Ore reduction and smelting process, reactor and gas deflector and load descent regulator
The reactor system using self-reducing briquettes and carbonaceous materials in the metal production process addresses the inefficiencies and environmental issues of traditional methods, achieving cost-effective and sustainable metal production with reduced emissions.
Patent Information
- Application Number
- PCT/BR2024/050171
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-22
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Current metal production processes, such as blast furnaces and electric reduction furnaces, face high capital and production costs, energy inefficiency, and a significant carbon footprint due to the use of coke or charcoal, leading to environmental concerns and unsustainable steel production.
A reactor system utilizing self-reducing briquettes made of metallic compounds and carbonaceous briquettes, with the carbon element already incorporated, replaces traditional sinter or pellets, allowing for energy-efficient reduction and fusion of metals with lower capital and production costs, and the use of biomass as a carbon source to reduce greenhouse gas emissions.
The process significantly reduces production and capital costs, enhances energy efficiency, and minimizes the carbon footprint by using abundant, lower-value raw materials, achieving a 30-50% reduction in production costs and aiming for zero greenhouse gas emissions in metal production.
Smart Images

Figure BR2024050171_31102024_PF_FP_ABST
Abstract
Description
ORE REDUCTION AND FUSION PROCESS, GAS REACTOR AND DEFLECTOR AND LOAD DECREASE REGULATOR FIELD OF INVENTION
[0001] The present invention consists of a process and equipment for producing metals and their alloys from their natural or residual compounds with high energy efficiency and extreme flexibility in terms of raw materials and sources of carbonaceous elements applicable to the process.
[0002] The process begins with composites or agglomerates of the metal compounds being produced, containing carbonaceous elements of fossil origin or biomass from industrial, agricultural, or urban waste in proportions suitable for metallization of these compounds when heated to the melting point of each metal. It also contains fluxing agents to form slag with the gangue of natural or residual metallic compounds and the ash of carbonaceous elements, plus binders to enable low-temperature curing of the composites or agglomerates of metallic compounds, giving them resistance to processing at the melting point of each metal.
[0003] The energy required for the process is generated by burning composites or agglomerates of carbonaceous elements of different degrees of carbonization, of fossil origin or biomass from industrial, agricultural or urban waste, also containing fluxing elements for the ash of the carbonaceous elements, plus binders to allow curing at low temperatures, providing properties for burning by pre-heated air or not with proportions of O2 up to 100%. BACKGROUND OF THE INVENTION: STATE OF THE ART
[0004] Two technological routes are currently used to reduce the melting of the metals that are the subject of the present invention: shaft furnaces and electric reduction furnaces.
[0005] Shaft furnaces, more specifically blast furnaces, are used to produce pig iron and, to a lesser extent, manganese iron and high nickel pig iron (NPI).
[0006] Blast furnaces require the use of high-temperature prepared feedstock such as sinter, pellets, and coke, which require significant energy expenditure and high capital expenditure (CAPEX), as well as a significant environmental impact and carbon footprint. In blast furnaces, to produce charcoal, it is very common to cultivate industrial-energy eucalyptus forests, which have high capital expenditure (CAPEX) and charcoal production costs (OPEX), and low energy efficiency.
[0007] In electric reduction furnaces, a raw, sintered, calcined or preheated oxide charge is mixed with reducing agents, coke or coal, fossil or vegetable, before being loaded into the furnaces.
[0008] In these furnaces, electrodes generate electric arcs and electric currents submerged in the load that melt the mixture of oxides and reducers, leading to their reduction-fusion.
[0009] Electric reduction furnaces are used to produce ferroalloys such as ferromanganese, ferrochrome and ferronickel.
[0010] Electric reduction furnaces have high capital (CAPEX) and production (OPEX) costs due to the intensive use of energy, coke and electrodes, with low energy efficiency, high environmental impact and a high carbon footprint.
[0011] The CAPEX and OPEX of the current state of the art, for example, of a plant for the production of pig iron in blast furnaces, can be estimated between: CAPEX 800 to 1,000 US$ / t of annual installed capacity; OPEX 300 to 350 US$ / t of metal; The present invention allows these figures to be reduced to: CAPEX 300 to 350 US$ / t of annual installed capacity; OPEX 200 to 250 US$ / t of metal.
[0012] New technologies, some under development and others at different stages of industrial use, are present in the current steel industry, the main ones being:
[0013] The Tecnored Furnace is a modular rectangular reactor, each module consisting of two tanks—a smaller one at the top and a larger one at the bottom. Each tank has one or more rows of tuyeres and a common gas outlet duct that feeds the self-reducing agglomerates. It is notable for being an iron production system that uses biocarbon or coal agglomerates in any proportion as an energy source, as well as self-reducing agglomerates that use coal or biomass fines as a reductant, but which must be processed in the Tecnored furnace with secondary combustion of the gases from the primary combustion to supply the energy required for self-reduction.
[0014] The OXYCUP Process is based on the production of large self-reducing agglomerates to be reduced and melted together with reasonable amounts of metal charge in a hot air cupola with a high percentage of O2 in the air blow. It incorporates fine residual agglomerates from the steel industry into the mass, hence its preferred installation. as a unit dedicated to the use of this waste and internal scrap that is difficult to digest in the usual furnaces.
[0015] The HISARNA (High Strength and Resource-Saving) process consists of a cyclonic reactor superimposed on a converter where the molten metal undergoes reductive fusion of pre-reduced iron oxide in the cyclonic reactor. The main feature of the HISARNA process is the replacement of coke with coal as the reducing agent. It has high capital (CAPEX) and production (OPEX) costs.
[0016] The ITmK3 process, developed in Japan to treat self-reducing agglomerates from steel mill waste, utilizes the RHF (Rotary Hearth Furnace) equipment. It promotes, in consecutive sections of its circular hearth, self-reduction, the fusion of iron and slag, and, finally, the consequent separation and solidification of these two phases, resulting in the iron taking on the final "nugget" shape. The ITmk3 process essentially consists of a rotary hearth furnace, into which pellets made of iron oxides mixed with fines of reducing agents and binders are loaded, resulting in the production of iron nodules. This is a highly efficient process, given its rapid reduction kinetics.
[0017] Blast furnaces operate by generating reducing gas and energy by burning coke or charcoal, injecting preheated air, enriched with O2 or not, into the coke or charcoal column at the base of the furnace (coke or coal foot), and permeating the generated gas (CO + N2) in countercurrent with the descending charge. Reduction-fusion occurs through penetration and progressive reaction of the gas in the charge. The dilution of the reducing gas fraction (CO) by N2 in the air and the need for gas penetration through the pores of the charge materials make this reaction very slow—in the case of blast furnaces, approximately 8 hours for the charge to descend from the top to the base—which requires a high furnace height. from which its name derives, and the requirement for forming the base of the charge column (coke or coal foot) with high-density, high-strength, and high-cost coke or charcoal. The reliance on coal also implies a high carbon footprint of the process.
[0018] It is clear that there is currently no viable, economically viable solution for progressive implementation to the problems related to high production and capital costs, and the high carbon footprint of steel production and the production of base metals and their alloys. OBJECTIVES OF THE INVENTION
[0019] The present invention aims to reveal a reactor for the production of metals and metal alloys from their natural or residual compounds with high energy efficiency and extreme flexibility in terms of raw materials and sources of carbon elements applicable to the process.
[0020] More specifically, the present invention, based on the principle of self-reduction, aims to replace the use of coke or charcoal with briquettes of coal fines or biomass, in any proportions, and to replace the charge of oxides to be reduced in the current hot-produced agglomerates, sinter or pellets, adapted to the gas / solid reaction model of current furnaces, with cold, self-reducing agglomerates, the reducing carbon element, formed by fines of mineral coal or biomass, in any proportions, being incorporated into the agglomerates in a mixture with the oxides to be reduced, that is, metallized, and the replacement of fossil carbon by biomass leads to the progressive circularization of steel production and of these metals and their alloys, in the medium term achieving the objective of zero greenhouse gas (GHG) emissions in a progressive and economically viable manner, transforming the production of these metals and their alloys, on a global scale. economically, socially and environmentally sustainable, encouraging a considerable expansion of the supply of biomass carbon to the market. GENERAL LINE SOLUTION The present invention discloses a reactor with a cylindrical casing comprising at its top at least one exhaust pipe and at least one load distributor, with the loads entering the system through double bell type airlocks or spherical valves that allow loading without loss of process gases, with a load distributor of one of the various alternative designs available, discharging into the cylindrical casing of the reactor self-reducing briquettes of metallic compounds and carbonaceous briquettes arranged in concentric load columns, with the carbonaceous briquettes being loaded in the outermost column, within reach of the blowing of the tuyeres and the self-reducing briquettes of metallic compounds being loaded in an adjacent concentric column, limited by a slope formed up to the center of the reactor.
[0021] The reactor may optionally be equipped with at least one gas deflector and load descent regulator and, at its base, must have at least one circle of tuyeres.
[0022] Air is injected through the tuyeres, generating a flame whose gases will form, in front of each tuyere, gaps for the passage of flame gases through the load (raceway), enabling the transfer of energy contained in the flame gases to the load of self-reducing briquettes of metallic compounds, carrying out the reduction and fusion of these briquettes and permeating and preheating this load until it exits through the load slope, which favors the exit through the central zone to the exhaust tubes at the top of the reactor.
[0023] Additionally, solid, liquid or gaseous fuels and other solid, liquid or gaseous materials of any nature may or may not be injected through the tuyeres.
[0024] The injected air is preheated, or not, and enriched with O2, or not.
[0025] The reactor comprises below the tuyeres line at least one crucible to receive liquid metal evacuated through a siphon hole and slag that floats above the metal, also evacuated continuously.
[0026] The gas deflector and load descent regulator, if optionally adopted, shall comprise at least one circular row of fins around the entire circumference of the reactor at mid-height between the base and the top of the reactor.
[0027] The present invention also discloses a process of reduction and fusion by self-reduction of ores in the following steps: a) manufacture of carbonaceous briquettes; b) manufacture of self-reducing briquettes of metallic compounds; and c) production of metal using carbonaceous briquettes and self-reducing briquettes of metallic compounds.
[0028] Step a) comprises the addition in a mixer of at least one binding agent in a proportion of 5% to 15% by mass with a tolerance typically of 2% depending on the binding agents used and biomass biocarbon fines, in a proportion of 85% to 95% by mass with a typical tolerance of 2%.
[0029] Biocarbon fines are obtained by the pyrolysis of, for example, sugarcane bagasse, forestry and agricultural waste, urban waste or even sewage sludge.
[0030] Biochar is a type of biocarbon that, when used, is ground before being added to the process and the binding agent used is calcium hydroxide or Ca(OH)2 or other traditional binders such as thermosetting resins.
[0031] In step a), in addition to the binding agent and biocarbon, industrial water is used in the mixer, in a proportion of 8% to 10% with a tolerance of 5%.
[0032] In step a), after all the inputs are processed in the mixer, generating carbon briquettes, there is at least one drying and curing step.
[0033] In step a), after the drying and curing step, there is at least one screening step, in which the fine carbonaceous briquettes are separated and sent back to the mixer.
[0034] Step b) comprises the addition in a mixer of at least one binding agent in a proportion of 5% to 10% by mass depending on the agent used, with a tolerance of 2% plus biocarbon of 15% to 25% by mass depending on the analysis of the biocarbon used and the desired carbon content in the primary metal to be produced, with a tolerance of 2%, iron ore fines in a proportion of 55% to 70% by mass depending on the metal content of the oxide used and slag-forming agents in a proportion of 7% to 10% by mass depending on the gangue present in the oxides used with a tolerance of 2%.
[0035] In step b), after all the inputs are processed in the mixer and subsequent briquetting, generating self-reducing briquettes of metallic compounds, there is at least one drying and curing step.
[0036] In step b), after the drying and curing step, there is at least one screening step, in which the fine self-reducing briquettes of metallic compounds are separated and returned to the mixer.
[0037] In step c) the carbonaceous briquettes and the self-reducing briquettes of metallic compounds are loaded into the reactor, with the carbonaceous briquettes being added in a proportion of 10% to 15% depending on their composition with a tolerance of 2% and the self-reducing briquettes of metallic compounds being loaded in a proportion of 85% to 90% with a tolerance of 2% in the case where the injection of powdered coal through the tuyeres is used.
[0038] In step c), at least liquid metal and slag are generated in the crucible.
[0039] In step c), process gases are generated and evacuated from the top of the reactor, and the gases generated are substantially composed of CO, CO2, H2O, H2, CH4 and N2 in proportions that depend on the analysis of the feed materials and process conditions.
[0040] The process of reducing and melting minerals also involves the incidence of flame gases on the load of self-reducing briquettes of metallic compounds, forming a reduction and melting zone. DESCRIPTION OF DRAWINGS
[0041] Figure 1 illustrates a vertical section of an embodiment of the proposed reactor.
[0042] Figure 2 illustrates an enlargement of the reduction and fusion zone traversed by the flame gases up to the load of self-reducing briquettes of metallic compounds.
[0043] Figure 3 illustrates the gas deflector and optional mobile load descent regulator acting on the conduction of gases and the descent of the load column.
[0044] Figure 4 illustrates in detail the gas deflector and optional mobile load descent regulator, explaining the function of the fins in forming a protective layer, forcing the load to roll over the retained load layer, preventing wear due to continuous friction.
[0045] Figure 5 illustrates a flowchart describing a configuration of the manufacturing process for self-reducing briquettes of metallic compounds, in which the ore used is MUSA type iron ore.
[0046] Figure 6 illustrates a flowchart describing a configuration of the carbonaceous briquettes manufacturing process.
[0047] Figure 7 illustrates a flowchart describing a metal production process configuration using carbonaceous briquettes and self-reducing metallic compound briquettes, in addition to other inputs.
[0048] The reference numbers used in this application are: 1 - reactor; 2 - self-reducing briquettes of metallic compounds; 3 - carbonaceous briquettes; 4 - cylindrical casing; 5 - charge distributor; 6 - charge column; 7 - tuyeres; 8 - air; 9 - oxygen (O2); 10 - solid, liquid or gaseous fuels; 11 - other solid, liquid or gaseous materials; 12 - slope; 13 - central charge zone; 14 - flame; 15 - reduction and melting zone; 16 - charge; 17 - liquid metal; 18 - slag; 19 - crucible; 20 - continuous outlet holes; 21 - gas deflector and charge descent regulator; 22 - gases; and 23 - exhaust pipes. DETAILED DESCRIPTION OF THE INVENTION
[0049] The invention is based on the reduction-fusion of metal compounds containing carbonaceous elements, fluxes and binders appropriately dosed in their core, with the energy generated by the high-energy-efficient burning of carbonaceous agglomerates also with fluxes and binders in its mass, in a single reactor of simple design and easy operation, with a capital cost (CAPEX) much lower than that of current technological routes.
[0050] The characteristics of the reactor used in this invention allow the use of compounds of various metals in levels not usable in current technological routes, as well as low-cost carbonaceous elements, whether of fossil or biomass origin. The highly efficient generation and utilization of energy in the reactor also results in a production cost (OPEX) much lower than that of current routes.
[0051] The proposed process radically changes the reduction-melting method of producing base metals and their alloys as currently practiced in both shaft furnaces and electric reduction furnaces, by adopting reactor 1 capable of producing these same metals and their alloys with lower CAPEX, lower OPEX and lower carbon footprint.
[0052] In the case of blast furnaces, for example, current models consist of generating gas and energy by burning coke and injecting powdered coal (PCI) through the tuyeres at the base, and slowly reducing the sinter and / or pellet load by the gas generated, in countercurrent to the load's descent, along the shaft until melting at the base, generating liquid metal and slag, in a load residence time of approximately 8 hours, from the top to the base.
[0053] The proposed solution replaces sinter and pellets with self-reducing briquettes of metallic compounds 2 with the carbon element already incorporated into their core, which eliminates the need for the slow penetration of the reducing gas into the sinter or pellets of the charge, since the reducing carbon is already inserted into the mass of the self-reducing briquettes of metallic compounds 2, depending only on the transmission of energy in the reactor, with a high thermal gradient, to obtain the reduction and fusion of the metallic compounds, with a residence time of the charge of around 20 to 30 minutes, that is, 16 to 24 times less than in current ovens, with a positive impact on the productivity and energy efficiency of the process.
[0054] The reactor 1, which in a preferred configuration has a cylindrical casing 4, comprises at its top at least one exhaust pipe 23 and at least one load distributor 5.
[0055] The loads enter the system from the top through double bell airlocks or spherical valves that prevent the passage of process gases to the atmosphere, and the load distributor 5 discharges into the cylindrical casing 4 of the reactor 1 in concentric vertical columns loads of self-reducing briquettes of metallic compounds 2 and loads of carbonaceous briquettes 3, and in the load column of self-reducing briquettes of metallic compounds 2 a slope is formed up to the center of the reactor 1 where a central load zone 13 is formed.
[0056] The central charge zone 13 deals with the most porous region within the reactor 1.
[0057] In a preferred configuration, two exhaust pipes 23 and a charge distributor 5 are used.
[0058] In an alternative configuration to using a cylindrical casing 4 in reactor 1, a conical casing may be used.
[0059] Reactor 1 comprises at its base at least one circle of tuyeres 7, and air 8 is injected through tuyeres 7, generating a flame 14 whose gases will form a passage zone for hot gases from the flame (raceway) transmitting heat for reduction and fusion 15 at the base of the load 16 of self-reducing briquettes of metallic compounds 2 permeating this load 16 until it exits through the slope through the central load zone 13, reaching the top of reactor 1 until reaching the exhaust pipes 23.
[0060] In a preferred configuration, two tuyeres 7 are used in the tuyere circle 7, in opposite positions of the cylindrical casing 4 of the reactor 1.
[0061] Through the tuyeres 7, solid, liquid or gaseous fuels 10 are injected, or not, and other solid, liquid or gaseous materials 11 of any nature, or not.
[0062] Preferably, the air 7 is preheated and enriched with O2. Alternatively, it is not enriched with O2.
[0063] The reactor is heated by burning biocarbon briquettes with preheated air enriched with oxygen in different proportions, and can also use the burning of carbonaceous fines injected through the tuyeres (PCI) with air enriched with oxygen or not.
[0064] The reactor 1 comprises below the tuyere line 7 at least one crucible 19 for receiving liquid metal 17 and slag 18, which are evacuated, the metal through continuous outlet holes 20 and the slag through a continuous outlet hole. Preferably, there is only one crucible 19.
[0065] A movable gas deflector and load descent regulator 21 is configured for optional use in reactor 1, comprising at least one circular row of fins for retaining a protective layer of load, forcing the load to descend by rolling over the retained layer.
[0066] The gas deflectors and load descent regulators 21 contribute to avoiding the wall effect in the upward flow of flame gases 14 and regulating the load descent 16, with the gas deflectors and load descent regulators 21 being equipped with fins to retain a protective load layer, avoiding wear due to continued friction.
[0067] The process of reducing and smelting minerals comprises the following steps: a) manufacture of carbonaceous briquettes 3; b) manufacture of self-reducing briquettes of metallic compounds 2; c) production of metal using carbonaceous briquettes 3 and self-reducing briquettes of metallic compounds 2.
[0068] Steps a) and b) do not necessarily need to occur in the order presented or in sequence, and may even be carried out in parallel and in locations far from each other.
[0069] Step a) comprises adding to a mixer at least one binding agent in a proportion of 5% to 15% by mass with a tolerance of 2% and biocarbon fines in a proportion of 85% to 95% by mass with a tolerance of 2%.
[0070] The term "biocarbon" refers to biomass carbonized through pyrolysis, such as sugarcane bagasse and plant residues. In the context of this invention, biocarbon is defined as a carbonaceous material produced by the pyrolysis of biomass, such as agricultural residues, wood, or other organic materials, under low-oxygen conditions. This pyrolysis process transforms organic matter into a carbon-rich product with high porosity and surface area.
[0071] In the context of biocarbon, biochar is a type of biocarbon that consists primarily of carbon. In addition to carbon, it can contain a variety of elements and compounds depending on the raw material used and production conditions. These components can include hydrocarbons, minerals, water, volatile gases, volatile organic compounds, and ash. The exact composition of biochar can vary significantly, which can affect its specific properties and applications.
[0072] An example of the composition of the raw material found in a type of biochar used in the present invention - bagasse biochar - is found in Table 1, with the respective mass percentages. Table 1 - composition of an example of biochar.
[0073] Preferably, the binding agent used in step a) is calcium hydroxide or Ca(OH)2. An example of a possible composition is shown in Table 2. Table 2 - composition of an example of a binding agent.
[0074] In an alternative configuration, thermosetting resins, polymers, tars or pitch can be used as binding agents.
[0075] In step a), in addition to the binding agent and biocarbon, which can be of the biochar type, water (H2O) is used in the mixer, in a proportion of 8% to 10% by mass with a tolerance of 5%.
[0076] In a preferred configuration, in step a), after all inputs are processed in the mixer, generating the carbonaceous briquettes 3, there is a drying and curing step. After the drying and curing step, there is preferably a screening step, in which the fines of carbonaceous briquettes 3 are separated and returned to the mixer.
[0077] An example of the composition of the carbonaceous briquette 3 obtained at the end of step a) is found in Table 3, with the respective mass percentages. Table 3 - composition of an example of a carbonaceous briquette 3.
[0078] Step b) comprises the addition in a mixer of at least one binding agent in a proportion of 5% to 10% by mass with a tolerance of 2%, biocarbon in a proportion of 15% to 25% by mass with a tolerance of 2%, iron ore in a proportion of 55% to 70% by mass with a tolerance of 2% and slag in a proportion of 7% to 10% by mass with a tolerance of 2%.
[0079] Preferably, the biocarbon is ground before being added to the process.
[0080] An example of iron ore used in the present invention - MUSA - is found in Table 4, with the respective mass percentages. Table 4 - composition of an example of iron ore (MUSA).
[0081] In the context of the present invention, the term MUSA refers to Mineração Usiminas SA, that is, it is the origin or supplier of iron ore.
[0082] In a preferred configuration, in step b), after all inputs are processed in the mixer, generating the self-reducing briquettes of metallic compounds 2, there is a drying and curing step. After the drying and curing step, there is a screening step in which the fines of self-reducing briquettes of metallic compounds 2 are separated and returned to the mixer.
[0083] An example of the composition of the self-reducing briquette of metallic compounds 2 produced in step b) of the present invention is found in Table 5, with the respective mass percentages. Table 5 - composition of an example of a briquette of metallic compounds 2.
[0084] In step c) the carbonaceous briquettes 3 and the self-reducing briquettes of metallic compounds 2 are poured into the reactor 1, with the carbonaceous briquettes 3 being added in a proportion of 10% to 15% by mass with a tolerance of 2% and the self-reducing briquettes of metallic compounds 2 being added in a proportion of 85% to 95% by mass with a tolerance of 2%.
[0085] Furthermore, in a preferred configuration, PCI (powdered charcoal) and oxygen 9 are added at a temperature of 60°C with a tolerance of 10°C. Additionally, air 8 and oxygen 9 are added at a temperature of 1200°C with a tolerance of 50°C.
[0086] In step c), liquid metal 17 and slag 18 are generated as output.
[0087] The liquid metal is composed substantially of C, Si, Mn, P, S, and Fe, with Fe found in the largest percentage.
[0088] Gases 22 are also generated in the process, and gases 22 are substantially composed of CO, CO2, H2, N2, CPU, H2O and H2S.
[0089] The process of reducing and melting minerals involves the incidence of gases from the flame 14 on the load 16 of self-reducing briquettes of metallic compounds 2, forming a reduction and melting zone 15.
[0090] Reactor 1 produces a reduction and melting zone 15 by the gases from the flame 14 obtained by the optimized burning of carbonaceous briquettes 3 capable of reaching the temperatures and generating energy necessary for the reduction and melting of these same alloys.
[0091] The generation of a reduction and melting zone with a temperature and energy transmission gradient suitable for the production of base metals and their alloys, in reactor 1, is achieved by maximum energy generation in the burning of carbonaceous briquettes 3 by the calibration of the Boudouard reaction, by the size of the carbonaceous briquettes 3, by the length or penetration of the flame 14 defined by the air flow rate 8 and by the relationship between the size of the carbonaceous briquettes 3 and the diameter of the tuyeres 7 by the Hatano equation, with the temperature of the reduction and melting zone 15 also defined by the variables of air preheating temperature 8, addition of O2 9 and optional injections through the tuyeres 7 of solid, liquid or gaseous fuels 10 or other solid, liquid or gaseous materials 11 and by the nature of the metallic compounds themselves present in the self-reducing briquettes of metallic compounds 2.
[0092] Flame optimization 14 for maximum energy generation is done by calibrating the variables listed above for minimum CO production.
[0093] The reactions at the heart of self-reducing briquettes of metallic compounds 2 occur as follows:
[0094] The burning reaction of carbonaceous briquettes 3 occurs as follows: (z) C + (p+2q) / 2 02 = (p) CO + (q) CO2 (3) Where: p + q = z (4) p / q = minimum (5)
[0095] After the reduction and melting zone 15, the gases from the flame 14 will flow through the load 16 of self-reducing briquettes of metallic compounds 2, descending in a countercurrent, preheating the load 16 until exiting through the slope 12 or through the more porous central load zone 13, with the flow of gases 22 being governed by the Ergun equations that define permeability as a cubic function of the porosity and the squares of the velocity and diameter of the granulated materials.
[0096] The gases 22 extracted by the exhaust pipes 23 will be used in the production of electrical energy through cogeneration or as fuel for various uses.
[0097] The adoption of the reactor and process described in the present invention allows a significant increase in energy efficiency and a reduction in production and capital costs, replacing high-temperature prepared charge, sinter or pellets, with cold-cured agglomerates of metallic compounds, already containing carbonaceous elements dosed for their complete reduction and fusion, also dispensing with the use of metallurgical coke or coarse charcoal, obtained from industrial forests or by deforestation of natural forests.
[0098] The energy for the process is generated by injecting preheated air, enriched with O2 or not, into cold-produced carbon agglomerates from lower-value fines, fossils or residual biomass. Energy generation is optimized by eliminating the need to generate reducing gas in the reactor, as the carbon for reducing the agglomerates is already present in their mass.
[0099] Increasing the overall energy efficiency of the steel plant increases energy credits by reducing production costs and the direct and indirect carbon footprint.
[0100] The use of fine carbonaceous elements, both in self-reducing briquettes of metallic compounds and in carbonaceous briquettes, expands the range of raw materials, both residual or natural metallic compounds, of lower value, and carbonaceous fines, which can be obtained from biomass from agricultural, forestry and urban waste, such as garbage and sewage sludge, with economic circularization of the production of basic metals and their alloys, zeroing, in the medium term, greenhouse gas (GHG) emissions, in addition to adding an oxygen credit to the environment, through the production of these metals and their alloys, economically, through the market, without excessive dependence on subsidies or carbon taxes.
[0101] The proposed solution allows the use of abundant raw materials, which are cheaper because they cannot be used by current furnaces, with an increase in the energy efficiency of the process, reducing the production cost of base metals and their alloys by 30% to 50%.
[0102] In addition to reducing the current fossil carbon footprint in the production of base metals and their alloys and the possibility of using carbon from waste biomass in any proportions, the present invention provides a definitive solution for the production of these metals and their alloys with zero greenhouse gas (GHG) emissions and an extra supply of oxygen to the environment.
[0103] The production of metal alloys in electric reduction furnaces will also have its capital and production costs greatly reduced by adopting the reactor and process described in the present invention, by eliminating heavy investments in electrical infrastructure and the high cost of intensive use of electrical energy and electrodes, replacing the use of electrical energy by burning carbon briquettes, reversing the current situation of this industry, from a demander to a supplier of electrical energy through cogeneration.
[0104] The conversion of current shaft furnaces and electric reduction furnaces to the process object of the present invention is technically and economically viable, due to the OPEX and CAPEX reductions it provides, with a rapid return on investment without excessive support from subsidies or carbon taxes.
[0105] In addition to the examples mentioned throughout the detailed description of the present invention, additional examples of possible compositions of raw materials used throughout the ore reduction and fusion process can be mentioned, as will be demonstrated below.
[0106] An example of return fines generated and / or used in the present invention is found in Table 6, with the respective mass percentages. Table 6 - composition of an example of return fines.
[0107] An example of PCI (powdered charcoal) used in the present invention is found in Table 7, with the respective mass percentages. Table 7 - composition of an example of PCI.
[0108] An example of slag generated and / or used in the present invention is found in Table 8, with the respective mass percentages. Table 8 - composition of an example of slag.
[0109] An example of a desulfurizing agent (De-S) used in the present invention is found in Table 9, with the respective mass percentages. Table 9 - composition of an example of De-S.
[0110] An example of raw material flows and reaction products of the present invention is found in Table 10, where the flows in kg / h of some of the inputs and products of the processes shown in figures 5, 6 and 7 for the production of 115 t / h of pig iron are shown. Table 10 - example of input flow for the biocarbon briquette production process
[0111] An example of raw material consumption in step c), shown in the flowchart in Figure 7, is found in Table 11, where the raw material consumption of the process is shown in their respective units of measurement. Table 11 - example of raw material consumption in the manufacture of self-reducing briquettes and in the reduction furnace
[0112] An example of inputs that enter the furnace in step c), shown in the flowchart in Figure 7, is shown in Table 12, where the furnace input consumption is shown in their respective units of measurement. Table 12 - example of inputs in step c).
[0113] A first example of outputs that leave the furnace in step c), visualized in the flowchart in Figure 7, is seen in Table 13, where the products resulting from the furnace are shown in their respective units of measurement. Table 13 - example of furnace outputs in step c).
[0114] An example of the compositions of the outputs listed above, visualized in the flowchart in Figure 7, are verified in Tables 14, 15 and 16, where the compositions of the products resulting from the furnace are shown in their respective units of measurement. Table 14 - example of slag composition. Table 15 - example of metal composition. Table 16 - example of gas composition.
[0115] Having described some preferred examples of embodiment of the invention, it is worth highlighting that the scope of protection conferred by this document encompasses all other alternative forms applicable to the execution of the invention, and this is defined and limited only by the content of the attached claims table.
[0116] Since such modifications are trivial for a person skilled in the art, it is understood that these constitute only alternative configurations of the present invention, still being encompassed by the scope of protection of the present invention.
[0117] It should be noted that the drawings presented are not necessarily to scale and are merely conceptual in nature. Nevertheless, it is expressly provided that all combinations of elements that perform the same function in substantially the same manner to achieve the same results as the elements claimed herein are within the scope of the present invention. Finally, it should be noted that the scope of protection of the present invention encompasses other possible variations and is not limited solely by the content of the claims alone, including possible equivalents.
Claims
CLAIMS 1. Reactor (1) with cylindrical casing (4) characterized by the fact that it comprises at its top at least one exhaust pipe (23) and at least one load distributor (5); wherein, the loads enter the reactor (1) through a double bell type sluice system or by spherical valves; wherein, the load distributor (5) discharges into the cylindrical casing (4) of the reactor (1) in concentric vertical columns loads of self-reducing briquettes of metallic compounds (2) and carbonaceous briquettes (3); and wherein, in the load column of self-reducing briquettes of metallic compounds (2) a slope is formed up to the center of the reactor (1) where a central load zone (13) is formed.
2. Reactor (1), according to claim 1, characterized by the fact that it incorporates at least one gas deflector and load descent regulator (21).
3. Reactor (1) according to any one of claims 1 and 2, characterized in that it comprises at its base at least one circle of tuyeres (7); and air (8) is injected through the tuyeres (7), generating a flame (14) whose gases will form a reduction and fusion zone (15) at the base of the load (16) of self-reducing briquettes of metallic compounds (2), permeating this load (16) until exiting through the slope (12) or through the central load zone (13), up to the top of the reactor (1) where the exhaust pipes (23) are located.
4. Reactor (1), according to claim 3, characterized in that solid, liquid or gaseous fuels (10) are injected through the tuyeres (7).
5. Reactor (1), according to claim 3, characterized by the fact that other solid, liquid or gaseous materials (11) of any nature are injected through the tuyeres (7).
6. Reactor (1) according to claim 3, characterized in that the air (7) is preheated.
7. Reactor (1) according to claim 3, characterized in that the air (7) is enriched with O2.
8. Reactor (1) according to any one of claims 1 to 7, characterized in that it comprises below the tuyeres line (7) at least one crucible (19) for receiving liquid metal (17) and slag (18) evacuated by continuous outlet holes (20).
9. Gas deflector and load descent regulator (21), movable, configured for use in a reactor (1), according to claim 2, characterized by the fact that it comprises at least one circular line of fins around the entire circumference of the reactor (1) at half height between the base and the top of the reactor (1).
10. Process of reduction and fusion of minerals, characterized by the fact that it comprises the following steps: a) manufacture of carbonaceous briquettes (3); b) manufacture of self-reducing briquettes of metallic compounds (2); c) production of metal using carbonaceous briquettes (3) and self-reducing briquettes of metallic compounds (2).
11. Process for reducing and smelting minerals, according to claim 10, characterized in that step a) comprises the addition in a mixer of at least one binding agent in a proportion of 5% to 15% by mass with a tolerance of 2% and biomass biocarbon fines in a proportion of 85% to 95% by mass with a tolerance of 2%.
12. Process for reducing and smelting minerals, according to claim 11, characterized in that the binding agent is calcium hydroxide or Ca(OH)2.
13. Process for reducing and smelting minerals, according to claim 11, characterized in that in step a), in addition to the binding agent and the biocarbon, industrial water is used in the mixer, in a proportion of 8% to 10% by mass with a tolerance of 5%.
14. Mineral reduction and fusion process, according to claim 13, characterized by the fact that in step a), after all the inputs are processed in the mixer, generating the carbonaceous briquettes (3), there is at least one drying and curing step.
15. Process for reducing and smelting minerals, according to claim 14, characterized in that in step a), after the drying and curing step, there is at least one screening step, in which the fine carbonaceous briquettes (3) are separated and returned to the mixer.
16. Process for reducing and smelting minerals, according to claim 10, characterized in that step b) comprises the addition in a mixer of at least one binding agent in a proportion of 5% to 10% by mass with a tolerance of 2%, biocarbon in a proportion of 15% to 25% by mass with a tolerance of 2%, iron ore fines in a proportion of 55% to 70% by mass and slag-forming agents in a proportion of 7% to 10% by mass with a tolerance of 2%.
17. Process for reducing and smelting minerals, according to claim 16, characterized by the fact that in step b), after all the inputs are processed in the mixer and subsequent briquetting, generating self-reducing briquettes of metallic compounds (2), there is at least one drying and curing step.
18. Process for reducing and smelting minerals, according to claim 17, characterized by the fact that in step b), after the drying and curing step, there is at least one screening step, in which the fines of self-reducing briquettes of metallic compounds (2) are separated and returned to the mixer.
19. Mineral reduction and fusion process, according to claim 16, characterized by the fact that the biocarbon used is of the biochar type; and that the biochar is ground before being added to the process.
20. Process for reducing and smelting minerals, according to claim 10, characterized in that in step c) the carbonaceous briquettes (3) and the self-reducing briquettes of metallic compounds (2) are loaded into the reactor (1), with the carbonaceous briquettes (3) being added in a proportion of 10% to 15% by mass with a tolerance of 2%; and the self-reducing briquettes of metallic compounds (2) being added in a proportion of 85% to 95% by mass with a tolerance of 2%.
21. Process for reducing and smelting minerals, according to claim 20, characterized in that in step c), at least liquid metal (17) and slag (18) are generated as output.
22. Process for reducing and smelting minerals, according to claim 20, characterized in that in step c) gases (22) are generated; and the gases (22) are substantially composed of CO, CO2, H2O, H2, CH4 and N2.
23. Process for reducing and fusion of minerals, according to claim 10, characterized by the fact that it comprises the incidence of gases from the flame (14) on the load (16) of briquettes self-reducing metallic compounds (2) forming a reduction and fusion zone (15).
24. Process for reducing and smelting minerals, according to claim 10, characterized in that it comprises the following steps: a) manufacturing of carbonaceous briquettes (3); b) manufacturing of self-reducing briquettes of metallic compounds (2); c) production of metal using the carbonaceous briquettes (3) and the self-reducing briquettes of metallic compounds (2); wherein, step a) comprises the addition in a mixer of at least one binding agent in a proportion of 5% to 15% by mass and biomass biocarbon fines in a proportion of 85% to 95% by mass; wherein, in step a), after all the inputs are processed in the mixer, generating the carbonaceous briquettes (3), there is at least one drying and curing step and at least one screening step, in which the carbonaceous briquette fines (3) are separated and returned to the mixer;wherein, step b) comprises the addition in a mixer of at least one binding agent in a proportion of 5% to 10% by mass, biocarbon in a proportion of 15% to 25% by mass, iron ore fines in a proportion of 55% to 70% by mass and slag-forming agents in a proportion of 7% to 10% by mass; wherein, in step b), after all the inputs are processed in the mixer and in the briquette machines, generating the self-reducing briquettes of metallic compounds (2), there is still at least one drying and curing step and at least one screening step, in which the fines of self-reducing briquettes of metallic compounds (2) are separated and returned to the mixer; wherein, in step c) the carbonaceous briquettes (3) and the metallic compound briquettes (2) are loaded into the reactor (1); wherein the carbonaceous briquettes (3) are added in a proportion of 10% to 15% by mass; and wherein, the self-reducing metallic compound briquettes (2) are added in a proportion of 85% to 95% by mass.
Citation Information
Patent Citations
METALLURGICAL OVEN FOR METAL ALLOYS
BR102015005373A2
PROCESS AND EQUIPMENT FOR CONVERTING BLAST FURNACES TO SELF-REDUCTION MODE
BR102019007542A2
Solid aggregate for use in reduction steelmaking furnaces.
BR102021018410A2
APPLICATION PROCESS OF CARBON NANOTUBES IN AGGLOMERATES OF FINE ORE PARTICULATES TO INCREASE MECHANICAL STRENGTH
BR112014005488A2
Method for operating shaft furnace
EP0261432A1