Adhesive film and article provided with adhesive film

The integration of a high-pigment fluororesin layer with a silane coupling agent and specific additives in the adhesive film addresses the poor adhesiveness of fluororesin films, achieving robust bonding and UV resistance for outdoor applications.

WO2024219397A1PCT designated stage expired Publication Date: 2024-10-24AGC INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015143
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-04-16
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Fluororesin films exhibit poor adhesiveness, which compromises the adhesive strength between the base material and the fluororesin film, especially after weather resistance tests, necessitating an enhancement in adhesive properties to ensure durable bonding.

Method used

Incorporating a fluororesin layer with a pigment content of 1.0% by mass or more, combined with a silane coupling agent having functional groups such as amino, epoxy, or acrylic groups, and using a specific thickness and composition of the adhesive layer to enhance adhesion, while also employing titanium oxide and aluminum oxide for improved ultraviolet shielding and catalytic activity suppression.

Benefits of technology

The resulting adhesive film demonstrates excellent adhesive strength to the base material even after weather resistance tests, with enhanced ultraviolet shielding and reduced deterioration from UV rays, ensuring long-term durability and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing: an adhesive film having excellent adhesive strength with respect to a base material even after having undergone a weathering test; and an article provided with an adhesive film having excellent adhesive strength with respect to a base material even after having undergone a weathering test. An adhesive film according to the present invention comprises: a fluororesin layer containing a fluororesin and a pigment; and an adhesive layer that contains a silane coupling agent having a functional group and that is provided at at least a portion of the fluororesin layer. The content of the pigment in the fluororesin layer is 1.0 mass% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive film and article comprising adhesive film

[0001] The present invention relates to an adhesive film and an article comprising the adhesive film.

[0002] Fluororesin films made from fluororesins have excellent properties such as weather resistance and water and oil repellency, and are used as protective films for various substrates. In particular, in recent years, they have been expected to be used as protective films for substrates used outdoors, and UV-shielding functionality is required to protect the substrate from sunlight.

[0003] Patent Document 1 describes a resin film containing, in a resin containing a fluororesin, composite particles in which the surfaces of titanium oxide particles have a coating layer containing aluminum oxide, and composite particles in which the surfaces of zinc oxide particles have a coating layer containing silicon oxide, for the purpose of improving weather resistance.

[0004] International Publication No. 2014 / 021436

[0005] However, since the adhesiveness of the fluororesin film itself is poor, it is desired to impart adhesiveness to the fluororesin film in order to improve the adhesive strength between the substrate and the fluororesin film. Patent Document 1 also describes that when the fluororesin film is used as a back sheet for a solar cell, a two-component curing urethane adhesive may be used to bond the fluororesin film and the moisture-proof layer via the adhesive layer.

[0006] As described in Patent Document 1, there are applications in which sufficient adhesive strength is achieved by using a two-component curing urethane adhesive to bond a fluororesin film to a substrate, but when the film is exposed to an outdoor environment for a long period of time, a fluororesin film having an adhesive layer that exhibits even greater adhesive strength with the substrate in a weather resistance test is desired, and it is desired to propose a method for imparting optimal adhesive strength between the fluororesin film and the substrate. One aspect of the present disclosure aims to provide an adhesive film that exhibits excellent adhesive strength with the substrate even after a weather resistance test, and an article that includes an adhesive film that exhibits excellent adhesive strength with the substrate even after a weather resistance test.

[0007] Specific means for achieving the above object are as follows. <1> An adhesive film having a fluororesin layer containing a fluororesin and a pigment, and an adhesive layer at least partially on the fluororesin layer containing a silane coupling agent having a functional group, wherein the content of the pigment in the fluororesin layer is 1.0 mass% or more. <2> The adhesive film according to <1>, wherein the pigment contains at least one selected from the group consisting of titanium oxide and carbon black. <3> The adhesive film according to <1> or <2>, wherein the pigment contains titanium oxide and aluminum oxide. <4> The adhesive film according to any one of <1> to <3>, wherein the functional group of the silane coupling agent contains at least one selected from the group consisting of an amino group, an epoxy group, and an acrylic group. <5> An adhesive film wherein the amount of functional groups of the silane coupling agent contained in the adhesive layer is 0.01 mmol / m 2 or more. <6> The adhesive film according to any one of <1> to <5>, wherein the fluororesin contains an ethylene-tetrafluoroethylene copolymer. <7> The adhesive film according to any one of <1> to <6>, wherein the fluororesin layer satisfies the following relational formula (1): Formula (1) 100<content of the pigment in the fluororesin layer (% by mass)×average thickness of the fluororesin layer (μm)<2100 <8> The adhesive film according to any one of <1> to <7>, wherein the transmittance of the adhesive film at a wavelength of 360 nm is 1.0% or less. <9> The adhesive film according to any one of <1> to <8>, wherein the adhesive layer has an average thickness of 0.5 μm or less. <10> The adhesive film according to any one of <1> to <8>, wherein the amount of functional groups of the silane coupling agent contained in the adhesive layer is 0.01 to 0.7 mmol / m 2<1> The adhesive film according to any one of <1> to <9>, which is a protective film for outdoor use. <11> The adhesive film according to any one of <1> to <10>, which is a protective film for outdoor use. <12> An article comprising the adhesive film according to any one of <1> to <11> and a substrate, the article comprising the fluororesin layer, the adhesive layer, and the substrate in this order. <13> The article according to <12>, wherein the substrate comprises at least one selected from the group consisting of glass, polycarbonate, polyvinyl chloride, epoxy resin, acrylic resin, ethylene-vinyl acetate copolymer resin, modified polyethylene, and fiber-containing resin. <14> The article according to <12> or <13>, wherein the adhesive film is a protective film. <15> The article according to any one of <12> to <14>, which is used outdoor.

[0008] According to one aspect of the present disclosure, it is possible to provide an adhesive film that has excellent adhesion to a substrate even after a weather resistance test, and an article that includes an adhesive film that has excellent adhesion to a substrate even after a weather resistance test.

[0009] 1 is a schematic cross-sectional view illustrating the layer structure of an example of an adhesive film of the present disclosure. 2 is a schematic cross-sectional view illustrating the layer structure of an example of an adhesive film of the present disclosure.

[0010] Embodiments of the present disclosure are described in detail below. However, the present disclosure is not limited to the following embodiments. In the following embodiments, components (including elementary steps, etc.) are not essential unless otherwise specified. The same applies to numerical values ​​and their ranges, and do not limit the present disclosure. In the present disclosure, numerical ranges indicated using "to" include the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present disclosure, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in the numerical ranges described in the present disclosure, the upper or lower limit of that numerical range may be replaced with a value shown in the examples. In the present disclosure, each component may contain multiple corresponding substances. When multiple substances corresponding to each component are present in a composition, the content or amount of each component means the total content or amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, the particles corresponding to each component may contain multiple types of particles. When multiple types of particles corresponding to each component are present in a composition, the particle size of each component refers to the value for the mixture of those multiple types of particles present in the composition, unless otherwise specified. In this disclosure, the term "layer" includes cases where the layer is formed throughout the entire region when observing the region in which the layer exists, as well as cases where the layer is formed only in a portion of the region. When embodiments are described with reference to drawings in this disclosure, the configuration of the embodiment is not limited to the configuration shown in the drawings. Furthermore, the sizes of components in the drawings are conceptual, and the relative size relationships between components are not limited to these.

[0011] In this disclosure, the term "unit" of a polymer refers to a portion derived from a monomer that exists in the polymer and constitutes the polymer. The term "unit" also refers to a unit obtained by chemically converting the structure of a unit after polymer formation. In some cases, units derived from individual monomers are referred to by the name of the monomer followed by "unit." In this disclosure, films and sheets are referred to as "films" regardless of their thickness.

[0012] <Adhesive film> An adhesive film according to one embodiment of the present disclosure has a fluororesin layer containing a fluororesin and a pigment, and an adhesive layer at least partially on the fluororesin layer, the adhesive layer containing a silane coupling agent having a functional group, the content of the pigment in the fluororesin layer being 1.0 mass% or more. The reason why the adhesive film having the above-described configuration has excellent adhesion to a substrate even after a weather resistance test is presumed to be, but is not limited to, the following presumption.

[0013] The adhesive film of one embodiment of the present disclosure contains a pigment in the fluororesin layer at 1.0% by mass or more, and therefore the amount of ultraviolet light that passes through the fluororesin layer is reduced, thereby reducing the amount of ultraviolet light that reaches the adhesive layer and the substrate, thereby preventing deterioration of the adhesive layer and the substrate due to ultraviolet light and providing an adhesive film that has excellent adhesive strength even after a weather resistance test.

[0014] Possible methods for imparting adhesiveness to a fluororesin layer include surface treatment of the fluororesin layer by corona discharge treatment, plasma treatment, etc., and providing an adhesive layer of urethane or the like on the surface-treated fluororesin layer. Among these various adhesive methods, the adhesive film of one embodiment of the present disclosure has an adhesive layer containing a silane coupling agent having a functional group, and therefore has excellent adhesion to various substrates, and the adhesive function between the fluororesin layer and the substrate is fully exhibited. It is believed that the sufficient adhesive function exhibited by the adhesive layer containing such a silane coupling agent is achieved by further containing 1.0 mass % or more of a pigment in the fluororesin.

[0015] [Fluororesin Layer] The fluororesin layer in one embodiment of the present disclosure contains a fluororesin and a pigment, and the content of the pigment in the fluororesin layer is 1.0 mass % or more.

[0016] In one embodiment of the present disclosure, the average thickness of the fluororesin layer is preferably 10 μm or more, more preferably 12 μm or more, and even more preferably 20 μm or more. The lower limit is preferably 300 μm or less, and even more preferably 250 μm or less. Within the above range, excellent followability is achieved during lamination with a substrate or processing. When the average thickness of the fluororesin layer can be measured with a micrometer, it may be measured at five locations with a micrometer and the average value calculated. When it cannot be measured with a micrometer, it may be measured in accordance with ISO 4591:1992 (JIS K7130:1999, Method B1, Thickness measurement method by mass method for samples taken from plastic film or sheet). In the present disclosure, the measurement is performed in accordance with ISO 4591:1992 (JIS K7130:1999, Method B1, Thickness measurement method by mass method for samples taken from plastic film or sheet).

[0017] (Resin) The resin contained in the fluororesin layer includes at least a fluororesin. One type of fluororesin may be used alone, or two or more types may be used in combination. The fluororesin is not particularly limited as long as it contains fluorine in the molecular structure of the resin, and is preferably a thermoplastic resin. Known fluororesins can be used, and a fluoroolefin-based polymer is preferred. The fluoroolefin-based polymer is a polymer having a fluoroolefin unit. The fluoroolefin-based polymer may further have other monomer units other than the fluoroolefin unit.

[0018] Examples of the fluoroolefin unit include units derived from tetrafluoroethylene, vinyl fluoride, vinylidene fluoride, trifluoroethylene, hexafluoropropylene, chlorotrifluoroethylene, etc. Among these, the tetrafluoroethylene unit is preferred from the viewpoint of excellent weather resistance, heat resistance, contamination resistance, etc. One type of fluoroolefin unit may be used alone, or two or more types may be used in combination.

[0019] Examples of polymers having tetrafluoroethylene units as fluoroolefin units include tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymers (hereinafter also referred to as "PFA"), tetrafluoroethylene-hexafluoropropylene-perfluoro(alkyl vinyl ether) copolymers, tetrafluoroethylene-hexafluoropropylene copolymers (hereinafter also referred to as "FEP"), ethylene-tetrafluoroethylene copolymers (hereinafter also referred to as "ETFE"), and ethylene-trichlorofluoroethylene copolymers (hereinafter also referred to as "ECTFE"). Polymers having tetrafluoroethylene units may be used alone or in combination of two or more. Of these, PFA, FEP, ETFE, and ECTFE are preferred. Among these, ETFE is particularly preferred from the standpoint of cost and mechanical strength.

[0020] ETFE is a copolymer having ethylene (hereinafter also referred to as "E") units (hereinafter also referred to as "E units") and tetrafluoroethylene (hereinafter also referred to as "TFE") units (hereinafter also referred to as "TFE units"). ETFE may further have structural units derived from other monomers than E and TFE, as necessary. The molar ratio of E units / TFE units in ETFE is preferably 40 / 60 to 70 / 30, more preferably 40 / 60 to 60 / 40. The total content of E units and TFE units in 100 mol% of all units constituting ETFE is preferably 90 mol% or more, more preferably 95 mol% or more, and may be 100 mol%.

[0021] The other monomer units in ETFE may be copolymerizable with E and TFE, for example, CF 2 = CFCl, CF 2 =CH 2 fluorine-containing ethylene units derived from monomers such as CF 2 =CFCF 3 , C.F. 2 = CHCF 3 fluorine-containing propylene units derived from monomers such as CH 2 = CHC 2 F 5 , C.H. 2 = CHC4 F 9 , C.H. 2 = CFC 4 F 9 , C.H. 2 =CF(CF 2 ) 3 fluorine-containing alkylethylene units having a fluoroalkyl group having 2 to 10 carbon atoms derived from a monomer such as H; 2 = CFO (CF 2 CFXO) m R f (In the formula, R f represents a perfluoroalkyl group having 1 to 6 carbon atoms, X represents a fluorine atom or a trifluoromethyl group, and m represents an integer of 1 to 5; 2 = CFOCF 2 CF 2 CF 2 COOCH 3 , C.F. 2 = CFOCF 2 CF (CF 3 ) OCF 2 CF 2 SO 2 Examples of the other monomer units include vinyl ether units having a group that can be converted into a carboxylic acid group or a sulfonic acid group, which are derived from a monomer such as F. One type of other monomer unit may be used alone, or two or more types may be used in combination.

[0022] When ETFE has other monomer units, the content of the other monomer units in 100 mol% of all units constituting ETFE is preferably 0.01 to 10 mol%, more preferably 0.05 to 5 mol%, and still more preferably 0.1 to 4 mol%.

[0023] The resin contained in the fluororesin layer may contain a resin other than the fluororesin. Examples of the other resin include acrylic resin, polycarbonate resin, polyethylene resin, polypropylene resin, polyethylene terephthalate, polybutylene terephthalate, nylon, etc. The resin other than the fluororesin may be used alone or in combination of two or more. The proportion of the fluororesin in the fluororesin layer is preferably 50% by mass or more, more preferably 90% by mass or more, even more preferably 98% by mass or more, and particularly preferably 100% by mass. When the proportion of the fluororesin in the fluororesin layer is 50% by mass or more, the heat resistance is excellent.

[0024] (Pigment) Known pigments can be used as the pigment contained in the fluororesin layer, and from the viewpoint of excellent weather resistance, those that reduce transmittance in the ultraviolet region and have excellent ultraviolet shielding properties are preferred. Examples include black pigments such as carbon black, blue pigments such as cobalt oxide, red pigments such as iron oxide, yellow pigments such as cerium oxide, and white pigments such as titanium oxide, silicon oxide, and zinc oxide. Among these, from the viewpoint of excellent ultraviolet shielding properties, carbon black or titanium oxide is preferred, and titanium oxide is particularly preferred. One type of pigment may be used alone, or two or more types may be used in combination. Furthermore, the pigment may be coated with other pigments, inorganic substances, organic substances, or combinations thereof, as long as the ultraviolet shielding ability is not impaired.

[0025] The pigment content in the fluororesin layer is 1.0% by mass or more, more preferably 2.0% by mass or more, and particularly preferably 2.5% by mass or more. The upper limit is preferably 15.0% by mass or less, more preferably 13.0% by mass or less, and even more preferably 11.0% by mass or less. A pigment content of 1.0% by mass or more reduces the amount of UV light transmitted through the fluororesin layer and the amount of UV light reaching the adhesive layer and the substrate, thereby providing excellent UV shielding and suppressing UV-induced deterioration of the adhesive layer and the substrate, thereby enabling the production of an adhesive film with excellent adhesion even after a weather resistance test. A pigment content of less than the upper limit is preferred because it provides excellent kneading properties when the pigment is kneaded into the resin, and the resulting adhesive film has excellent substrate concealment properties. The substrate concealment properties refer to the inability to view patterns, letters, fibers, etc., on the substrate when the adhesive film and the substrate are laminated together. Excellent substrate concealment properties result in excellent design properties for articles in which the adhesive film and the substrate are laminated together.

[0026] When a pigment having catalytic activity is used as the pigment, the catalytic activity of the pigment is expressed by light or heat during outdoor use, and may react with the fluororesin in the fluororesin layer to cause voids and other deterioration of the fluororesin layer. However, if the pigment content is 1.0 mass% or more, even if the catalytic activity of a portion of the pigment is expressed, the remaining pigment amount is sufficient to fully exhibit the ultraviolet shielding effect, and successive expression of the catalytic activity of the pigment due to light or heat can be suppressed.

[0027] The content of the pigment contained in the fluororesin layer may be calculated as a theoretical value from the amount of pigment added when the fluororesin layer was produced, or may be calculated by baking the fluororesin layer to burn off the resin, and measuring the weight before and after baking using an analytical balance (for example, AUX320 manufactured by Shimadzu Corporation).

[0028] The pigment content in the fluororesin layer is preferably adjusted appropriately according to the average thickness of the fluororesin layer to fully exhibit the UV-shielding effect. When the average thickness of the fluororesin layer is 10 μm or more and less than 20 μm, the pigment content is preferably 10.0% by mass or more and 15.0% by mass or less. When the average thickness of the fluororesin layer is 20 μm or more and less than 50 μm, the pigment content is preferably 5.0% by mass or more and 15.0% by mass or less. When the average thickness of the fluororesin layer is 50 μm or more and less than 75 μm, the pigment content is preferably 2.0% by mass or more and 15.0% by mass or less, more preferably 12.0% by mass or more and 15.0% by mass or less. When the average thickness of the fluororesin layer is 75 μm or more and less than 100 μm, the pigment content is preferably 2.0% by mass or more and 15.0% by mass or less, more preferably 7.0% by mass or more and 13.0% by mass or less. When the average thickness of the fluororesin layer is 100 μm or more and less than 150 μm, the pigment content is preferably 1.0% by mass or more and 15.0% by mass or less, and more preferably 6.0% by mass or more and 10.0% by mass or less. When the average thickness of the fluororesin layer is 150 μm or more and less than 200 μm, the pigment content is preferably 1.0% by mass or more and 14.0% by mass or less, and more preferably 5.0% by mass or more and 6.0% by mass or less. When the average thickness of the fluororesin layer is 200 μm or more and less than 250 μm, the pigment content is preferably 1.0% by mass or more and 10.0% by mass or less, more preferably 2.5% by mass or more and 5.0% by mass or less, and may be 3.0% by mass or more and 5.0% by mass or less. When the average thickness of the fluororesin layer is 250 μm or more and less than 300 μm, the pigment content is preferably 1.0% by mass or more and 7.0% by mass or less, and more preferably 2.0% by mass or more and 3.0% by mass or less.

[0029] The fluororesin layer preferably satisfies the following relational expression (1): 100<Pigment content in the fluororesin layer (% by mass) × Average thickness of the fluororesin layer (μm) < 2100. The pigment content in the fluororesin layer (% by mass) × Average thickness of the fluororesin layer (μm) is preferably 100 to 2100, more preferably 500 to 1500, and more preferably 610 to 1000. Within the above range, the adhesive film exhibits excellent UV blocking properties and substrate concealment effects. Furthermore, the formability of the fluororesin layer and the formability when laminating the adhesive film to the substrate are excellent. Furthermore, the adhesive film exhibits excellent adhesion after a weather resistance test. The above-mentioned ranges are preferred for the pigment content in the fluororesin layer and the average thickness of the fluororesin layer. Table 1 shows an example of how to calculate the relational expression (1).

[0030]

[0031] The average particle size of the pigment is preferably 0.10 to 5.0 μm, and more preferably 0.15 to 2.0 μm. If the average particle size of the pigment is within the above range, the ultraviolet ray blocking function is excellent. The average particle size of the pigment is measured by observing the fluororesin layer with a scanning electron microscope, measuring the particle sizes of 20 randomly selected particles, and averaging these values.

[0032] When the pigment contains titanium oxide, it preferably contains titanium oxide and aluminum oxide. Because titanium oxide has catalytic activity, titanium oxide composite particles (hereinafter also referred to as "titanium oxide composite particles") having a coating layer containing at least aluminum oxide on the surface of the titanium oxide are more preferred. The proportion of titanium oxide in the titanium oxide composite particles is preferably 95% by mass or more, more preferably 95.5% by mass or more, relative to 100% by mass of the total mass of the titanium oxide composite particles (total of titanium oxide and coating layer). When the proportion of titanium oxide is 95% by mass or more, excellent ultraviolet shielding effect is exhibited in the fluororesin. The upper limit of the proportion of titanium oxide in the titanium oxide composite particles is not particularly limited, but is, for example, 99.9% by mass. The proportion of the coating layer in the titanium oxide composite particles is preferably 0.6 to 4.5% by mass, more preferably 1.0 to 4.0% by mass, and even more preferably 1.0 to 3.5% by mass, relative to 100% by mass of the total mass of the titanium oxide composite particles. When the proportion of the coating layer in the titanium oxide composite particles is 3.5% by mass or less, foam streaks are less likely to occur during molding of the fluororesin layer, and a fluororesin layer with good appearance is more likely to be obtained. In another embodiment, the proportion of the coating layer in the titanium oxide composite particles is, for example, 0.6 to 2.5% by mass, for example, 1.0 to 2.5% by mass, or 1.0 to 2.0% by mass, relative to 100% by mass of the total mass of the titanium oxide composite particles.

[0033] The coating layer of the titanium oxide composite particles contains at least aluminum oxide. By containing aluminum oxide, the coating layer of the titanium oxide composite particles has the effect of preventing aggregation of the composite particles and the effect of reducing the catalytic activity of titanium oxide. The proportion of aluminum oxide in the titanium oxide composite particles is preferably 0.6 to 2.5 mass%, more preferably 1.0 to 2.5 mass%, and even more preferably 1.0 to 2.0 mass%, relative to 100 mass% of the total mass of the titanium oxide composite particles. When the proportion of aluminum oxide in the titanium oxide composite particles is 2.5 mass% or less, foam streaks are less likely to occur during molding of the fluororesin layer, making it easier to obtain a fluororesin layer with good appearance.

[0034] The coating layer of the titanium oxide composite particles may contain inorganic components other than aluminum oxide. Examples of such inorganic components include phosphorus oxide, sodium oxide, silicon oxide, zirconium oxide, and cerium oxide. These inorganic components may be used singly or in combination. The total amount of silicon oxide, zirconium oxide, and cerium oxide is preferably 2.5% by mass or less, more preferably 2.0% by mass or less, and may be 1.0% by mass or less, or even 0.8% by mass or less, relative to 100% by mass of the total mass of the titanium oxide composite particles. Meanwhile, phosphorus oxide, particularly phosphate ions, may be contained in any proportion as long as the total amount with aluminum oxide is 4% by mass or less, preferably 3% by mass or less, relative to 100% by mass of the total mass of the titanium oxide composite particles.

[0035] The coating layer of the titanium oxide composite particles may be a single layer or multiple layers. When the coating layer of the titanium oxide composite particles contains an inorganic component other than aluminum oxide, the inorganic component may be contained in the same layer as the aluminum oxide or in a different layer. Among the inorganic components, phosphorus oxide and sodium oxide may be contained in the aluminum oxide layer as impurities. When silicon oxide or zirconium oxide is contained, it is preferable that a silicon oxide layer or zirconium oxide layer is provided separately from the aluminum oxide layer. In this case, it is preferable that the aluminum oxide layer is provided outside the other layer (silicon oxide layer or zirconium oxide layer).

[0036] The coating layer of the titanium oxide composite particles may have a surface treatment agent layer as the outermost layer. Examples of the surface treatment agent constituting the surface treatment agent layer include antioxidants and hydrophobizing agents. When an antioxidant is used as the surface treatment agent, coloration during compounding can be prevented. When a hydrophobizing agent is used as the surface treatment agent, aggregation of the titanium oxide composite particles in the fluororesin layer can be suppressed. As the antioxidant, known antioxidants such as phosphorus-containing antioxidants, phenolic antioxidants, and sulfur-containing antioxidants can be used.

[0037] Examples of the hydrophobizing agent include a silane coupling agent having an alkyl group, a silicone compound, etc. Examples of the silane coupling agent having an alkyl group include trialkoxysilanes such as isobutyltrimethoxysilane, hexyltrimethoxysilane, and (3,3,3-trifluoropropyl)trimethoxysilane; silazanes such as hexamethyldisilazane; and chlorosilanes such as dimethyldichlorosilane. Of these, isobutyltrimethoxysilane is preferred.

[0038] The silicone compound is an organopolysiloxane having an organic group. The organic group is preferably an alkyl group or a phenyl group having 4 or less carbon atoms. Silicone compounds commonly known as silicone oils can be used. Examples of silicone oils include straight silicone oils such as dimethyl silicone oil and phenylmethyl silicone oil, alkyl-modified silicone oil, alkylaralkyl-modified silicone oil, and fluorinated alkyl-modified silicone oil. Among these, dimethyl silicone oil is preferred from the viewpoint of cost, and phenylmethyl silicone oil is preferred from the viewpoint of heat resistance. Commercially available silicone compounds can be used. Examples of dimethyl silicone oils with various molecular weights (viscosities) include SH200 (product name) manufactured by Dow Corning Toray Silicone Co., Ltd., KF96 (product name) manufactured by Shin-Etsu Chemical Co., Ltd., and TSF451 (product name) manufactured by Momentive Performance Materials, Inc. Examples of phenylmethyl silicone oils include SH510 (product name), SH550 (product name), and SH710 (product name) manufactured by Toray Dow Corning Silicone Co., Ltd., and KF54 (product name) manufactured by Shin-Etsu Chemical Co., Ltd.

[0039] Silicone compounds are preferred as hydrophobizing agents. When silicone compounds are used, the fluororesin layer is less likely to harden even after long-term outdoor exposure, and flexibility is more likely to be maintained. The reason for this is unclear, but it is presumed that silicone compounds have the effect of inhibiting the crystallization of the fluororesin.

[0040] When a surface treatment agent layer is provided, the proportion of the surface treatment agent layer in the titanium oxide composite particles is preferably 0.3 to 2.5 mass% and more preferably 0.5 to 1.5 mass% relative to the total mass of the composite particles before the surface treatment agent layer is provided, i.e., the total mass of particles (inorganic particles) composed of inorganic components such as titanium oxide and aluminum oxide. A proportion of 0.3 mass% or more ensures sufficient effects of providing the surface treatment agent layer. If the proportion exceeds 2.5 mass%, and if the surface treatment agent has low heat resistance, a large amount of thermal decomposition products of the surface treatment agent may be generated during film molding and adhere to the die, potentially necessitating frequent lip cleaning.

[0041] The titanium oxide composite particles may be produced by a known production method, or commercially available products may be used. Examples of commercially available products that can be used as titanium oxide composite particles include Ti-Pure (registered trademark) R-101, R-102, R-103, R-104, and R-350 manufactured by Chemours; TiONA (registered trademark) RCL-69, TiONA (registered trademark) 188, and TRONOX (registered trademark) CR470 manufactured by TRONOX; 2230 and 2233 manufactured by Kronos; and CR50 and CR63 manufactured by Ishihara Sangyo Kaisha, Ltd. A surface treatment agent layer may be further provided on these commercially available products.

[0042] When titanium oxide composite particles are used as the pigment, the content of the titanium oxide composite particles in the fluororesin layer is preferably 1.0% by mass or more, more preferably 2.0% by mass or more, and even more preferably 2.5% by mass or more. The upper limit is preferably 15.0% by mass or less, more preferably 13.0% by mass or less, and even more preferably 11.0% by mass or less. If the content of titanium oxide composite particles in the fluororesin layer is 1.0% by mass or more, the amount of ultraviolet light transmitted through the fluororesin layer is reduced, and the amount of ultraviolet light reaching the adhesive layer and the substrate can be further reduced, thereby suppressing deterioration of the adhesive layer and the substrate due to ultraviolet light and obtaining an adhesive film with superior adhesive strength after a weather resistance test. If the content is below the upper limit, the kneading property when kneading the pigment into the fluororesin is superior.

[0043] The content of each component in the titanium oxide composite particles can be measured by subjecting the fluororesin layer to a scanning X-ray fluorescence analyzer (for example, ZSX Primus II manufactured by Rigaku Corporation).

[0044] The average particle size of the titanium oxide composite particles is preferably 0.15 to 0.40 μm, and more preferably 0.17 to 0.30 μm. If the average particle size is 0.15 μm or more, the specific surface area of ​​titanium oxide in the titanium oxide composite particles is reduced, and the development of catalytic activity is effectively suppressed. From the viewpoint of effectively suppressing the development of catalytic activity, the average particle size is preferably 0.15 μm or more in order to reduce the specific surface area of ​​titanium oxide in the titanium oxide composite particles. If the average particle size is 0.40 μm or less, the ultraviolet shielding function is excellent. The average particle size of the titanium oxide composite particles is determined by observing the fluororesin layer with an electron microscope, measuring the particle sizes of 20 randomly selected particles, and averaging the measured values.

[0045] As the pigment, zinc oxide particles may be used, or zinc oxide composite particles having a coating layer containing at least silicon oxide on the surface of zinc oxide particles may be used. The zinc oxide composite particles are preferably used in combination with titanium oxide or titanium oxide composite particles. In particular, when the content of titanium oxide or titanium oxide composite particles in the fluororesin layer is 5.0 mass% or less, the combined use of zinc oxide composite particles and titanium oxide or titanium oxide composite particles can sufficiently suppress the catalytic activity of the titanium oxide or titanium oxide composite particles, resulting in better weather resistance. This effect is thought to be due to the synergistic interaction of the zinc oxide composite particles, which function as an ultraviolet shielding agent, thereby reducing the amount of ultraviolet light hitting the titanium oxide or titanium oxide composite particles, and the zinc oxide composite particles, which function as an acid acceptor for hydrofluoric acid produced by photodecomposition of the fluororesin, thereby suppressing the chain reaction of photodecomposition of the fluororesin caused by hydrofluoric acid.

[0046] The mass ratio of zinc oxide to silicon oxide in the zinc oxide composite particles (ZnO / SiO 2) is preferably 40 / 60 to 85 / 15, more preferably 50 / 50 to 85 / 15, even more preferably 50 / 50 to 80 / 20, and may be 60 / 40 to 80 / 20. 2 Within the above range, the effect of gradually and efficiently neutralizing hydrofluoric acid is exhibited, resulting in an adhesive film with better weather resistance. When the mass ratio is equal to or less than the upper limit, the neutralizing effect against hydrofluoric acid tends to be maintained for a long period of time. When the mass ratio is equal to or more than the lower limit, aggregation of the zinc oxide composite particles is effectively suppressed.

[0047] The coating layer of the zinc oxide composite particles may contain inorganic components other than silicon oxide. Examples of other inorganic components include phosphorus oxide, sodium oxide, aluminum oxide, zirconium oxide, and cerium oxide. The total amount of zinc oxide and silicon oxide in the zinc oxide composite particles is preferably 80% by mass or more, more preferably 85% by mass or more. When the total amount is 80% by mass or more, the above-mentioned effects are sufficiently exhibited.

[0048] The coating layer of the zinc oxide composite particles may be a single layer or multiple layers. When the coating layer of the zinc oxide composite particles contains an inorganic component other than silicon oxide, the inorganic component may be contained in the same layer as the silicon oxide or in a different layer. Among the inorganic components, phosphorus oxide and sodium oxide may be contained in the silicon oxide layer as impurities. When aluminum oxide or zirconium oxide is contained, it is preferable that an aluminum oxide layer or zirconium oxide layer is provided separately from the silicon oxide layer. In this case, it is preferable that the aluminum oxide layer is provided outside the other layer (aluminum oxide layer or zirconium oxide layer).

[0049] The coating layer of the zinc oxide composite particles may have a surface treatment agent layer as the outermost layer. Examples of surface treatment agents constituting the surface treatment agent layer include those similar to those mentioned in the description of the titanium oxide composite particles. When a surface treatment agent layer is provided, the proportion of the surface treatment agent layer in the zinc oxide composite particles is preferably 1 to 5 mass %, more preferably 1.5 to 4 mass %, relative to the total mass of the zinc oxide composite particles before the surface treatment agent layer is provided, i.e., the total mass of particles (inorganic particles) composed of inorganic components such as zinc oxide and silicon oxide. When the proportion is 1 mass % or more, the effect of providing the surface treatment agent layer is sufficiently obtained. When the proportion is 5 mass % or less, the generation of thermal decomposition products of the surface treatment agent during film formation is effectively suppressed.

[0050] The zinc oxide composite particles may be produced by a known production method or may be commercially available. The zinc oxide composite particles may have a surface area of, for example, 25 to 50 m 2 / g of zinc oxide particles are coated with silicon oxide. Examples of the method for coating with silicon oxide include a method utilizing a sol-gel reaction using alkoxysilane and a method of producing from water glass (for example, JP-A-11-256133). Commercially available zinc oxide composite particles include, for example, MZ-510HPSX (ZnO / SiO 2 These commercially available products include those that have been subjected to hydrophobic treatment, and may further be provided with a surface treatment agent layer.

[0051] When titanium oxide composite particles and zinc oxide composite particles are contained, the total content of the titanium oxide composite particles and the zinc oxide composite particles in the fluororesin layer is preferably 1.0 to 15.0 mass%, more preferably 2.0 to 13.0 mass%. The content of the zinc oxide composite particles is preferably 0.05 to 0.5 mass%, more preferably 0.1 to 0.3 mass%, relative to the fluororesin. When the content of the zinc oxide composite particles is 0.05 mass% or more relative to the fluororesin, hydrofluoric acid produced by decomposition of the fluororesin during exposure of the fluororesin layer to light can be sufficiently neutralized. When the content of the zinc oxide composite particles is 0.5 mass% or less relative to the fluororesin, the content of silicon oxide is sufficiently reduced, which makes it difficult for foam streaks to occur during film molding, and makes it easy to obtain a fluororesin layer with good appearance.

[0052] The content of each component in the zinc oxide composite particles can be measured using a scanning X-ray fluorescence analyzer (for example, ZSX Primus II manufactured by Rigaku Corporation). The content of each component may also be measured using a pressed sheet of the zinc oxide composite particles.

[0053] The average particle size of the zinc oxide composite particles is preferably 0.1 to 5 μm, and more preferably 0.2 to 2 μm. If the average particle size is 0.1 μm or more, the use of a surface hydrophobizing agent can be effectively suppressed, and the occurrence of streaks during film formation can be effectively suppressed. If the average particle size is 5 μm or less, the film will have excellent smoothness. The average particle size of the zinc oxide composite particles is measured by observing the fluororesin layer with a scanning electron microscope, measuring the particle sizes of 20 randomly selected particles, and averaging these values.

[0054] (Other Components) The fluororesin layer according to one embodiment of the present disclosure may contain additives other than the fluororesin and the pigment, as necessary. Examples of the additives include copper compounds such as copper oxide and copper iodide, hydrophobizing agents, antioxidants, mica, and antibacterial agents. Among the above, the inclusion of a copper compound improves the heat resistance of the resin film.

[0055] Examples of the hydrophobizing agent and antioxidant include the same agents as those listed as surface treatment agents in the description of the titanium oxide composite particles.

[0056] The fluororesin layer according to one embodiment of the present disclosure can be produced by a known method, for example, by melt-kneading a fluororesin, a pigment, and other optional components to form a resin composition, and then forming the resin composition into a film by a known molding method. Furthermore, if necessary, a surface treatment may be applied.

[0057] In order to improve the coatability of the adhesive layer, it is preferable to surface-treat the surface of the fluororesin layer that comes into contact with the adhesive layer. The surface treatment is not particularly limited, and examples thereof include corona discharge treatment, plasma discharge treatment, UV ozone treatment, flame treatment, and chemical conversion treatment. Among these, corona discharge treatment or plasma discharge treatment is preferred, and corona discharge treatment is more preferred, from the viewpoints of simplicity of the equipment and ease of introduction into industrial processes. Corona discharge treatment or plasma discharge treatment generates hydrophilic functional groups on the surface, thereby reducing surface energy. The surface wetting index of the fluororesin layer obtained by the surface treatment is preferably 20 mN / m or more, more preferably 30 mN / m or more, and particularly preferably 35 mN / m or more, from the viewpoints of the coatability of the adhesive layer and the adhesion between the adhesive layer and the fluororesin layer. The upper limit of the wetting tension is not particularly limited, and may be 80 mN / m or less. The surface wettability index of the fluororesin layer of the present disclosure is a value obtained by subjecting at least one surface of the fluororesin layer to a corona treatment and measuring the corona-treated surface using a wettability index reagent manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. in accordance with JIS K6768:1999.

[0058] [Adhesive Layer] The adhesive layer in one embodiment of the present disclosure is disposed on at least a portion of the fluororesin layer and contains a silane coupling agent having a functional group. Known silane coupling agents can be used as the silane coupling agent having a functional group. Examples of functional groups include amino groups, epoxy groups, mercapto groups, isocyanate groups, and acrylic groups. Silane coupling agents having at least one selected from the group consisting of amino groups, epoxy groups, and acrylic groups are preferred from the viewpoint of easily forming a bond at the interface between the substrate and the adhesive layer and providing excellent adhesion between the substrate and the adhesive layer. Silane coupling agents having an amino group as a functional group are particularly preferred from the viewpoint of requiring heating in the bonding step with the substrate or providing excellent adhesion to substrates with unevenness. The silane coupling agents having a functional group may be used alone or in combination of two or more.

[0059] Examples of silane coupling agents having an amino group include N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, N-phenyl-3-aminopropylmethyldimethoxysilane, and N-phenyl-3-aminopropylmethyldiethoxysilane are preferred, and from the viewpoint of obtaining stable adhesive strength, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and 3-aminopropylmethyldimethoxysilane are particularly preferred.

[0060] As the silane coupling agent having an epoxy group, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane are preferred.

[0061] As the silane coupling agent having a mercapto group, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, and 3-mercaptopropyltriethoxysilane are preferred.

[0062] As the silane coupling agent having an isocyanate group, 3-isocyanate propyl methyl dimethoxy silane, 3-isocyanate propyl trimethoxy silane, 3-isocyanate propyl methyl diethoxy silane, and 3-isocyanate propyl triethoxy silane are preferred.

[0063] As the silane coupling agent having an acrylic group, 3-acryloxypropyltrimethoxysilane and 3-acryloxypropyltriethoxysilane are preferred.

[0064] The amount of functional groups in the silane coupling agent contained in the adhesive layer is 0.01 mmol / m 2 More preferably, 0.015 mmol / m or more 2 More preferably, 0.05 mmol / m or more 2 The upper limit is 5.0 mmol / m 2 Preferably, 2.5 mmol / m or less 2 More preferably, 1.0 mmol / m or less 2 More preferably, 0.7 mmol / m or less 2 The following is particularly preferred: 0.2 mmol / m 2 The following is highly preferred: The amount of functional groups of the silane coupling agent contained in the adhesive layer is 0.01 mmol / m 2 A content of 5.0 mmol / m or more is preferable in terms of excellent initial adhesion to the substrate and adhesion after a weather resistance test. 2 When the amount of functional groups in the silane coupling agent contained in the adhesive layer is 1.0 mmol / m or less, the amount of the silane coupling agent used is prevented from becoming unnecessarily large. 2 In the following cases, hydrophilicity is maintained for 100 days or more in a hydrophilicity retention evaluation at 80°C, and is particularly excellent for outdoor use.

[0065] The amount of functional groups in the silane coupling agent contained in the adhesive layer is determined from the following theoretical value: Theoretical value: When a coating liquid containing the silane coupling agent (solid content) is applied with a bar coater and dried to form an adhesive layer, the amount is determined by multiplying the wire number of the bar coater by 2.29, multiplying the result by the concentration (= mass of silane coupling agent / mass of coating liquid), and dividing the result by the molecular weight of the silane coupling agent.

[0066] The average thickness of the adhesive layer is preferably 0.5 μm or less, more preferably 0.1 μm or less, and even more preferably 0.05 μm or less. The lower limit is preferably 0.001 μm or more, more preferably 0.003 μm or more, and even more preferably 0.01 μm or more. A thickness within the above range is preferable in that stable adhesive strength can be obtained. When a coating liquid containing a silane coupling agent (solid content) is applied with a bar coater and dried to form an adhesive layer, the average thickness (μm) of the adhesive layer is determined by multiplying the wire number of the bar coater by 2.29, multiplying this by the concentration (= mass of silane coupling agent / mass of coating liquid), and dividing the result by the specific gravity of the silane coupling agent.

[0067] In addition to the silane coupling agent having a functional group, the adhesive layer may further contain a leveling agent, a solvent, etc. The solvent, which serves to dilute the silane coupling agent having a functional group and improve the coatability when forming the adhesive layer, is removed by drying, but may remain in the adhesive layer.

[0068] The solvent may be any solvent capable of dissolving or dispersing the silane coupling agent having a functional group, and examples thereof include aromatic hydrocarbons such as benzene, toluene, and xylene, alicyclic hydrocarbons such as cyclohexane, aliphatic hydrocarbons such as hexane and octane, ethers, ketones, and esters such as diacetone alcohol, diethylene glycol, butyl carbitol, isophorone, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, 4-hydroxy-4-methyl-2-pentanone, and ethyl acetate, halogenated hydrocarbons such as dichloromethane and carbon tetrachloride, organic solvents containing two or more functional groups such as dimethylformamide, butyl carbitol acetate, and diethanolamine, and monohydric or polyhydric alcohols such as methanol, ethanol, propanol, 2-propanol, butanol, 2-methyl-1-propanol, and ethylene glycol. The solvents may be used alone or in combination of two or more.

[0069] The adhesive layer may be formed by applying an adhesive liquid containing a silane coupling agent having a functional group, a solvent, a leveling agent, and any other optional components as a coating liquid. The coating liquid may be a dispersion or a solution. The content of the solvent in the coating liquid is set so as to obtain a viscosity suitable for the layer formation method to be applied, such as coating or printing. Typically, the solvent is contained in an amount of 10 to 100 parts by mass per 10 parts by mass of the silane coupling agent having a functional group, but this is not limited thereto. Furthermore, the leveling agent is contained in an amount of 0.01 to 0.10 parts by mass per 10 parts by mass of the silane coupling agent having a functional group, but this is not limited thereto. The content of any other components contained therein may also be adjusted appropriately.

[0070] Examples of a method for applying an adhesive liquid to form an adhesive layer include wet coating. Examples of wet coating include spin coating, bar coating, microgravure coating, and direct gravure coating. Of these, spin coating, bar coating, and microgravure coating, which allow application in small amounts, are preferred.

[0071] [Layer structure] Figure 1 shows a schematic cross-sectional view illustrating the layer structure of an example of an adhesive film of the present disclosure. The adhesive film (10) in Figure 1 is composed of a fluororesin layer (2) and an adhesive layer (4) provided in this order. The fluororesin layer (2) contains a pigment (6).

[0072] The average thickness of the adhesive film in one embodiment of the present disclosure is preferably 10 μm or more, more preferably 12 μm or more, and even more preferably 20 μm or more. The upper limit is preferably 300 μm or less, and even more preferably 250 μm or less. Within the above range, excellent conformability to the substrate during lamination processing is achieved. The average thickness of the adhesive film is determined by measuring the thickness at five points and calculating the arithmetic mean value. If measurement is possible with a micrometer, the five points may be measured with a micrometer and the average value may be calculated. If measurement with a micrometer is not possible, the adhesive film may be cut, the cross section observed with a metallurgical microscope or electron microscope, and the five points may be measured by comparison with a scale bar or the like, and the average value may be calculated.

[0073] (Other Layers) The adhesive film may have an antifouling layer as another layer on the side of the fluororesin layer that does not have the adhesive layer. Examples of the antifouling layer include a water-repellent layer, an oil-repellent layer, an anti-fingerprint layer, and a hydrophilic layer. A hydrophilic layer is particularly preferred.

[0074] The hydrophilic layer serving as the antifouling layer can be formed by applying a hydrophilizing agent. The hydrophilizing agent is not particularly limited, and known agents can be used. The hydrophilizing agent preferably contains hydrophilic inorganic fine particles (average particle size of about 0.01 μm) such as silica fine particles or alumina fine particles, and more preferably a mixture of silica fine particles and boehmite fine particles. The hydrophilizing agent typically used is one in which inorganic fine particles are dispersed in a binder such as a silane coupling agent or polyvinyl alcohol (PVA). The hydrophilizing agent may contain a solvent such as ion-exchanged water or a pH adjuster such as nitric acid.

[0075] The thickness of the hydrophilic layer is preferably 0.01 to 1 μm.

[0076] When an antifouling layer is provided, it is preferable to surface-treat the substrate to which the hydrophilizing agent is applied in order to improve the coatability of the hydrophilizing agent. The surface treatment is not particularly limited, and examples thereof include corona discharge treatment, plasma discharge treatment, ozone treatment, flame treatment, chemical conversion treatment, and primer treatment. Corona discharge treatment is more preferable as the surface treatment. The primer treatment may be performed using a primer treatment liquid. The primer treatment liquid preferably contains an aminosilane. The primer treatment liquid may further contain a leveling agent, a solvent, and the like.

[0077] [Physical Properties of Adhesive Film] In one embodiment of the present disclosure, the adhesive film preferably has a transmittance of 1.0% or less at a wavelength of 360 nm, more preferably 0.5% or less, more preferably 0.1% or less, and even more preferably 0.03% or less, in order to block ultraviolet rays and improve adhesion to the substrate after a weather resistance test. The transmittance at a wavelength of 360 nm may be 0.0%. Furthermore, from the viewpoint of suppressing deterioration due to ultraviolet rays, the transmittance at a wavelength of 400 nm is preferably 1.0% or less, more preferably 0.4% or less, even more preferably 0.3% or less, and particularly preferably 0.1% or less. The transmittance at a wavelength of 400 nm may be 0.0%. Furthermore, from the viewpoint of the obtained adhesive film having an excellent effect of concealing the substrate, the transmittance at a wavelength of 550 nm is preferably 10.0% or less, and preferably 8.0% or less. The transmittance at a wavelength of 550 nm may be 0.0%. The transmittance at each wavelength is measured in % at 360 nm, 400 nm and 550 nm in accordance with DIN EN 410 1998 using an ultraviolet-visible-near infrared spectrophotometer (for example, Shimadzu UV-PC3600 measuring instrument).

[0078] In the adhesive film according to one embodiment of the present disclosure, an uneven structure may be provided on at least one surface of the fluororesin layer. When an uneven structure is provided on the surface of the fluororesin layer that is in contact with the adhesive layer, this is preferred in terms of increasing the surface area and providing excellent adhesion to the substrate. Furthermore, when an uneven structure is provided on the surface of the fluororesin layer that is not provided with the adhesive layer, this is preferred in terms of providing excellent suppression of light reflection.

[0079] The arithmetic mean roughness Ra of the surface having a concave-convex structure is preferably 0.3 to 3.5 μm, more preferably 0.3 to 3.0 μm, even more preferably 0.8 to 3.0 μm, particularly preferably 1.0 to 3.0 μm, and may be 1.0 to 2.5 μm. The depth of the concave-convex structure may be set shallower, in which case Ra is preferably 0.3 to 2.0 μm, more preferably 0.8 to 1.8 μm, and even more preferably 1.0 to 1.6 μm. On the other hand, the depth of the concave-convex structure may be set deeper, in which case Ra is preferably 0.6 to 3.0 μm, more preferably 1.7 to 3.0 μm, and even more preferably 1.8 to 3.0 μm.

[0080] The maximum height roughness Rz of the surface having the uneven structure is preferably 1 to 25 μm, more preferably 4 to 25 μm, and even more preferably 4 to 22 μm. When the depth of the unevenness is set to be shallow, Rz is preferably 1 to 8 μm, more preferably 4 to 7 μm, and even more preferably 4 to 6 μm. When the depth of the unevenness is set to be deep, Rz is preferably 12 to 25 μm, more preferably 13 to 25 μm, and even more preferably 14 to 22 μm, and may be 15 to 25 μm or 18 to 22 μm.

[0081] The arithmetic mean roughness Ra and the maximum height roughness Rz refer to values ​​measured by the method described in JIS B0601:2013 (ISO4287:1997, Amd.1:2009).

[0082] The adhesive film of the present disclosure has excellent adhesion after weather resistance testing, and is therefore suitable for use as a protective film for outdoor use. Examples of protective films for outdoor use include building exterior materials, solar cells, wind power generation blades, vehicle exterior materials, ship exterior materials, exterior materials for aerospace vehicles such as rockets and balloons, and communication infrastructure. Furthermore, since the adhesive film of the present disclosure contains a pigment and is colored, it can also be used as a building interior material and an interior material for aerospace vehicles such as rockets and balloons from the perspective of design.

[0083] <Article> An article according to one embodiment of the present disclosure includes the adhesive film according to one embodiment of the present disclosure and a substrate, and is provided with a fluororesin layer, an adhesive layer, and a substrate in this order. FIG. 2 shows a schematic cross-sectional view illustrating the layer structure of an example of an article according to the present disclosure. The article (20) of FIG. 2 is provided with a fluororesin layer (2), an adhesive layer (4), and a substrate (8) in this order. The fluororesin layer (2) contains a pigment (6). Another substrate (not shown) may be provided on the surface of the substrate (8) opposite the adhesive layer (4).

[0084] The material (including composition) constituting the substrate is not particularly limited, and known materials can be used. Materials usable for the substrate include glass, polymethylpentene, syndiotactic polystyrene, polycycloolefin, silicone rubber, polyester elastomer, polyethylene terephthalate, polybutylene terephthalate, unstretched nylon, polycarbonate, polyvinyl chloride, epoxy resin, acrylic resin, ethylene-vinyl acetate copolymer resin, modified polyethylene, and fiber-containing resin. From the viewpoint of a substrate having heat resistance that does not deform when heated and bonded to an adhesive film, glass, polycarbonate, polyvinyl chloride, epoxy resin, acrylic resin, ethylene-vinyl acetate copolymer resin, modified polyethylene, and fiber-containing resin are preferred. Fiber-containing resins are particularly preferred from the viewpoints of high strength, light weight, corrosion resistance, and moldability into various sizes. These substrates may be used alone or in combination of two or more types.

[0085] Examples of fibers contained in fiber-containing resins include glass fibers, carbon fibers, boron fibers, and aramid fibers. Resins used in fiber-containing resins include thermosetting resins such as epoxy resins, phenolic resins, and unsaturated polyester resins, and thermoplastic resins such as polypropylene resins and polyamide resins. Particularly preferred substrates include glass fiber-reinforced plastics (GFRP), which are fiber-containing resins containing glass fibers; thermosetting carbon fiber-reinforced plastics (CFRP), which are made from carbon fibers and thermosetting resins such as epoxy resins; and thermoplastic carbon fiber-reinforced plastics (CFRTP), which are made from carbon fibers and thermoplastic resins such as polypropylene resins. Fiber-containing resins are lightweight and have high elastic modulus, heat resistance, and impact resistance, making them suitable for use as structural materials for outdoor applications and aircraft. The adhesive film of one embodiment of the present disclosure exhibits excellent adhesion to substrates, both initially and after weathering tests, making it suitable for use with fiber-containing resins.

[0086] The average thickness of the substrate is not particularly limited and is selected according to various applications. When the average thickness of the substrate can be measured with a micrometer, it may be measured at five locations using a micrometer and the average value calculated. Alternatively, the article may be cut, the cross section observed using a metallurgical microscope or electron microscope, and the five locations measured by comparison with a scale bar or the like, and the average value calculated. In the present disclosure, the thickness was measured in accordance with ISO 4591:1992 (JIS K7130:1999 B1 method, a method for measuring the thickness of a sample taken from a plastic film or sheet using a mass method).

[0087] When laminating a substrate and an adhesive film, the surface in contact with the adhesive layer may be surface-treated to improve the adhesive strength between the adhesive layer and the substrate. The surface treatment is not particularly limited, and examples thereof include corona discharge treatment, plasma discharge treatment, UV ozone treatment, flame treatment, chemical conversion treatment, and primer treatment. A preferred surface treatment method is selected according to the type of substrate. From the viewpoint of ease of introduction into industrial processes, corona discharge treatment or plasma discharge treatment is preferred, and corona discharge treatment is more preferred. The surface wetting index of the substrate after surface treatment is preferably 30 mN / m or more, more preferably 36 mN / m or more, and particularly preferably 40 mN / m or more. The upper limit of the wetting tension is not particularly limited, and may be 60 mN / m or less.

[0088] The method for laminating the substrate and the adhesive film to produce an article is not particularly limited, and known methods can be used. Examples include a lamination method using a hand roller at room temperature and normal pressure, and a lamination method in which heating and pressure are applied in a vacuum. If air bubbles are introduced between the adhesive film and the substrate during lamination, the adhesive strength and the strength of the article will decrease, so it is preferable to remove the air bubbles using a hand roller, a brush, or in a vacuum.

[0089] The adhesive strength at the interface between the adhesive film and the substrate in the article of the present disclosure was measured using a Tensilon universal testing machine (RTC-1210A manufactured by A&D Co., Ltd.) at 180°C and 50 mm / min using a 180° peel method. After the start of the test, the average value of the peel force over 20 mm over a travel distance of 10 to 30 mm was calculated as the adhesive strength. The initial adhesive strength at the interface between the adhesive film and the substrate is preferably 3 N / cm or more, more preferably 6 N / cm or more, and even more preferably 10 N / cm or more. Furthermore, even after a weather resistance test, the adhesive strength at the interface between the adhesive film and the substrate is preferably maintained at 3 N / cm or more, and even more preferably 6 N / cm or more.

[0090] (Other Layers) The article may have an antifouling layer as another layer on the surface of the article that is not in contact with the adhesive layer. Examples of the antifouling layer include a water-repellent layer, an oil-repellent layer, an anti-fingerprint layer, and a hydrophilic layer. A hydrophilic layer is particularly preferred. Examples of hydrophilic layers as antifouling layers include those described above.

[0091] The article of the present disclosure has an adhesive film that exhibits excellent adhesion after weather resistance testing, and is therefore suitable for use in articles for outdoor use by using the adhesive film as a protective film. Examples of articles for outdoor use include building exterior materials, solar cells, wind power generation blades, vehicle exterior materials, ship exterior materials, exterior materials for aerospace vehicles such as rockets and balloons, and communication infrastructure. Furthermore, because the article of the present disclosure contains a pigment and has a colored adhesive film, it can also be used as a building interior material and an interior material for aerospace vehicles such as rockets and balloons from the standpoint of design.

[0092] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. Of Examples 1 to 17, Examples 1 to 5, 11, and 13 to 17 are working examples, and Examples 6 to 10 and 12 are comparative examples. The evaluation methods and materials used in each example are shown below.

[0093] [Evaluation Method] (Thickness) The average thickness (μm) of the fluororesin layer was measured in accordance with ISO 4591:1992 (JIS K7130:1999 B1 method, a method for measuring thickness by the mass method of a sample taken from a plastic film or sheet). When an adhesive layer is formed by applying a coating liquid containing a silane coupling agent (solid content) with a bar coater and drying it, the average thickness (μm) of the adhesive layer was determined by multiplying the wire number of the bar coater by 2.29, multiplying the result by the concentration (= mass of silane coupling agent / mass of coating liquid), and dividing the result by the specific gravity of the silane coupling agent.

[0094] (Transmittance (%)) For test specimens of adhesive films immediately after production, the transmittance (%) at 360 nm, 400 nm and 550 nm was measured in accordance with DIN EN 410 1998 using an ultraviolet-visible-near infrared spectrophotometer (Shimadzu Corporation UV-PC3600 measuring instrument).

[0095] (Adhesive strength (N / cm)) The obtained test piece was cut into a width of 10 mm to prepare an evaluation sample. This evaluation sample was subjected to a peel test using a Tensilon universal material testing machine (RTC-1210A manufactured by A&D Co., Ltd.) at 180°C and at 50 mm / min by the 180° peel method. After the start of the test, the average value of the peel strength over a 20 mm travel distance of 10 to 30 mm was calculated as the adhesive strength. The evaluation criteria for adhesive strength are as follows: A (good): 6 N / cm or more B (fair): 3 N / cm or more and less than 6 N / cm C (poor): less than 3 N / cm

[0096] (Weather Resistance Test) The obtained test specimen was cut into a size of 15 cm x 7 cm to prepare an evaluation sample. This evaluation sample was placed in a weather resistance accelerated test device (Iwasaki Electric, Eye Super UV Tester) and irradiated with light at a wavelength of 300 to 450 nm and an intensity of 1500 mW / cm. 2 While irradiating the specimen with ultraviolet light, the specimen was exposed to the same cycle (12 hours and 20 seconds per cycle) consisting of (i) 10 hours of ultraviolet light irradiation under conditions of a BP (black panel) temperature of 63°C and a relative humidity of 50% RH, (ii) a 10-second shower, (iii) 2 hours of dark condensation under conditions of a BP temperature of 30°C and a relative humidity of 100% RH, and (iv) a 10-second shower, for a total of 500 hours of exposure. The ultraviolet light irradiation to the specimen was carried out from the fluororesin layer side. The adhesive strength of the evaluation sample after exposure was measured in the same manner as above. The evaluation criteria for adhesive strength were also the same as above.

[0097] (Hydrophilicity Retention Test) An adhesive film with a hydrophilic layer was prepared, in which a hydrophilic layer was provided on the adhesive layer of an adhesive film. An evaluation sample measuring 14 cm long x 8 cm wide was cut out from this adhesive film with a hydrophilic layer. The environmental test chamber was maintained at a constant temperature of 20°C, and the thermostatic water bath was maintained at 80°C. A stainless steel (SUS) roof-type frame was installed at a 15° inclination relative to the horizontal plane. The evaluation sample was placed on the frame with the hydrophilic layer facing down and left for up to 100 days, after which the evaluation sample was removed. The evaluation sample was removed 1 day, 10 days, and 100 days after setting, and the state of water droplets on the surface of the hydrophilic layer of the sample was observed to confirm the hydrophilicity retention. The criteria for determining whether hydrophilicity was retained were as follows: Hydrophilicity retained: Water droplets spread in the form of a film on the surface of the hydrophilic layer and ran down. Hydrophilicity not retained: Water droplets remained as beads on the surface of the hydrophilic layer and did not run down. The hydrophilic layer was prepared using a hydrophilizing agent prepared by mixing the following liquids 1 and 2. Liquid 1: 1.5 parts by mass of 1N nitric acid was added to 16.1 parts by mass of ion-exchanged water, and 9.7 parts by mass of silica sol (product name "Snowtex (registered trademark) S", manufactured by Nissan Chemical Industries, Ltd., pH 10, solid content concentration: 30% by mass) was added with stirring. Stirring was continued for 30 minutes, and the mixture was then allowed to stand at room temperature (25°C) for 1 day. Liquid 2: 2 parts by mass of 1N nitric acid was added to 2.75 parts by mass of ion-exchanged water, and while stirring, 50 parts by mass of industrial ethanol (product name "Solmix AP-1", manufactured by Japan Alcohol Sales Co., Ltd.), 17.8 parts by mass of boehmite (product name "K-Touch Z20A", manufactured by K.I. Chemical Co., Ltd., pH 4.0, solids concentration: 20% by mass), and 0.2 parts by mass of aminosilane (product name "KBM903", manufactured by Shin-Etsu Chemical Co., Ltd.) were added. Stirring was continued for 30 minutes, and then the mixture was allowed to stand at room temperature (25°C) for 1 day. The obtained hydrophilizing agent was applied by the bar coating method using a No. 5 bar coater and dried at 80°C for 60 seconds to form a layer with a thickness of 0.3 μm, thereby obtaining a film with the hydrophilizing agent. The evaluation criteria for the hydrophilicity retention test are as follows: A (good): Hydrophilicity was maintained for 100 days or more. B (Acceptable): The hydrophilicity was maintained for 10 days or more but less than 100 days. C (Poor): The hydrophilicity was maintained for less than 10 days.

[0098] [Materials Used] (Pigment) (Production of b1) 100 parts by mass of titanium oxide composite particles having a coating layer containing aluminum oxide on the surface of titanium oxide (average particle size: 0.25 μm; in the titanium oxide composite particles, the ratio of titanium oxide was 96.7% by mass, the ratio of aluminum oxide was 1.4% by mass, the total ratio of silicon oxide, zirconium oxide, and cerium oxide was 1.9% by mass, the total ratio of phosphorus oxide and aluminum oxide was 1.6% by mass, and the ratio of the coating layer was 3.3% by mass; Ti-Pure (registered trademark) R-350, manufactured by Chemours) were added to and mixed with a solution in which 2 parts by mass of dimethyl silicone oil (product name "SH200", manufactured by Dow Corning Toray Co., Ltd.) was dispersed in isopropyl alcohol, and the mixture was baked at 140° C. for 2 hours to obtain pigment (b1).

[0099] (Production of b2) According to the description in JP-A-11-256133, a pigment (b2) of silica-coated zinc oxide particles containing 60% by mass of zinc oxide and 40% by mass of silica was produced.

[0100] Example 1 Fluon (registered trademark) C-88AX (ETFE resin, manufactured by AGC) was used as the fluororesin. 100 parts by mass of Fluon C-88AX and 9.05 parts by mass of pigment (b1) were blended and then extruded using a 35 mm co-rotating twin-screw kneading extruder (TEM35, manufactured by Toshiba Machine) at a temperature of 320°C and a throughput of 20 kg per hour to obtain titanium oxide-containing pellets. The content of pigment (b1) contained in the fluororesin layer was 8.3 mass%. The titanium oxide-containing pellets were dried at 150°C for 1 hour and then extruded into a film to form a fluororesin layer with an average thickness of 75 μm. The film emerging from the T-die was passed through a mirror-finished roll maintained at 150°C and a surface-embossed roll maintained at 100°C while being nipped. Both surfaces were then subjected to a surface treatment using corona discharge to obtain a fluororesin film having a surface wettability index of 40 mN / m and one surface having an uneven structure. The surface having the uneven structure had an Ra of 2.8 μm and an Rz of 14.8. The surface wettability index in this disclosure is a value measured in accordance with JIS K6768:1999 using a wettability index reagent manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. The transmittance of the obtained fluororesin film at a wavelength of 360 nm was 0.0%.

[0101] An adhesive liquid was applied to the surface of the corona discharge-treated fluororesin film that did not have a textured structure by a bar coating method using a No. 5 bar, and the coated fluororesin film was dried at 80°C for 5 seconds to obtain an average thickness of 0.34 μm and a coating amount of 0.34 g / m. 2 An adhesive layer of 1.92 mmol / m was formed, and an adhesive film test specimen was obtained. The adhesive liquid used was a solution containing 3 mass% of a silane coupling agent having a primary amino group as an organic functional group (product name "KBM-903", manufactured by Shin-Etsu Chemical Co., Ltd., 3-aminopropyltrimethoxysilane), 0.05 mass% of a leveling agent (product name "Surfynol 420", manufactured by Shin-Etsu Chemical Co., Ltd.), and 96.95 mass% of industrial ethanol (product name "Solmix AP-1", manufactured by Japan Alcohol Sales Co., Ltd.). The amount of functional groups in the silane coupling agent contained in the adhesive layer was 1.92 mmol / m 2 It was.

[0102] The resulting adhesive film specimen was cut into a size of 15 cm x 7 cm. A 40 cm square SUS plate, a 40 cm square 125 μm polyimide film (product name "UPILEX (registered trademark)-S, product number 125S" manufactured by UBE), the adhesive film, a 220 μm uncured epoxy-based CFRP prepreg substrate (product name "TR3110 381GM" manufactured by Mitsubishi Rayon Co., Ltd.), and the SUS plate were laminated in this order, and then placed on the table of a high-temperature vacuum press (Kitagawa Seiki Co., Ltd., KVHC-2). When laminating the adhesive film to the substrate, the article was arranged so that it contained the fluororesin, adhesive layer, and substrate in this order. After creating a vacuum (vacuum degree 1.0 kPa), the article was pressed at 180°C for 90 minutes. The pressure was then returned to atmospheric pressure, and the sample temperature was confirmed to be below 40°C. The sample was then removed to obtain a test article having a layer structure of fluororesin layer / adhesive layer / CFRP.

[0103] The adhesive film specimens and article specimens obtained were subjected to the above evaluations. The results are shown in Table 2.

[0104] [Example 2] An adhesive layer was formed in the same manner as in Example 1, except that the amount of KBM-903 in the adhesive solution was changed to 0.3 mass % and adjusted by the amount of ethanol, to obtain a test specimen of an adhesive film and a test specimen of an article. The adhesive layer in the adhesive film of Example 2 had an average thickness of 0.034 μm, and the amount of functional groups of the silane coupling agent contained in the adhesive layer was 0.19 mmol / m 2 The adhesive film specimen and the article specimen of Example 2 were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0105] [Example 3] An adhesive layer was formed in the same manner as in Example 1, except that the amount of KBM-903 in the adhesive solution was changed to 0.03 mass % and adjusted by the amount of ethanol, to obtain a test specimen of an adhesive film and a test specimen of an article. The adhesive layer in the adhesive film of Example 3 had an average thickness of 0.0034 μm, and the amount of functional groups of the silane coupling agent contained in the adhesive layer was 0.019 mmol / m 2 The adhesive film specimen and the article specimen of Example 3 were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0106] Example 4 Using the same method as in Example 1, titanium oxide-containing pellets were prepared so that the content of pigment (b1) contained in the fluororesin layer was 3.0% by mass, and a fluororesin film having an average thickness of 200 μm and an uneven structure on one side was obtained. The Ra of the uneven structured surface was 3.0 μm and Rz was 16.8. In addition, an adhesive layer was formed using the same method as in Example 1, except that the amount of KBM-903 in the adhesive solution was changed to 1.0% by mass and adjusted with the amount of ethanol, and an adhesive film specimen and an article specimen were obtained. The adhesive layer in the adhesive film of Example 4 had an average thickness of 0.11 μm, and the amount of functional groups in the silane coupling agent contained in the adhesive layer was 0.64 mmol / m 2 The adhesive film specimen and the article specimen of Example 4 were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0107] [Example 5] 100 parts by mass of Fluon C-88AX, 3.1 parts by mass of pigment (b1), and 0.21 parts by mass of pigment (b2) were blended, and titanium oxide-containing pellets were prepared using the same method as in Example 1, to obtain a fluororesin film with an average thickness of 200 μm. The content of pigment (b1) contained in the fluororesin was 3.0% by mass, and the content of pigment (b2) was 0.2% by mass. In addition, an adhesive layer was formed using the same method as in Example 1, except that the amount of KBM-903 in the adhesive solution was changed to 0.3% by mass and adjusted with the amount of ethanol, and an adhesive film specimen and an article specimen were obtained. The adhesive layer in the adhesive film of Example 5 had an average thickness of 0.034 μm, and the amount of functional groups in the silane coupling agent contained in the adhesive layer was 0.19 mmol / m 2 The adhesive film specimen and the article specimen of Example 5 were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0108] [Example 6] An adhesive film specimen and an article specimen were obtained in the same manner as in Example 2, except that a pigment-free ETFE fluororesin film (trade name "Aflex 50N", manufactured by AGC) with an average thickness of 50 μm was used instead of the fluororesin film. The adhesive film specimen and the article specimen of Example 6 were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0109] [Example 7] Instead of the fluororesin film of Example 1, a fluororesin film of ETFE containing no pigment and having an average thickness of 50 μm (product name "Aflex 50N", manufactured by AGC) was used, and instead of the corona discharge treatment, one side of the fluororesin film was subjected to a 300 W min / m 2 irradiation in a mixed gas atmosphere consisting of argon gas / ethylene gas / carbon dioxide gas = 100 / 10 / 2 (molar ratio). 2 An atmospheric pressure plasma discharge treatment was carried out at 100°C at 100°C to obtain a fluororesin film having a surface wettability index of 44 mN / m. The obtained fluororesin film was laminated to a substrate in the same manner as in Example 1 without forming an adhesive layer, to obtain a test specimen of an article. At this time, the surface that had been subjected to the atmospheric pressure plasma discharge treatment was placed in contact with the substrate. The test specimen of the adhesive film and the test specimen of the article of Example 7 were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0110] [Example 8] Instead of the fluororesin film of Example 1, an ETFE fluororesin film (trade name "Aflex 50N", manufactured by AGC) having an average thickness of 50 μm was used, and surface treatment by corona discharge was performed on one side in the same manner as in Example 1 to obtain a fluororesin film with a surface wetting index of 50 mN / m. The obtained fluororesin film was laminated to a substrate in the same manner as in Example 1 without forming an adhesive layer, to obtain a test specimen of an article. At this time, the surface that had been subjected to corona discharge treatment was placed so as to contact the substrate. The test specimen of the adhesive film and the test specimen of the article of Example 8 were evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0111] Example 9 A fluororesin film of ETFE (trade name "Aflex 50N", manufactured by AGC) having an average thickness of 50 μm was subjected to a surface treatment by corona discharge on both sides to obtain a fluororesin film having a surface wetting index of 40 mN / m in the same manner as in Example 1. The pressure-sensitive adhesive composition described below was applied to one of the surface-treated sides with an applicator so as to give a thickness of 25 μm after drying, and the applied layer was dried at 70° C. for 5 minutes to form an adhesive layer. The adhesive composition used contained 100 parts by mass of SK-2094 (Soken Chemical & Engineering Co., Ltd., solids content 25% by mass), 1 part by mass of crosslinking agent M-5A (Soken Chemical & Engineering Co., Ltd., solids content 100% by mass), 5 parts by mass of UV absorber (BASF Japan, product name "TINUVIN 479"), and 1.5 parts by mass of light stabilizer (BASF Japan, product name "TINUVIN 123"). A CFRP substrate was placed on the resulting adhesive layer and attached at room temperature using a hand roller to avoid air bubbles. This resulted in a test specimen of an article with a layer structure of fluororesin layer / UV absorber-containing adhesive layer / CFRP. The adhesive film test specimen and the article test specimen of Example 9 were evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0112] Example 10 A fluororesin film of ETFE (trade name "Aflex 50N", manufactured by AGC) having an average thickness of 50 μm was subjected to a surface treatment by corona discharge on both sides in the same manner as in Example 1, to obtain a fluororesin film with a surface wetting index of 40 mN / m. The adhesive composition described below was applied to one of the surface-treated sides with an applicator so as to give a thickness of 10 μm after drying, and the applied layer was dried at 70° C. for 5 minutes to form an adhesive layer. The adhesive layer was prepared by mixing 100 parts by mass (solids) of HD-1013 (trade name "HD-1013", 60% solids by mass, manufactured by Rock Paint Co., Ltd.), a polyurethane resin base, 18.8 parts by mass (solids) of H-62 (isocyanate content: 10% by mass, 75% solids by mass, manufactured by Rock Paint Co., Ltd.), a curing agent, 7 parts by mass of TINUVIN 479 (hydroxyphenyltriazine-based UV absorber, manufactured by BASF Japan Co., Ltd.), and 1.5 parts by mass of TINUVIN 123 (hindered amine-based light stabilizer, manufactured by BASF Japan Co., Ltd.), to prepare an adhesive composition. The resulting adhesive layer was overlaid with a CFRP substrate and attached at room temperature using a hand roller, taking care not to introduce air bubbles. This resulted in a test specimen of an article having a layer structure of fluororesin layer / UV absorber-containing adhesive layer / CFRP. The adhesive film specimen and the article specimen of Example 10 were evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0113] Example 11 The adhesive film prepared in Example 2 was cut into a size of 15 cm x 7 cm. A 50 cm square PTFE glass cloth, a 40 cm square tempered glass, a 50 cm square PTFE glass cloth, a 2 mm polycarbonate (PC) resin substrate (product name "PC-1600" manufactured by Takiron C.I.), the adhesive film prepared in Example 2, and a 50 cm square PTFE glass cloth were laminated in this order, and then placed on the table of a vacuum laminator (manufactured by NPC Corporation, LM-50S) set to 120°C. When laminating the adhesive film to the substrate, the article was arranged so that it had the fluororesin, adhesive layer, and substrate in that order. The article was then preheated in a vacuum state (vacuum degree 100 Pa) for 3 minutes, pressurized at 100 Pa for 30 minutes, returned to atmospheric pressure, and the sample was confirmed to have reached room temperature before being removed. A test specimen having a layer structure of fluororesin layer / adhesive layer / polycarbonate resin was obtained. The test specimens of the article of Example 11 were evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0114] Example 12 A test specimen of an article having a substrate of polycarbonate (PC) resin was obtained in the same manner as in Example 11, without forming an adhesive layer on the fluororesin film described in Example 1. The adhesive film test specimen and the article test specimen of Example 12 were evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0115] Example 13 A test specimen of an article having a layer structure of fluororesin layer / adhesive layer / glass epoxy resin was obtained using the same method as in Example 11, except that the substrate was changed to a 2 mm glass epoxy (EG) resin (product name "T-932", manufactured by Sumitomo Bakelite Co., Ltd.) instead of polycarbonate resin. The test specimen of the article of Example 13 was evaluated using the same method as in Example 1. The results are shown in Table 3.

[0116] Example 14 A test specimen of an article having a layer structure of fluororesin layer / adhesive layer / polyvinyl chloride resin was obtained using the same method as in Example 11, except that the substrate was changed to a 2 mm polyvinyl chloride (PVC) resin (product name "SUMILITE (registered trademark) EL-3762", manufactured by Takiron C.I. Co., Ltd.) instead of polycarbonate resin. The surface of the polyvinyl chloride resin in contact with the adhesive layer was subjected to corona discharge treatment to give a surface wetting index of 50 mN / m. The test specimen of the article of Example 14 was evaluated using the same method as in Example 1. The results are shown in Table 3.

[0117] Example 15 A specimen of an article having a layer structure of fluororesin layer / adhesive layer / methacrylic resin was obtained using the same method as in Example 11, except that the substrate was changed to a 2 mm methacrylic (PMMA) resin (product name "Acrylite (registered trademark) L#001", manufactured by Mitsubishi Chemical Corporation) instead of a polycarbonate resin. The surface in contact with the methacrylic resin adhesive layer was subjected to a corona discharge treatment to give a surface wetting index of 40 mN / m. The specimen of the article of Example 15 was evaluated using the same method as in Example 1. The results are shown in Table 3.

[0118] Example 16 A specimen of an article having a layer structure of fluororesin layer / adhesive layer / glass was obtained using the same method as in Example 11, except that the substrate was changed to 3 mm glass (product name "FL3", manufactured by AGC) instead of polycarbonate resin. The specimen of the article of Example 16 was evaluated using the same method as in Example 1. The results are shown in Table 3.

[0119] Example 17 The adhesive film prepared in Example 2 was cut into a size of 15 cm x 8 cm. A 50 cm square PTFE glass cloth, a 40 cm square tempered glass, a 50 cm square PTFE glass cloth, the adhesive film prepared in Example 2, a 450 μm ethylene vinyl acetate (EVA) resin substrate (product name "F806" manufactured by Fostech), the atmospheric pressure plasma-treated fluororesin film prepared in Example 7, and a 50 cm square PTFE glass cloth were laminated in this order, and placed on the table of a vacuum laminator (manufactured by NPC Corporation, LM-50S) set to 145°C. When laminating the adhesive film to the substrate, the article was arranged so that it had the fluororesin, adhesive layer, and substrate in that order. The sample was then preheated in a vacuum state (vacuum degree 100 Pa) for 3 minutes, then pressurized at 100 Pa for 15 minutes, and returned to atmospheric pressure. After confirming that the sample temperature had returned to room temperature, the sample was removed to obtain a test specimen of an article having a layer structure of fluororesin layer / adhesive layer / EVA resin / fluororesin film (atmospheric pressure plasma treatment). The test specimen of the article of Example 17 was evaluated in the same manner as in Example 1. For the evaluation of adhesive strength, the interface between the fluororesin layer / adhesive layer and the EVA resin was measured. The results are shown in Table 3.

[0120]

[0121]

[0122] The adhesive films of Examples 1 to 5, 11, and 13 to 17 maintained sufficient adhesion to various substrates even after a 500-hour accelerated weathering test. In particular, articles using the adhesive films of Examples 1 to 5 and CFRP as a substrate maintained excellent adhesion even after a 500-hour accelerated weathering test. Furthermore, an adhesive film containing zinc oxide as a pigment in addition to titanium oxide, as in Example 5, also exhibited particularly excellent adhesion after a 500-hour accelerated weathering test. On the other hand, adhesive films in which the pigment content in the fluororesin was less than 1% by mass, as in Examples 6 to 8, had an initial adhesion strength of 3 N / cm or more with the substrate, but after a 500-hour accelerated weathering test, the adhesion strength with the substrate fell to less than 3 N / cm, failing to maintain sufficient adhesion. Furthermore, fluororesin films not having an adhesive layer according to the present disclosure, as in Examples 7 to 10, had an initial adhesion strength of 3 N / cm or more with the substrate, but after a 500-hour accelerated weathering test, the adhesion strength with the substrate fell to less than 3 N / cm, failing to maintain sufficient adhesion. As in Example 12, depending on the type of substrate, it was found that the initial adhesive strength was also poor in the case of a fluororesin film of the present disclosure that did not have an adhesive layer.

[0123] Further, the results of evaluation of hydrophilicity retention for Examples 1 to 5 are shown in Table 4.

[0124]

[0125] In Examples 2 to 5, the hydrophilicity was maintained even after the hydrophilicity retention test, and excellent weather resistance was demonstrated even in an actual outdoor environment exposed to rain. On the other hand, in Example 1, it was difficult to maintain the hydrophilicity for 10 days or more after the hydrophilicity retention test.

[0126] The disclosure of Japanese Patent Application No. 2023-068089 is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards in this disclosure are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

[0127] The adhesive film of the present disclosure is suitable for use as a protective film for substrates used outdoors, and from the viewpoint of design, is also suitable for use as a colored protective film for interior use.

Claims

1. An adhesive film having a fluororesin layer containing a fluororesin and a pigment, and an adhesive layer on at least a portion of the fluororesin layer containing a silane coupling agent having a functional group, wherein the content of the pigment in the fluororesin layer is 1.0 mass% or more.

2. The adhesive film according to claim 1, wherein the pigment comprises at least one selected from the group consisting of titanium oxide and carbon black.

3. The adhesive film according to claim 1 or 2, wherein the pigment comprises titanium oxide and aluminum oxide.

4. An adhesive film according to claim 1 or 2, wherein the functional group of the silane coupling agent includes at least one selected from the group consisting of an amino group, an epoxy group, and an acrylic group.

5. The amount of functional groups in the silane coupling agent contained in the adhesive layer is 0.01 mmol / m 2 The adhesive film according to claim 1 or 2.

6. The adhesive film according to claim 1 or 2, wherein the fluororesin comprises an ethylene-tetrafluoroethylene copolymer.

7. The adhesive film according to claim 1 or 2, wherein the fluororesin layer satisfies the following relational formula (1): 100<content of the pigment in the fluororesin layer (mass%)×average thickness of the fluororesin layer (μm)<2100.

8. An adhesive film according to claim 1 or 2, wherein the transmittance of the adhesive film at a wavelength of 360 nm is 1.0% or less.

9. The adhesive film according to claim 1 or 2, wherein the average thickness of the adhesive layer is 0.5 μm or less.

10. The amount of functional groups of the silane coupling agent contained in the adhesive layer is 0.01 to 1.0 mmol / m 2 The adhesive film according to claim 1 or 2, 11. The adhesive film according to claim 1 or 2, which is a protective film for outdoor use.

12. An article comprising the adhesive film according to claim 1 or 2 and a substrate, the article comprising the fluororesin layer, the adhesive layer and the substrate in this order.

13. The article according to claim 12, wherein the substrate comprises at least one selected from the group consisting of glass, polycarbonate, polyvinyl chloride, epoxy resin, acrylic resin, ethylene-vinyl acetate copolymer resin, modified polyethylene, and fiber-containing resin.

14. The article of claim 12, wherein the adhesive film is a protective film.

15. The article of claim 12, which is for outdoor use.

Citation Information

Patent Citations

  • Surface-treating method of fluorine based member and method for bonding fluorine based member

    JP1992145139A

  • Production of composite material and obtained composite material

    JP2001079948A

  • Back sheet for solar cell

    JP2008282873A

  • Bonded body and method for producing the same

    JP2018168218A

  • Light-scattering fluororesin film for agricultural applications, and method for producing same

    WO2010047338A1