Aluminum and phosphorus co-doped heterostructure cobaltosic oxide / nickel ferrite / foamed nickel composite nano material as well as preparation method and application of aluminum and phosphorus co-doped heterostructure cobaltosic oxide / nickel ferrite / foamed nickel composite nano material
Through the co-doping of aluminum and phosphorus heterostructured cobalt tetroxide/nickel ferrate/nickel foam composite nanomaterials, the problem of slow kinetics of precious metal catalysts in electrochemical water decomposition is solved, and the electrocatalytic performance and feasibility of large-scale production is improved. , realizes high-efficiency oxygen evolution reaction in an alkaline environment.
Patent Information
- Application Number
- CN202411033515.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The high price, extremely scarce and poor durability of precious metal catalysts cannot meet the demand for large-scale hydrogen production. Especially in the slow kinetics of the oxygen analysis reaction in electrochemical water decomposition, resulting in large energy losses, which hinders the large amount of hydrogen. produce.
Design a heterostructured co-doped cobalt tetroxide/nickel ferrate/foam nickel composite nanomaterial, and change the electronic structures of Co3O4 and NiFe2O4 through aluminum and phosphorus co-doping to form a two-dimensional nanosheet layer growing on nanowires Heterostructure, improves electrocatalytic performance, and is prepared by simple hydrothermal method and low-temperature calcination method, suitable for large-scale production.
It significantly improves the intrinsic activity and conductivity of the catalyst, provides more active sites, and improves the oxygen evolution reaction activity in an alkaline environment, which is suitable for large-scale utilization and promotion.
Smart Images

Figure CN118957662A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of material preparation, and in particular to an aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nano material and a preparation method and application thereof. Background Art
[0002] Many studies have been devoted to the development of clean, sustainable and renewable energy sources. Among them, electrochemical water splitting into hydrogen and oxygen is an eco-friendly, economically feasible large-scale hydrogen production solution. Generally speaking, the overall water electrolysis process includes hydrogen evolution reaction (HER) and oxygen evolution reaction (OER). However, compared with the two-electron transfer hydrogen evolution reaction (HER), the oxygen evolution reaction (OER) involves a slower kinetics of four-electron proton coupling transfer, which is considered to be the rate-determining step of water splitting. The high overpotential of OER leads to huge energy losses, hindering the large-scale production of hydrogen. In order to improve the catalytic efficiency of electrocatalytic water splitting, it is extremely important to design highly active, low-cost and stable OER catalysts.
[0003] Currently, precious metal catalysts such as RuO2 and IrO2 have high catalytic activity for OER under alkaline conditions, but their high price, extreme scarcity and poor durability make it difficult for them to meet the huge demand for large-scale hydrogen production in the future. Studies have shown that non-precious metal compounds often show better catalytic stability and durability than carbon-based materials in harsh electrolysis environments. Three-dimensional transition metal compounds, especially spinel materials, have attracted widespread attention due to their good stability, abundant reserves, low cost, easy synthesis, and diverse structures. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of noble metal catalysts that are difficult to meet large-scale production due to their high price, extreme scarcity and poor durability, and thus provide an aluminum-phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial and a preparation method and application thereof. The aluminum-phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial has a heterostructure of two-dimensional nanosheet layers grown on nanowires, which is conducive to the transfer of mass and charge. The electronic structures of Co3O4 and NiFe2O4 are changed by aluminum-phosphorus co-doping, and the electrocatalytic performance thereof is further improved. At the same time, the raw materials and process equipment used in the preparation method of the aluminum-phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial are simple and low in cost, which is conducive to large-scale production and is expected to produce good social and economic effects. In addition, the composite nanomaterial has good catalytic activity for oxygen evolution in electrolytic water under alkaline conditions.
[0005] In order to achieve the above-mentioned object, in the first aspect, the present invention provides an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial, wherein the chemical formula of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial is AP-Co3O4@NiFe2O4 / NF, wherein:
[0006] The structure of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial is a heterostructure in which two-dimensional nanosheet layers are grown on nanowires.
[0007] In a second aspect, the present invention provides a method for preparing an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial, the preparation method comprising:
[0008] 1) Preparation of aluminum-doped cobalt oxide / nickel foam composite nanomaterial: in the presence of a first solvent, cobalt salt, aluminum salt and alkaline substance are first mixed, and then pretreated nickel foam is added to perform a first hydrothermal reaction, and calcined to obtain aluminum-doped cobalt oxide / nickel foam composite nanomaterial;
[0009] 2) Preparation of aluminum and phosphorus co-doped cobalt tetroxide / nickel foam composite nanomaterial: under an inert atmosphere, the aluminum-doped cobalt tetroxide / nickel foam composite nanomaterial described in step 1) is phosphated with a phosphorus source to obtain an aluminum and phosphorus co-doped cobalt tetroxide / nickel foam composite nanomaterial;
[0010] 3) Preparation of aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterials: In the presence of a second solvent, nickel salt, iron salt and reducing agent are mixed for a second time, and the aluminum and phosphorus co-doped cobalt oxide / nickel foam composite nanomaterials described in step 2) are added to carry out a second hydrothermal reaction.
[0011] In a third aspect, the present invention provides an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial prepared by the method described in the second aspect.
[0012] In a fourth aspect, the present invention provides an application of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial described in the first aspect or the third aspect as an electrocatalyst in catalyzing oxygen evolution reaction by electrolysis of water.
[0013] Through the above technical scheme, the linear Co3O4 in the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial (AP-Co3O4@NiFe2O4 / NF) of the present invention is covered by NiFe2O4 sheets to form a rich heterostructure, which is conducive to the transfer of mass and charge. Al and P elements are co-doped in Co3O4@NiFe2O4 / NF, which increases oxygen vacancies, promotes charge transfer, and achieves the best balance of surface chemical states. These improvements significantly improve the intrinsic activity of Co3O4@NiFe2O4 / NF catalysts. In addition, the synergistic effect of oxygen vacancies and AP-Co3O4@NiFe2O4 / NF heterostructure improves the conductivity of the electrocatalyst and provides more active sites involved in OER.
[0014] At the same time, the preparation method of the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of the present invention first adopts a simple hydrothermal method and a low-temperature calcination method to grow Al-Co3O4 / NF on a three-dimensional NF conductive skeleton, then obtains AP-Co3O4 / NF by a low-temperature gas phase phosphating method, and finally adopts a secondary mild hydrothermal method to mix nickel salt, iron salt, and a reducing agent in a solvent to obtain oxygen vacancy-rich AP-Co3O4@NiFe2O4 / NF heterostructure composite nanomaterial. The present invention is beneficial to the diffusion of ions and the release of gas products by designing a suitable liquid phase reaction system, provides a fast electron channel for electrocatalysis, and has the advantages of simple operation, economical and environmentally friendly reagents, low cost, easy operation, and suitability for mass production.
[0015] The aluminum and phosphorus co-doped heterogeneous structure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of the present invention is used as an electrocatalyst for oxygen evolution reaction. The heterogeneous structure aluminum and phosphorus co-doped cobalt oxide / nickel ferrite / nickel foam composite nanomaterial can be used to catalyze oxygen evolution reaction in an alkaline environment, has good electrocatalytic oxygen evolution reaction activity, and is conducive to large-scale utilization and promotion.
[0016] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:
[0018] Figure 1 The X-ray powder diffraction pattern of the aluminum-doped cobalt tetroxide / nickel foam composite nanomaterial obtained in step (1) of Example 1;
[0019] Figure 2This is a scanning electron microscope image of the aluminum-doped cobalt tetroxide / nickel foam composite nanomaterial obtained in step (1) of Example 1;
[0020] Figure 3 This is a scanning electron microscope image of the aluminum and phosphorus co-doped cobalt tetroxide / nickel foam composite nanomaterial obtained in step (2) of Example 1;
[0021] Figure 4 The X-ray powder diffraction pattern spectrum of the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 1;
[0022] Figure 5 This is a scanning electron microscope image of the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 1;
[0023] Figure 6 This is a transmission electron microscope image of the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 1;
[0024] Figure 7 This is a scanning electron microscope image of the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 2;
[0025] Figure 8 This is a scanning electron microscope image of the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 3;
[0026] Fig. 9 This is a scanning electron microscope image of the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 4;
[0027] Fig.10 This is a scanning electron microscope image of the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 5;
[0028] Fig.11 This is a scanning electron microscope image of the composite nanomaterial of Comparative Example 1;
[0029] Fig.12 This is a scanning electron microscope image of the composite nanomaterial of Comparative Example 2;
[0030] Fig.13 The X-ray powder diffraction pattern spectrum of the cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Comparative Example 3;
[0031] Fig.14 This is a scanning electron microscope image of the nickel ferrite / nickel foam composite nanomaterial of Comparative Example 4;
[0032] Fig.15Polarization curves of the AP-Co3O4@NiFe2O4 / NF composite nanomaterial obtained in Example 1, the Co3O4@NiFe2O4 / NF composite nanomaterial obtained in Comparative Example 3, and the NiFe2O4 / NF composite nanomaterial obtained in Comparative Example 4 for catalytic oxygen evolution reaction in 1 mol / L KOH solution. DETAILED DESCRIPTION
[0033] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0034] In a first aspect, the present invention provides an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial, wherein the chemical formula of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial is AP-Co3O4@NiFe2O4 / NF, wherein:
[0035] The structure of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial is a heterostructure in which two-dimensional nanosheet layers are grown on nanowires.
[0036] In the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial (AP-Co3O4@NiFe2O4 / NF) of the present invention, the linear Co3O4 is covered by NiFe2O4 sheets to form a rich heterostructure, which is conducive to the transfer of mass and charge. Al and P elements are co-doped in Co3O4@NiFe2O4 / NF, which increases oxygen vacancies, promotes charge transfer, and achieves the best balance of surface chemical states. These improvements significantly improve the intrinsic activity of the Co3O4@NiFe2O4 / NF catalyst. In addition, the synergistic effect of oxygen vacancies and the AP-Co3O4@NiFe2O4 / NF heterostructure improves the conductivity of the electrocatalyst and provides more active sites involved in OER.
[0037] In a preferred embodiment of the present invention, the thickness of the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial is 8-12 nm.
[0038] In a second aspect, the present invention provides a method for preparing an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial, the preparation method comprising:
[0039] 1) Preparation of aluminum-doped cobalt oxide / nickel foam composite nanomaterial: in the presence of a first solvent, cobalt salt, aluminum salt and alkaline substance are first mixed, and then pretreated nickel foam is added to perform a first hydrothermal reaction, and calcined to obtain aluminum-doped cobalt oxide / nickel foam composite nanomaterial;
[0040] 2) Preparation of aluminum and phosphorus co-doped cobalt tetroxide / nickel foam composite nanomaterial: under an inert atmosphere, the aluminum-doped cobalt tetroxide / nickel foam composite nanomaterial described in step 1) is phosphated with a phosphorus source to obtain an aluminum and phosphorus co-doped cobalt tetroxide / nickel foam composite nanomaterial;
[0041] 3) Preparation of aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterials: In the presence of a second solvent, nickel salt, iron salt and reducing agent are mixed for a second time, and the aluminum and phosphorus co-doped cobalt oxide / nickel foam composite nanomaterials described in step 2) are added to carry out a second hydrothermal reaction.
[0042] The preparation method of the aluminum and phosphorus co-doped heterogeneous structure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of the present invention first adopts a simple hydrothermal method and a low-temperature calcination method to grow Al-Co3O4 / NF on a three-dimensional NF conductive skeleton, then obtains AP-Co3O4 / NF by a low-temperature gas phase phosphating method, and finally adopts a secondary mild hydrothermal method to mix nickel salt, iron salt and a reducing agent in a solvent to obtain oxygen vacancy-rich AP-Co3O4@NiFe2O4 / NF heterogeneous structure composite nanomaterial. The present invention is conducive to the diffusion of ions and the release of gas products by designing a suitable liquid phase reaction system, provides a fast electron channel for electrocatalysis, and has the advantages of simple operation, economical and environmentally friendly reagents, low cost, easy operation, and suitability for mass production.
[0043] In a preferred embodiment of the present invention, in order to remove dust, oil stains and some oxides on the surface of the nickel foam, the pretreatment step includes: cutting the nickel foam into 3 cm × 4 cm slices, soaking them in 6 mol / L hydrochloric acid for 15 minutes, and then rinsing them with deionized water and anhydrous ethanol for 3 times respectively, and finally placing the nickel foam material in a 50 ° C vacuum drying oven for 10 hours for standby use.
[0044] In a preferred embodiment of the present invention, in order to obtain an aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial with better catalytic activity, in step 1), the molar ratio of the aluminum salt to the cobalt salt is 1:2-25, wherein the aluminum salt is calculated as aluminum atoms and the cobalt salt is calculated as cobalt atoms. For example, the molar ratio of the aluminum salt to the cobalt salt can be 1:2, 1:5, 1:10, 1:15, 1:20 or 1:25.
[0045] In a preferred embodiment of the present invention, in order to obtain an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial with better catalytic activity, the cobalt salt is cobalt nitrate and / or cobalt sulfate.
[0046] In a preferred embodiment of the present invention, in order to obtain an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial with better catalytic activity, the aluminum salt is aluminum nitrate and / or aluminum sulfate.
[0047] In a preferred embodiment of the present invention, in order to obtain an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial with better catalytic activity, the alkaline substance is one or more of urea, ammonium fluoride and sodium carbonate.
[0048] In a preferred embodiment of the present invention, the concentration of the alkaline substance is 0.3-0.4 mol / L, preferably 0.357 mol / L.
[0049] In a preferred embodiment of the present invention, the first solvent is water, and the water can be common experimental and production water such as deionized water, ultrapure water and distilled water.
[0050] In a preferred embodiment of the present invention, in step 1), the conditions of the first mixing include: a time of 20-40 min and a stirring rate of 600-1000 rpm, for example, a time of 20 min and a stirring rate of 600 rpm; a time of 25 min and a stirring rate of 700 rpm; a time of 30 min and a stirring rate of 800 rpm; a time of 35 min and a stirring rate of 900 rpm or a time of 40 min and a stirring rate of 1000 rpm.
[0051] In a preferred embodiment of the present invention, in order to obtain an aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial with better catalytic activity, the conditions of the first hydrothermal reaction include: under closed conditions, the temperature is 100-160°C, and the time is 8-14h, for example, the temperature is 100°C, and the time is 8h; the temperature is 110°C, and the time is 10h; the temperature is 120°C, and the time is 12h; the temperature is 130°C, and the time is 14h; the temperature is 140°C, and the time is 14h; the temperature is 150°C, and the time is 12h or the temperature is 160°C, and the time is 10h.
[0052] In a preferred embodiment of the present invention, in order to obtain an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial with better catalytic activity, the calcination conditions include: a temperature of 200-500°C and a time of 1-4h, for example, a temperature of 200°C and a time of 1h; a temperature of 300°C and a time of 2h; a temperature of 400°C and a time of 3h or a temperature of 500°C and a time of 4h.
[0053] In a preferred embodiment of the present invention, in order to obtain an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial with better catalytic activity, in step 2), the amount ratio of the phosphorus source to the aluminum-doped cobalt oxide / nickel foam composite nanomaterial is 1:1-4, wherein the phosphorus source is calculated as phosphorus atoms, for example, the amount ratio of the phosphorus source to the aluminum-doped cobalt oxide / nickel foam composite nanomaterial is 1:1, 1:2, 1:3 or 1:4.
[0054] In a preferred embodiment of the present invention, in order to obtain an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial with better catalytic activity, the phosphorus source is sodium hypophosphite and / or red phosphorus.
[0055] In a preferred embodiment of the present invention, in order to obtain an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial with better catalytic activity, the phosphating conditions include: a temperature of 200-500°C, a time of 1-4h, and a heating rate of 15-25°C·min -1 For example, the temperature is 200℃, the time is 1h, and the heating rate is 15℃·min -1 ; Temperature is 300℃, time is 2h, heating rate is 20℃·min -1 ; Temperature is 400℃, time is 3h, heating rate is 25℃·min -1 Or the temperature is 500℃, the time is 4h, and the heating rate is 20℃·min -1 .
[0056] In a preferred embodiment of the present invention, the inert atmosphere is an argon atmosphere and / or a nitrogen atmosphere.
[0057] In a preferred embodiment of the present invention, in order to obtain an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial with better catalytic activity, in step 3), the molar ratio of the nickel salt to the iron salt is 1:1-6, wherein the nickel salt is calculated as nickel atoms and the iron salt is calculated as iron atoms; for example, the molar ratio of the nickel salt to the iron salt can be 1:1, 1:2, 1:3, 1:4, 1:5 or 1:6.
[0058] In a preferred embodiment of the present invention, the reducing agent is ascorbic acid and / or sodium citrate.
[0059] In a preferred embodiment of the present invention, the concentration of the reducing agent is 6-8 mmol / L, preferably 7 mmol / L.
[0060] In a preferred embodiment of the present invention, the second solvent is water, and the water can be common experimental and production water such as deionized water, ultrapure water and distilled water.
[0061] In a preferred embodiment of the present invention, in order to obtain an aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial with better catalytic activity, in step 3), the conditions of the second hydrothermal reaction include: under closed conditions, the temperature is 100-160°C, and the time is 8-14h, for example, the temperature is 100°C, and the time is 8h; the temperature is 110°C, and the time is 9h; the temperature is 120°C, and the time is 10h; the temperature is 130°C, and the time is 11h; the temperature is 140°C, and the time is 12h; the temperature is 150°C, and the time is 13h or the temperature is 160°C, and the time is 14h.
[0062] In a third aspect, the present invention provides an aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial prepared by the method described in the second aspect.
[0063] In a fourth aspect, the present invention provides an application of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial described in the first aspect or the third aspect as an electrocatalyst in catalyzing oxygen evolution reaction by electrolysis of water.
[0064] The aluminum and phosphorus co-doped heterogeneous structure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of the present invention is used as an electrocatalyst for oxygen evolution reaction. The heterogeneous structure aluminum and phosphorus co-doped cobalt oxide / nickel ferrite / nickel foam composite nanomaterial can be used to catalyze oxygen evolution reaction in an alkaline environment, has good electrocatalytic oxygen evolution reaction activity, and is conducive to large-scale utilization and promotion.
[0065] The present invention will be described in detail below by way of examples. In the following examples, all drugs not specifically specified are conventional commercial products.
[0066] Example 1
[0067] (1) Before the experiment, the nickel foam was cut into 3.0×4.0 cm 2 The thin slices were soaked in 6M HCl for 15 minutes, and then rinsed three times with deionized water and anhydrous ethanol to remove surface oil and oxides; 2.5mmol cobalt nitrate hexahydrate, 0.25mmol aluminum nitrate nonahydrate, 5mmol ammonium fluoride and 7.5mmol urea were added to 35.0mL deionized water and stirred continuously for 30 minutes to obtain a red clear solution; the mixed red clear solution was charged into a 50mL polytetrafluoroethylene autoclave containing clean nickel foam, and hydrothermally reacted at 120°C for 10 hours. After the reaction system was cooled to room temperature, the product was taken out, rinsed alternately with deionized water and anhydrous ethanol for 3 times, and then dried in a vacuum oven at 60°C. Subsequently, the product was placed in a muffle furnace and calcined at 350°C for 2 hours to obtain aluminum-doped cobalt oxide / nickel foam composite nanomaterials, recorded as Al-Co3O4 / NF;
[0068] (2) Using the Al-Co3O4 / NF prepared in step (1) as a precursor and Na2HPO2 as a P source, Al-Co3O4 / NF and Na2HPO2 were placed at two different positions in the porcelain boat, wherein 0.1 g of Na2HPO2 was placed upstream of the tube and heated at 2 °C min in an Ar atmosphere. -1 The heating rate was 350℃ for 2h to obtain the aluminum and phosphorus co-doped cobalt tetroxide / nickel foam composite nanomaterial, which was recorded as AP-Co3O4 / NF.
[0069] (3) 0.25 mmol of nickel nitrate hexahydrate, 0.5 mmol of ferrous chloride tetrahydrate and 0.25 mmol of ascorbic acid were added to 35.0 mL of deionized water and stirred continuously for 30 min to obtain a clear green solution; the mixed clear green solution was charged into a 50 mL polytetrafluoroethylene high-pressure reactor containing AP-Co3O4 / NF and subjected to hydrothermal reaction at 180°C for 10 h. After the reaction system was cooled to room temperature, the product was taken out and rinsed alternately with deionized water and anhydrous ethanol for 3 times, and then dried in a vacuum oven at 60°C to obtain an aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial, recorded as AP-Co3O4@NiFe2O4 / NF (the Al doping amount was 1.19%).
[0070] Depend on Figure 1 It can be seen from the X-ray powder diffraction pattern of the aluminum-doped cobalt tetroxide / nickel foam composite nanomaterial obtained in step (1) of Example 1 that its main diffraction peak corresponds to the characteristic peak of Co3O4 (PDF#43-1003) on the X-ray powder diffraction standard card, indicating that the product obtained in step (1) of Example 1 is Co3O4.
[0071] Depend on Figure 2 From the scanning electron microscope image of the aluminum-doped cobalt tetroxide / nickel foam composite nanomaterial obtained in step (1) of Example 1, it can be seen that the prepared Al-Co3O4 / NF is a nanowire structure.
[0072] Depend on Figure 3 From the scanning electron microscope image of the aluminum and phosphorus co-doped cobalt oxide / nickel foam composite nanomaterial obtained in step (2) of Example 1, it can be seen that the phosphorus doping in step (2) does not change the shape structure of the Al-Co3O4 / NF nanowires.
[0073] Depend on Figure 4From the X-ray powder diffraction pattern spectrum of the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 1, it can be seen that its main diffraction peaks are consistent with Co3O4 (PDF#43-1003) of the X-ray powder diffraction standard card, indicating that the product obtained in Example 1 is AP-Co3O4@NiFe2O4 / NF composite material.
[0074] Depend on Figure 5 From the scanning electron microscope image of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 1, it can be seen that the AP-Co3O4@NiFe2O4 / NF composite material prepared in Example 1 is a heterostructure material with two-dimensional nanosheets grown on nanowires, and the thickness of the two-dimensional nanosheets is about 10 nm.
[0075] Depend on Figure 6 From the transmission electron microscope image of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 1, it can be seen that the AP-Co3O4@NiFe2O4 / NF composite material prepared in Example 1 is a thin layer of nanosheet structure uniformly grown on the surface of the Co3O4 nanowire, with a thickness of about 10 nm.
[0076] Example 2
[0077] The method of Example 1 was followed, except that the "0.25 mmol aluminum nitrate nonahydrate" in step (1) was replaced by "0.125 mmol aluminum nitrate nonahydrate" to obtain an aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial, recorded as AP-Co3O4@NiFe2O4 / NF (Al doping amount 0.45%).
[0078] Depend on Figure 7 From the scanning electron microscope image of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 2, it can be seen that the AP-Co3O4@NiFe2O4 / NF composite material prepared in Example 2 is a heterostructure material of two-dimensional nanosheet layers grown on nanowires, with a thickness of about 8 nm.
[0079] Example 3
[0080] The method of Example 1 was followed, except that the "0.25 mmol aluminum nitrate nonahydrate" in step (1) was replaced by "0.5 mmol aluminum nitrate nonahydrate" to obtain an aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial, recorded as AP-Co3O4@NiFe2O4 / NF (Al doping amount 1.99%).
[0081] Depend on Figure 8From the scanning electron microscope image of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 3, it can be seen that the AP-Co3O4@NiFe2O4 / NF composite material prepared in Example 3 is a heterostructure material of two-dimensional nanosheet layers grown on nanowires, with a thickness of about 12 nm.
[0082] Example 4
[0083] The method of Example 1 was followed, except that the "0.25 mmol aluminum nitrate nonahydrate" in step (1) was replaced by "0.75 mmol aluminum nitrate nonahydrate" to obtain an aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial, recorded as AP-Co3O4@NiFe2O4 / NF (Al doping amount 2.54%).
[0084] Depend on Fig. 9 From the scanning electron microscope image of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 4, it can be seen that the AP-Co3O4@NiFe2O4 / NF composite material prepared in Example 4 is a heterostructure material of two-dimensional nanosheet layers grown on nanowires, with a thickness of about 9 nm.
[0085] Example 5
[0086] The method of Example 1 was followed, except that the "hydrothermal reaction at 180°C for 10 h" in step (3) was replaced by "hydrothermal reaction at 160°C for 12 h" to obtain an aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial, recorded as AP-Co3O4@NiFe2O4 / NF (Al doping amount 1.19%).
[0087] Depend on Fig.10 From the scanning electron microscope image of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial of Example 5, it can be seen that the AP-Co3O4@NiFe2O4 / NF composite material prepared in Example 5 is a heterostructure material of two-dimensional nanosheet layers grown on nanowires, with a thickness of about 10 nm.
[0089] Comparative Example 1
[0090] The method of Example 1 was followed, except that the step (3) of "hydrothermal reaction at 180°C for 10 h" was replaced by "hydrothermal reaction at 120°C for 10 h", and the obtained composite nanomaterial was recorded as D1 (Al doping amount: 1.19%).
[0091] Depend on Fig.11From the scanning electron microscope image of the composite nanomaterial of Comparative Example 1, it can be seen that no thin layer of nanosheet structure has grown on the Co3O4 nanowires of the composite nanomaterial of Comparative Example 1, and Comparative Example 1 only lowers the temperature of the second hydrothermal reaction relative to Example 1, which leads to a significant change in the morphology of the nanomaterial, indicating that the experimental conditions of the present invention also need to be controlled and cannot be changed at will.
[0092] Comparative Example 2
[0093] The method of Example 1 was followed, except that the "hydrothermal reaction at 180°C for 10 h" in step (3) was replaced by "hydrothermal reaction at 200°C for 10 h", and the obtained composite nanomaterial was recorded as D2 (Al doping amount 1.19%).
[0094] Depend on Fig.12 From the scanning electron microscope image of the composite nanomaterial of Comparative Example 2, it can be seen that the Co3O4 nanowire structure in the composite nanomaterial of Comparative Example 2 collapses directly, and Comparative Example 2 only increases the temperature of the second hydrothermal reaction relative to Example 1, which leads to a significant change in the morphology of the nanomaterial, indicating that the experimental conditions of the present invention also need to be controlled and cannot be changed at will.
[0095] Comparative Example 3
[0096] The method of Example 1 is followed, except that the aluminum source in step (1) is not added, and the phosphating in step (2) is not performed, to obtain a cobalt tetroxide / nickel ferrite / nickel foam composite nanomaterial, denoted as Co3O4@NiFe2O4 / NF.
[0097] Depend on Fig.13 From the X-ray powder diffraction pattern spectrum of the cobalt tetroxide / nickel ferrite / nickel foam composite nanomaterial of Comparative Example 3, it can be seen that the main diffraction peaks of the cobalt tetroxide / nickel ferrite / nickel foam composite nanomaterial of Comparative Example 3 correspond to the characteristic peaks of Co3O4 (PDF#43-1003) of the X-ray powder diffraction standard card, and NiFe2O4 is amorphous, so there is no characteristic peak corresponding to it, indicating that the product obtained in Comparative Example 3 is a cobalt tetroxide / nickel ferrite / nickel foam composite nanomaterial.
[0098] Comparative Example 4
[0099] The method of Example 1 is followed, except that only step (3) is performed, and the AP-Co3O4 / NF in step (3) is replaced by pretreated nickel foam to obtain nickel ferrite / nickel foam composite nanomaterial, which is recorded as NiFe2O4 / NF.
[0100] Depend on Fig.14From the scanning electron microscope image of the nickel ferrite / nickel foam composite nanomaterial of Comparative Example 4, it can be seen that the nickel ferrite / nickel foam composite nanomaterial of Comparative Example 4 is a honeycomb two-dimensional nanosheet structure.
[0101] Application Example 1
[0102] The application of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial in the field of catalytic electrolysis of water and oxygen evolution reaction is specifically described as follows:
[0103] The AP-Co3O4@NiFe2O4 / NF composite nanomaterial obtained in Example 1, the Co3O4@NiFe2O4 / NF composite nanomaterial obtained in Comparative Example 3, and the NiFe2O4 / NF composite nanomaterial obtained in Comparative Example 4 were used as catalysts to test the catalytic performance of oxygen evolution reaction in alkaline water electrolysis, and the steps were as follows:
[0104] At room temperature, 1M KOH solution was used as the electrolyte solution in the alkaline environment for testing. A standard three-electrode system was used for testing. A graphite rod was used as the counter electrode, and a silver / silver chloride (Ag / AgCl) electrode was used as the reference electrode. The AP-Co3O4@NiFe2O4 / NF composite nanomaterial obtained in Example 1, the Co3O4@NiFe2O4 / NF composite nanomaterial obtained in Comparative Example 3, and the NiFe2O4 / NF composite nanomaterial obtained in Comparative Example 4 were cut into a size of 1*1 cm and clamped on an electrode clamp as working electrodes. The catalytic oxygen evolution and hydrogen evolution reaction performance tests were carried out by linear sweep voltammetry. The results are shown in FIG. Fig.15 shown.
[0105] Depend on Fig.15 The polarization curves of the AP-Co3O4@NiFe2O4 / NF composite nanomaterial obtained in Example 1, the Co3O4@NiFe2O4 / NF composite nanomaterial obtained in Comparative Example 3, and the NiFe2O4 / NF composite nanomaterial obtained in Comparative Example 4 for catalyzing oxygen evolution reaction in 1 mol / L KOH solution can be seen. When the current density is 10 mA / cm 2The overpotential of the Co3O4@NiFe2O4 / NF composite nanomaterial obtained in Comparative Example 3 is 331 mV, the overpotential of the NiFe2O4 / NF composite nanomaterial obtained in Comparative Example 4 is 251 mV, and the overpotential of the AP-Co3O4@NiFe2O4 / NF composite nanomaterial obtained in Example 1 is only 170 mV. The test results show that compared with the Co3O4@NiFe2O4 / NF composite nanomaterial obtained in Comparative Example 3 and the NiFe2O4 / NF composite nanomaterial obtained in Comparative Example 4, the AP-Co3O4@NiFe2O4 / NF composite nanomaterial prepared by the preparation method of the present invention has better catalytic oxygen evolution reaction performance in an alkaline environment, can provide better economic benefits, and thus can be better applied.
[0106] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0107] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0108] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. An aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial, characterized in that: The chemical formula of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial is AP-Co3O4@NiFe2O4 / NF, wherein: The structure of the aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial is a heterostructure in which two-dimensional nanosheet layers are grown on nanowires.
2. The aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial according to claim 1, characterized in that: The thickness of the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial is 8-12 nm.
3. A method for preparing aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial, characterized in that: The preparation method is: 1) Preparation of aluminum-doped cobalt oxide / nickel foam composite nanomaterial: in the presence of a first solvent, cobalt salt, aluminum salt and alkaline substance are first mixed, and then pretreated nickel foam is added to perform a first hydrothermal reaction, and calcined to obtain aluminum-doped cobalt oxide / nickel foam composite nanomaterial; 2) Preparation of aluminum and phosphorus co-doped cobalt tetroxide / nickel foam composite nanomaterial: under an inert atmosphere, the aluminum-doped cobalt tetroxide / nickel foam composite nanomaterial described in step 1) is phosphated with a phosphorus source to obtain an aluminum and phosphorus co-doped cobalt tetroxide / nickel foam composite nanomaterial; 3) Preparation of aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterials: In the presence of a second solvent, nickel salt, iron salt and reducing agent are mixed for a second time, and the aluminum and phosphorus co-doped cobalt oxide / nickel foam composite nanomaterials described in step 2) are added to carry out a second hydrothermal reaction.
4. The preparation method according to claim 3, characterized in that: In step 1), the molar ratio of the aluminum salt to the cobalt salt is 1:2-25, wherein the aluminum salt is calculated as aluminum atoms and the cobalt salt is calculated as cobalt atoms; Preferably, the cobalt salt is cobalt nitrate and / or cobalt sulfate; More preferably, the aluminum salt is aluminum nitrate and / or aluminum sulfate; Further preferably, the alkaline substance is one or more of urea, ammonium fluoride and sodium carbonate; More preferably, the concentration of the alkaline substance is 0.3-0.4 mol / L; More preferably, the first solvent is water.
5. The preparation method according to claim 3 or 4, characterized in that: In step 1), the first mixing conditions include: a time of 20-40 min and a stirring rate of 600-1000 rpm; Preferably, the conditions of the first hydrothermal reaction include: in a closed environment, the temperature is 100-160° C., and the time is 8-14 h; More preferably, the calcination conditions include: temperature of 200-500° C., time of 1-4 h;.
6. The preparation method according to any one of claims 3 to 5, characterized in that: In step 2), the mass ratio of the phosphorus source to the aluminum-doped cobalt tetroxide / nickel foam composite nanomaterial is 1:1-4, wherein the phosphorus source is calculated as phosphorus atoms; Preferably, the phosphorus source is sodium hypophosphite and / or red phosphorus; More preferably, the phosphating conditions include: temperature of 200-500°C, time of 1-4h, heating rate of 15-25°C·min -1 ; Further preferably, the inert atmosphere is an argon atmosphere and / or a nitrogen atmosphere.
7. The preparation method according to any one of claims 3 to 6, characterized in that: In step 3), the molar ratio of the nickel salt to the iron salt is 1:1-6, wherein the nickel salt is calculated as nickel atoms and the iron salt is calculated as iron atoms; Preferably, the reducing agent is ascorbic acid and / or sodium citrate; More preferably, the concentration of the reducing agent is 6-8 mmol / L; More preferably, the second solvent is water.
8. The preparation method according to any one of claims 3 to 7, characterized in that: In step 3), the conditions of the second hydrothermal reaction include: under closed conditions, the temperature is 100-160° C., and the time is 8-14 h.
9. Aluminum and phosphorus co-doped heterostructured cobalt oxide / nickel ferrite / nickel foam composite nanomaterial prepared by the preparation method according to any one of claims 3 to 8.
10. Use of the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial according to claim 1 or 2 or the aluminum and phosphorus co-doped heterostructure cobalt oxide / nickel ferrite / nickel foam composite nanomaterial according to claim 9 as an electrocatalyst in catalyzing oxygen evolution reaction by electrolysis of water.
Citation Information
Patent Citations
Phosphorus-doped ferronickel oxide nitrogen-doped carbon nanofiber composite material and preparation method and application thereof
CN110975914A
Efficient oxygen evolution electrocatalyst and preparation method thereof
CN111790416A
Preparation method of phosphorus-doped cobalt nanowire array for reducing nitrate nitrogen in water
CN111807474A
Copper-doped cobalt phosphide bifunctional water electrolysis catalytic material in hollow nanotube structure
CN111939951A
Preparation method of double transition metal phosphide catalyst
CN116837404A
Cited By
Porous metal-based composite material as well as preparation method and application thereof
CN119972137A