Method for manufacturing high-strength carbon fiber wet nonwoven fabric through recycling

The method enhances carbon fiber wet nonwoven fabric production by using a dispersant with acrylic acid and acrylamide-based monomers, applying filtrate for secondary drying, and reusing it, addressing strength and cost challenges in existing processes.

WO2024219708A1PCT designated stage expired Publication Date: 2024-10-24HANSOL CHEM
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/004170
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-04-01
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing methods for manufacturing carbon fiber wet nonwoven fabrics face challenges in achieving high tensile strength, surface bonding force, and dispersibility due to the use of binder fibers like polyvinyl alcohol and polymers, which impede fiber dispersion and increase manufacturing costs.

Method used

A method involving the preparation of a prewetting solution with carbon fibers and a binder fiber, addition of a dispersant containing acrylic acid-based and acrylamide-based monomer units, filtration, primary drying, and secondary drying with the application of filtrate to enhance dispersibility and tensile strength, while reusing the filtrate to reduce costs.

Benefits of technology

The method significantly improves the dispersibility, tensile strength, and surface bonding force of carbon fiber wet nonwoven fabrics, allowing for cost-effective production by reusing the filtrate and reducing the front/back strength difference and porosity issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024004170_24102024_PF_FP_ABST
    Figure KR2024004170_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a high-strength carbon fiber wet nonwoven fabric through recycling. More specifically, the present invention relates to a method for manufacturing a carbon fiber wet nonwoven fabric, the method comprising a step for coating the top of a carbon fiber wet nonwoven fabric by spraying same with a filtrate produced by filtering a carbon fiber dispersion solution, thus making it possible to manufacture a carbon fiber nonwoven fabric having significantly improved drying efficiency, dispersibility, tensile strength, and surface bonding strength, and as the filtrate can be reused, process costs can be drastically reduced compared to existing processes.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing high-strength carbon fiber wet-laid nonwoven fabric through recycling

[0001] The present invention relates to a method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric through recycling. More specifically, the present invention relates to a method for manufacturing a carbon fiber wet-laid nonwoven fabric, which comprises a step of filtering a carbon fiber dispersion during the manufacturing of the carbon fiber wet-laid nonwoven fabric and spraying the resulting filtrate onto the top of the carbon fiber wet-laid nonwoven fabric, thereby manufacturing a carbon fiber nonwoven fabric with significantly improved drying efficiency, dispersibility, tensile strength, and surface bonding strength, and wherein the filtrate can be reused, thereby drastically reducing process costs compared to existing processes.

[0002]

[0003] Carbon fiber possesses excellent physical properties, including a specific strength-to-weight ratio six times that of steel and a specific modulus three times that of steel. It also possesses exceptional thermal, heat-resistant, and electrical conductivity. Carbon fiber wet-laid nonwoven fabrics, made based on these properties, possess heat resistance, lightness, electrical, and thermal conductivity, and are used in carbon fiber-reinforced composites (CFRP), planar heaters, fuel cells, and redox flow batteries.

[0004]

[0005] The properties of carbon fiber wet-laid nonwovens are affected by factors such as fiber length, the degree of carbon fiber dispersion, and the type and content of the binder fiber used. Conventional binder fibers, such as polyvinyl alcohol (PVA), low-melting-point polyester (LM-PET), and polyethylene (PE), used in carbon fiber wet-laid nonwovens, suffer from differences in strength between the front and back of the fabric when producing high-bay-weight wet-laid nonwovens. Furthermore, the use of polymers such as cellulose and latex can impede carbon fiber dispersion, reducing strength and other properties. Furthermore, the need for large quantities of these polymers can clog the pores of the nonwoven fabric, reducing electrical conductivity and other properties. Furthermore, these polymers can prevent the resin used in composite material production from penetrating the pores, limiting the applications of carbon fiber wet-laid nonwovens. Therefore, technological improvements are needed to improve the dispersibility, tensile strength, and surface bonding of carbon fiber wet-laid nonwovens, including the development of dispersants, manufacturing methods, and cost reduction.

[0006]

[0007] Meanwhile, the applicant disclosed in Korean Patent Application No. 10-2022-0081800 (July 4, 2022) a copolymer solution containing an acrylic acid series monomer unit and an acrylamide series monomer unit as a carbon fiber dispersion solution that effectively disperses carbon fibers in an aqueous system.

[0008]

[0009] As a result of the present inventors' diligent efforts to solve the problems of the above-mentioned prior art, i) when the dispersant disclosed in Patent Application No. 10-2022-0081800 is used as a carbon fiber dispersant, the dispersion stability of carbon fibers increases, thereby exhibiting significantly improved drying efficiency and tensile strength, ii) by adding a step of filtering the carbon fiber dispersion, applying the resulting filtrate to the top of a carbon fiber wet nonwoven fabric, and secondary drying, not only can the tensile strength and surface bonding force of the carbon fiber wet nonwoven fabric be significantly increased, but also iii) by spraying the carbon fiber dispersion onto the carbon fiber wet nonwoven fabric, the problems of the prior art, such as the difference in strength between the front and back sides when manufacturing a high basis weight wet nonwoven fabric and the reduction in porosity of the wet nonwoven fabric due to excessive use, can be improved, and thus the present invention has been completed.

[0010] The inventors of the present invention also confirmed that even when the remaining filtrate is supplied and reused during the manufacture of a carbon fiber dispersion after applying the filtrate to a carbon fiber wet nonwoven fabric, the properties of the carbon fiber wet nonwoven fabric are not affected, and thus the recycled liquid can be used without a separate additive. In addition, the filtrate can be recaptured and used in the dispersion process after concentration correction, so that the process cost can be drastically reduced compared to the existing process.

[0011]

[0012] However, the problems that the present invention seeks to solve are not limited to the problems mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the description below.

[0013]

[0014] According to the first embodiment, the present invention

[0015] (1) A step of preparing a prewetting solution by mixing carbon fiber, binder fiber, and wetting agent in a dispersion medium;

[0016] (2) A step of preparing a carbon fiber dispersion by adding a dispersant to the above prewetting solution;

[0017] (3) A step of filtering the carbon fiber dispersion and drying the filtered carbon fiber to form a carbon fiber wet nonwoven fabric; and

[0018] (4) A method for manufacturing a high-strength carbon fiber wet nonwoven fabric is disclosed, including a step of filtering the carbon fiber dispersion solution, applying the resulting filtrate to the top of a carbon fiber wet nonwoven fabric, and secondary drying to manufacture a high-strength carbon fiber wet nonwoven fabric.

[0019] In the present invention, the method may further include a step (5) of applying the filtrate to the upper part of a carbon fiber wet nonwoven fabric and then supplying the remaining filtrate to the step (2) for reuse.

[0020] In the present invention, the carbon fiber may include fibers using as precursors infusible polyacrylonitrile (PAN)-based fibers (PAN-based flame-resistant fibers), infusible pitch-based fibers, infusible lignin-based fibers, infusible polyacetylene-based fibers, infusible polyethylene-based fibers, polybenzoxazole-based fibers, etc., carbon fiber waste, or mixtures thereof.

[0021] In the present invention, the binder fiber may include polyvinyl alcohol, polyvinyl chloride, acrylic, ethylene vinyl acetate, polyester, polyurethane, latex, or a mixture thereof.

[0022] In the present invention, the surfactant may include an EO (ethylene oxide) / PO (propylene oxide) copolymer surfactant, a PEO (polyethylene oxide) surfactant, a PEG (polyethylene glycol) surfactant, or a mixture thereof.

[0023] In the present invention, the weight ratio of carbon fiber: binder fiber: wetting agent may be 1:0.01-0.5:0.01-0.5.

[0024] In the present invention, the dispersant is a copolymer including an acrylic acid series monomer unit and an acrylamide series monomer unit, and the mol% ratio of the acrylic acid series monomer unit and the acrylamide series monomer unit based on 100 mol% of the total content of the copolymer may be 10:90 to 90:10.

[0025] In the present invention, the monomer polymerized with the acrylic acid series monomer unit may include acrylic acid, methacrylic acid, itaconic acid, 2-acrylamido-2-methylpropane sulfonic acid, maleic acid, or a mixture thereof, and the monomer polymerized with the acrylamide series monomer unit of the copolymer may include acrylamide, methacrylamide, or a mixture thereof.

[0026] In the present invention, the weight ratio of the carbon fiber and the dispersant may be 1:1-50.

[0027] In the present invention, the filtration may use a filter of 20 mesh to 200 mesh.

[0028] In the present invention, the primary drying can be performed in an oven at 80°C to 150°C for 1 to 30 minutes.

[0029] In the present invention, the application may include spray application.

[0030] In the present invention, the secondary drying can be performed in an oven at 80°C to 150°C for 1 to 30 minutes.

[0031]

[0032] According to the second embodiment, the present invention

[0033] A high-strength carbon fiber wet-laid nonwoven fabric having a dispersibility of 300 or less and a tensile strength of 20 kgf / ㎠ or more, manufactured by the above method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric, is disclosed.

[0034] In the present invention, the high-strength carbon fiber wet nonwoven fabric can have a dispersibility of 200 to 250 and a tensile strength of 110 to 200 kgf / ㎠.

[0035]

[0036] According to the method for manufacturing a high-strength carbon fiber wet nonwoven fabric of the present invention, a method for manufacturing a high-strength carbon fiber wet nonwoven fabric with significantly improved drying efficiency, dispersibility, tensile strength, and surface bonding strength can be provided by including a step of filtering a carbon fiber dispersion solution and spraying the resulting filtrate onto the top of the carbon fiber wet nonwoven fabric.

[0037] In addition, according to the method for manufacturing a high-strength carbon fiber wet nonwoven fabric of the present invention, the remaining filtrate after applying the filtrate to the carbon fiber wet nonwoven fabric can be reused, so that the process cost can be drastically reduced compared to the existing process.

[0038]

[0039] Meanwhile, the scope of the present invention is not limited by the effects described above.

[0040]

[0041] Figure 1 shows an exemplary schematic diagram of a method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention.

[0042] Figure 2 is a photograph showing the dispersibility of carbon fibers in carbon paper according to the measurement values ​​measured by the 2D lab formation sensor equipment.

[0043] Figure 3 is a photograph showing the degree of damage to the surface of a carbon fiber wet nonwoven fabric classified as high, medium, and low after generating friction on the surface (top surface during manufacturing) of the carbon fiber wet nonwoven fabric by operating the friction fastness test equipment (QM680, QMESYS) 10 times.

[0044]

[0045] Hereinafter, a method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric through recycling according to a specific embodiment of the invention will be described in detail. However, this is presented as one example of the invention, and the scope of the invention is not limited thereby. It will be apparent to those skilled in the art that various modifications to the embodiment are possible within the scope of the invention. Unless otherwise specified, throughout this specification, "include" or "comprising" refers to including a certain component (or component) without any particular limitation, and cannot be interpreted as excluding the addition of other components (or components).

[0046]

[0047] 1. Manufacturing method of high-strength carbon fiber wet-laid nonwoven fabric

[0048] The present invention provides a method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric, the method comprising:

[0049] (1) A step of preparing a prewetting solution by mixing carbon fiber, binder fiber, and wetting agent in a dispersion medium;

[0050] (2) A step of preparing a carbon fiber dispersion by adding a dispersant to the above prewetting solution;

[0051] (3) A step of filtering the carbon fiber dispersion and drying the filtered carbon fiber to form a carbon fiber wet nonwoven fabric; and

[0052] (4) It includes a step of filtering the carbon fiber dispersion solution, applying the resulting filtrate to the top of a carbon fiber wet nonwoven fabric, and secondary drying to manufacture a high-strength carbon fiber wet nonwoven fabric.

[0053] In addition, the method for manufacturing a high-strength carbon fiber wet nonwoven fabric according to the present invention may further include a step (5) of applying the filtrate to the upper part of the carbon fiber wet nonwoven fabric and then supplying the remaining filtrate to the step (2) for reuse.

[0054] An exemplary schematic diagram of a method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention is shown in Fig. 1.

[0055]

[0056] (1) Prewetting solution preparation step

[0057] The present invention comprises, in a first step, a step of preparing a prewetting solution by mixing carbon fibers, binder fibers, and a wetting agent with a dispersion medium. The first step involves introducing the carbon fibers, binder fibers, and wetting agent into the dispersion medium and stirring the mixture to introduce hydrophilic groups capable of forming hydrogen bonds with water onto the hydrophobic surface of the carbon fibers, thereby enabling water dispersion.

[0058] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the carbon fiber may include carbon fibers and carbon fiber wastes or mixtures thereof, which are precursors of, but are not limited to, infusible polyacrylonitrile (PAN)-based fibers (PAN-based flame-resistant fibers), infusible pitch-based fibers, cellulose-based fibers, infusible lignin-based fibers, infusible polyacetylene-based fibers, infusible polyethylene-based fibers, polybenzoxazole-based fibers, etc.

[0059] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the average length of the carbon fibers may be 5 mm or more, for example, 6 mm or more, 10 mm or more, 12 mm or more, 15 mm or more, or 20 mm or more.

[0060] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the binder fiber may include, but is not limited to, polyvinyl alcohol, polyvinyl chloride, acrylic, ethylene vinyl acetate, polyester, polyurethane, latex, or a mixture thereof.

[0061] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the weight ratio of the carbon fiber and the binder fiber may be 1:0.01-0.5, for example, 1:0.1.

[0062] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the prewetting solution may further include a surfactant as a wetting agent. The surfactant may include a cationic surfactant, an anionic surfactant, a nonionic surfactant, or a mixture thereof. For example, the surfactant may include, but is not limited to, an EO (ethylene oxide) / PO (propylene oxide) copolymer surfactant, a PEO (polyethylene oxide)-based surfactant, a PEG (polyethylene glycol)-based surfactant, or a mixture thereof.

[0063] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the weight ratio of the carbon fiber and the wetting agent may be 1:0.5-2, for example, 1:1.

[0064] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the weight ratio of carbon fiber: binder fiber: wetting agent may be 1:0.01-0.5:0.01-0.5, for example, 1:0.1:.

[0065] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the dispersion medium may include water, but is not limited thereto.

[0066] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the step of preparing a prewetting solution by mixing the carbon fiber, binder fiber, and dispersion medium can be performed by stirring, and the stirring can be performed at 500 rpm to 3,000 rpm, for example, 1,000 rpm, for 1 minute to 30 minutes, for example, 5 minutes.

[0067]

[0068] (2) Carbon fiber dispersion manufacturing step

[0069] The present invention may include a second step of preparing a carbon fiber dispersion by adding a dispersant to the prewetting solution. The second step may induce dispersion of carbon fibers by electrostatic repulsion by adding and mixing the dispersant to the prewetting solution, while simultaneously preventing re-agglomeration of the carbon fibers by utilizing steric hindrance.

[0070] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the dispersant may be a copolymer or copolymer solution described in Korean Patent Application No. 10-2022-0081800, which may include an acrylic acid-based monomer unit and an acrylamide-based monomer unit. In the case of conventionally used cellulose-based polymers including CMC, they may decompose over time, making recycling difficult. On the other hand, the copolymer including an acrylic acid-based monomer unit and an acrylamide-based monomer unit according to the present invention has a low possibility of decomposition, and thus has the advantage of being recyclable.

[0071] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the mol% ratio of the acrylic acid series monomer unit and the acrylamide series monomer unit (mol% of the acrylic acid series monomer unit: mol% of the acrylamide series monomer unit) based on 100 mol% of the total content of the copolymer of the dispersant may be 10:90 to 90:10. For example, the mol% ratio of the acrylic acid series monomer unit and the acrylamide series monomer unit may be 90:10, 80:20, 70:30, 60:40, 50:50, 40:60, 30:70, 20:80, 10:90, and 30:70 to 70:30. The monomer polymerized into the acrylic acid series monomer unit of the above copolymer may include acrylic acid, methacrylic acid, itaconic acid, 2-acrylamido-2-methylpropane sulfonic acid, maleic acid, or a mixture thereof, and the monomer polymerized into the acrylamide series monomer unit of the above copolymer may include acrylamide, methacrylamide, or a mixture thereof.

[0072] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the weight ratio of the carbon fiber and the dispersant may be 1:1-50, for example, 1:20.

[0073] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the step of adding a dispersant to the prewetting solution to prepare a carbon fiber dispersion may be performed by stirring, and the stirring may be performed at 100 rpm to 1,000 rpm, for example, 300 rpm, for 1 minute to 30 minutes, for example, 5 minutes.

[0074]

[0075] (3) Filtration and primary drying stage

[0076] The present invention may include a third step of filtering the carbon fiber dispersion and drying the filtered carbon fibers to form a carbon fiber wet nonwoven fabric. The present invention can improve the drying efficiency of the carbon fiber wet nonwoven fabric by using the dispersant described in Republic of Korea Patent Application No. 10-2022-0081800.

[0077] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the filtration may use a filter of 20 mesh to 200 mesh.

[0078] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the primary drying can be performed in an oven at 80°C to 150°C for 1 to 30 minutes.

[0079]

[0080] (4) Application of filtrate and secondary drying step

[0081] The present invention may include, as a fourth step, a step of filtering the carbon fiber dispersion, applying the resulting filtrate to the top of a carbon fiber wet nonwoven fabric, and secondary drying to produce a high-strength carbon fiber wet nonwoven fabric. The present invention has the advantage of being able to collect and apply the filtrate without a separate storage tank, and the filtrate remaining after spraying can be collected in a subsequent step and reused in the dispersion process through concentration correction.

[0082] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the application may include spray application. The present invention adopts a spray-type application method, thereby improving the problems such as the difference in strength between the front and back sides in the production of conventional high-basis-weight wet-laid nonwoven fabrics and the reduction in porosity of the wet-laid nonwoven fabric due to excessive use.

[0083] In the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the primary drying can be performed in an oven at 80°C to 150°C for 1 to 30 minutes.

[0084]

[0085] (5) Filtrate reuse stage

[0086] The present invention may include, as a fifth step, a step of applying the filtrate to a carbon fiber wet nonwoven fabric in the filtrate application step, and then reusing the remaining filtrate by supplying the filtrate to (2) the carbon fiber dispersion production step. Since the present invention can be used by supplying the filtrate as a dispersant to the carbon fiber dispersion production step, the process cost due to the use of the dispersant can be reduced.

[0087]

[0088] 2. High-strength carbon fiber wet nonwoven fabric

[0089] The present invention aims to provide a high-strength carbon fiber wet-laid nonwoven fabric manufactured by the above method.

[0090] In the high-strength carbon fiber wet nonwoven fabric according to the present invention, the carbon fiber wet nonwoven fabric is manufactured with a basis weight of 16 g / ㎡ and a thickness of 120 to 150 ㎛, and the dispersibility (uniformity) measured using a 2D rapometry sensor device may be 300 or less, for example, 200 to 250.

[0091] In the high-strength carbon fiber wet-laid nonwoven fabric according to the present invention, the tensile strength of the carbon fiber wet-laid nonwoven fabric may be 20 kgf / ㎠ or more, preferably 100 kgf / ㎠ or more, for example, 110 to 200 kgf / ㎠.

[0092]

[0093] Below, various examples are presented to aid understanding of the invention. These examples are provided solely to facilitate understanding of the invention and are not intended to limit the scope of protection of the invention.

[0094]

[0095] <Manufacturing Example>

[0096] Manufacturing Example 1. Manufacturing of dispersant

[0097] Acrylic acid monomer (AA), acrylamide monomer (AM), and water were placed in a three-necked flask reactor, and after attaching a thermometer, the temperature was increased to 70°C under nitrogen purging. The weight ratio of acrylic acid monomer (AA), acrylamide monomer (AM), and water (weight of acrylic acid monomer (AA) + acrylamide monomer (AM): weight of water) was 2:8. Next, ammonium persulfate (APS) was dissolved in water and added dropwise over 30 minutes (0.1 part by weight of APS was used per 100 parts by weight of the total content of acrylic acid monomer (AA), acrylamide monomer (AM), and water). After completion of the addition, the mixture was maintained at 70°C for 7 hours, cooled, and then adjusted to pH 70 with NaOH to produce a polymer having a solid content of 25% and a weight average molecular weight of 100,000 g / mol.

[0098] The mol% ratio of acrylic acid monomer (AA) and acrylamide monomer (AM) based on the total content of 100 mol% of the above polymer (mol% of acrylic acid monomer (AA): mol% of acrylamide monomer (AM)) is 70:30 (CDS-2500P, Hansol).

[0099]

[0100] <Example>

[0101] A high-strength carbon fiber wet nonwoven fabric was manufactured according to the amount of dispersant and carbon fiber wet nonwoven fabric shown in Table 1 below.

[0102] No. Dispersion system amount Example 1 CDS-2500P (hansol.co.ltd) 10g Example 220g Example 3 Filtrate of Example 1 10g Comparative Example 1 CDS-2500P 0g Comparative Example 2 CMC 1% 0g Comparative Example 3 CMC 1% 10g Comparative Example 4 Filtrate of Comparative Example 2 0g Comparative Example 5 Filtrate of Comparative Example 3 10g

[0103] Example 1. Preparation of carbon fiber wet-laid nonwoven fabric

[0104] (1) Prewetting solution preparation step: 3.75 g of 12 mm carbon fiber (Zolteck), 0.375 g of polyvinyl alcohol (PVA) fiber (VPB-101, Kurary), and 3.75 g of a nonionic surfactant series wetting agent (HPW-500, Hansol) were mixed in a solvent (water, 492.125 g), and then a pulper was applied to prepare a prewetting solution that went through a prewetting step at approximately 1000 rpm.

[0105] (2) Carbon fiber dispersion preparation step: About 500 g of the above prewetting solution was added to a solvent (water, about 1.925 g) in which 75 g of a dispersant (CDS-2500P, Hansol) was dissolved, and the mixture was stirred at a low speed of about 350 rpm using an impeller that generates less vortex formation, thereby preparing a carbon fiber dispersion.

[0106] (3) Filtration and primary drying step: The carbon fiber dispersion was filtered through a 100 mesh filter to filter out carbon fibers, and primary drying was performed at 120°C for 10 min using a 25x25㎠ laboratory handsheet machine to form a carbon fiber wet nonwoven fabric having a basis weight of 60 g / ㎡ and a thickness of about 480 to 520 ㎛ after drying.

[0107] (4) Application of filtrate and secondary drying step: 10 g of the filtrate produced by filtering the carbon fiber dispersion was sprayed onto the top of the first-dried carbon fiber wet nonwoven fabric, and secondary drying was performed at 120°C for 10 min.

[0108]

[0109] Example 2. Preparation of carbon fiber wet-laid nonwoven fabric

[0110] A carbon fiber wet-laid nonwoven fabric was manufactured using the same method as in Example 1, except that 20 g of the filtrate was applied instead of 10 g.

[0111]

[0112] Example 3. Preparation of carbon fiber wet-laid nonwoven fabric

[0113] A carbon fiber wet-laid nonwoven fabric was manufactured using the same method as in Example 1, except that the filtrate produced in Example 1 was used instead of CDS-2500 as a dispersing agent.

[0114]

[0115] Comparative Example 1. Manufacturing of Carbon Fiber Wet-Laid Nonwoven Fabric

[0116] A carbon fiber wet-laid nonwoven fabric was manufactured using the same method as in Example 1, except that step (4) was omitted.

[0117]

[0118] Comparative Example 2. Manufacturing of Carbon Fiber Wet-Laid Nonwoven Fabric

[0119] A carbon fiber wet-laid nonwoven fabric was manufactured using the same method as in Comparative Example 1, except that 1% CMC was used instead of CDS-2500 as a dispersant.

[0120]

[0121] Comparative Example 3. Manufacturing of Carbon Fiber Wet-Laid Nonwoven Fabric

[0122] A carbon fiber wet-laid nonwoven fabric was manufactured using the same method as Example 1, except that 1% of CMC was used instead of CDS-2500 as the dispersant.

[0123]

[0124] Comparative Example 4. Manufacturing of Carbon Fiber Wet-Laid Nonwoven Fabric

[0125] A carbon fiber wet-laid nonwoven fabric was manufactured using the same method as in Comparative Example 1, except that a filtrate was used instead of CDS-2500 as a dispersant.

[0126]

[0127] Comparative Example 5. Manufacturing of Carbon Fiber Wet-Laid Nonwoven Fabric

[0128] A carbon fiber wet-laid nonwoven fabric was manufactured using the same method as in Comparative Example 2, except that a filtrate was used instead of 1% CMC as a dispersant.

[0129]

[0130] <Experimental Example>

[0131] Experimental Example 1. Characteristic Evaluation of Carbon Fiber Wet-Laid Nonwoven Fabric

[0132] The solid content of the dispersion liquid, the solid content of the filtrate, the dryness during the first drying, and the dispersibility, tensile strength, and surface bonding strength of the carbon fiber wet nonwoven fabric manufactured in the above examples and comparative examples were evaluated by the following methods, and the results are shown in Table 2.

[0133] (1) Solid content of dispersion

[0134] In the above example, 10 g of a dispersion was prepared without adding fibers, and the solid content was measured after hot air drying at 105°C for 2 hours.

[0135] (2) Solid content of filtrate

[0136] The carbon fiber dispersion was filtered, 10 g of the resulting filtrate was collected, and the solid content was measured after drying with hot air at 105°C for 2 hours.

[0137] (3) Whether it is dry during the first drying

[0138] Drying was evaluated by drying at 120°C for 10 min, and subsequent evaluations (dispersibility, tensile strength, and surface bonding strength) were performed after complete drying through additional heat treatment.

[0139] (4) Dispersibility

[0140] The dispersibility (uniformity) of the carbon fiber wet nonwoven fabric was measured using the 2d lab formation sensor equipment of Techpap SAS (France). The dispersibility of the carbon fiber wet nonwoven fabric can be evaluated through the number and distribution of flocs measured by the 2d lab formation sensor equipment, and it can be evaluated that the lower the measurement value, the better the dispersibility (Figure 2).

[0141] (5) Tensile strength

[0142] The tensile strength of the carbon fiber wet nonwoven fabric was measured using the AGS-X 10N-10KN equipment of Shimadzu at a speed of 2 m / min.

[0143] (6) Surface bonding strength

[0144] The surface bonding strength was classified as upper, middle, and lower according to the degree of peeling of the surface of the wet nonwoven fabric after driving the equipment 10 times with the top surface of the wet nonwoven fabric as the surface when manufacturing the wet nonwoven fabric. It can be evaluated that the closer it is to the upper, the better the surface bonding strength (Figure 3).

[0145]

[0146] Experimental Example 2. Results

[0147] No.Solid content of dispersion liquidSolid content of filtrateDrying during first dryingDryingDispersibilityTensile strengthSurface bonding strengthExample 10.750.75O236.12116.63UpperExample 20.750.75O234.53149.67UpperExample 30.750.75O224.36118.01UpperComparative Example 10.750.75O238.6897.19LowerComparative Example 20.750.61X420.6755.46LowerComparative Example 30.750.62X415.3694.23UpperComparative Example 40.610.28X532.4215.56LowerComparative Example 50.620.27X523.1231.35Upper

[0148] (1) Evaluation of the possibility of reusing the filtrate based on the comparison of the solid content in the filtrate When using 1% CMC (Comparative Examples 2 and 3) as a dispersing agent, the solid content in the filtrate was found to be somewhat reduced compared to the solid content in the dispersion, and in particular, in Comparative Examples 4 and 5 using the filtrate of Comparative Examples 2 and 3, the solid content in the filtrate was found to be significantly reduced compared to the solid content in the dispersion, and therefore, the filtrate of 1% CMC was found to be unreusable.

[0149] On the other hand, when CDS-2500P (Examples 1 and 2) and its filtrate (Example 3) were used as a dispersant, it was confirmed that the filtrate of CDS-2500P could be reused as the solid content in the dispersion and the solid content in the filtrate were the same.

[0150]

[0151] (2) Evaluation of the properties of carbon fiber wet nonwoven fabrics by adding a filtrate application step

[0152] The tensile strength (94.23 kgf / cm2) and surface bonding force (top) of Comparative Example 3, which included a filtrate application step using 1% CMC as a dispersant, were found to have increased compared to the tensile strength (55.46 kgf / cm2) and surface bonding force (bottom) of Comparative Example 2, which did not include a filtrate application step.

[0153] Meanwhile, the tensile strength (116.63 kgf / cm2) and surface bonding force (top) of Example 1 including the filtrate application step using CDS-2500P as a dispersant were found to be significantly improved compared to the tensile strength (97.19 kgf / cm2) and surface bonding force (bottom) of Comparative Example 1 not including the filtrate application step.

[0154] Therefore, it was confirmed that when a step of applying a filtrate is added during the manufacture of a carbon fiber wet nonwoven fabric according to the present invention, the tensile strength and surface bonding strength of the carbon fiber wet nonwoven fabric can be improved.

[0155]

[0156] (3) Evaluation of the properties of carbon fiber wet-laid nonwoven fabric using CDS-2500P as a dispersant

[0157] The drying efficiency (O), dispersibility (238.68), and tensile strength (97.19 kgf / cm2) of Comparative Example 1 using CDS-2500P as a dispersant were found to be higher than the drying efficiency (X), dispersibility (420.67), and tensile strength (55.46 kgf / cm2) of Comparative Example 2 using 1% CMC as a dispersant.

[0158] In particular, the drying efficiency (O), dispersibility (236.12), and tensile strength (116.63 kgf / cm2) of Example 1, which includes a filtrate application step using CDS-2500P as a dispersant, were shown to be significantly improved compared to the drying efficiency (X), dispersibility (415.36), and tensile strength (94.23 kgf / cm2) of Comparative Example 3, which uses 1% CMC as a dispersant.

[0159] Therefore, it was confirmed that when CDS-2500P is used as a dispersant in the production of a carbon fiber wet-laid nonwoven fabric according to the present invention, the drying efficiency, dispersibility, and tensile strength of the carbon fiber wet-laid nonwoven fabric can be improved.

[0160]

[0161] (4) Evaluation of the properties of carbon fiber wet-laid nonwoven fabrics according to filtrate reuse

[0162] The dispersibility (532.42), tensile strength (11.56 kgf / cm2) and surface bonding force (bottom) of Comparative Example 4, which reused the filtrate of Comparative Example 2, were significantly reduced in tensile strength compared to the dispersibility (420.67), tensile strength (55.46 kgf / cm2) and surface bonding force (bottom) of Comparative Example 2, and the dispersibility (523.12), tensile strength (31.36 kgf / cm2) and surface bonding force (top) of Comparative Example 5, which reused the filtrate of Comparative Example 3 and included the filtrate application step, were significantly reduced in tensile strength compared to the dispersibility (523.12), tensile strength (94.23 kgf / cm2) and surface bonding force (top) of Comparative Example 3.

[0163] On the other hand, Example 3, which reused the filtrate of Example 1 and included a filtrate application step, showed dispersibility (224.36), tensile strength (118.01 kgf / cm2), and surface bonding strength (top) similar to those of Example 1 in terms of dispersibility (236.12), tensile strength (116.63 kgf / cm2), and surface bonding strength (top), confirming that reusing the filtrate did not affect the properties of the manufactured carbon fiber wet-laid nonwoven fabric.

[0164]

[0165] While specific aspects of the present invention have been described in detail above, it should be apparent to those skilled in the art that these specific descriptions are merely preferred implementation examples and are not intended to limit the scope of the present invention. Therefore, the substantial scope of the present invention is defined by the appended claims and their equivalents.

[0166]

[0167] The method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric of the present invention enables the development of a high-strength carbon fiber wet-laid nonwoven fabric with significantly improved drying efficiency, dispersibility, tensile strength, and surface bonding strength. Furthermore, the method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric of the present invention allows the residual filtrate after applying the filtrate to the carbon fiber wet-laid nonwoven fabric to be reused, thereby enabling a dramatic reduction in process costs compared to existing processes.

Claims

1. (1) A step of preparing a pre-wetting solution by mixing carbon fiber, binder fiber, and wetting agent in a dispersion medium; (2) A step of preparing a carbon fiber dispersion by adding a dispersant to the above prewetting solution; (3) A step of filtering the carbon fiber dispersion and drying the filtered carbon fiber to form a carbon fiber wet nonwoven fabric; and (4) A step of filtering the carbon fiber dispersion solution, applying the resulting filtrate to the top of a carbon fiber wet nonwoven fabric, and drying it a second time to manufacture a high-strength carbon fiber wet nonwoven fabric; A method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric, comprising:

2. In paragraph 1, A method for manufacturing a high-strength carbon fiber wet nonwoven fabric, characterized in that the method further includes a step of (5) applying the filtrate to the top of a carbon fiber wet nonwoven fabric and then supplying the remaining filtrate to the step (2) to reuse it.

3. In paragraph 1, A method for producing a high-strength carbon fiber wet-laid nonwoven fabric, characterized in that the carbon fiber comprises a fiber having as a precursor an infusible polyacrylonitrile (PAN)-based fiber (PAN-based flame-resistant fiber), an infusible pitch-based fiber, an infusible lignin-based fiber, an infusible polyacetylene-based fiber, an infusible polyethylene-based fiber, or a polybenzoxazole-based fiber, and carbon fiber waste, or a mixture thereof.

4. In paragraph 1, A method for producing a high-strength carbon fiber wet-laid nonwoven fabric, characterized in that the binder fiber comprises polyvinyl alcohol, polyvinyl chloride, acrylic, ethylene vinyl acetate, polyester, polyurethane, latex, or a mixture thereof.

5. In paragraph 1, A method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric, characterized in that the surfactant comprises an EO (ethylene oxide) / PO (propylene oxide) copolymer surfactant, a PEO (polyethylene oxide)-based surfactant, a PEG (polyethylene glycol)-based surfactant, or a mixture thereof.

6. In paragraph 1, A method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric, characterized in that the weight ratio of the carbon fiber: binder fiber: wetting agent is 1:0.01-0.5:0.01-0.

5.

7. In paragraph 1, The above dispersant is a copolymer containing an acrylic acid series monomer unit and an acrylamide series monomer unit, A method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric, characterized in that the mol% ratio of the acrylic acid series monomer unit and the acrylamide series monomer unit is 10:90 to 90:10 based on 100 mol% of the total content of the copolymer.

8. In paragraph 7, The monomer polymerized with the above acrylic acid series monomer unit includes acrylic acid, methacrylic acid, itaconic acid, 2-Acrylamido-2-methylpropane sulfonic acid, maleic acid or a mixture thereof. A method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric, characterized in that the monomer polymerized as an acrylamide series monomer unit of the above copolymer includes acrylamide, methacrylamide, or a mixture thereof.

9. In paragraph 1, A method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric, characterized in that the weight ratio of the carbon fiber and the dispersant is 1:1-50.

10. In paragraph 1, A method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric, characterized in that the above filtration uses a filter of 20 mesh to 200 mesh.

11. In paragraph 1, A method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric, characterized in that the above primary drying is performed in an oven at 80°C to 150°C for 1 to 30 minutes.

12. In paragraph 1, A method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric, characterized in that the above application includes spray application.

13. In paragraph 1, A method for manufacturing a high-strength carbon fiber wet-laid nonwoven fabric, characterized in that the above secondary drying is performed in an oven at 80°C to 150°C for 1 to 30 minutes.

14. A high-strength carbon fiber wet-laid nonwoven fabric manufactured by a method according to any one of claims 1 to 13, having a dispersibility of 300 or less and a tensile strength of 20 kgf / ㎠ or more.

15. In paragraph 14, A high-strength carbon fiber wet-laid nonwoven fabric characterized by having a dispersibility of 200 to 250 and a tensile strength of 110 to 200 kgf / ㎠.

Citation Information

Patent Citations

  • Sizing agent for carbon fiber

    JP2015074837A

  • Nonwoven fabric and resin molding comprising the nonwoven fabric

    JP2018131693A

  • Nonwoven fabric and method of manufacturing nonwoven fabric

    JP2019112727A

  • Carbon fiber dispersant composition, carbon fiber dispersant kit, carbon fiber dispersing composition, and carbon fiber sheet manufacturing method

    JP2019150773A

  • Carbon fiber nonwoven fabric and carbon fiber-reinforced resin composite

    JP2020165048A