Electromagnetic hot-melt tin alloy solder, and preparation and soldering method therefor
Through the combination of electromagnetic heat-melting tin alloy solder and electromagnetic wave heating equipment, problems such as oxidation and leakage during the welding process of tin alloy solder are solved, the welding quality and cost-effectiveness are improved, environmental pollution is reduced, and product life is extended.
Patent Information
- Application Number
- PCT/CN2023/118437
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2023-09-13
- Publication Date
- 2024-10-31
AI Technical Summary
Existing tin alloy solders are prone to oxidation, leakage, false welding, false welding and other problems due to high temperatures during the welding process, and the welding quality is difficult to control, resulting in high failure rates of electronic products, as well as high costs and environmental pollution.
Using electromagnetic heat-melting tin alloy solder, through a specific proportion of particulate metal laminated materials and special electromagnetic wave heating equipment, rapid heating and welding from the inside out, reducing the amount of flux and power loss, avoiding high temperature damage to components, and achieving seamless Contact heating.
Significantly improve soldering quality, reduce soldering costs and environmental pollution, extend product service life, avoid high temperature damage to components and welding quality problems, and reduce soldering quality control costs.
Smart Images

Figure CN2023118437_31102024_PF_FP_ABST
Abstract
Description
Electromagnetic heat-melting tin alloy solder and its preparation and soldering method Technical Field
[0001] The invention relates to the field of electronic product manufacturing, and in particular to an electromagnetic hot-melting tin alloy solder and a preparation method thereof, and a soldering method. Background Art
[0002] Tin alloy solder is a fusible metal with a lower melting point than the metal being welded. When the solder melts, it can wet the surface of the metal being welded without melting the metal being welded, and form an alloy layer at the contact surface to connect the metal to the metal being welded. In general electronic product assembly, it is commonly known as solder.
[0003] Tin alloy solder is often processed and shaped into specified sizes when used, and comes in a variety of forms, including sheets, blocks, pastes, strips, balls, and wires.
[0004] 1) Filamentous solder - usually called solder wire, with rosin wrapped in the center, called resin core wire, commonly used in manual soldering. The outer diameter of resin core wire is usually 0.5mm, 0.6mm, 0.8mm, 1.0mm, 1.2mm, 1.6mm, 2.0mm, 2.3mm, 3.0mm, etc.
[0005] 2) Flake solder - commonly used for welding silicon wafers and other sheet-shaped parts;
[0006] 3) Strip solder - commonly used in automatic assembly production lines, where an automatic welding machine is used to punch out a section of the strip solder for welding to improve production efficiency;
[0007] 4) Solder paste - solder and flux are mixed together to make it. When soldering, the solder paste is first applied to the printed circuit board and then soldered. It has been widely used in automatic placement technology.
[0008] Existing tin alloy solders consist of solder resist and a tin alloy in specific proportions. These alloys primarily include tin-lead, tin-bismuth, and tin-silver-copper alloys, with typical ratios being SN63 / PB37, SN42BI58, SN96.5CU0.5AG3.0, and SN99CU0.7AG0.3. Before lead-free requirements were introduced, the most commonly used alloy was Sn63 / Pb37. Lead-free tin alloy solders primarily consist of tin / silver / copper, such as SN96.5CU0.5AG3.0 and SN99CU0.7AG0.3. Silver and copper replace the original lead component, along with a small amount of antioxidants. For low-temperature requirements, melting point-lowering elements are added.
[0009] Soldering is the process of welding with tin alloys. Soldering has a low temperature and can be performed with simple tools. It's a simple method, making it easy to repair solder joints and replace components. Therefore, it's the most common soldering method used in electronics assembly.
[0010] Existing tin alloy solders are primarily heated from the surface to the inside using a heating tool such as a soldering iron or a flat soldering station, or through non-contact heating such as laser heating or air heating such as reflow soldering. The solder paste melts from the surface to the inside, and the alloy components cool and solidify, forming a solder joint between the two objects being soldered, achieving the metallurgical connection. Existing tin alloy solders using existing hot-melt soldering processes have the following disadvantages:
[0011] 1. Current soldering methods, such as direct contact heating with a soldering iron or soldering station, can easily lead to soldering quality issues like false joints and cold joints due to factors such as the power and temperature of the soldering iron or soldering station, the type and quantity of the solder alloy, the heat dissipation of the object being soldered, ambient temperature, air flow, the type of soldering tip, the contact pressure, contact area and angle when transferring heat to the workpiece, and the operator's proficiency. In particular, when using a soldering iron for contact heating, the tip's prolonged exposure to high temperatures and weakly acidic substances like flux can easily oxidize and deposit a layer of black impurities on its surface. These impurities form an insulating layer, which, if not cleaned promptly, hinders heat transfer between the tip and the workpiece, compromising soldering quality. Furthermore, carbonized material on the tip's surface can remain between the solder joints, affecting aesthetics and even causing leakage, impacting product quality. Excessive temperatures on the soldering iron or soldering station can easily damage components or PCBs. Even using the soldering iron tip to directly contact and heat the tin to melt it, once the soldering iron tip leaks electricity, it will damage the static-sensitive components, causing significant economic losses. If the performance of the components is degraded, it will trigger large-scale after-sales incidents, thus causing a huge negative impact on the product's brand image.
[0012] 2. Existing tin alloy solders are used in the surface mount soldering (SMT) process for electronic products in the form of solder paste. Solder paste is printed and applied to the pads of a printed circuit board (PCB). Surface mount components are then precisely placed onto the solder-paste-coated pads. The PCB is then placed in a reflow oven (hot air heating equipment) that heats the PCB according to a specific reflow profile, melting the solder paste. Once the alloy cools and solidifies, a solder joint is formed between the component and the PCB, achieving soldering. Many factors can affect SMT solder quality: for example, a mismatch between the reflow temperature setting and the type of solder paste can cause overheating and oxidation, while insufficient temperature or insufficient melting time can lead to cold soldering. Uneven hot air flow in the reflow oven can lead to a soldering problem known as tombstoning (different levels of solder paste melting on either side of the PCB, causing the component to stand upright). The preheat zone of the reflow profile is used to raise the PCB temperature from ambient to the required activation temperature. In this zone, the product temperature rises continuously at a rate of no more than 2-5°C per second. A rapid temperature rise can cause defects, such as fine cracks in ceramic capacitors, while a slow temperature rise can overheat the solder paste, preventing the PCB from reaching active temperature and resulting in poor solder quality. The preheat zone setting is affected by factors such as ambient temperature, solder type, component density, PCB size, and PCB copper foil thickness, making it difficult to avoid soldering defects. The SMT process is a continuous, high-temperature operation, placing high demands on the heat resistance of both the PCB and surface-mount components. Even the slightest carelessness can damage these components, and these high heat resistance requirements can significantly increase costs. Furthermore, reflow equipment must maintain a constant high temperature during operation and exhaust the high-temperature evaporation gases from the flux, making the production process energy-intensive and costly.
[0013] 3. Existing tin alloy solder is used in the wave soldering and dip soldering processes of circuit boards in the form of a high-temperature liquid tin alloy. This production process is used for most PCBs with a large number of interposers. The tin alloy solder is placed in a molten tin bath in a tin furnace and heated to a liquid state using electric heating tubes. After the interposer is sprayed with flux, it comes into contact with the solder liquid, where the tin alloy adheres to the PCB pads and the interposer pins, completing the soldering process. This process is affected by factors such as the heat dissipation of the soldered components, ambient temperature, flux quality, solder resist amount, tin alloy solder quality, and operator proficiency, making it prone to soldering quality issues such as false solder joints and cold joints. Because the soldering process requires constant high temperatures, the tin surface is easily oxidized and requires prompt cleaning, resulting in large amounts of tin slag and significant solder loss. Since residues from the high temperatures of flux and solder adhere to the PCB surface, they are not only unsightly but can also cause electrical leakage. Therefore, most PCBs require cleaning with detergents or ultrasonic cleaning after the wave soldering or dip soldering process, increasing process costs and environmental pollution.
[0014] Statistics show that nearly half of all electronic product failures are caused by poor soldering. An electronic device can have tens of thousands of solder joints, and it's common for one, two, or even just a few to cause the entire product to malfunction. These issues often lead to serious accidents, resulting in personal injury and national property losses. However, identifying the solder joints that cause failures in an electronic device with tens of thousands of solder joints is a complex task. Cold or false solder joints are particularly difficult to detect, and can appear normal immediately, but over time, due to increased oxidation, cause the device to malfunction. Especially for high-frequency and high-voltage equipment, burrs, pinholes, and air bubbles in solder joints can cause tip discharge or excessive internal resistance at the weld, leading to overheating and fire. Due to the limitations of existing tin alloy solders and the outside-in heating and welding process, despite significant quality control investments, product quality issues caused by solder quality have been ineffective. Furthermore, existing tin alloy solders and soldering processes consume significant amounts of solder and electrical energy, causing significant environmental pollution and high costs. Summary of the Invention
[0015] To address the above-mentioned issues, the present invention provides an electromagnetically fused tin alloy solder, its preparation, and soldering method. The solder contains a specific ratio of microparticle-shaped metal laminates that can be heated by a specific electromagnetic field. Using dedicated electromagnetic wave heating equipment, the inventive tin alloy solder is rapidly heated and fused from the inside out, completing the soldering process. This improves solder quality, significantly reduces tin alloy and flux usage, and significantly reduces power loss. Furthermore, the post-soldering cleaning step can be eliminated, thereby reducing costs and environmental pollution. In particular, it avoids damage to components caused by high temperatures and extends product life. This material is poised to completely replace existing tin alloy solders.
[0016] The present invention is achieved through the following technical solutions: an electromagnetically fused tin alloy solder, comprising:
[0017] High-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials, high-purity copper or other highly conductive metal materials and synthetic materials, high-purity zinc or other metal materials that easily form eutectic alloys with tin, and tin alloys constitute electromagnetic hot-melt tin alloy solder, which is a microparticle-shaped metal laminate material.
[0018] As a preferred technical solution, the mass percentage of high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials is 28-40%.
[0019] As a preferred technical solution, the mass percentage of high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials is 38.8%.
[0020] As a preferred technical solution, the mass percentage of high-purity copper or other highly conductive metal materials and synthetic materials is 5-15%.
[0021] As a preferred technical solution, the mass percentage of high-purity copper or other highly conductive metal materials and synthetic materials is 8.73%.
[0022] As a preferred technical solution, the mass percentage of high-purity zinc or other metal materials that can easily form a eutectic alloy with tin is 10-22%.
[0023] As a preferred technical solution, the mass percentage of high-purity zinc or other metal materials that can easily form a eutectic alloy with tin is 17.68%.
[0024] A method for preparing an electromagnetically fused tin alloy solder according to the present invention comprises the following steps:
[0025] S1. Prepare iron with a purity of 99.5% or more and a mass percentage of 38.8%, copper with a purity of 99.5% or more and a mass percentage of 8.73%, and zinc with a purity of 99.5% or more and a mass percentage of 17.68%;
[0026] S2. Prepare an appropriate amount of tin alloy;
[0027] S3. Copper with a purity of 99.5% or more and a mass percentage of 8.73%, zinc with a purity of 99.5% or more and a mass percentage of 17.68%, and an appropriate amount of tin alloy are plated on the outside of the high-purity iron in sequence;
[0028] S4, preparing electromagnetically heated molten tin alloy solder.
[0029] The invention discloses a method for soldering tin alloy solder by using electromagnetic heat. The method melts the tin alloy solder by electromagnetic heat and utilizes a special electromagnetic wave heating device to quickly heat and fuse the solder from the inside out to complete the soldering process.
[0030] The beneficial effects of the present invention are: 1. Since the surface heating time is short and the probability of oxidation is small, the invented tin alloy solder can reduce the content of flux, thereby reducing the harmful gases and residues generated by the flux after high temperature, thereby reducing air pollution and the risk of PCB leakage;
[0031] 2. The tin alloy solder powder of the present invention can be used in a non-contact specific electromagnetic field heating soldering process, eliminating the need for direct contact between the electric heater and the solder, thereby preventing damage to electrostatically sensitive components caused by leakage from the electric heater.
[0032] 3. The tin alloy solder powder of the present invention utilizes dedicated electromagnetic wave heating equipment to simultaneously heat and fuse the entire tin alloy solder inside and out. This method is virtually unaffected by factors such as the heat dissipation of the soldered object, ambient temperature, and operator proficiency. High-temperature solder residue is virtually nonexistent, significantly improving solder quality and reducing solder quality control costs. In particular, it avoids the significant loss of electrical energy and solder slag due to oxidation and contamination that necessitates solder replacement during conventional hand-dip and wave soldering processes.
[0033] 4. The tin alloy solder powder of the present invention can also be used in the form of solder paste in the surface mount soldering (SMT) process for electronic products. Using dedicated electromagnetic wave heating equipment, the tin alloy solder of the present invention is rapidly heated and fused from the inside out to complete the soldering process. This avoids the soldering quality issues, high energy consumption, and significant air pollution associated with existing tin alloy solder reflow equipment (hot air heating equipment). Furthermore, because the tin alloy solder of the present invention is simultaneously heated and fused internally and externally, it does not require refrigeration to maintain surface activity, thus reducing production steps and the quality issues that arise from these steps, thereby reducing production costs and losses.
[0034] 5. The tin alloy solder of the present invention reduces the content of tin alloy, greatly reducing the cost of using solder. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0036] FIG1 is a schematic cross-sectional view of a single particle of type 6 tin alloy solder powder according to the present invention;
[0037] FIG2 is a schematic diagram of the axis monolayer atomic sequence structure of a single particle of type 6 tin alloy solder powder according to the present invention. Implementation Method
[0038] All features disclosed in this specification, or all steps in the disclosed methods or processes, except mutually exclusive features and / or steps, can be combined in any manner.
[0039] Any feature disclosed in this specification (including any appended claims, abstract, and drawings), unless otherwise stated, may be replaced by other equivalent or similar features. In other words, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.
[0040] In the description of the present invention, it should be understood that the terms "one end", "the other end", "outside", "upper", "inside", "horizontal", "coaxial", "center", "end", "length", "outer end" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they should not be understood as limiting the present invention.
[0041] In addition, in the description of the present invention, “a plurality of” means at least two, for example, two, three, etc., unless otherwise clearly and specifically defined.
[0042] Terms indicating spatial relative positions, such as "upper," "above," "lower," and "below," are used herein for ease of description to describe the relationship of one unit or feature relative to another unit or feature as shown in the accompanying drawings. Spatially relative terms may be intended to encompass different orientations of the device in use or operation in addition to the orientation shown in the drawings. For example, if the device in the drawings were turned over, units described as being "below" or "beneath" other units or features would be "above" the other units or features. Thus, the exemplary term "below" encompasses both above and below orientations. The device may be otherwise oriented (rotated 90 degrees or in other orientations), and the spatially relative descriptors used herein interpreted accordingly.
[0043] In the present invention, unless otherwise expressly specified or limited, terms such as "disposed," "socketed," "connected," "through," and "inserted" should be understood in a broad sense. For example, they may refer to fixed or detachable connections, or integration; mechanical or electrical connections; direct or indirect connections through an intermediate medium; and internal communication between two components or interaction between two components, unless otherwise expressly specified or limited. Those skilled in the art will understand the specific meanings of the above terms in the present invention based on specific circumstances. Example
[0044] The electromagnetically molten tin alloy solder of the present invention comprises high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials, high-purity copper or other highly conductive metal materials and synthetic materials, high-purity zinc or other metal materials that easily form eutectic alloys with tin, and tin alloys, constituting the electromagnetically molten tin alloy solder. The electromagnetically molten tin alloy solder is a microparticle-shaped metal laminate material.
[0045] In this embodiment, the mass percentage of high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials is 28-40%. Specifically, in this embodiment, high-purity iron is used, and its mass percentage is 28%.
[0046] The mass percentage of high-purity copper or other highly conductive metal materials and synthetic materials is 5-15%. Specifically, in this embodiment, high-purity copper is used, and its mass percentage is 5%.
[0047] The mass percentage of high-purity zinc or other metal materials that easily form a eutectic alloy with tin is 10-22%. Specifically, in this embodiment, high-purity zinc is used, and its mass percentage is 10%. Example
[0048] The electromagnetically molten tin alloy solder of the present invention comprises high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials, high-purity copper or other highly conductive metal materials and synthetic materials, high-purity zinc or other metal materials that easily form eutectic alloys with tin, and tin alloys, constituting the electromagnetically molten tin alloy solder. The electromagnetically molten tin alloy solder is a microparticle-shaped metal laminate material.
[0049] In this embodiment, the mass percentage of high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials is 28-40%. Specifically, in this embodiment, high-purity iron is used, and its mass percentage is 38.8%.
[0050] The mass percentage of high-purity copper or other highly conductive metal materials and synthetic materials is 5-15%. Specifically, in this embodiment, high-purity copper is used, and its mass percentage is 8.73%.
[0051] The mass percentage of high-purity zinc or other metal materials that can easily form a eutectic alloy with tin is 10-22%. Specifically, in this embodiment, high-purity zinc is used, and its mass percentage is 17.68%.
[0052] The mass percentage in this embodiment is the optimal configuration. Example
[0053] The electromagnetically molten tin alloy solder of the present invention comprises high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials, high-purity copper or other highly conductive metal materials and synthetic materials, high-purity zinc or other metal materials that easily form eutectic alloys with tin, and tin alloys, constituting the electromagnetically molten tin alloy solder. The electromagnetically molten tin alloy solder is a microparticle-shaped metal laminate material.
[0054] In this embodiment, the mass percentage of high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials is 28-40%. Specifically, in this embodiment, high-purity iron is used, and its mass percentage is 40%.
[0055] The mass percentage of high-purity copper or other highly conductive metal materials and synthetic materials is 5-15%. Specifically, in this embodiment, high-purity copper is used, and its mass percentage is 15%.
[0056] The mass percentage of high-purity zinc or other metal materials that easily form a eutectic alloy with tin is 10-22%. Specifically, in this embodiment, high-purity zinc is used, and its mass percentage is 22%.
[0057] The present invention provides a method for preparing an electromagnetically fused tin alloy solder, taking iron, copper, zinc and a tin alloy as examples, comprising the following steps: (1) preparing iron with a purity of 99.5% or more and a mass percentage of 38.8%, copper with a purity of 99.5% or more and a mass percentage of 8.73%, and zinc with a purity of 99.5% or more and a mass percentage of 17.68%; (2) preparing an appropriate amount of tin alloy; (3) sequentially plating copper with a purity of 99.5% or more and a mass percentage of 8.73%, zinc with a purity of 99.5% or more and a mass percentage of 17.68%, and an appropriate amount of tin alloy on the outside of the high-purity iron; and (4) obtaining the electromagnetically fused tin alloy solder.
[0058] Taking type 6 tin alloy solder powder as an example, its single particle is prepared by sequentially plating pure iron spherical particles with a diameter of about 4.14um with 128nm thick pure copper, 270nm thick pure zinc, and 400nm thick tin alloy (various commercial tin alloys such as SN63 / PB37, SN42BI58, SN96.5CU0.5AG3.0 and SN99CU0.7AG0.3 can be selected according to actual needs), as shown in Figures 1 and 2. In the figure, the width of the iron atom is about 4.14um, the width of the copper atom is about 128nm, the width of the zinc atom is about 270nm, and the width of the tin alloy atom is about 400nm.
[0059] The present invention relates to an inventive tin alloy solder powder containing a specific proportion of a metal laminate material that can be heated by a specific electromagnetic field. Using specialized electromagnetic wave heating equipment, the inventive tin alloy solder is rapidly heated and welded from the inside out to complete the soldering process. This improves solder quality, significantly reduces tin alloy and flux usage, and significantly reduces power loss. Furthermore, post-soldering cleaning can be eliminated, thereby reducing costs and environmental pollution. In particular, it avoids damage to components caused by high temperatures and extends product life. This invention is poised to completely replace existing tin alloy solders.
[0060] The invention of tin alloy solder can be used to quickly heat and fuse from the inside out using a dedicated electromagnetic wave heating device to complete the soldering process. The invention has the following advantages:
[0061] 1. Due to the short surface heating time and low chance of oxidation, the invention of tin alloy solder can reduce the flux content, thereby reducing the harmful gases and residues generated by the flux at high temperature, thereby reducing air pollution and the risk of PCB leakage;
[0062] 2. The tin alloy solder powder of the present invention can be used in a non-contact specific electromagnetic field heating soldering process, eliminating the need for direct contact between the electric heating element and the solder, thereby preventing damage to electrostatically sensitive components caused by leakage current from the electric heating element.
[0063] 3. The tin alloy solder powder of the present invention utilizes dedicated electromagnetic wave heating equipment to simultaneously heat and fuse the entire tin alloy solder inside and out. This method is virtually unaffected by factors such as the heat dissipation of the soldered object, ambient temperature, and operator proficiency. High-temperature solder residue is virtually nonexistent, significantly improving solder quality and reducing solder quality control costs. In particular, it avoids the significant loss of electrical energy and solder slag due to oxidation and contamination that necessitates solder replacement during conventional hand-dip and wave soldering processes.
[0064] 4. The tin alloy solder powder of the present invention can also be used in the form of solder paste in the surface mount soldering (SMT) process for electronic products. Using dedicated electromagnetic wave heating equipment, the tin alloy solder of the present invention is rapidly heated and fused from the inside out to complete the soldering process. This avoids the soldering quality issues, high energy consumption, and significant air pollution associated with existing tin alloy solder reflow equipment (hot air heating equipment). Furthermore, because the tin alloy solder of the present invention is simultaneously heated and fused internally and externally, it does not require refrigeration to maintain surface activity, thus reducing production steps and the quality issues that arise from these steps, thereby reducing production costs and losses.
[0065] 5. The tin alloy solder of the present invention reduces the content of tin alloy, greatly reducing the cost of using solder.
[0066] The foregoing description is merely a specific embodiment of the present invention and a preferred embodiment thereof, but the scope of protection of the present invention is not limited thereto. Any similar substitutions or variations based on the principles described in the scope of the present application are intended to be covered by the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope of protection defined in the claims.
Claims
1. An electromagnetically fused tin alloy solder, characterized in that: include: High-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials, high-purity copper or other highly conductive metal materials and synthetic materials, high-purity zinc or other metal materials that easily form eutectic alloys with tin, and tin alloys constitute electromagnetic hot-melt tin alloy solder, which is a microparticle-shaped metal laminate material.
2. The electromagnetically fused tin alloy solder according to claim 1, characterized in that: The mass percentage of high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials is 28~40%.
3. The electromagnetically fused tin alloy solder according to claim 2, characterized in that: The mass percentage of high-purity iron or other magnetic transition metals and some rare earth metals or other magnetic synthetic materials is 38.8%.
4. The electromagnetically fused tin alloy solder according to claim 1, characterized in that: The mass percentage of high-purity copper or other highly conductive metal materials and synthetic materials is 5~15%.
5. The electromagnetically fused tin alloy solder according to claim 4, characterized in that: The mass percentage of high-purity copper or other high-conductivity metal materials and synthetic materials is 8.73%.
6. The electromagnetically fused tin alloy solder according to claim 1, characterized in that: The mass percentage of high-purity zinc or other metal materials that can easily form a eutectic alloy with tin is 10-22%.
7. The electromagnetically fused tin alloy solder according to claim 1, characterized in that: The mass percentage of high-purity zinc or other metal materials that can easily form a eutectic alloy with tin is 17.68%.
8. A method for preparing electromagnetically molten tin alloy solder, characterized in that: The following steps are involved: S1. Prepare iron with a purity of 99.5% or more and a mass percentage of 38.8%, copper with a purity of 99.5% or more and a mass percentage of 8.73%, and zinc with a purity of 99.5% or more and a mass percentage of 17.68; S2. Prepare an appropriate amount of tin alloy; S3, copper with a purity of 99.5% or more and 8.73% by mass, zinc with a purity of 99.5% or more and 17.68% by mass, and an appropriate amount of tin alloy are plated on the outside of the high-purity iron in sequence; S4, preparing electromagnetically heated molten tin alloy solder.
9. A method for soldering by using electromagnetic heat to melt tin alloy solder, characterized in that: The electromagnetically heated tin alloy solder according to any one of claims 1 to 8 is used, and a dedicated electromagnetic wave heating device is used to quickly heat and fuse the soldering process from the inside out.
Citation Information
Patent Citations
Solder ball and manufacturing method thereof
CN102672365A
Solder ball used for small-space PoP (package on package) structure
CN104485318A
Cu core ball, solder paste, formed solder, cu core column, and solder joint
CN105873716A
Solder ball structure, solder and manufacturing method
CN111283345A
Electromagnetic hot melting tin alloy solder and preparation and tin soldering method thereof
CN116441786A