Liquid epoxy molding compound and preparation method therefor
By adjusting the ratio of inorganic silicone fillers and epoxy resin, combined with premixing and grinding processes, the problem of excessive warpage height of liquid epoxy plastic sealant was solved, achieving a low-warpage packaging structure and improving cost-effectiveness.
Patent Information
- Application Number
- PCT/CN2023/092798
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2023-05-08
- Publication Date
- 2024-10-31
AI Technical Summary
The existing liquid epoxy plastic sealant warps too high during the packaging process, causing the packaged electronic products to be unable to be used normally and increasing production costs.
By adjusting the mass fraction and particle size of inorganic silicon fillers, combined with the use of naphthalene-type epoxy resin and acid anhydride curing agents, and using pre-mixing and grinding processes, the thermal expansion coefficient of the liquid epoxy molding compound is reduced, thereby reducing the warpage height.
It effectively reduces the warpage height of the liquid epoxy plastic sealant, improves the mechanical properties and thermal conductivity of the packaging structure, reduces production costs, and improves the success rate of packaging.
Smart Images

Figure CN2023092798_31102024_PF_FP_ABST
Abstract
Description
Liquid epoxy molding compound and preparation method thereof
[0001] Cross-references to related publications
[0002] This disclosure claims priority to Chinese patent disclosure No. 202310462294.9, filed on April 26, 2023, entitled “A liquid epoxy molding compound and its preparation method,” the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present disclosure relates to the field of microelectronic packaging materials, and in particular to a liquid epoxy molding compound and a preparation method thereof. Background Art
[0004] As electronic products become increasingly miniaturized, the semiconductor encapsulation structures used to package them are also becoming thinner and lighter. Traditional packaging materials typically use epoxy molding compounds, but these cannot meet the stringent requirements of miniaturization, such as the shortened spacing between metal leads and the reduced thickness of packaged devices. Liquid epoxy encapsulant represents the third revolutionary evolution in microelectronics packaging technology and is a key material for globular array arrays and chip-scale packages. It is primarily composed of a low-viscosity liquid alicyclic epoxy resin, spherical silica powder, an epoxy curing agent and accelerator, a silica powder surface treatment agent, and other functional additives, prepared through appropriate processes. Due to surface tension and intermolecular forces during the molding process, the edges of electronic products encapsulated with this epoxy molding compound can warp to varying degrees. This is particularly true for encapsulated chips, where excessive warpage can render the encapsulated electronic product unusable.
[0005] Calculated based on the warpage height of liquid epoxy molding compound (7.5cm×2.5cm×0.1cm), when the warpage height is above 3cm, although the package thickness is appropriate, the excessive warpage will affect the use of the packaged chip. In addition, the warpage height of the packaged chip is generally required to be between 2cm and 3cm for convenient use. Packaged products with a warpage height of more than 3cm will be treated as defective products in industrial production, which indirectly increases the packaging cost. Therefore, how to provide a liquid epoxy molding compound with low warpage height to achieve low-cost packaging of electronic products is a technical problem that urgently needs to be solved.
[0006] Summary of the Invention
[0007] The purpose of the present disclosure is to provide a liquid epoxy molding compound and a preparation method thereof, so as to solve the technical problem of excessively high warpage height of liquid epoxy molding compounds in the prior art.
[0008] According to the first aspect of the present disclosure, a liquid epoxy molding compound is provided, in which the raw materials include, by mass fraction: inorganic silicon filler: 83% to 88%, naphthalene-type epoxy resin: 5% to 10%, anhydride curing agent: 5% to 10% and accelerator: 0.1% to 0.5%; wherein, the particle size of the inorganic silicon filler is less than 50μm to 100μm, accounting for 99%.
[0009] According to the second aspect of the present disclosure, a method for preparing the liquid epoxy molding compound described in the first aspect is provided, comprising: mixing the naphthalene-type epoxy resin, the curing agent, the accelerator and the inorganic silicon filler, and premixing to obtain a mixture; grinding the mixture to a target particle size, and then performing vacuum degassing to obtain a liquid epoxy molding compound. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] FIG1 shows a schematic diagram of a process for preparing a liquid epoxy molding compound according to some embodiments of the present disclosure;
[0011] FIG2 is a schematic diagram showing a method for testing warpage height according to some embodiments of the present disclosure;
[0012] FIG3 shows a scanning electron microscope image of silicon dioxide with a D99 of 75 μm provided in Comparative Example 1 of the present disclosure. DETAILED DESCRIPTION
[0013] The present disclosure will be described in detail below with reference to specific embodiments and examples, and the advantages and various effects of the present disclosure will be more clearly presented. Those skilled in the art will understand that these specific embodiments and examples are used to illustrate the present disclosure, not to limit the present disclosure. Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as having the meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present disclosure belongs. If there is a conflict, the present specification takes precedence. Unless otherwise specifically stated, the various raw materials, reagents, instruments and equipment used in the present disclosure can be purchased commercially or can be obtained by existing methods. The various embodiments of the present disclosure may be presented in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be understood as a rigid limitation on the scope of the present disclosure; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within the range. For example, it should be considered that the description of a range from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any quoted numbers (fractions or integers) within the indicated range. In this disclosure, unless otherwise stated, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of this disclosure, the terms "including", "comprising" and the like mean "including but not limited to". Moreover, the terms "including", "comprising" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device comprising a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply the existence of any such actual relationship or order between these entities or operations. In this document, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. For an association relationship of more than three associated objects described with "and / or", it means that any one of the three associated objects can exist alone, or at least two of them can exist at the same time. For example, for A, and / or B, and / or C, it can mean that any one of A, B, and C exists alone, or any two of them exist at the same time, or three of them exist at the same time. In this document, "at least one" means one or more, and "more" means two or more."At least one," "at least one of the following," or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c," or "at least one of a, b, and c," can all mean: a, b, c, a~b (i.e., a and b), a~c, b~c, or a~b~c, where a, b, and c can each be single or plural.
[0014] The present disclosure provides a liquid epoxy molding compound. The raw materials of the liquid epoxy molding compound include, by mass fraction, 83% to 88% of an inorganic silicon filler, 5% to 10% of a naphthalene-type epoxy resin, 5% to 10% of an anhydride curing agent, and 0.1% to 0.5% of an accelerator. The inorganic silicon filler has a particle size of less than 50 μm to 100 μm, accounting for 99%.
[0015] The positive effect of controlling the mass fraction of inorganic silicone fillers to 83% to 88% is that within this mass fraction range, the inorganic silicone fillers can reduce the shrinkage of the liquid epoxy molding compound, impart appropriate mechanical properties and thermal conductivity, and reduce the expansion coefficient of the liquid epoxy molding compound. The positive effect of controlling the mass fraction of naphthalene epoxy resin to 5% to 10% is that, as a material matrix, naphthalene epoxy resin has relatively high rigidity and, after curing, has a higher storage modulus than other epoxy resins, thereby improving the mechanical properties of the liquid epoxy molding compound. The positive effect of controlling the mass fraction of anhydride curing agent to 5% to 10% is that within this mass fraction range, the curing effect of the anhydride curing agent is maximized, thereby achieving rapid solidification of the liquid epoxy molding compound from liquid to solid, forming a packaging structure that meets the desired warpage height. The positive effect of an accelerator mass fraction of 0.1% to 0.5% is that within this mass fraction range, it can catalyze the rapid curing of naphthalene-based epoxy resin, thereby improving the curing effect of liquid epoxy molding compound. The positive effect of controlling the particle size of inorganic silicone fillers to less than 50μm to 100μm, accounting for 99%, is that the degree of warpage of liquid epoxy molding compound is related to its thermal expansion coefficient, and the smaller the thermal expansion coefficient, the smaller the warpage. Therefore, controlling the specific particle size of inorganic silicone fillers can effectively reduce the thermal expansion coefficient of liquid epoxy molding compound, thereby reducing the degree of warpage of the package structure formed after curing.
[0016] In some embodiments, the inorganic silicon-based filler includes inorganic silica.
[0017] By limiting the specific inorganic silicon fillers, on the one hand, the mechanical properties and heat resistance of the liquid epoxy molding compound are improved by inorganic silica, and on the other hand, the gaps between the particles are reduced by the fine particles of inorganic silica, thereby reducing the thermal expansion coefficient of the liquid epoxy molding compound, and obtaining a liquid epoxy molding compound that meets the expected warpage height.
[0018] In some embodiments, the naphthalene-based epoxy resin includes 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate.
[0019] By controlling the specific naphthalene-type epoxy resin, on the one hand, 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexyl carboxylate can evenly disperse inorganic silicones, and on the other hand, the naphthalene-type epoxy resin can be combined with a curing agent to achieve rapid curing of the liquid epoxy molding compound.
[0020] In some embodiments, the anhydride curing agent includes tetrahydrophthalic anhydride.
[0021] Defining a specific anhydride curing agent can further improve the curing effect, achieve rapid curing of the liquid epoxy molding compound, and form a packaging structure that meets the expected warpage height.
[0022] In some embodiments, the accelerator includes 2-ethyl-4-methylimidazole.
[0023] The specific accelerator is limited to promote the effect of catalyzing the rapid curing of naphthalene-type epoxy resin, and the accelerator can only react at a certain temperature, thereby enabling the liquid epoxy molding compound to be quickly cured while ensuring its convenience in use.
[0024] Referring to Figure 1, the present disclosure provides a method for preparing the liquid epoxy molding compound, the method comprising: S1. mixing the naphthalene-type epoxy resin, the curing agent, the accelerator and the inorganic silicon filler, and premixing to obtain a mixture; S2. grinding the mixture to a target particle size, and then performing vacuum degassing to obtain the liquid epoxy molding compound.
[0025] By premixing and then grinding, the particle size of the inorganic silicon filler can be further refined, thereby further reducing the thermal expansion coefficient of the liquid epoxy molding compound, and thus further reducing the warpage height of the package structure formed by the liquid epoxy molding compound. This method is a method for preparing the above-mentioned liquid epoxy molding compound. The specific composition and specific ratio of the liquid epoxy molding compound can be referred to the above-mentioned embodiments. Since this method adopts some or all of the technical solutions of the above-mentioned embodiments, it at least has all the beneficial effects brought about by the technical solutions of the above-mentioned embodiments, and will not be further described here.
[0026] In some embodiments, the premixing includes premixing in a manner combining a first revolution stirring and a first self-rotation stirring; the rotation speed of the first revolution stirring is 800rpm to 1400rpm; and / or, the rotation speed of the first self-rotation stirring is 500rpm to 1000rpm; and / or, the premixing time is 150s to 300s.
[0027] Controlling the speed of the first revolution stirring and the speed of the first rotation stirring in the premixing stage, and controlling the specific time of premixing at the same time, can promote the mixing degree of the raw materials, so that the inorganic silicon filler is evenly distributed in the liquid epoxy molding compound, and can promote the effect of the inorganic silicon filler in reducing the thermal expansion coefficient of the liquid epoxy molding compound.
[0028] In some embodiments, the target particle size is 25 μm to 50 μm.
[0029] Controlling the specific target particle size not only further reduces the particle size of the inorganic silicon filler, but also allows the inorganic silicon filler to reduce the thermal expansion coefficient of the liquid epoxy molding compound. A three-roller grinding machine is used for grinding, with the gap between the three rollers set to 50μm to 100μm at the inlet and 25μm to 50μm at the outlet. This allows the particle size of the inorganic silicon filler entering the grinding stage to be within the range of 50μm to 100μm, thus preventing the presence of large particles of inorganic silicon filler in the liquid epoxy molding compound, which would affect the inorganic silicon filler's ability to reduce the thermal expansion coefficient of the liquid epoxy molding compound.
[0030] In some embodiments, the vacuum degree of the vacuum degassing is ≤100 kPa.
[0031] By controlling the specific vacuum degree of vacuum degassing, the presence of bubbles in the formed liquid epoxy molding compound can be reduced or even avoided, so as to prevent the bubbles from affecting the distribution of the inorganic silicon filler, thereby enabling the inorganic silicon filler to reduce the thermal expansion coefficient of the liquid epoxy molding compound.
[0032] In some embodiments, the vacuum degassing includes degassing by combining a second orbital stirring and a second self-rotation stirring; the rotation speed of the second orbital stirring is 800rpm~1400rpm; and / or, the rotation speed of the second self-rotation stirring is 80rpm~140rpm; and / or, the time of the vacuum degassing is 60s~90s.
[0033] Controlling the specific second revolution stirring speed and the second rotation stirring speed during vacuum degassing, and controlling the vacuum degassing time at the same time, can not only reduce the bubbles in the formed liquid epoxy molding compound by stirring, but also make the various components mix evenly, and can promote the effect of inorganic silicon fillers in reducing the thermal expansion coefficient of the liquid epoxy molding compound.
[0034] The present disclosure will be further described below with reference to specific examples. It should be understood that these examples are intended to illustrate the present disclosure only and are not intended to limit the scope of the present disclosure. Experimental methods in the following examples where specific conditions are not specified are generally measured in accordance with national standards. If no corresponding national standards are available, the methods were performed in accordance with commonly used international standards, conventional conditions, or conditions recommended by the manufacturer.
[0035] Example 1: The raw materials of the liquid epoxy molding compound include, by mass fraction, 86% silicon dioxide, 7% 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, 7% tetrahydrophthalic anhydride, and 0.3% 2-ethyl-4-methylimidazole; wherein, 99% of the inorganic silicon filler has a particle size of less than 75 μm. A scanning electron microscope image of the silicon dioxide is shown in FIG4 . The specific steps for preparing the above-mentioned liquid epoxy molding compound are as follows: 1. Ingredients: Add the raw materials of each component into the mixing cup; 2. Premixing: Place the mixing cup containing the ingredients into the blender and stir evenly, with an orbital speed of 1000 rpm, an autorotation speed of 800 rpm, and a stirring time of 200 s; 3. Grinding: Add the stirred premixed material to the three-roller drum, with a gap of 100 μm between the feed port of the three rollers and a gap of 50 μm between the discharge port; 4. Degassing: Place the mixing cup containing the ground material into the blender for degassing, with a vacuum degree of -100 kPa, an orbital speed of 1000 rpm, an autorotation speed of 100 rpm, and a stirring time of 80 s.
[0036] Example 2: Example 2 is compared with Example 1. The difference between Example 2 and Example 1 is that, calculated by mass fraction, the raw materials of the liquid epoxy molding compound include: silicon dioxide: 86%, 3,4-epoxycyclohexylmethyl-3', 4'-epoxycyclohexylcarboxylate: 7%, tetrahydrophthalic anhydride: 7% and 2-ethyl-4-methylimidazole: 0.3%; among which, the particle size of the inorganic silicon filler is less than 75 μm, accounting for 99%. The specific steps for preparing the above-mentioned liquid epoxy molding compound are as follows: 1. Ingredients: Add the raw materials of each component into the mixing cup; 2. Premixing: Place the mixing cup containing the ingredients into the blender and stir evenly, with an orbital speed of 1000 rpm, an autorotation speed of 800 rpm, and a stirring time of 200 s; 3. Grinding: Add the stirred premixed material to a three-roller drum, with a gap of 60 μm between the feed port of the three rollers and a gap of 30 μm between the discharge port; 4. Degassing: Place the mixing cup containing the ground material into the blender for degassing, with a vacuum degree of -100 kPa, an orbital speed of 1000 rpm, an autorotation speed of 100 rpm, and a stirring time of 80 s.
[0037] Comparative Example 1: Comparative Example 1 is compared with Example 1. The difference between Comparative Example 1 and Example 1 is that, by mass fraction, the raw materials of the liquid epoxy molding compound include: silicon dioxide: 86%, 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate: 7%, tetrahydrophthalic anhydride: 7% and 2-ethyl-4-methylimidazole: 0.3%; wherein 99% of the inorganic silicon filler has a particle size of 75 μm. The specific steps for preparing the above-mentioned liquid epoxy molding compound are as follows: 1. Ingredients: Add the raw materials of each component into the mixing cup; 2. Premixing: Place the mixing cup containing the ingredients into the blender and stir evenly, with an orbital speed of 1000 rpm, an autorotation speed of 800 rpm, and a stirring time of 200 s; 3. Grinding: Add the stirred premixed material to the three-roller drum, with a gap of 200 μm between the feed port of the three rollers and a gap of 100 μm between the discharge port; 4. Degassing: Place the mixing cup containing the ground material into the blender for degassing, with a vacuum degree of -100 kPa, an orbital speed of 1000 rpm, an autorotation speed of 100 rpm, and a stirring time of 80 s.
[0038] Comparative Example 2: Comparative Example 2 is compared with Example 1. The difference between Comparative Example 2 and Example 1 is that, calculated by mass fraction, the raw materials of the liquid epoxy molding compound include: silicon dioxide: 86%, 3,4-epoxycyclohexylmethyl-3', 4'-epoxycyclohexylcarboxylate: 7%, tetrahydrophthalic anhydride: 7% and 2-ethyl-4-methylimidazole: 0.3%; among which, the particle size of the inorganic silicon filler is less than 75 μm, accounting for 99%. The specific steps for preparing the above-mentioned liquid epoxy molding compound are as follows: 1. Ingredients: Add the raw materials of each component into the mixing cup; 2. Premixing: Place the mixing cup containing the ingredients into the blender and stir evenly, with an orbital speed of 1000 rpm, an autorotation speed of 800 rpm, and a stirring time of 200 s; 3. Grinding: Add the stirred premixed material to the three-roller drum, with a gap of 150 μm between the feed port of the three rollers and a gap of 75 μm between the discharge port; 4. Degassing: Place the mixing cup containing the ground material into the blender for degassing, with a vacuum degree of -100 kPa, an orbital speed of 1000 rpm, an autorotation speed of 100 rpm, and a stirring time of 80 s.
[0039] Comparative Example 3: Comparative Example 3 is compared with Example 1. The difference between Comparative Example 3 and Example 1 is that, calculated by mass fraction, the raw materials of the liquid epoxy molding compound include: silicon dioxide: 86%, 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate: 7%, tetrahydrophthalic anhydride: 7% and 2-ethyl-4-methylimidazole: 0.3%; wherein, 50% of the particle size of the inorganic silicon filler is 75 μm. The specific steps for preparing the above-mentioned liquid epoxy molding compound are as follows: 1. Ingredients: Add the raw materials of each component into the mixing cup; 2. Premixing: Place the mixing cup containing the ingredients into the blender and stir evenly, with an orbital speed of 1000 rpm, an autorotation speed of 800 rpm, and a stirring time of 200 s; 3. Grinding: Add the stirred premixed material to a three-roller drum, with a gap of 10 μm between the feed port of the three rollers and a gap of 5 μm between the discharge port; 4. Degassing: Place the mixing cup containing the ground material into the blender for degassing, with a vacuum degree of -100 kPa, an orbital speed of 1000 rpm, an autorotation speed of 100 rpm, and a stirring time of 80 s.
[0040] Related experiments and effect data: Warpage test method: The liquid epoxy molding compound obtained in each embodiment and comparative example is evenly scraped on a glass slide (7.5cm×2.5cm×0.1cm), the material thickness is 0.1cm, and the curing condition is 130℃ / 1h. After cooling, the height of the warped end of the glass slide is measured, which is the warpage height, as shown in Figure 2. The measured results are shown in Table 1. Thermal expansion coefficient test method: Reference standard: ASTM E831-2019, take a sample that is completely cured at 150℃ for 1h, and prepare a test sample with a size of 5mm*5mm*2mm. The thermal expansion coefficient of the sample was measured using TMA (compression mode); TMA parameter settings were: preload force: 0.05 N, first scan: room temperature to 250°C (heating rate 10°C / min), second scan: room temperature to 250°C (heating rate 10°C / min), and data from the second heating period curve was collected. The CTE1 temperature range was 40°C to 100°C, and the CTE2 temperature range was 150°C to 200°C. The measured results are shown in Table 1. Particle size measurement method: A laser particle size analyzer was used, and the measured results are shown in Table 1.
[0041] Table 1 Test results of liquid epoxy molding compound obtained in each embodiment and comparative example
[0042] As shown in Table 1, the present application can effectively reduce the thermal expansion coefficient of the liquid epoxy molding compound during the molding stage. Since the degree of warping of the liquid epoxy molding compound is related to the magnitude of its thermal expansion coefficient, and the smaller the thermal expansion coefficient, the smaller the warping degree, the warping height of the liquid epoxy molding compound can be reduced, and the warping height can be ensured to be close to or equal to 0 mm. At the same time, in conjunction with Figure 3, it can be seen that the refined silica particles have a larger specific surface area and a larger contact surface with the epoxy resin, which makes the silica and epoxy resin bond more tightly, thereby reducing the material's thermal expansion coefficient.
[0043] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages: (1) The embodiments of the present application provide a liquid epoxy molding compound. Compared with the components of traditional liquid epoxy molding compounds, the large particles of silicon dioxide are ground into small particles of silicon dioxide, which can reduce the increase in the length of the liquid epoxy molding compound in a certain direction per unit temperature during the molding stage, thereby effectively reducing the thermal expansion coefficient of the liquid epoxy molding compound during the molding stage and effectively reducing the warpage height of the liquid epoxy molding compound. (2) The embodiments of the present application provide a liquid epoxy molding compound. In the process of forming a packaging structure, not only can a low-warpage packaging structure be obtained, but also production costs can be reduced and the packaging success rate of electronic products can be improved.
[0044] The foregoing description is intended only to provide specific embodiments of the present disclosure, intended to enable those skilled in the art to understand and implement the present disclosure. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present disclosure. Therefore, the present disclosure is not to be limited to the embodiments shown herein, but is to be construed in the broadest manner consistent with the principles and novel features claimed herein.
Claims
1. A liquid epoxy molding compound, wherein the raw materials of the liquid epoxy molding compound include, by mass fraction: Inorganic silicon filler: 83% to 88%, naphthalene epoxy resin: 5% to 10%, anhydride curing agent: 5% to 10% and accelerator: 0.1% to 0.5%; Among them, the particle size of the inorganic silicon filler is less than 50 μm to 100 μm, accounting for 99%.
2. The liquid epoxy molding compound according to claim 1, wherein: The inorganic silicon-based filler includes inorganic silicon dioxide.
3. The liquid epoxy molding compound according to claim 1, wherein: The naphthalene-based epoxy resin includes 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate.
4. The liquid epoxy molding compound according to claim 1, wherein: The acid anhydride curing agent includes tetrahydrophthalic anhydride.
5. The liquid epoxy molding compound according to claim 1, wherein: The accelerator includes 2-ethyl-4-methylimidazole.
6. A method for preparing the liquid epoxy molding compound according to any one of claims 1 to 5, comprising: Mixing the naphthalene epoxy resin, the curing agent, the accelerator and the inorganic silicon filler, and premixing to obtain a mixture; as well as The mixed material is ground to a target particle size, and then vacuum degassing is performed to obtain a liquid epoxy molding compound.
7. The method according to claim 6, wherein: The premixing includes premixing in a manner of combining first revolution stirring and first rotation stirring; wherein, The rotation speed of the first revolution stirring is 800 rpm to 1400 rpm, the rotation speed of the first rotation stirring is 500 rpm to 1000 rpm, and the premixing time is 150 s to 300 s.
8. The method according to claim 6, wherein: The target particle size is 25 μm to 50 μm.
9. The method according to claim 6, wherein: The vacuum degree of the vacuum degassing is ≤100 kPa.
10. The method according to claim 6, wherein: The vacuum degassing comprises degassing in a manner of combining a second revolution stirring and a second rotation stirring; wherein, The rotation speed of the second revolution stirring is 800 rpm to 1400 rpm, the rotation speed of the second rotation stirring is 80 rpm to 140 rpm, and the time of the vacuum degassing is 60 s to 90 s.
Citation Information
Patent Citations
Epoxy resin composition for electronic packaging and preparation method thereof
CN109486100A
Encapsulating epoxy resin composition for ball grid array package, cured epoxy resin object, and electronic component / device
CN111527146A
Resin composition and application thereof
CN111909486A
Chip packaging material, chip packaging structure and packaging method
CN113604184A
Mold sealing adhesive for chip packaging and packaging structure
CN113621332A