Aluminum-magnesium-zirconium co-doped tricobalt tetraoxide, preparation method therefor and use thereof
By co-doping aluminum, magnesium and zirconium with cobalt tetraoxide, the problem of uneven distribution of doping elements is solved, and a lithium cobalt oxide cathode material with high capacity and high rate performance is achieved to meet the demand for increasing the energy density of lithium-ion batteries.
Patent Information
- Application Number
- PCT/CN2023/111984
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-23
- Filing Date
- 2023-08-09
- Publication Date
- 2024-10-31
Smart Images

Figure CN2023111984_31102024_PF_FP_ABST
Abstract
Description
Aluminum-magnesium-zirconium co-doped cobalt oxide and its preparation method and application Technical Field
[0001] The present application belongs to the technical field of lithium-ion batteries and relates to aluminum-magnesium-zirconium co-doped cobalt oxide and its preparation method and application. Background Art
[0002] Lithium cobalt oxide is widely used as a positive electrode material for lithium-ion batteries in the 3C consumer market due to its high compaction density and good cycle stability. With the in-depth study of lithium cobalt oxide, the charging voltage of most commercial lithium cobalt oxide materials can reach 4.45V or higher, and its specific capacity reaches 180mAh / g. However, with the rapid development of 3C digital products, in order to improve the electrical performance of lithium cobalt oxide materials, the structural stability of lithium cobalt oxide during the charge and discharge process can be improved by doping its precursor, cobalt tetroxide, so as to release more lithium ions, thereby increasing the cutoff voltage of lithium cobalt oxide and improving the specific capacity of lithium-ion batteries. The commonly used cobalt tetroxide bulk doping element on the market is aluminum, which improves the stability of lithium cobalt oxide materials under high voltage through the "pillar" effect of aluminum atoms. For example, CN112993243A discloses a method for preparing high-density aluminum-doped cobalt oxide, which includes the following steps: 1) adding a cobalt salt solution, an alkaline solution, and an oxidant to a reactor for reaction. When the D50 reaches 2.0-2.5 μm, adding an aluminum-cobalt solution to the reaction system for reaction. When the D50 reaches 3.5-4.0 μm, the addition of the aluminum-cobalt solution is stopped and the reaction is continued while maintaining other conditions unchanged until the D50 reaches the desired particle size, at which point the reaction is stopped to obtain an aluminum-containing cobalt oxyhydroxide slurry; 2) aging, dehydrating, washing, and drying the aluminum-containing cobalt oxyhydroxide slurry to obtain an aluminum-containing cobalt oxyhydroxide powder; and 3) calcining the aluminum-containing cobalt oxyhydroxide powder to obtain the target product. However, as the amount of inert element aluminum doping increases, its specific capacity is limited.
[0003] In order to obtain high-capacity lithium cobalt oxide materials, researchers began to try to dope the cobalt oxide body with multiple elements. For example, CN110534719A discloses a method for preparing aluminum-magnesium-nickel-manganese-doped spherical cobalt oxide. By controlling the pH and stirring intensity to control the synthesis reaction rate and the dispersion of the primary particles, the doping elements in the synthesized cobalt oxyhydroxide are evenly distributed. The lithium cobalt oxide material thus synthesized has a first-week discharge capacity of 179 mAh / g at a 1C rate. However, its four-element doping places high demands on the quality control of the element content of the product, and the physical state of each element in the cobalt oxyhydroxide is not characterized, which brings potential risk iterations of product instability and also puts higher requirements on the energy density of lithium-ion batteries.
[0004] Therefore, how to obtain doped cobalt tetroxide with high specific capacity and uniform distribution of doping elements is a technical problem that needs to be solved urgently.
[0005] Summary of the Invention
[0006] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0007] The purpose of this application is to provide an aluminum-magnesium-zirconium co-doped cobalt oxide, its preparation method, and application. This application stabilizes the multi-element doping wet synthesis process by doping the cobalt oxide with aluminum, magnesium, and zirconium, and characterizing the physical state of the doped elements during the synthesis process. This allows for precise control at the atomic level, and by combining the advantages of Al, Mg, and Zr, the synergistic effects result in a lithium cobalt oxide positive electrode material with high capacity and high rate performance.
[0008] To achieve this goal, this application adopts the following technical solutions:
[0009] In a first aspect, an embodiment of the present application provides a method for preparing aluminum-magnesium-zirconium co-doped cobalt oxide, the preparation method comprising the following steps:
[0010] (1) adding a mixed salt solution of cobalt, aluminum, magnesium, and zirconium and a precipitant solution in parallel to perform a coprecipitation reaction, wherein during the coprecipitation reaction, sampling is performed once every target time period for XRD testing until the target particle size is reached and the reaction is stopped to obtain aluminum-magnesium-zirconium co-doped cobalt oxyhydroxide;
[0011] (2) sintering the cobalt oxyhydroxide described in step (1) to obtain the aluminum-magnesium-zirconium co-doped cobalt tetroxide;
[0012] Wherein, the mixed salt solution of cobalt, aluminum, magnesium and zirconium includes a complexing agent solution.
[0013] In the embodiment of the present application, the phase of the sample was monitored by XRD test, and the phase state was: Co2AlO4 and (Mg 0.18 Co 0.82 )(Zr 0.20 Co 1.80 )O4, there is no element segregation in the sample.
[0014] The present invention embodiment performs aluminum, magnesium and zirconium doping on the cobalt oxide body and characterizes the phase state during the synthesis of the doped elements, thereby stabilizing the wet synthesis process of multi-element doping and achieving precise control at the atomic level. By combining the advantages of Al, Mg and Zr, the conductivity of the material can be increased by doping with magnesium, and the structure can be stabilized by replacing the cobalt site with aluminum. At the same time, the large radius of the zirconium ion is used to expand the spacing of the lithium cobalt oxide layer structure, thereby improving the Li +The transmission capacity and synergistic effect achieve uniform distribution of doping elements and cobalt elements without element segregation, and obtain a small-particle structure with stable elements and uniform distribution of aluminum-magnesium-zirconium co-doped cobalt tetroxide precursor material, thereby obtaining a lithium cobalt oxide positive electrode material with high capacity and high rate performance.
[0015] In the embodiment of the present application, if the phase analysis of the sample is not performed by performing interval XRD testing, it is difficult to ensure that all doping elements are lattice-doped at the atomic level. However, through XRD testing at intervals, the process can be accurately and timely controlled so that each doping element is co-precipitated with the cobalt atoms without segregation. At the same time, in the embodiment of the present application, the three elements of aluminum, magnesium and zirconium must be doped at the same time. Without any of the three elements, the improvement of specific capacity and the enhancement of cycle stability cannot be achieved.
[0016] In one embodiment, the mass concentration of cobalt ions in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in step (1) is 125-135 g / L, for example, 125 g / L, 126 g / L, 127 g / L, 128 g / L, 129 g / L, 130 g / L, 131 g / L, 132 g / L, 133 g / L, 134 g / L or 135 g / L, etc.
[0017] In one embodiment, the mass concentration of aluminum ions in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in step (1) is 1.4 to 1.6 g / L, for example, 1.4 g / L, 1.43 g / L, 1.45 g / L, 1.48 g / L, 1.5 g / L, 1.53 g / L, 1.55 g / L, 1.58 g / L or 1.6 g / L, etc.
[0018] In one embodiment, the mass concentration of magnesium ions in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in step (1) is 0.65 to 0.75 g / L, for example, 0.65 g / L, 0.66 g / L, 0.67 g / L, 0.68 g / L, 0.69 g / L, 0.7 g / L, 0.71 g / L, 0.72 g / L, 0.73 g / L, 0.74 g / L or 0.75 g / L, etc.
[0019] In one embodiment, the mass concentration of zirconium ions in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in step (1) is 0.1 to 0.2 g / L, for example, 0.1 g / L, 0.11 g / L, 0.12 g / L, 0.13 g / L, 0.14 g / L, 0.15 g / L, 0.16 g / L, 0.17 g / L, 0.18 g / L, 0.19 g / L or 0.2 g / L, etc.
[0020] In the embodiments of the present application, the mass concentration range of cobalt, aluminum, magnesium and zirconium in the mixed salt solution of cobalt, aluminum, magnesium and zirconium is regulated, thereby regulating the doping amount of aluminum, magnesium and zirconium, and further regulating the role of each doping element in the electrical properties of the material; if the mass concentration of any element is not within the above range, it will lead to a decrease in electrical properties.
[0021] In one embodiment, the molar concentration of the complexing agent solution in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in step (1) is 0.1 to 2 mol / L, for example, 0.1 mol / L, 0.25 mol / L, 0.5 mol / L, 0.75 mol / L, 1 mol / L, 1.25 mol / L, 1.5 mol / L, 1.75 mol / L or 2 mol / L.
[0022] In one embodiment, the complexing agent solution includes an EDTA solution.
[0023] In one embodiment, during the coprecipitation reaction in step (1), the flow rate of the mixed salt solution of cobalt, aluminum, magnesium and zirconium is 150 to 300 L / h, for example, 150 L / h, 160 L / h, 170 L / h, 180 L / h, 190 L / h, 200 L / h, 210 L / h, 220 L / h, 230 L / h, 240 L / h, 250 L / h, 260 L / h, 270 L / h, 280 L / h, 290 L / h or 300 L / h, etc.
[0024] In one embodiment, the coprecipitation reaction in step (1) is carried out under an air atmosphere.
[0025] In one embodiment, the air flow rate is 6 to 20 m 3 / h, for example 6m 3 / h、7m 3 / h、8m 3 / h、9m 3 / h、10m 3 / h、11m 3 / h、12m 3 / h、13m 3 / h、14m 3 / h、15m 3 / h、16m 3 / h、17m 3 / h、18m 3 / h、19m 3 / h or 20m 3 / h, etc.
[0026] In one embodiment, the pH value during the coprecipitation reaction in step (1) is 9-11, for example, 9, 9.3, 9.5, 9.8, 10, 10.3, 10.5, 10.8 or 11.
[0027] In one embodiment, the reaction temperature during the coprecipitation reaction in step (1) is 50-80°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C.
[0028] In one embodiment, the stirring speed during the coprecipitation reaction in step (1) is 600-800 rpm, for example, 600 rpm, 650 rpm, 700 rpm, 750 rpm or 800 rpm.
[0029] In one embodiment, the target time period in step (1) ranges from 3 to 6 hours, such as 3 hours, 4 hours, 5 hours or 6 hours.
[0030] In the embodiment of the present application, if the target time period is too short, the result of the XRD test will not be satisfactory, resulting in a waste of test resources, while if the time period is too long, the process cannot be accurately controlled in a timely manner.
[0031] In one embodiment, the sintering temperature in step (2) is 650-850°C, for example, 650°C, 700°C, 750°C, 800°C or 850°C.
[0032] In one embodiment, the sintering time in step (2) is 3 to 6 hours.
[0033] As an optional technical solution, the preparation method includes the following steps:
[0034] (1) Add the mixed salt solution of cobalt, aluminum, magnesium and zirconium at a flow rate of 150 to 300 L / h and the precipitant solution in parallel, and add the mixed salt solution of cobalt, aluminum, magnesium and zirconium at a flow rate of 6 to 20 m / h. 3 / h in an air atmosphere, maintaining a pH value of 9-11, performing a coprecipitation reaction at a temperature of 50-80°C and a stirring speed of 600-800 rpm. During the coprecipitation reaction, sampling is performed every 3-6 hours for XRD testing until the target particle size is reached and the reaction is stopped to obtain aluminum-magnesium-zirconium co-doped cobalt oxyhydroxide.
[0035] (2) sintering the cobalt oxyhydroxide described in step (1) at 650-850° C. for 3-6 hours to obtain the aluminum-magnesium-zirconium co-doped cobalt oxide; the mass concentration of cobalt ions in the cobalt-aluminum-magnesium-zirconium mixed salt solution described in step (1) is 125-135 g / L; the mass concentration of aluminum ions in the cobalt-aluminum-magnesium-zirconium mixed salt solution described in step (1) is 1.4-1.6 g / L; the mass concentration of magnesium ions in the cobalt-aluminum-magnesium-zirconium mixed salt solution described in step (1) is 0.65-0.75 g / L; the mass concentration of zirconium ions in the cobalt-aluminum-magnesium-zirconium mixed salt solution described in step (1) is 0.1-0.2 g / L; the molar concentration of the complexing agent solution in the cobalt-aluminum-magnesium-zirconium mixed salt solution described in step (1) is 0.1-2 mol / L.
[0036] In a second aspect, an embodiment of the present application provides an aluminum-magnesium-zirconium co-doped cobalt tetroxide, wherein the aluminum-magnesium-zirconium co-doped cobalt tetroxide is prepared by the preparation method of aluminum-magnesium-zirconium co-doped cobalt tetroxide as described in the first aspect.
[0037] In one embodiment, the tap density of the aluminum-magnesium-zirconium co-doped cobalt oxide is 2.5 to 2.7 g / cm 3 , for example 2.5g / cm 3 , 2.53g / cm 3 , 2.55g / cm 3 , 2.58g / cm 3 , 2.6g / cm 3 , 2.63g / cm 3 , 2.65g / cm 3 , 2.68g / cm 3 or 2.7g / cm 3 wait.
[0038] In one embodiment, the specific surface area of the aluminum-magnesium-zirconium co-doped cobalt oxide is 0.9 to 1.2 m 2 / g, for example 0.9m 2 / g、1m 2 / g, 1.1m 2 / g or 1.2m 2 / g, etc.
[0039] In a third aspect, an embodiment of the present application provides a lithium cobalt oxide positive electrode material, which is obtained by mixing and sintering a lithium source and cobalt oxide co-doped with aluminum magnesium zirconium as described in the second aspect.
[0040] In a fourth aspect, an embodiment of the present application further provides a lithium-ion battery, wherein the lithium-ion battery comprises the lithium cobalt oxide positive electrode material as described in the third aspect.
[0041] Compared with the prior art, this application has the following beneficial effects:
[0042] This application stabilizes the wet synthesis process of multi-element doping by doping the cobalt oxide body with aluminum, magnesium and zirconium, and characterizes the phase state during the synthesis of the doped elements, achieving precise control at the atomic level. By combining the advantages of Al, Mg and Zr, the conductivity of the material can be increased by doping with magnesium, and the structure can be stabilized by replacing the cobalt site with aluminum. At the same time, the large radius of the zirconium ion is used to expand the spacing of the lithium cobalt oxide layer structure to increase the Li + The transmission capacity and synergistic effect achieve uniform distribution of doping elements and cobalt elements without element segregation, and obtain a small-particle structure with stable elements and uniform distribution of aluminum-magnesium-zirconium co-doped cobalt tetroxide precursor material, thereby obtaining a lithium cobalt oxide positive electrode material with high capacity and high rate performance.
[0043] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.
[0045] FIG1 is an XRD pattern of aluminum-magnesium-zirconium co-doped cobalt oxide provided in Example 1. DETAILED DESCRIPTION
[0046] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.
[0047] Example 1
[0048] This embodiment provides a method for preparing aluminum-magnesium-zirconium co-doped cobalt oxide, the preparation method being as follows:
[0049] (1) preparing a mixed solution of doped cobalt chloride with a cobalt ion concentration of 130 g / L, an aluminum ion concentration of 1.5 g / L, a magnesium ion concentration of 0.7 g / L, and a zirconium ion concentration of 0.15 g / L, then adding 0.5 mol / L of chelating agent EDTA to the cobalt solution and mixing thoroughly (a mixed salt solution of cobalt, aluminum, magnesium, and zirconium);
[0050] (2) adding pure water (the volume of water is 40% of the volume of the reactor) to the reactor, adjusting the pH value to 9.8, and simultaneously adding the cobalt mixed solution and 10 mol / L sodium hydroxide solution to the reactor under an air pressure of 0.35 MPa. The temperature is 50° C. and the rotation speed is 650 rpm to carry out a coprecipitation reaction. During the reaction process, samples are taken and dried every 4 hours for XRD characterization to monitor the phase state of the doping element. When the phase characterization results are consistent with FIG1 , the coprecipitation reaction can be continued. When the particle size of the aluminum-magnesium-zirconium cobalt oxyhydroxide is 3.5 μm, the reactor is stopped, washed, and dried to obtain aluminum-magnesium-zirconium co-doped cobalt oxyhydroxide; and calcined.
[0051] (3) The aluminum-magnesium-zirconium co-doped cobalt oxyhydroxide was sintered in a muffle furnace at 800° C. for 3 h to obtain the aluminum-magnesium-zirconium co-doped cobalt tetroxide (its final phase state is also shown in FIG1 ).
[0052] Example 2
[0053] This embodiment provides a method for preparing aluminum-magnesium-zirconium co-doped cobalt oxide, the preparation method being as follows:
[0054] (1) preparing a mixed solution of doped cobalt chloride with a cobalt ion concentration of 125 g / L, an aluminum ion concentration of 1.4 g / L, a magnesium ion concentration of 0.65 g / L, and a zirconium ion concentration of 0.1 g / L, then adding 0.1 mol / L of a complexing agent EDTA to the cobalt solution and mixing thoroughly to obtain a mixed salt solution of cobalt, aluminum, magnesium, and zirconium;
[0055] (2) adding pure water (the volume of water is 40% of the volume of the reactor) to the reactor, adjusting the pH value to 10.5, and simultaneously adding the cobalt mixed solution and 10 mol / L sodium hydroxide solution to the reactor under an air pressure of 0.35 MPa, at a temperature of 60° C. and a rotation speed of 600 rpm, to carry out a coprecipitation reaction; sampling and drying every 3 hours during the reaction process to perform XRD characterization and monitor the phase state of the doping element; the coprecipitation reaction can be continued when the phase characterization results are consistent with FIG1 ; when the particle size of the aluminum-magnesium-zirconium cobalt oxyhydroxide is 3.5 μm, stopping the reactor, washing, and drying to obtain aluminum-magnesium-zirconium co-doped cobalt oxyhydroxide; and calcining;
[0056] (3) The aluminum-magnesium-zirconium co-doped cobalt oxyhydroxide is sintered at 650° C. for 6 h in a muffle furnace to obtain the aluminum-magnesium-zirconium co-doped cobalt tetroxide.
[0057] Example 3
[0058] This embodiment provides a method for preparing aluminum-magnesium-zirconium co-doped cobalt oxide, the preparation method being as follows:
[0059] (1) preparing a mixed solution of doped cobalt chloride with a cobalt ion concentration of 135 g / L, an aluminum ion concentration of 1.6 g / L, a magnesium ion concentration of 0.75 g / L, and a zirconium ion concentration of 0.2 g / L, then adding 2 mol / L of chelating agent EDTA to the cobalt solution and mixing thoroughly (a mixed salt solution of cobalt, aluminum, magnesium, and zirconium);
[0060] (2) adding pure water (the volume of water is 40% of the volume of the reactor) to the reactor, adjusting the pH value to 9, and simultaneously adding the cobalt mixed solution and 10 mol / L sodium hydroxide solution to the reactor under an air pressure of 0.35 MPa, at a temperature of 50° C. and a rotation speed of 800 rpm, to carry out a coprecipitation reaction; sampling and drying every 6 hours during the reaction process to perform XRD characterization and monitor the phase state of the doping element; the coprecipitation reaction can be continued when the phase characterization results are consistent with FIG1 ; when the particle size of the aluminum-magnesium-zirconium cobalt oxyhydroxide is 3.5 μm, stopping the reactor, washing, and drying to obtain aluminum-magnesium-zirconium co-doped cobalt oxyhydroxide; and calcining;
[0061] (3) The aluminum-magnesium-zirconium co-doped cobalt oxyhydroxide is sintered at 700° C. for 4 hours in a muffle furnace to obtain the aluminum-magnesium-zirconium co-doped cobalt tetroxide.
[0062] Example 4
[0063] The difference between this embodiment and embodiment 1 is that the mass concentration of aluminum ions in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in this embodiment is 1.2 g / L.
[0064] The rest of the preparation methods and parameters were the same as those in Example 1.
[0065] Example 5
[0066] The difference between this embodiment and embodiment 1 is that the mass concentration of magnesium ions in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in this embodiment is 1 g / L.
[0067] The rest of the preparation methods and parameters were the same as those in Example 1.
[0068] Example 6
[0069] The difference between this embodiment and embodiment 1 is that the mass concentration of zirconium ions in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in this embodiment is 0.05 g / L.
[0070] The rest of the preparation methods and parameters were the same as those in Example 1.
[0071] Comparative Example 1
[0072] The difference between this comparative example and Example 1 is that magnesium is not doped in this comparative example.
[0073] The rest of the preparation methods and parameters were the same as those in Example 1.
[0074] Comparative Example 2
[0075] The difference between this comparative example and Example 1 is that zirconium is not doped in this comparative example.
[0076] The rest of the preparation methods and parameters were the same as those in Example 1.
[0077] The cobalt oxide precursor materials provided in Examples 1-6 and Comparative Examples 1-2 were mixed with lithium hydroxide and sintered to obtain a lithium cobalt oxide positive electrode material. The lithium cobalt oxide positive electrode material, a conductive agent, and a binder were mixed to obtain a positive electrode slurry. The slurry was coated on aluminum foil by a coater and dried at low temperature. A button battery was obtained using a lithium sheet as a counter electrode and lithium hexafluorophosphate, EC, and DMC as electrolytes.
[0078] The button cells provided in Examples 1-6 and Comparative Examples 1-2 were subjected to electrochemical performance testing using the following test conditions: The assembled CR2032 button cell cases were tested using a CT3001A blue battery test system. The test voltage ranged from 3.0 to 4.58 V at room temperature (25°C), with discharge rates of 0.2C, 0.5C, 1.0C, and 2.0C, respectively; and at high temperature (45°C), with a test voltage range of 3.0 to 4.58 V. The test results are shown in Table 1.
[0079] Table 1
[0080] It can be seen from the data results of Examples 1 and 4-6 that when the mass concentration range of cobalt, aluminum, magnesium and zirconium in the mixed salt solution of cobalt, aluminum, magnesium and zirconium provided in the present application is not within the preferred range, it is not conducive to improving the specific capacity or maintaining the cycle stability.
[0081] From the data results of Example 1 and Comparative Examples 1-2, it can be seen that the three elements of aluminum, magnesium and zirconium in this application work synergistically and none of them can be missing. Without any one of them, it is impossible to obtain a lithium cobalt oxide material precursor with excellent specific capacity and cyclability.
[0082] In summary, this application stabilizes the wet synthesis process of multi-element doping by doping the cobalt oxide body with aluminum, magnesium and zirconium, and characterizes the phase state during the synthesis of the doped elements, thereby achieving precise control at the atomic level. By combining the advantages of Al, Mg and Zr, the conductivity of the material can be increased by doping with magnesium, and the structure can be stabilized by replacing the cobalt site with aluminum. At the same time, the large radius of the zirconium ion is used to expand the spacing of the lithium cobalt oxide layer structure to improve Li +The transmission capacity and synergistic effect achieve uniform distribution of doping elements and cobalt elements without element segregation, and obtain a small-particle structure with stable elements and uniform distribution of aluminum-magnesium-zirconium co-doped cobalt tetroxide precursor material, thereby obtaining a lithium cobalt oxide positive electrode material with high capacity and high rate performance.
[0083] The applicant declares that the above is only a specific implementation method of the present application, but the protection scope of the present application is not limited thereto. Technical personnel in the relevant technical field should understand that any changes or substitutions that can be easily thought of by technical personnel in the relevant technical field within the technical scope disclosed in this application fall within the protection scope and disclosure scope of this application.
Claims
1. A method for preparing aluminum-magnesium-zirconium co-doped cobalt oxide, the preparation method comprising the following steps: (1) adding a cobalt, aluminum, magnesium, and zirconium mixed salt solution and a precipitant solution in parallel to perform a coprecipitation reaction, wherein during the coprecipitation reaction, sampling is performed once every target time period for XRD testing until the target particle size is reached and the reaction is stopped to obtain aluminum, magnesium, and zirconium co-doped cobalt oxyhydroxide; (2) sintering the cobalt oxyhydroxide described in step (1) to obtain the aluminum-magnesium-zirconium co-doped cobalt tetroxide; Wherein, the mixed salt solution of cobalt, aluminum, magnesium and zirconium includes a complexing agent solution.
2. The method for preparing aluminum-magnesium-zirconium co-doped cobalt oxide according to claim 1, wherein: The mass concentration of cobalt ions in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in step (1) is 125-135 g / L; Optionally, the mass concentration of aluminum ions in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in step (1) is 1.4 to 1.6 g / L; Optionally, the mass concentration of magnesium ions in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in step (1) is 0.65 to 0.75 g / L; Optionally, the mass concentration of zirconium ions in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in step (1) is 0.1 to 0.2 g / L; Optionally, the molar concentration of the complexing agent solution in the mixed salt solution of cobalt, aluminum, magnesium and zirconium in step (1) is 0.1 to 2 mol / L.
3. The method for preparing aluminum-magnesium-zirconium co-doped cobalt oxide according to claim 1 or 2, wherein: The complexing agent solution includes EDTA solution.
4. The method for preparing aluminum-magnesium-zirconium co-doped cobalt oxide according to any one of claims 1 to 3, wherein: During the coprecipitation reaction in step (1), the flow rate of the mixed salt solution of cobalt, aluminum, magnesium and zirconium is 150 to 300 L / h; Optionally, the coprecipitation reaction in step (1) is carried out under an air atmosphere; Optionally, the air flow rate is 6 to 20 m 3 / h.
5. The method for preparing aluminum-magnesium-zirconium co-doped cobalt oxide according to any one of claims 1 to 4, wherein: The pH value during the coprecipitation reaction in step (1) is 9 to 11; Optionally, the reaction temperature during the coprecipitation reaction in step (1) is 50 to 80° C.; Optionally, the stirring speed during the coprecipitation reaction in step (1) is 600-800 rpm; Optionally, the target time period in step (1) ranges from 3 to 6 hours.
6. The method for preparing aluminum-magnesium-zirconium co-doped cobalt oxide according to any one of claims 1 to 5, wherein: The sintering temperature in step (2) is 650-850° C. Optionally, the sintering time in step (2) is 3 to 6 hours.
7. The method for preparing aluminum-magnesium-zirconium co-doped cobalt oxide according to any one of claims 1 to 6, wherein: The preparation method comprises the following steps: (1) Add the mixed salt solution of cobalt, aluminum, magnesium and zirconium at a flow rate of 150 to 300 L / h and the precipitant solution in parallel, and the flow rate is 6 to 20 m 3 / h in an air atmosphere, maintaining a pH value of 9 to 11, performing a coprecipitation reaction at a temperature of 50 to 80°C and a stirring speed of 600 to 800 rpm. During the coprecipitation reaction, sampling is performed every 3 to 6 hours for XRD testing until the target particle size is reached, and the reaction is stopped to obtain aluminum-magnesium-zirconium co-doped cobalt oxyhydroxide; (2) sintering the cobalt oxyhydroxide described in step (1) at 650-850° C. for 3-6 hours to obtain the aluminum-magnesium-zirconium co-doped cobalt tetroxide; the mass concentration of cobalt ions in the cobalt-aluminum-magnesium-zirconium mixed salt solution described in step (1) is 125-135 g / L; the mass concentration of aluminum ions in the cobalt-aluminum-magnesium-zirconium mixed salt solution described in step (1) is 1.4-1.6 g / L; the mass concentration of magnesium ions in the cobalt-aluminum-magnesium-zirconium mixed salt solution described in step (1) is 0.65-0.75 g / L; the mass concentration of zirconium ions in the cobalt-aluminum-magnesium-zirconium mixed salt solution described in step (1) is 0.1-0.2 g / L; the complexing agent solution in the cobalt-aluminum-magnesium-zirconium mixed salt solution described in step (1) The molar concentration is 0.1~2mol / L.
8. A cobalt oxide co-doped with aluminum, magnesium and zirconium, wherein the cobalt oxide co-doped with aluminum, magnesium and zirconium is prepared by the method for preparing cobalt oxide co-doped with aluminum, magnesium and zirconium according to any one of claims 1 to 7.
9. The aluminum-magnesium-zirconium co-doped cobalt oxide according to claim 8, wherein: The tap density of the aluminum-magnesium-zirconium co-doped cobalt oxide is 2.5-2.7 g / cm 3 ; Optionally, the specific surface area of the aluminum-magnesium-zirconium co-doped cobalt oxide is 0.9 to 1.2 m 2 / g.
10. A lithium cobalt oxide positive electrode material, which is obtained by mixing and sintering a lithium source and the aluminum-magnesium-zirconium co-doped cobalt oxide as claimed in claim 8 or 9.
11. A lithium ion battery, comprising the lithium cobalt oxide positive electrode material according to claim 10.
Citation Information
Patent Citations
A metal oxide and preparation method
CN109004198A
Method for detecting performance of aluminum-doped cobaltosic oxide material
CN112763522A
Preparation method of magnesium-aluminum co-doped lithium cobalt oxide precursor
CN114349066A
Aluminum-magnesium-zirconium co-doped cobaltosic oxide as well as preparation method and application thereof
CN116375102A
Non-aqueous electrolyte secondary battery and charging method thereof
CN1825674A
Cited By
Mg-F co-doped cobaltosic oxide as well as preparation method and application thereof
CN121470555A