium hexafluorophosphate. Among these, imidazole-based compounds are preferred from the viewpoint of obtaining excellent curing properties.

[0110] When the photosensitive resin composition of the present embodiment contains the curing accelerator (H), the content of the curing accelerator (H) is not particularly limited, but from the viewpoint of further improving the heat resistance and the dielectric constant, it is preferably 0.01 to 10 mass %, more preferably 0.05 to 5 mass %, and even more preferably 0.1 to 2 mass %, based on the total amount of the resin components of the photosensitive resin composition.

[0111] <(I) Photopolymerization initiator> The photosensitive resin composition of this embodiment preferably further contains a photopolymerization initiator as component (I). By containing the photopolymerization initiator (I), the photosensitive resin composition of this embodiment tends to further improve the resolution of vias. The photopolymerization initiator (I) may be used alone or in combination of two or more. From the viewpoint of the resolution of vias, the photosensitive resin composition of this embodiment preferably contains two or more types of component (I).

[0112] The (I) photopolymerization initiator is not particularly limited as long as it can photopolymerize an ethylenically unsaturated group, and can be appropriately selected from commonly used photopolymerization initiators. Examples of the (I) photopolymerization initiator include benzoin-based compounds such as benzoin, benzoin methyl ether, and benzoin isopropyl ether; acetophenone-based compounds such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-[4-(methylthio)benzoyl]-2-(4-morpholinyl)propane, and N,N-dimethylaminoacetophenone; 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and the like. ketal compounds such as acetophenone dimethyl ketal and benzil dimethyl ketal; acridine compounds such as 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane; acylphosphine oxide compounds such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide; and oxime ester compounds such as 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzoyloxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(O-acetyloxime), and 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime].

[0113] Among these, oxime ester compounds and acylphosphine oxide compounds are preferred, with 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyloxime) and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide being more preferred. Oxime ester compounds have the advantage of improving photocurability, while acylphosphine oxide compounds have the advantage of improving the degree of cure at the bottom of the cured product obtained by curing a photosensitive resin film and suppressing undercut. The combined use of an oxime ester compound and an acylphosphine oxide compound tends to further improve via resolution.

[0114] When the photosensitive resin composition of this embodiment contains (I) a photopolymerization initiator, the content of the (I) photopolymerization initiator is not particularly limited, but is preferably 0.01 to 20 mass%, more preferably 0.05 to 10 mass%, even more preferably 0.05 to 3 mass%, and particularly preferably 0.05 to 1.0 mass%, based on the total amount of resin components of the photosensitive resin composition. When the content of the (I) photopolymerization initiator is equal to or greater than the lower limit, elution of the exposed portion during development tends to be reduced, while when it is equal to or less than the upper limit, heat resistance tends to be improved.

[0115] <(J) Photosensitizer> The photosensitive resin composition of this embodiment may contain a photosensitizer as component (J) as needed. The photosensitizer (J) may be used alone or in combination of two or more. From the viewpoint of via resolution, the photosensitive resin composition of this embodiment may contain two or more components (J). Examples of the (J) photosensitizer include thioxanthone compounds such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; tertiary amines such as trialkylamine and triethanolamine; dialkylaminobenzoic acid alkyl esters such as ethyl N,N-dimethylaminobenzoate and amyl N,N-dimethylaminobenzoate; bis(dialkylamino)benzophenones such as 4,4'-bis(dimethylamino)benzophenone and 4,4'-bis(diethylamino)benzophenone; phosphine compounds such as triphenylphosphine; toluidine compounds such as N,N-dimethyltoluidine; anthracene compounds such as 9,10-dimethoxyanthracene, 2-ethyl-9,10-dimethoxyanthracene, and 2-ethyl-9,10-diethoxyanthracene; perylene compounds; and coumarin compounds. As the (J) photosensitizer, from the viewpoint of improving via resolution and via shape, bis(dialkylamino)benzophenone is preferred, and 4,4'-bis(diethylamino)benzophenone is more preferred.

[0116] When the photosensitive resin composition of this embodiment contains a (J) photosensitizer, the content of the (J) photosensitizer is not particularly limited, but is preferably 0.01 to 5 mass%, more preferably 0.05 to 3 mass%, even more preferably 0.1 to 1.5 mass%, and particularly preferably 0.1 to 1.0 mass%, based on the total amount of resin components of the photosensitive resin composition. When the content of the (J) photosensitizer is equal to or greater than the lower limit, the degree of cure of the bottom of the cured product obtained by curing the photosensitive resin film tends to be sufficiently high, while when the content is equal to or less than the upper limit, the degree of cure of the bottom of the cured product tends to be appropriately low.

[0117] <(K) Additives> The photosensitive resin composition of the present embodiment may contain, as necessary, various known and commonly used additives, such as pigments such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, carbon black, and naphthalene black; adhesion aids such as melamine; foam stabilizers such as silicone compounds; polymerization inhibitors; thickeners; and flame retardants. The content of these (K) additives may be adjusted appropriately depending on the respective purposes, and is preferably 0.01 to 5 mass%, alternatively 0.05 to 3 mass%, or alternatively 0.1 to 1 mass%, based on the total amount of resin components in the photosensitive resin composition.

[0118] <Diluent> The photosensitive resin composition of this embodiment may contain a diluent as needed. Examples of the diluent include organic solvents. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ether compounds such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, butyl cellosolve acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha. These diluents may be used alone or in combination.

[0119] When the photosensitive resin composition of this embodiment contains a diluent, the content of the diluent may be appropriately selected for the purpose of adjusting the concentration of the total solid content in the photosensitive resin composition to preferably 40 to 90 mass %, more preferably 50 to 85 mass %, and even more preferably 60 to 80 mass %. By adjusting the amount of the diluent used to within the above range, the coatability of the photosensitive resin composition is improved, and it becomes possible to form a higher-resolution pattern.

[0120] The photosensitive resin composition of this embodiment can be obtained by kneading and mixing the components using a roll mill, a bead mill, or the like. The photosensitive resin composition of this embodiment may be used in a liquid state (liquid state) or in a film state (film-like state). When used in a liquid state, the coating method for the photosensitive resin composition of this embodiment is not particularly limited, and various coating methods such as printing, spin coating, spray coating, jet dispensing, inkjet coating, and dip coating are examples. Among these, printing and spin coating are preferred from the viewpoint of more easily forming a photosensitive layer. When used in a film state, the composition can be used, for example, in the form of a photosensitive resin film described below. In this case, a photosensitive layer of the desired thickness can be formed by laminating it on a carrier film using a laminator or the like. Using the composition in a film state is preferred because it increases the production efficiency of printed wiring boards.

[0121] Since the photosensitive resin composition of this embodiment is suitable for via formation by photolithography (also referred to as photovia formation), the present disclosure also provides a photosensitive resin composition for photovia formation comprising the photosensitive resin composition of this embodiment. The photosensitive resin composition of this embodiment is useful as an interlayer insulating layer for printed wiring boards, and is also useful for solder resist applications.

[0122] [Photosensitive Resin Film] The photosensitive resin film of this embodiment contains the photosensitive resin composition of this embodiment, in other words, is formed using the photosensitive resin composition of this embodiment. The photosensitive resin film is useful as a photosensitive layer for forming an interlayer insulating layer. The photosensitive resin film of this embodiment is formed using the photosensitive resin composition of this embodiment, and therefore contains 10 to 70 volume % of the particles (X). The components and their contents in the photosensitive resin film are as described for the components and their contents in the photosensitive resin composition of this embodiment.

[0123] The photosensitive resin film of this embodiment may be provided on a carrier film. The photosensitive resin film of this embodiment can be formed, for example, by applying the photosensitive resin composition of this embodiment to a carrier film using a known coating device such as a comma coater, bar coater, kiss coater, roll coater, gravure coater, or die coater, followed by drying. Examples of the carrier film include polyesters such as polyethylene terephthalate and polybutylene terephthalate; and polyolefins such as polypropylene and polyethylene. The thickness of the carrier film is preferably 5 to 100 μm, more preferably 10 to 60 μm, and even more preferably 15 to 45 μm.

[0124] Furthermore, the photosensitive resin film of this embodiment may have a protective film on the surface opposite to the surface in contact with the carrier film. Polymer films such as polyethylene and polypropylene may be used as the protective film. The same polymer film as the carrier film described above may be used, or a different polymer film may be used.

[0125] The coating film formed by applying the photosensitive resin composition can be dried using hot air drying, a dryer using far infrared rays, or a dryer using near infrared rays. The drying temperature is preferably 60 to 150°C, more preferably 70 to 120°C, and even more preferably 80 to 110°C. The drying time is preferably 1 to 60 minutes, more preferably 2 to 30 minutes, and even more preferably 5 to 20 minutes. The content of the remaining diluent in the photosensitive resin film after drying is preferably 3% by mass or less, more preferably 2% by mass or less, and even more preferably 1% by mass or less, from the viewpoint of avoiding diffusion of the diluent during the manufacturing process of the printed wiring board.

[0126] The thickness (thickness after drying) of the photosensitive resin film (photosensitive layer) is not particularly limited, but from the viewpoint of thinning the printed wiring board, it is preferably 1 to 100 μm, more preferably 3 to 50 μm, and even more preferably 5 to 40 μm.

[0127] The photosensitive resin film of this embodiment has excellent via resolution and adhesive strength with copper plating, and is therefore suitable primarily as an interlayer insulating layer for printed wiring boards, but is also useful as a solder resist.

[0128] [Printed Wiring Board] The printed wiring board of this embodiment is obtained by the above-mentioned manufacturing method and contains the photosensitive resin composition of this embodiment or the photosensitive resin film of this embodiment. In other words, it contains an interlayer insulating layer formed using the photosensitive resin composition of this embodiment or the photosensitive resin film of this embodiment. Here, the expression "containing an interlayer insulating layer" includes cases where the interlayer insulating layer is contained as is, and cases where the interlayer insulating layer is contained in a state after being subjected to, for example, processing such as via formation, various treatments such as roughening treatment, and wiring formation. The printed wiring board of this embodiment allows the formation of fine wiring and has excellent adhesion to copper plating, so it can also be used as an interposer for semiconductor packages.

[0129] [Semiconductor Package] The present disclosure also provides a semiconductor package including the printed wiring board of the present embodiment and a semiconductor element. The semiconductor package of the present embodiment can be manufactured by mounting a semiconductor element such as a semiconductor chip or memory at a predetermined position on the printed wiring board of the present embodiment and then encapsulating the semiconductor element with an encapsulating resin or the like.

[0130] The present embodiment will be described in more detail below using examples, but the present disclosure is not limited to these examples. The acid value and weight average molecular weight of component (A) were measured according to the following methods. Furthermore, the properties of the photosensitive resin compositions obtained in each example were evaluated according to the following methods.

[0131] <Method for Measuring Acid Value> The acid value of component (A) was calculated from the amount of aqueous potassium hydroxide solution required to neutralize component (A).

[0132] <Method for measuring weight-average molecular weight> The weight-average molecular weight of component (A) was measured using the following GPC measurement device and measurement conditions, and the value converted using the calibration curve of standard polystyrene was used as the weight-average molecular weight. The calibration curve was created using a set of five standard polystyrene samples ("PStQuick MP-H" and "PStQuick B", manufactured by Tosoh Corporation). (GPC measurement device) Device: High-speed GPC device "HCL-8320GPC", detector: differential refractometer or UV, manufactured by Tosoh Corporation Column: column TSKgel SuperMultipore HZ-H (column length: 15 cm, column inner diameter: 4.6 mm), manufactured by Tosoh Corporation (Measurement conditions) Solvent: tetrahydrofuran (THF) Measurement temperature: 40°C Flow rate: 0.35 ml / min Sample concentration: 10 mg / 5 ml THF Injection amount: 20 μl

[0133] [1. Surface Roughness (Ra)] In each of the Examples and Comparative Examples, the surface of the evaluation laminate A after the desmear treatment was measured for the surface roughness (Rz) of the prepreg surface produced in each Example using a high-performance non-contact three-dimensional surface profile roughness measurement system (Wyko NT9100, manufactured by Bruker Japan K.K.) by white light interferometry.

[0134] [2. Evaluation of Adhesion Strength with Copper Plating] The perpendicular peel strength of the evaluation laminate B produced in each example and comparative example was measured at 23° C. in accordance with JIS C6481 (1996).

[0135] Synthesis Example 1 Synthesis of Photopolymerizable Compound (A1) Having an Ethylenically Unsaturated Group and an Acidic Substituent 350 parts by mass of dicyclopentadiene-type epoxy resin ("XD-1000" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 252 g / eq, softening point 74.2°C, component (a1), number of ring carbon atoms in alicyclic skeleton: 10), 70 parts by mass of acrylic acid (component (a2)), 0.5 parts by mass of methylhydroquinone, and 120 parts by mass of carbitol acetate were charged and heated to 90°C with stirring to react and dissolve the mixture. Next, the resulting solution was cooled to 60°C, and 2 parts by mass of triphenylphosphine was added. The mixture was heated to 100°C and reacted until the acid value of the solution reached 1 mgKOH / g. To the reacted solution, 98 parts by mass of tetrahydrophthalic anhydride (component (a3)) and 85 parts by mass of carbitol acetate were added, heated to 80°C, and reacted for 6 hours. Thereafter, the mixture was cooled to room temperature to obtain a photopolymerizable compound (A1) having an ethylenically unsaturated group and an acidic substituent, with a solids concentration of 73% by mass [acid value: 60 mg KOH / g, weight average molecular weight: 2,000].

[0136] Synthesis Example 2 Synthesis of Photopolymerizable Compound (A2) Having an Ethylenically Unsaturated Group and an Acidic Substituent 350 parts by mass of cresol novolac epoxy resin (EOCN-104S, component (a1) manufactured by Nippon Kayaku Co., Ltd.), 70 parts by mass of acrylic acid (component (a2)), 0.5 parts by mass of methylhydroquinone, and 120 parts by mass of carbitol acetate were charged and heated to 90°C with stirring to react and dissolve the mixture. Next, the resulting solution was cooled to 60°C, and 2 parts by mass of triphenylphosphine was added. The mixture was heated to 100°C and reacted until the acid value of the solution reached 1 mgKOH / g. To the reacted solution, 98 parts by mass of tetrahydrophthalic anhydride (component (a3)) and 85 parts by mass of carbitol acetate were added, heated to 80°C, and reacted for 6 hours. Thereafter, the mixture was cooled to room temperature to obtain a photopolymerizable compound (A2) having an ethylenically unsaturated group and an acidic substituent, with a solids concentration of 73% by mass [acid value: 60 mgKOH / g, weight average molecular weight: 6,500].

[0137] Examples 1 to 12 and Comparative Examples 1 to 6 (1) Preparation of Photosensitive Resin Compositions Compositions were formulated according to the formulations shown in Table 1 (the units of values ​​in the table are parts by mass, and in the case of solutions, the amounts are equivalent to the solid content) (note that particles (X) were previously mixed with component (A)), and then kneaded using a three-roll mill. Methyl ethyl ketone was then added to adjust the solid content concentration to 65% by mass, thereby obtaining a photosensitive resin composition. (2) Preparation of Photosensitive Resin Films A 16 μm-thick polyethylene terephthalate film (manufactured by Teijin Limited, product name "G2-16") was used as a carrier film. The photosensitive resin composition prepared in each example was applied onto the carrier film, adjusting the film thickness to 25 μm after drying, and then dried at 100°C for 10 minutes using a hot air convection dryer to form a photosensitive resin film (photosensitive layer). Next, a polyethylene film (manufactured by Tamapoly Co., Ltd., product name "NF-15") was laminated as a protective film on the surface opposite to the side in contact with the carrier film of the photosensitive resin film (photosensitive layer), and a photosensitive resin film having the carrier film and protective film laminated thereon was produced.

[0138] (Lamination step (1)) While peeling the protective film from the "photosensitive resin film having a carrier film and a protective film bonded thereto" produced by the above method, lamination was performed on a 1.0 mm thick copper-clad laminate substrate using a press-type vacuum laminator (manufactured by Meiki Seisakusho Co., Ltd., product name "MVLP-500") at a pressure of 0.4 MPa, a press hot plate temperature of 75°C, a vacuum time of 25 seconds, a lamination press time of 25 seconds, and an air pressure of 4 kPa or less, to obtain a laminate. The obtained laminate was exposed to 200 mJ / cm using a parallel light exposure machine (manufactured by Oak Seisakusho Co., Ltd., product name "EXM-1201") using an ultra-high pressure mercury lamp as a light source. 2 The entire surface was exposed to 2,000 mJ / cm 2 UV light (wavelength 365 nm). 2 After the exposure, the copper-clad laminate was heated at 170° C. for 1 hour to obtain a cured product on the copper-clad laminate, which was called a "laminate for evaluation."

[0139] (Photovia Formation Step (2)) The evaluation laminate was exposed to 210 mJ / cm 2 from above the carrier film using an i-line stepper (UX-7, manufactured by Ushio Inc.) and a step tablet and a via evaluation mask. 2 The substrate was exposed to a 365 nm wavelength. After peeling off the carrier film, the substrate was developed for 40 seconds at 30°C with a 1% by mass aqueous sodium carbonate solution using a spray developer, forming vias with a size of approximately 60 μm. Images of the vias obtained by scanning electron microscope (SEM) measurement (magnification: 2,500x) for Examples 2 and 11 are shown in FIGS. 7 and 8, respectively. In FIG. 7 (Example 2), the via top opening diameter was 55.6 μm, and the via bottom opening diameter was 53.6 μm. In FIG. 8 (Example 11), the via top opening diameter was 56.0 μm, and the via bottom opening diameter was 53.8 μm. It can be seen that the via resolution was excellent in both cases.

[0140] (Roughening Treatment Step (3-1): Roughening Treatment with Roughening Solution) Next, first, 2 L of "Swelling Dip Securigant MV" (trade name, manufactured by Atotech Japan Co., Ltd.) [sodium hydroxide concentration: 3 g / L] as a swelling solution was heated to 70°C, and the evaluation laminate was immersed in the solution for 5 minutes. Thereafter, the solution was rinsed with stored water at 25°C for 1 minute, and then rinsed with running water at 25°C for 3 minutes. Next, 2 L of "Dosing Securigant PMV" (trade name, manufactured by Atotech Japan Co., Ltd.) [sodium hydroxide concentration: 40 g / L] as a roughening solution was heated to 60°C, and the evaluation laminate was immersed in the solution for 5 minutes. Thereafter, the solution was rinsed with stored water at 70°C for 1 minute in pure water.

[0141] (Particle (X) Dissolving Step (3-2): Although particles (X) were not used in each Comparative Example, this step was performed in the same manner as in the Examples.) Next, "Reduction Solution Securigant MV" (trade name, manufactured by Atotech Japan Co., Ltd.) (total volume: 2,000 ml) to which an aqueous sulfuric acid solution had been added so that the sulfuric acid concentration was 48 ml / L was heated to the temperature shown in Table 1, and the evaluation laminate was then immersed for the time shown in Table 1. Thereafter, the evaluation laminate was washed in stored water at 25°C for 1 minute, and then washed in running water at 25°C for 3 minutes. This evaluation laminate after the particle (X) dissolving step (3-2) is referred to as Evaluation Laminate A. Here, in Examples 2, 5, 8, and 11 and Comparative Example 5, the surface of the evaluation laminate A was measured using a scanning electron microscope (SEM), and surface images were taken. The results are shown in Figures 9 to 13.

[0142] (Circuit Pattern Forming Step (4)) Next, the evaluation laminate was treated with an alkaline cleaner "Cleaner Securigant 902" (trade name, manufactured by Atotech Japan Co., Ltd.) at 60°C for 5 minutes, followed by degreasing and cleaning. After cleaning, the evaluation laminate was treated with a pre-dip liquid "Pre-dip Neogant B" (trade name, manufactured by Atotech Japan Co., Ltd.) at 23°C for 1 minute. Thereafter, the evaluation laminate was treated with an activator liquid "Activator Neogant 834" (trade name, manufactured by Atotech Japan Co., Ltd.) at 35°C for 5 minutes, and then the evaluation laminate was treated with a reducing liquid "Reducer Neogant WA" (trade name, manufactured by Atotech Japan Co., Ltd.) at 30°C for 5 minutes. The evaluation laminate thus obtained was placed in a chemical copper solution ("Basic Printganth MV-TP1," "Copper Printganth MV-TP1," "Moderator Printganth MV-TP1," "Stabilizer Printganth MV-TP1," and "Reducer Cu" (all trade names manufactured by Atotech Japan Co., Ltd.) and sodium hydroxide), and electroless plating was performed until the plating thickness reached approximately 0.5 μm. After the electroless plating, an annealing treatment was performed at a temperature of 120°C for 30 minutes to remove residual hydrogen gas. Thereafter, copper sulfate electroplating was performed, and an annealing treatment was performed at 180°C for 60 minutes to form a conductor layer with a thickness of 25 μm. This evaluation laminate is referred to as Evaluation Laminate B. A circuit pattern was then formed on Evaluation Laminate B by a semi-additive process. The measurement and evaluation results are shown in Table 1.

[0143]

[0144] The components used in Table 1 are as follows: [(A) Photopolymerizable Compound Having an Ethylenically Unsaturated Group and an Acidic Substituent] A1: Photopolymerizable compound (A1) having an ethylenically unsaturated group and an acidic substituent obtained in Synthesis Example 1, containing an alicyclic skeleton. A2: Photopolymerizable compound (A2) having an ethylenically unsaturated group and an acidic substituent obtained in Synthesis Example 2, not containing an alicyclic skeleton.

[0145] [(B) Thermosetting Resin] B1: "YX-4000" (manufactured by Mitsubishi Chemical Corporation, biphenyl aralkyl epoxy resin, epoxy equivalent: 180 to 192 g / eq)

[0146] [(C) Crosslinking Agent] C1: "DPHA" (dipentaerythritol hexaacrylate) C2: "TMPTA" (trimethylolpropane triacrylate)

[0147] [(D) Elastomer] D1: "Ricon (registered trademark) 131MA17" (manufactured by Cray Valley Corporation, maleic acid-modified polybutadiene, number average molecular weight 54,000 (catalog value))

[0148] [(X) Particles (particles that dissolve at least 95% by mass in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L at 70°C for 20 minutes)] X1; Magnesium hydroxide 1: "ECOMAG (registered trademark) Z-10" (magnesium hydroxide, volume average particle diameter 1.2 μm, manufactured by Tateho Chemical Industries Co., Ltd.) X2; "Magthermo MS-S" (magnesium carbonate, volume average particle diameter 1.2 μm, manufactured by Konoshima Chemical Co., Ltd.) X3; "LPZINC-KS-2" (zinc oxide, volume average particle diameter 2 μm, manufactured by Sakai Chemical Industry Co., Ltd.) X4; Magnesium hydroxide 2: "Magseeds (registered trademark) V-6F" (magnesium hydroxide, volume average particle diameter 0.9 μm, manufactured by Konoshima Chemical Co., Ltd.)

[0149] [(E) Inorganic Filler] E1: Spherical fused silica (volume average particle diameter 0.5 μm)

[0150] [(I) Photopolymerization initiator] I1: Photopolymerization initiator 1: 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, an acetophenone-based compound I2: Photopolymerization initiator 2: 2,4-diethylthioxanthone, a thioxanthone-based compound

[0151] Table 1 shows that Examples 1 to 12 successfully increased the adhesive strength with copper plating while maintaining a low surface roughness of the interlayer insulating layer. This is presumably due to the dissolution of particles (X) present on the surface of the interlayer insulating layer, forming depressions, as shown in Figures 9 to 12. On the other hand, in Comparative Examples 1 to 3, in which particles (X) were used, the surface roughness was low due to the absence of particles, but in this case, the peel strength with copper plating was extremely low. Furthermore, in Comparative Examples 4 to 6, in which an inorganic filler other than particles (X) was used instead of particles (X), the peel strength with copper plating was low even when the surface roughness was low. As shown in Figure 13, this is presumably due to the presence of an inorganic filler on the surface of the interlayer insulating layer.

[0152] Example 13 and Comparative Example 7 In the same manner as in Example 1 and Comparative Example 4, each photosensitive resin film was prepared, and a cured product was formed on a copper-clad laminate substrate through the lamination step (1) to obtain a "laminate for evaluation." The following operations were then performed. (Roughening Treatment Step (3-1); Dry Etching) The surface of the evaluation laminate obtained above was plasma-treated using oxygen plasma under conditions of an output of 300 W, a temperature of 25°C, and a treatment time of 5 minutes. (Particle (X) Dissolving Step (3-2) and Circuit Pattern Forming Step (4)) Next, the laminate was treated with an alkaline cleaner "Cleaner Securigant 902" (trade name, manufactured by Atotech Japan Co., Ltd.) at 60°C for 5 minutes, followed by rinsing in stored water at 25°C for 1 minute and then rinsing in running water at 25°C for 3 minutes. Here, in Example 13, the surface of the obtained evaluation laminate was subjected to scanning electron microscope (SEM) measurement (magnification: 10,000 times), and surface images were taken. The results are shown in FIG. 14. Next, the surface of the evaluation laminate was treated with a mixed solution of sodium persulfate and an aqueous sulfuric acid solution (sulfuric acid concentration: 18.5 ml / L) at 27°C for 30 seconds to perform soft etching and dissolve the particles (X). This treatment was performed not only in Example 13 but also in Comparative Example 7, which did not use particles (X). Thereafter, the laminate was washed with stored water at 25°C for 1 minute, followed by running water at 25°C for 3 minutes. Here, in Example 13, the surface of the obtained evaluation laminate was measured with a scanning electron microscope (SEM) (magnification: 10,000 times), and a surface image was taken. The results are shown in Figure 15. After the above treatment, the evaluation laminate was treated with a pre-dip solution "Pre-Dip Neogant B" (trade name, manufactured by Atotech Japan Co., Ltd.) at 25°C for 1 minute. The evaluation laminate was then treated with an activator solution "Activator Neogant 834" (trade name, manufactured by Atotech Japan Co., Ltd.) at 40°C for 5 minutes, followed by running water at 25°C for 1 minute, followed by running water at 25°C for 3 minutes. Next, the evaluation laminate was treated with a reducing solution "Reducer Neogant WA" (trade name, manufactured by Atotech Japan Co., Ltd.) at 30°C for 5 minutes, rinsed in standing water at 25°C for 1 minute, and then rinsed in running water at 25°C for 3 minutes.The evaluation laminate thus obtained was placed in a chemical copper solution ("Basic Printganth MV-TP1," "Copper Printganth MV-TP1," "Moderator Printganth MV-TP1," "Stabilizer Printganth MV-TP1," and "Reducer Cu" (all trade names manufactured by Atotech Japan Co., Ltd.) and sodium hydroxide), and electroless plating was carried out until the plating thickness reached approximately 0.5 μm. After the electroless plating, an annealing treatment was carried out at a temperature of 120°C for 30 minutes to remove any remaining hydrogen gas. Thereafter, copper sulfate electroplating was carried out, and an annealing treatment was carried out at 180°C for 60 minutes to form a conductor layer with a thickness of 25 μm. This evaluation laminate is referred to as Evaluation Laminate C. A circuit pattern was then formed on Evaluation Laminate C by a semi-additive process. The measurement and evaluation results are shown in Table 2.

[0153]

[0154] As can be seen from Table 2, in Example 13, as can be seen from the change in the surface of the interlayer insulating layer from Figure 14 to Figure 15, the particles (X) dissolved after the particle (X) dissolving step (3-2), and as a result, it was possible to successfully increase the adhesive strength with the copper plating while keeping the surface roughness of the interlayer insulating layer small. On the other hand, in Comparative Example 7, in which an inorganic filler other than particles (X) was used instead of particles (X), the peel strength with the copper plating was low when the surface roughness was small.

[0155] Example 14 and Comparative Example 8 In the same manner as in Example 2 and Comparative Example 5, each photosensitive resin film was prepared, and a cured product was formed on a copper-clad laminate substrate through the lamination step (1), to obtain a "laminate for evaluation." Thereafter, the following operations were performed. (Roughening Treatment Step (3-1): Dry Etching) The surface of the laminate for evaluation obtained above was plasma-treated using oxygen plasma under conditions of an output of 300 W, a temperature of 25°C, and a treatment time of 5 minutes. (Particle (X) Dissolution Step (3-2)) The surface of the plasma-treated laminate for evaluation was heated to the temperature shown in Table 3 in "Reduction Solution Securigant MV" (trade name, manufactured by Atotech Japan Co., Ltd.) (total volume: 2,000 ml), to which an aqueous sulfuric acid solution had been added so that the sulfuric acid concentration was 49 ml / L. The temperature was then increased to the temperature shown in Table 3, and the laminate for evaluation was then immersed for the time shown in Table 3. This treatment was performed not only in Example 14, but also in Comparative Example 8, which did not use particles (X). (Circuit Pattern Forming Step (4)) Next, the evaluation laminate was treated with an alkaline cleaner "Cleaner Securigant 902" (trade name, manufactured by Atotech Japan Co., Ltd.) at 60°C for 5 minutes, followed by rinsing in stored water at 25°C for 1 minute and then rinsing in running water at 25°C for 3 minutes. Subsequently, the surface of the evaluation laminate was treated with a mixed solution of sodium persulfate and an aqueous sulfuric acid solution (sulfuric acid concentration: 18.5 ml / L) at 27°C for 0.5 minutes to perform soft etching. Thereafter, rinsing in stored water at 25°C for 1 minute and then rinsing in running water at 25°C for 3 minutes. After the above treatment, the evaluation laminate was treated with a pre-dip solution "Pre-Dip Neogant B" (trade name, manufactured by Atotech Japan Co., Ltd.) at 25°C for 1 minute. Thereafter, the evaluation laminate was treated with an activator solution "Activator Neogant 834" (trade name, manufactured by Atotech Japan Co., Ltd.) at 40°C for 5 minutes, followed by rinsing in stored water at 25°C for 1 minute and then rinsing in running water at 25°C for 3 minutes. Next, the evaluation laminate was treated with a reducing solution "Reducer Neogant WA" (trade name, manufactured by Atotech Japan Co., Ltd.) at 30°C for 5 minutes, rinsed in standing water at 25°C for 1 minute, and then rinsed in running water at 25°C for 3 minutes.The evaluation laminate thus obtained was placed in a chemical copper solution ("Basic Printganth MV-TP1," "Copper Printganth MV-TP1," "Moderator Printganth MV-TP1," "Stabilizer Printganth MV-TP1," and "Reducer Cu" (all trade names manufactured by Atotech Japan Co., Ltd.) and sodium hydroxide), and electroless plating was carried out until the plating thickness reached approximately 0.5 μm. After the electroless plating, an annealing treatment was carried out at a temperature of 120°C for 30 minutes to remove any remaining hydrogen gas. Thereafter, copper sulfate electroplating was carried out, and an annealing treatment was carried out at 180°C for 60 minutes to form a conductor layer with a thickness of 25 μm. This evaluation laminate is referred to as Evaluation Laminate C. A circuit pattern was then formed on Evaluation Laminate C by a semi-additive process. The measurement and evaluation results are shown in Table 2.

[0156]

[0157] From Table 3, it can be said that in Example 14, the particles (X) were dissolved after the particle (X) dissolving step (3-2), and as a result, it was possible to successfully increase the adhesive strength with the copper plating while keeping the surface roughness of the interlayer insulating layer small. On the other hand, in Comparative Example 8, in which an inorganic filler other than particles (X) was used instead of particles (X), the peel strength with the copper plating was low when the surface roughness was small.

[0158] 100A Printed wiring board 1 Particle (X) 2 Depression 101 Substrate 102 Circuit pattern 103 Interlayer insulating layer 104 Via (via hole) 105 Seed layer 106 Resist pattern 107 Copper circuit layer 108 Solder resist layer

Claims

1. A method for manufacturing a printed wiring board, comprising the following steps (1) to (4): (1) laminating a photosensitive resin film containing particles (X) that dissolve at least 95% by mass in a sulfuric acid aqueous solution having a concentration of 5 to 100 ml / L at 70°C for 20 minutes onto one or both sides of a circuit board; (2) forming an interlayer insulating layer having vias by exposing and developing the photosensitive resin film laminated in step (1); (3-1) roughening the surfaces of the vias and the interlayer insulating layer; (3-2) treating the roughened interlayer insulating layer with an acidic solution to dissolve the particles (X) present on the surface of the interlayer insulating layer; (4) forming a circuit pattern on the interlayer insulating layer.

2. The method for producing a printed wiring board according to claim 1, wherein the roughening treatment in (3-1) is carried out using a roughening liquid.

3. The method for producing a printed wiring board according to claim 1, wherein the roughening treatment in (3-1) is carried out by dry etching.

4. The method for producing a printed wiring board according to claim 1, wherein the surface roughness (Ra) of the interlayer insulating layer after the roughening treatment in (3-1) is 0.30 μm or less.

5. The method for producing a printed wiring board according to claim 1, wherein the acid solution used in (3-2) includes an aqueous sulfuric acid solution.

6. The method for producing a printed wiring board according to claim 1, wherein the particles (X) have a volume average particle size of 0.1 to 3 μm.

7. The method for producing a printed wiring board according to claim 1, wherein the photosensitive resin film contains 10 to 70 volume % of the particles (X).

8. A photosensitive resin composition comprising particles (X) that dissolve at 95% by mass or more in an aqueous sulfuric acid solution having a concentration of 5 to 100 ml / L at 70° C. for 20 minutes.

9. The photosensitive resin composition according to claim 8, further comprising (A) a photopolymerizable compound having an ethylenically unsaturated group and an acidic substituent, and (B) a thermosetting resin.

10. The photosensitive resin composition according to claim 9, wherein the component (A) contains an alicyclic skeleton represented by the following general formula (A-1): (In the formula, R A1 represents an alkyl group having 1 to 12 carbon atoms, and may be substituted anywhere in the alicyclic skeleton. 1 is an integer from 0 to 6. * is a binding site to other structures.) 11. The photosensitive resin composition according to claim 8, wherein the particles (X) have an average particle size of 0.1 to 3 μm.

12. The photosensitive resin composition according to claim 8, wherein the content of the particles (X) is 10 to 70 volume % based on the total solid content.

13. A photosensitive resin composition for forming a photovia, comprising the photosensitive resin composition according to claim 8.

14. A photosensitive resin film comprising the photosensitive resin composition according to claim 8.

15. A printed wiring board comprising the photosensitive resin composition according to claim 8 or the photosensitive resin film according to claim 14.

16. A semiconductor package comprising the printed wiring board according to claim 15 and a semiconductor element.

Citation Information

Patent Citations

  • Thermosetting resin composition, multilayered printed wiring board, and preparation thereof

    JP1995304931A

  • Photosensitive additive adhesive composition

    JP2000104034A

  • Photosensitive resin composition and method for forming resin pattern using the composition

    JP2004233835A

  • Photosensitive resin composition, and dry film, printed wiring board and method for manufacturing printed wiring board using the composition

    JP2017116652A

  • Photosensitive resin film laminate

    JP2019061224A