A method for preparing products from recycled glass fines
The method of mixing glass fines with a cellulose binder and heating them forms recyclable glass products, addressing the underutilization of glass fines by creating valuable, entirely glass products that can be recycled again, improving efficiency and sustainability.
Patent Information
- Application Number
- PCT/AU2024/050384
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-31
AI Technical Summary
Glass fines, a by-product of the recycling process, are underutilized due to their small size, color mix, and contaminants, making them difficult to sort and use as feedstock for traditional glass production.
A method involving mixing glass fines with a cellulose-based binder solution, forming the mixture into a shape, and heating it to create glass products such as tiles or bricks, which can be entirely recyclable back into glass fines.
This method enables the production of valuable glass products from previously unusable fines, providing a circular material stream and eliminating the need for glazing, thus enhancing efficiency and environmental sustainability.
Smart Images

Figure IMGF000010_0001 
Figure IMGF000010_0002 
Figure 00000014_0000
Abstract
Description
A method for preparing products from recycled glass finesField of the disclosure
[0001] The present disclosure broadly relates to a method of producing products from glass fines.Background of the disclosure
[0002] Any discussion of the prior art throughout this specification should in no way be considered as an admission that such prior art is widely known or forms part of the common general knowledge in the field.
[0003] Glass packaging such as bottles and jars makes up approximately 80% of glass consumed in Australia. In 2019, the Institute of Sustainable Futures at the University of Technology Sydney conducted a life cycle assessment of packaging in Australia on behalf of the Australian Packaging Covenant Organisation. Their research finds that in the 2017-18 financial year, 1 .3 million tonnes of glass packaging was consumed in Australia. Although 78% of this number was collected to be recycled and 50% recovered, only 36% was ultimately recycled back into glass packaging. The 14% gap between the recovery and recycling rate ends up as glass fines.
[0004] Throughout the recovery process, glass packaging is broken down into small pieces called cullet. Cullet can be separated into colours and recycled back into glass. However, as the cullet passes through each recovery stage, it continues to degrade, mixing with small particles from other waste streams, until it forms glass fines - pieces smaller than 8 mm. Glass fines are difficult to sort and unable to serve as feedstock for traditional glass production due to their size, colour mix and range of contaminants, making them the lowest value product in the waste stream. They are ultimately a by-product of the recovery process whereby a perfectly recyclable material is systematically broken down into a vast and underutilised resource. It would be advantageous if glass fines could be used to form a valuable product.Summary of the disclosure
[0005] In a first aspect of the disclosure, there is provided a method of preparing a glass product, the method comprising:(i) preparing a mixture comprising glass fines and a binder solution, wherein the binder solution comprises cellulose;(ii) forming the mixture into a shape; and(iii) heating the shape to form the glass product.
[0006] The following options may be used in conjunction with the first aspect of the disclosure, either individually or in any suitable combination.
[0007] The binder solution may further comprise water. The binder solution may comprise between about 1 -10% w / w cellulose. The binder solution may comprise about 6% w / w cellulose.
[0008] The binder solution may comprise carboxymethyl cellulose (CMC), microfibrillated cellulose (MFC), or a combination thereof. The binder solution may comprise between about 1 -7% w / w CMC. The binder solution may comprise about 4.5% w / w CMC. The binder solution may comprise between about 1 -3% w / w MFC. The binder solution may comprise about 1 .3% w / w MFC.
[0009] The binder solution may comprise CMC and MFC. The binder solution may comprise between about 1 -7% w / w CMC and between about 1 -3% w / w MFC. The binder solution may comprise about 4.5% w / w CMC and about 1 .3% w / w MFC.
[0010] The binder solution may comprise between about 90-98% w / w water.
[0011] The binder solution may consist of, or consist essentially of, cellulose and water. The binder solution may consist of, or consist essentially of, CMC, MFC, and water.
[0012] The mixture may comprise between about 75-95% w / w glass fines and between about 5-25% w / w binder solution. The mixture may comprise about 85% w / w glass fines and about 15% w / w binder solution. The mixture may consist of, or consist essentially of, glass fines and binder solution.
[0013] In step (ii) the mixture may be formed into the shape by hand building, extrusion, compression moulding, or 3D printing.
[0014] The method of the first aspect of the disclosure may further comprise a step (ii.a.) following step (ii) and before step (iii), of drying the shape.
[0015] In step (iii) the mixture may be heated at a temperature of between about 500-900 °C. The mixture may be heated at a temperature of about 760 °C. The mixture may be heated for a duration of between about 4 hours and about 12 hours.
[0016] The glass product may be selected from a tile, a brick, a cladding, a toilet, a bowl, a basin, a decorative item, a bead, a pendant, a mechanical component, or a filter.
[0017] The glass product may consist of, or consist essentially of, glass.
[0018] In a second aspect of the disclosure, there is provided a glass product prepared by the method of the first aspect of the disclosure.Definitions
[0019] The following are some definitions that may be helpful in understanding the description of the present disclosure. These are intended as general definitions and should in no way limit the scope of the present disclosure to those terms alone, but are put forth for a better understanding of the following description.
[0020] Throughout this specification, unless the context requires otherwise, the word "comprise", or variations such as "comprises" or "comprising", will be understood to imply the inclusion of a stated element, integer or step, or group of elements, integers or steps, but not the exclusion of any other element, integer or step, or group of elements, integers or steps.
[0021] The terms "a" and "an" are used herein to refer to one or to more than one (i.e. to at least one) of the grammatical object of the article. By way of example, "an element" means one element or more than one element.
[0022] The term "about" is understood to refer to ±10% of the recited value.
[0023] Any numerical range recited herein is intended to include all sub-ranges of the same numerical precision subsumed within the recited range. For example, a range of 1 .0 to 5.0 is intended to include all sub-ranges between (and including) the recited minimum value of 1 .0 and the recited maximum value of 5.0, that is, having a minimum value equal to or greater than 1.0 and a maximum value equal to or less than 5.0, such as 2.1 to 4.5. Any maximum numerical limitation recited herein is intended to include all lower numerical limitations subsumed therein and any minimum numerical limitation recited herein is intended to include all higher numerical limitations subsumed therein.
[0024] The term "consists of" is intended to mean that no integers other than those stated are present. The term "consists essentially of" also allows for the presence of other integers, commonly minor, which are not intentionally contributed and which do not substantially affect the operation of the invention.
[0025] The term "may" should be taken to imply that the contrary proposition is also contemplated. Thus, for example, the statement "A may be B" should be taken to incorporate both statements "A is B" and "A is not B".
[0026] Any description of prior art documents herein, or statements herein derived from or based on those documents, is not an admission that the documents or derived statements are part of the common general knowledge of the relevant art.
[0027] For the purposes of description, all documents referred to herein are hereby incorporated by reference in their entirety unless otherwise statedBrief Description of the Drawings
[0028] Figure 1. A life cycle diagram of a tile manufactured according to the method of the first aspect of the disclosure.
[0029] Figure 2. A manufacturing process flow diagram according to an embodiment of the method of the first aspect of the disclosure.
[0030] Figure 3. Tiles prepared according to the method of the first aspect of the disclosure.
[0031] Figure 4. XRD spectrum of tile prepared according to the method of the first aspect of the disclosure (designated 'Moondust') compared with a conventional ceramic tile. Q = peak characteristic of quartz.
[0032] Figure 5. TGA analysis of a glass product prepared according to the method of the first aspect of the disclosure. The area marked by the dashed line is the dehydroxylation region.Detailed Description
[0033] The present inventors have surprisingly found that useful glass products such as bricks and tiles can be formed by firing a mixture of glass fines and a binder solution comprising cellulose. As the finished glass products consist entirely of glass, they have the additional advantage of being completely recyclable back to glass fines, from which a new glass product can be formed, providing a 'circular' material, as depicted in Figure 1 .
[0034] Thus in a first aspect of the disclosure, there is provided a method of preparing a glass product, the method comprising:(i) preparing a mixture comprising glass fines and a binder solution, wherein the binder solution comprises cellulose;(ii) forming the mixture into a shape; and(iii) heating the shape to form the glass product
[0035] In step (i) of the method of the first aspect of the disclosure, glass fines are mixed with a binder solution. Glass fines are small particles of glass that are recovered from the processing of glass waste. In general, glass fines may be less than 8 mm in size. The glass fines used in the method of the first aspect of the disclosure may have a size of less than about 300 pm, or less than about 250, 200, 150, 100, or less than about 50 pm. The glass fines may have a size of less than about 150 pm. In this context, the 'size' of the glass fines refers to the length of the longest axis of a glass particle.
[0036] The binder solution comprises cellulose. Cellulose acts as a binder, that is, binds the glass fines together, enabling them to be stably formed into a shape. The binder solution may comprise between about 1 % and about 10% w / w cellulose, or between about 1 -2, 1 -3, 1 -4, 1 - 5, 1 -6, 1 -7, 1 -8, 1 -9, 2-3, 2-4, 2-5, 2-6, 2-7, 2-8, 2-9, 2-10, 3-4, 3-5, 3-6, 3-7, 3-8, 3-9, 3-10, 4-5, 4-6, 4-7, 4-8, 4-9. 4-10, 5-6, 5-7, 5-8, 5-9, 5-10, 6-7, 6-8, 6-9, 6-10, 7-8, 7-9, 7-10, 8-9, 8- 10, or between about 9% and about 10% w / w cellulose. The binder solution may comprise between about 2% and about 7% w / w cellulose. The binder solution may comprise between about 3% and about 8% w / w cellulose. The binder solution may comprise between about 5% and about 10% w / w cellulose. The binder solution may comprise about 1 % w / w cellulose, or about 2, 3, 4, 5, 6, 7, 8, 9, or about 10% w / w cellulose. The binder solution may comprise about 6% w / w cellulose.
[0037] The cellulose may be at least in part in the form of carboxymethyl cellulose (CMC), microfibrillated cellulose (MFC), or a combination thereof. In the context of this disclosure, the term "cellulose" should be taken to encompass both CMC and MFC as well as other forms of cellulose. The binder solution may comprise between about 1% and about 7% w / w CMC, or between about 1 -2, 1 -3, 1 -4, 1 -5, 1 -6, 2-3, 2-4, 2-5, 2-6, 2-7, 3-4, 3-5, 3-6, 3-7, 4-5, 4-6, 4-7, 5-6, 5-7, or between about 6% and about 7% w / w CMC. The binder solution may comprise between about 1% and about 5% w / w CMC. The binder solution may comprise between about 3% and about 6% w / w CMC. The binder solution may comprise between about 4% and about 5% w / w CMC. The binder solution may comprise about 1 % w / w CMC, or about 2, 3, 4, 4.5, 5,6, or about 7% w / w CMC. The binder solution may comprise about 4.5% w / w CMC. The binder solution may comprise between about 1% and about 3% w / w MFC, or between about 1 -1 .5, 1 -2, 1 -2.5, 1.5-2, 2.5-2.5, 1.5-3, 2-2.5, 2-3, or between about 2.5% and about 3% w / w MFC. The binder solution may comprise between about 1 % and about 2% w / w MFC. The binder solution may comprise between about 1% and about 1 .5% w / w MFC. The binder solution maycomprise about 1 % w / w MFC, or about 1.3, 1.5, 2, 2.5, or about 3% w / w MFC. The binder solution may comprise about 1 .3% w / w MFC.
[0038] The binder solution may comprise both CMC and MFC. The binder solution may further comprise water. The binder solution may comprise CMC, MFC, and water. The binder solution may consist of CMC, MFC, and water. The binder solution may consist essentially of CMC, MFC, and water. The binder solution may comprise between about 1 -7% w / w CMC and between about 1 -3% w / w MFC, as described in the preceding paragraph. The binder solution may comprise between about 1% and about 5% w / w CMC and between about 1% and about 2% w / w MFC. The binder solution may comprise between about 3% and about 6% w / w CMC between about 1 % and about 2% w / w MFC. The binder solution may comprise between about 4% and about 5% w / w CMC and between about 1 % and about 1 .5% w / w MFC. The binder solution may comprise about 4.5% w / w CMC and about 1 .3% w / w MFC. The binder solution may comprise between about 90% and about 98% w / w water. The binder solution may comprise water up to 100% w / w, i.e. the balance of the binder solution may be water.
[0039] The method of the first aspect of the disclosure may further comprise a step (a.i.) of preparing the binder solution. The binder solution may be prepared by mixing the cellulose and water. The binder solution may be prepared by mixing water and CMC and / or MFC. The binder solution may be prepared by mixing CMC and MFC. The cellulose may be provided in an aqueous solution or as a powder. For example, CMC may be provided in a 6% w / w aqueous solution or as a powder. The MFC may be provided in an aqueous solution having 10% w / w dry material content, or as an aqueous solution having 2% w / w dry material content. Thus preparing the binder solution may comprise, for example, mixing about 30 parts CMC powder, about 2 parts MFC 2% w / w dry material content aqueous solution, and about 12 parts water.
[0040] The binder solution may be mixed with the glass fines using any suitable mixer, such as a rotary blade mixer, shell mixer, ribbon mixer, or intensive mixer. The binder solution may be mixed with the glass fines using a rotary blade mixer. The mixture may comprise between about 75% and about 95% w / w glass fines, or between about 75-80, 75-85, 75-90, 80-85, 80- 90, 80-95, 85-90, 85-95, or between about 90% and about 95% w / w glass fines. The mixture may comprise between about 80% and about 90% w / w glass fines. The mixture may comprise about 75% w / w glass fines, or about 80, 85, 90, or about 95% w / w glass fines. The mixture may comprise about 85% w / w glass fines. The mixture may comprise between about 5% and about 25% w / w binder solution, or between about 5-10, 5-15, 5-20, 10-15, 10-20, 10-25, 15- 20, 15-25, or between about 20% and about 25% w / w binder solution. The mixture may comprise between about 10% and about 20% w / w binder solution. The mixture may comprise about 5% w / w binder solution, or about 10, 15, 20, or about 25% w / w binder solution. Themixture may comprise about 15% w / w binder solution. The mixture may comprise between about 75-95% w / w glass fines and between about 5-25% w / w binder solution. The mixture may comprise between about 10% and about 20% w / w binder solution and between about 80% and about 90% w / w glass fines. The mixture may consist, or consist essentially of, of glass fines and binder solution, in the proportions described above.
[0041] In step (ii) of the method of the first aspect of the disclosure, the mixture is formed into a shape. The shape may be any suitable shape, such as, for example a tile, a brick, a bowl, a basin, a decorative item, a bead, a pendant, a mechanical component, or a filter. The mixture may be formed into the shape by any suitable means, such as by hand building, extrusion, compression moulding, or 3D printing. In embodiments, the mixture may be compressed in a mould by a plunger, extruded and punched to produce irregularly shaped tiles and thinner tiles, or pressed using a ram press to provide heavily profiled tiles where extruded slugs of the tile body are pressed between two halves of a hard or porous mould mounted in a hydraulic press. The mixture may be formed into a shape by extrusion.
[0042] The method of the first aspect of the disclosure may further comprise a step (ii.a), following step (ii) and before step (iii), of drying the shape. If there is water present in the tiles during step (iii), the tiles may crack. The shape may be dried at a slow rate to prevent or inhibit the formation of cracks. The step of drying may be carried out over a period of between about 2 hours and about 20 hours, or between about 2-5, 2-10, 2-15, 5-10, 5-15, 5-20, 10-15, I Q- 20, or between about 15 hours and about 20 hours, or over a period of at least about 2, 5, 10 or 20 hours. The step of drying may be carried out over a period of between about 10 hours and about 20 hours. The shape may be dried for about 2 hours, or about 5, 10, 12, 15, or about 20 hours. The shape may be dried for about 12 hours. The shape may be dried at a temperature of between about 20 °C and about 50 °C, or between about 20-30, 20-40, 30-40, 30-50, or between about 40 °C and about 50 °C. The shape may be dried at a temperature of between about 30 °C and about 40 °C. The shape may be dried at a temperature of about 20 °C, or about 30, 40 or about 50 °C. The shape may be dried at a temperature of about 30 °C. The shape may be dried in continuous drier or a tunnel drier, where it is heated indirectly using gas or oil, infrared lamps, or microwave energy. The shape may be dried in a food dehydrator, such as a commercial food dehydrator. Infrared drying may be used for thin shapes, such as thin tiles, whereas microwave drying may be used for thick shapes. Alternatively, an impulse dryer may be used for creating pulses of hot air flowing to the shape.
[0043] In step (iii) of the method of the first aspect of the disclosure, the shape, which is formed from the mixture, is heated to form the glass product. The shape may be heated such that the binder solution (such as cellulose and water) is burnt off, leaving a ceramic product thatconsists entirely of, or essentially of, glass. The shape may be heated at a temperature of between about 500 °C and about 900 °C, or between about 500-600, 500-700, 500-800, 600- 700, 600-800, 600-900, 700-800, 700-900, or between about 800 °C and about 900 °C. The mixture may be heated at a temperature of between about 600 °C and about 800 °C. The mixture may be heated at a temperature of between about 700 °C and about 800 °C. The mixture may be heated at a temperature of between about 680 °C and about 900 °C. The shape may be heated at a temperature of about 500 °C, or about 550, 600, 650, 700, 750,760, 800, 850, or about 900 °C. The shape may be heated at a temperature of about 760 °C. The shape may be heated for a duration of between about 4 hours and about 12 hours, or between about 4-6, 4-8, 4-10, 6-8, 6-10, 6-12, 8-10, 8-12, or between about 10 hours and about 12 hours. The shape may be heated for about 2 hours, or about 4, 6, 8, 10, or about 12 hours. The shape may be heated for about 8 hours. The heating may take place in a kiln.
[0044] Conveniently, a glass product produced using the method of the first aspect of the disclosure does not require glazing. Because the product is made of glass, step (iii) commonly provides a product having a semi-gloss finish. Avoiding an additional step of glazing results in a process which is more efficient, environmentally friendly, and economical, compared to conventional processes for preparing ceramic products.
[0045] The method of the first aspect of the disclosure may further comprise a step (iv) of finishing. In an embodiment, the finishing step does not involve rectification. Rectification may not be necessary as glass products prepared by the method of the first aspect of the disclosure may be moulded accurately.
[0046] The method of the first aspect of the disclosure may further comprise a quality assurance process which is carried out at steps (i)-(iii), or (i)-(iv) using statistical process control. Random samples of the glass product may be tested to meet certain specifications regarding physical and chemical properties in accordance with predetermined standards. These may include properties such as mechanical strength, abrasion resistance, chemical resistance, water absorption, dimensional stability, frost resistance, linear coefficient of thermal expansion, and slip resistance.
[0047] The glass product produced using the method of the first aspect of the disclosure may be, for example, a tile, a brick, a cladding, a toilet, a bowl, a basin, a decorative item, a bead, a pendant, a mechanical component, or a filter. The product may consist, or consist essentially of, of glass.
[0048] An embodiment of the method of the first aspect of the disclosure is depicted in Figure 2. In this embodiment, the process (100) comprises step 101 of preparing raw materials, whereby recycled glass packaging is crushed to reduce into cullet using hammer or muller mills. A sieve may be used to filter out particles in a specific size range. This is followed by step 102 of mixing, wherein the glass fines and binder solution are combined to form a mixture. This is followed by step 103 of press forming, wherein the mixture is then pressed into tiles, and step 104, wherein the press formed tile is dried. The dried tile is then fired in a kiln in step 105. This is followed by step 106 of finishing. In this embodiment, glazing and rectification steps are not required.
[0049] In a second aspect of the disclosure, there is provided a glass product prepared by the method of the first aspect of the disclosure.Examples
[0050] The present disclosure is further described below by reference to the following nonlimiting examples.Example 1
[0051] A binder solution was prepared by mixing the following ingredients:
[0052] This is equivalent to:
[0053] The binder solution (11 parts by weight) was mixed with glass fines having a size of less than 150 pm (60 parts by weight) using a rotary blade mixer to form a mixture. The mixture was formed into tiles.
[0054] The tiles were then dried in a commercial food dehydrator at 30 °C for 12 hours, and then fired in a kiln at 760 °C.
[0055] Figure 3 shows an example of tiles prepared using the method of the invention. XRD analysis (Figure 4) indicates that the glass product has substantially the same composition (quartz) as the glass fines starting material. TGA analysis (Figure 5) indicates that following the dehydroxylation region (rectangle marked with dashed line in Figure 5), the mass of the glass product sample remains steady until the chamber reaches 1200 °C. The absence of any significant gain or loss of mass indicate that the material is homogenous and pure.
[0056] The inventors have investigated various biopolymers as potential binders, such as starch, various types of cellulose, and agar. Starches did not function well as binders because when mixed with water they become non-Newtonian fluids, so when put under pressure, for example during extrusion, they become solid and cannot be extruded. Agar was found to burn off too soon in the kiln, which meant the glass product crumbled and fell apart before the glass particles could fuse. However, it was found that cellulose can withstand high temperatures (up 580 °C) before it burns. The inventors first tested a binder containing only CMC and water, but the resulting mixture with glass fines did not extrude well because the mixture needed to be very wet to enable extrusion and thus became too wet and “sloppy”. To make the mixture less wet, the inventors combined the CMC with MFC and discovered that this combination worked well, in particular for extruding.
[0057] Those skilled in the art will appreciate that the disclosure described herein is susceptible to variations and modifications other than those specifically described. It is to be understood that the disclosure includes all such variations and modifications. The disclosure also includes all of the steps, features, compositions and compounds referred to or indicated in this specification, individually or collectively, and any and all combinations of an two or more of said steps, features, compositions and compounds.
Claims
Claims:1 . A method of preparing a glass product, the method comprising:(i) preparing a mixture comprising glass fines and a binder solution, wherein the binder solution comprises cellulose;(ii) forming the mixture into a shape; and(iii) heating the shape to form the glass product.
2. The method of claim 1 , wherein the binder solution further comprises water.
3. The method of claim 1 or claim 2, wherein the binder solution comprises between about 1 -10% w / w cellulose.
4. The method of any one of claims 1 to 3, wherein the binder solution comprises about 6% w / w cellulose.
5. The method of any one of claims 1 to 4, wherein the binder solution comprises carboxymethyl cellulose (CMC), m icrofibril lated cellulose (MFC), or a combination thereof.
6. The method of any one of claims 1 to 5, wherein the binder solution comprises between about 1-7% w / w CMC.
7. The method of any one of claims 1 to 6, wherein the binder solution comprises about 4.5% w / w CMC.
8. The method of any one of claims 1 to 7, wherein the binder solution comprises between about 1-3% w / w MFC.
9. The method of any one of claims 1 to 8, wherein the binder solution comprises about 1 .3% w / w MFC.
10. The method of any one of claims 1 to 9, wherein the binder solution comprises CMC and MFC.11 . The method of any one of claims 1 to 10, wherein the binder solution comprises between about 1-7% w / w CMC and between about 1 -3% w / w MFC.
12. The method of any one of claims 1 to 11 , wherein the binder solution comprises about 4.5% w / w CMC and about 1 .3% w / w MFC.
13. The method of any one of claims 1 to 12, wherein the binder solution comprises between about 90-98% w / w water.
14. The method of any one of claims 1 to 13, wherein the binder solution consists of cellulose and water.
15. The method of any one of claims 1 to 14, wherein the binder solution consists of CMC, MFC, and water.
16. The method of any one of claims 1 to 14, wherein the mixture comprises between about 75-95% w / w glass fines and between about 5-25% w / w binder solution.
17. The method of any one of claims 1 to 16, wherein the mixture comprises about 85% w / w glass fines and about 15% w / w binder solution.
18. The method of any one of claims 1 to 17, wherein the mixture consists of glass fines and binder solution.
19. The method of any one of claims 1 to 18, wherein in step (ii) the mixture is formed into the shape by hand building, extrusion, compression moulding, or 3D printing.
20. The method of any one of claims 1 to 19, further comprising a step (ii.a.) following step (ii) and before step (iii), of drying the shape.21 . The method of any one of claims 1 to 20, wherein in step (iii) the shape is heated at a temperature of between about 500-900 °C.
22. The method of any one of claims 1 to 21 , wherein in step (iii) the shape is heated at a temperature of about 760 °C.
23. The method of any one of claims 1 to 22, wherein in step (iii) the shape is heated for a duration of between about 4 hours and about 12 hours.
24. The method of any one of claims 1 to 23, wherein the glass product is selected from a tile, a brick, a cladding, a toilet, a bowl, a basin, a decorative item, a bead, a pendant, a mechanical component, or a filter.
25. The method of any one of claims 1 to 24, wherein the glass product consists of glass.
26. A glass product prepared by the method of any one of claims 1 to 25.
Citation Information
Patent Citations
Rice hull glass material and preparation method thereof
CN115557698A
Moldable and malleable glass mass for the production of jewelry, decorative and everyday objects by fusing
DE202010000606U1
Method of manufacturing stone-like articles
US20080076655A1
Dental glass ionomer cement compositions containing polysaccharide nanofiber
US20220015991A1
Compositions and methods for providing increased strength in ceiling, flooring, and building products
US20230060416A1