Preparation method for and use of na xfe 3-0.5x(so 4) 3@c positive electrode material

The NaxFe3-0.5x(SO4)3@C cathode material is prepared by mixing conductive carbon materials and active materials and then heating them with microwaves, which solves the problem of complex preparation processes for cathode materials in existing sodium-ion batteries and achieves high-efficiency and energy-saving materials. The preparation is suitable for industrial production and improves the performance of the material.

WO2024221957A1PCT designated stage expired Publication Date: 2024-10-31SHENZHEN INST OF ADVANCED TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/137599
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-12-08
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The preparation process of existing sodium-ion battery cathode materials is complex. The traditional solid-phase method is time-consuming and has low thermal energy utilization. The co-precipitation method has complex equipment and difficult wastewater and gas treatment, making it difficult to achieve industrial production.

Method used

The NaxFe3-0.5x(SO4)3@C cathode material is prepared by mixing conductive carbon materials and active materials and then heating them with microwaves. By adjusting the proportion of raw materials, heating power and time, the particle size and phase structure of the product are precisely controlled, simplifying the process and Improve the purity and conductivity of materials.

Benefits of technology

A NaxFe3-0.5x(SO4)3@C cathode material with high purity, high conductivity and stable structure has been achieved. It has high reversible capacity and good cycle performance. The process is energy-saving and environmentally friendly, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023137599_31102024_PF_FP_ABST
    Figure CN2023137599_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a preparation method for and a use of a NaxFe3 - 0.5x(SO4)3@C positive electrode material. The preparation method comprises mixing raw materials of an active material with a conductive carbon material and then performing microwave heating. The raw materials of the active material comprise sodium sulfate and ferrous sulfate. The weight proportion of the conductive carbon material in the active material is 1-40 wt%. The mixing method comprises ball milling. The prepared NaxFe3 - 0.5x(SO4)3@C positive electrode material has advantages such as high purity, excellent electrical conductivity, a stable structure, high reversible capacity, high coulombic efficiency, and excellent cycle performance. The preparation method is energy-saving, environment-friendly and efficient, is easy to operate and has low equipment requirements, has abundant, low-cost raw materials, and is suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

A Na x Fe 3-0.5x Preparation method and application of (SO4)3@C positive electrode material Technical Field

[0001] The present invention belongs to the technical field of new energy materials, and specifically relates to a Na x Fe 3-0.5x Preparation method and application of (SO4)3@C positive electrode material. Background Art

[0002] As a supplement to lithium-ion batteries, sodium-ion batteries are expected to be used in low-speed electric vehicles, communication base stations, large-scale energy storage and other fields. As a key component of sodium-ion batteries, cathode materials affect the cost, energy density, cycle life, etc. of sodium-ion batteries. The current mainstream cathode materials for sodium-ion batteries are oxides, polyanionic compounds and Prussian blue analogs. The structure of polyanionic sulfate compounds can be expressed as follows: x MM´(SO4) m Y n denoted by . A represents an alkali metal ion, such as Li, Na, or K; M or M´ represents a transition metal ion, such as Fe, V, Mn, Co, and Cr; and Y represents an anion, such as F, PO₄, and OH. Monoanionic sulfate compounds typically form a three-dimensional structural framework composed of M / M´O₆ octahedra and SO₄ tetrahedra connected by co-points, edges, or faces. The alkali metal ions are distributed in the interstices of the framework and can move completely or partially within it. In dianionic sulfate compounds, the MX₆ (X is F or O) in their structure forms a covalent unit with anions such as PO₄ and then connects with SO₄ tetrahedra to form a three-dimensional framework. Monoanionic sulfate compounds have a stable structure, minimal volume change during Na insertion and extraction, and low activation energy for ion diffusion. These compounds offer advantages such as the ability to control the potential by adjusting the transition metal ion environment. Furthermore, sulfate has a strong inductive effect, making it easy to obtain high-potential materials, making them promising cathode materials. Technical issues

[0003] Na2Fe2(SO4)3 is a monoanionic sulfate cathode. In the prior art, an alluaudite-type Na2Fe2(SO4)3 material has been reported. In this material, FeO6 octahedrons with two Fe ion sites share edges to form Fe2O 10These dimers, in turn, link with SO₄ tetrahedra to form a three-dimensional open framework with three Na sites. Current methods for preparing Na₂Fe₂(SO₄)₃ cathodes include solid-phase synthesis and co-precipitation. Traditional solid-phase methods suffer from long calcination times, low thermal efficiency, uneven heating of particles, and the susceptibility to the formation of impurity phases. While the co-precipitation method offers good chemical homogeneity in the precursor solution and small product particle size, it also suffers from complex equipment and processes, difficult wastewater and exhaust gas treatment, and a long synthesis cycle, making industrial production challenging.

[0004] Therefore, it is imperative to solve the problem of complex preparation process of current polyanionic sulfate compound positive electrode materials. Technical Solutions

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a Na x Fe 3-0.5x Preparation method of (SO4)3@C positive electrode material, preparation of Na x Fe 3-0.5x The (SO4)3@C positive electrode material has the advantages of high purity, good conductivity, stable structure, high reversible capacity, high coulombic efficiency, and good cycle performance. The preparation method provided by the present invention is energy-saving, environmentally friendly, and efficient, with simple operation, low equipment requirements, abundant raw materials, and low cost, and is suitable for large-scale industrial production.

[0006] The second aspect of the present invention provides an application of the positive electrode material obtained by the preparation method in a positive electrode sheet.

[0007] A third aspect of the present invention provides an application of a positive electrode plate in a sodium ion battery.

[0008] According to the first embodiment of the present invention, a Na x Fe 3-0.5x The preparation method of (SO4)3@C positive electrode material comprises mixing raw materials of active material and conductive carbon material and then heating with microwave;

[0009] The raw materials of the active material include sodium sulfate and ferrous sulfate;

[0010] The conductive carbon material accounts for 1 to 40 wt% of the raw materials of the active material;

[0011] The mixing method includes ball milling.

[0012] According to some embodiments of the present invention, the conductive carbon material accounts for 5-10 wt % of the raw material of the active material.

[0013] According to some embodiments of the present invention, the conductive carbon material accounts for 7.5 wt % of the raw materials of the active material.

[0014] According to some embodiments of the present invention, the molar ratio of sodium sulfate to ferrous sulfate is 0.5x:(3-0.5x), wherein the value range of x is 0<x<6.

[0015] According to some preferred embodiments of the present invention, the molar ratio of sodium sulfate to ferrous sulfate is 0.5x:(3-0.5x), wherein x is 2.

[0016] According to some embodiments of the present invention, the ball milling includes wet ball milling and dry ball milling.

[0017] According to some embodiments of the present invention, the rotation speed of the ball mill is 100-1000 r / min.

[0018] According to some preferred embodiments of the present invention, the rotation speed of the ball mill is 500-1000 r / min.

[0019] According to some preferred embodiments of the present invention, the rotation speed of the ball mill is 500 r / min.

[0020] According to some embodiments of the present invention, the ball milling time is 1 to 600 minutes.

[0021] According to some embodiments of the present invention, the ball milling time is 120-600 min.

[0022] According to some embodiments of the present invention, the ball milling time is 120 minutes.

[0023] According to some embodiments of the present invention, the solvent for wet ball milling includes at least one of methanol, anhydrous ethanol, acetone, ethylene glycol and pyridine.

[0024] According to some embodiments of the present invention, the solvent for wet ball milling includes anhydrous ethanol.

[0025] According to some embodiments of the present invention, the wet ball milling further includes drying.

[0026] According to some embodiments of the present invention, the drying temperature is 50-200°C.

[0027] According to some embodiments of the present invention, the drying temperature is 80-200°C.

[0028] According to some embodiments of the present invention, the drying temperature is 80°C.

[0029] According to some embodiments of the present invention, the dry ball milling method includes performing ball milling under an inert atmosphere.

[0030] According to some embodiments of the present invention, the inert atmosphere includes at least one of nitrogen, argon and hydrogen.

[0031] According to some embodiments of the present invention, the temperature of the microwave heating is 300-400° C.; and the time of the microwave heating is 1-120 min.

[0032] According to some preferred embodiments of the present invention, the temperature of the microwave heating is 350-400° C.; and the time of the microwave heating is 20-120 min.

[0033] According to some preferred embodiments of the present invention, the temperature of the microwave heating is 350° C.; and the time of the microwave heating is 20 min.

[0034] In the present invention, the particle size and phase structure of the product can be accurately controlled by adjusting parameters such as the raw material ratio, heating power and time.

[0035] According to some embodiments of the present invention, the conductive carbon material includes at least one of carbon nanotubes, carbon fibers, activated carbon, Ketjen black, acetylene black, super P, hard carbon, soft carbon, graphite, and graphene.

[0036] According to some embodiments of the present invention, the conductive carbon material includes graphene.

[0037] According to some embodiments of the present invention, the ferrous sulfate includes ferrous sulfate monohydrate or anhydrous ferrous sulfate.

[0038] According to some embodiments of the present invention, the raw material for preparing ferrous sulfate includes at least one of FeSO4·7H2O, FeSO4·5H2O, and FeSO4·4H2O.

[0039] According to some preferred embodiments of the present invention, the raw material for preparing ferrous sulfate includes FeSO4·7H2O.

[0040] According to some embodiments of the present invention, the method for preparing ferrous sulfate includes drying the raw materials for preparing ferrous sulfate.

[0041] According to some embodiments of the present invention, the drying method comprises microwave drying.

[0042] According to some embodiments of the present invention, the microwave drying temperature is 100-400° C., and the microwave drying time is 1-120 min.

[0043] According to some preferred embodiments of the present invention, the microwave drying temperature is 250° C., and the microwave drying time is 10 minutes.

[0044] According to an embodiment of the second aspect of the present invention, an application of the positive electrode material in a positive electrode sheet is proposed.

[0045] According to some embodiments of the present invention, the positive electrode sheet includes a current collector and a positive electrode material layer covering the current collector, the positive electrode material layer includes a positive electrode active material, a conductive agent and a binder, and the positive electrode active material is the Na x Fe 3-0.5x (SO4)3@C positive electrode material.

[0046] According to an embodiment of the third aspect of the present invention, an application of the positive electrode sheet in a sodium ion battery is proposed.

[0047] According to some embodiments of the present invention, the applications include mobile electronic communication devices, electric vehicles, two-wheeled electric bicycles, low-speed electric vehicles, energy storage batteries, power batteries and energy storage power stations. Beneficial effects

[0048] According to an embodiment of the present invention, a Na x Fe 3-0.5x The preparation method of (SO4)3@C positive electrode material has at least the following beneficial effects:

[0049] 1. The present invention adopts a method of ball milling conductive carbon material and active material together, which simplifies the process and reduces costs. The addition of conductive carbon material provides a larger contact area for the active material, which is conducive to the uniform dispersion of the active material. After the active material and the conductive carbon material are mixed and heated by microwaves, a carbon-coated polyanionic sulfate positive electrode material is formed, wherein the heterogeneous interface formed by the conductive carbon material and the active material promotes the improvement of the crystallinity of the active material and stabilizes the material structure. The conductive carbon material acts as a bridge for electron transfer between the particles of the active material, improving the defect of poor conductivity of the active material itself.

[0050] 2. The present invention adopts the method of synthesizing positive electrode materials by microwave heating, which can greatly shorten the synthesis time, achieve uniform heating, and have no hysteresis effect. x Fe 3-0.5x (SO4)3@C cathode materials offer advantages such as high purity, good conductivity, stable structure, high reversible capacity, high coulombic efficiency, and excellent cycling performance. The preparation method provided by the present invention is energy-efficient, environmentally friendly, and highly efficient, with simple operation, low equipment requirements, abundant raw materials, and low cost, making it suitable for large-scale industrial production.

[0051] 3. Other features and advantages of the present invention will be set forth in the following description, and in part will become apparent from the description, or may be understood by practicing the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the following description of the embodiments with reference to the accompanying drawings, in which:

[0053] FIG1 is a SEM image of a Na2Fe2(SO4)3@C powder sample of Example 1 of the present invention;

[0054] FIG2 is an XRD spectrum of Na2Fe2(SO4)3@C according to Example 1 of the present invention. Best Mode for Carrying Out the Invention

[0055] The following will clearly and completely describe the concept of the present invention and the technical effects produced in conjunction with the embodiments, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention. Unless otherwise specified, the test methods used in the embodiments are all conventional methods; the materials used, unless otherwise specified, can all be obtained from commercial channels.

[0056] Example 1

[0057] This embodiment discloses a method for preparing a polyanion sulfate cathode material, the molecular formula of which is Na2Fe2(SO4)3@C, and the specific steps are as follows:

[0058] S1: Weigh 556.02 g (2 mol) of FeSO4·7H2O into a microwave oven. Heat to 250°C under nitrogen and keep warm for 10 min to obtain anhydrous FeSO4.

[0059] S2: Weigh 142.04 g (1 mol) of anhydrous Na2SO4, 303.82 g (2 mol) of anhydrous FeSO4, and 33.44 g (7.5 wt%) of graphene;

[0060] S3: The raw materials in step S2 were mixed and added to a ball mill, and 40 ml of anhydrous ethanol was added as a grinding aid. The mixture was ball milled at a speed of 500 r / min for 120 min to obtain a highly dispersed precursor powder, which was then dried in an oven at 80°C for 0.5 h to completely evaporate the solvent;

[0061] S4: Place the precursor in a microwave oven, heat to 350°C and keep warm for 20 minutes, and finally cool to room temperature to obtain the Na2Fe2(SO4)3@C positive electrode material.

[0062] Figure 1 is an SEM image of Na2Fe2(SO4)3@C provided in Example 1 of the present invention. It can be seen from the figure that the particle size is between nanometers and micrometers, and has a large number of pores. There is no agglomeration between the particles, and the surface is covered with evenly distributed graphene.

[0063] Figure 2 is the XRD spectrum of Na2Fe2(SO4)3@C provided in Example 1 of the present invention, which proves that the prepared sample has good crystallinity and purity, no impurity peaks exist, and the addition of carbon material does not affect the phase composition of the material. Modes for Carrying Out the Invention

[0064] Example 2

[0065] This embodiment discloses a method for preparing a polyanionic sulfate cathode material having a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that FeSO4·4H2O is placed in a microwave oven, heated to 100°C under nitrogen protection, and kept warm for 120 minutes to obtain FeSO4·H2O.

[0066] Example 3

[0067] This embodiment discloses a method for preparing a polyanionic sulfate cathode material having a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that the 556.02 g (2 mol) FeSO4·7H2O in step S1 is replaced with 484.00 g (2 mol) Fe(SO4)·5H2O, which is then placed in a microwave oven and heated to 300°C under vacuum conditions and kept warm for 1 min to obtain anhydrous FeSO4.

[0068] Example 4

[0069] This embodiment discloses a method for preparing a polyanionic sulfate cathode material having a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that FeSO4·7H2O is placed in a microwave oven, heated to 400°C under vacuum conditions, and kept warm for 1 minute to obtain anhydrous FeSO4.

[0070] Example 5

[0071] This embodiment discloses a method for preparing a polyanionic sulfate cathode material having the molecular formula Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that acetone is used as a grinding aid to obtain a highly dispersed precursor powder, which is then baked in a 50°C oven for 0.5 h to completely evaporate the solvent.

[0072] Example 6

[0073] This embodiment discloses a method for preparing a polyanionic sulfate cathode material having the molecular formula Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that ethylene glycol is used as a grinding aid to obtain a highly dispersed precursor powder, which is then baked in an oven at 200°C for 0.5 h to completely evaporate the solvent.

[0074] Example 7

[0075] This embodiment discloses a method for preparing a polyanion sulfate cathode material with a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that dry ball milling is used, and after the ball milling is completed, the precursor is directly placed in a microwave oven for sintering.

[0076] Example 8

[0077] This embodiment discloses a method for preparing a polyanion sulfate positive electrode material with a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that the added conductive material is carbon nanotubes, and the rest is the same as that of Example 1.

[0078] Example 9

[0079] This embodiment discloses a method for preparing a polyanion sulfate positive electrode material with a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that the added conductive material is Ketjen black, and the rest is the same as that of Example 1.

[0080] Example 10

[0081] This embodiment discloses a method for preparing a polyanion sulfate positive electrode material with a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that the added conductive material is graphite, and the rest is the same as that of Example 1.

[0082] Example 11

[0083] This embodiment discloses a method for preparing a polyanion sulfate cathode material with a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that 4.46 g (1 wt%) of graphene is weighed, and the rest is the same as that of Example 1.

[0084] Example 12

[0085] This embodiment discloses a method for preparing a polyanionic sulfate cathode material with a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that 178.34 g (40 wt%) of graphene is weighed, and the rest is the same as that of Example 1.

[0086] Example 13

[0087] This embodiment discloses a method for preparing a polyanion sulfate cathode material with a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that the material is ball milled at a speed of 100 r / min for 600 min, and the rest is the same as that of Example 1.

[0088] Example 14

[0089] This embodiment discloses a method for preparing a polyanion sulfate cathode material with a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that the material is ball milled at a speed of 1000 r / min for 1 min, and the rest is the same as that of Example 1.

[0090] Example 15

[0091] This embodiment discloses a method for preparing a polyanion sulfate positive electrode material with a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that the material is heated to 300°C and kept warm for 120 minutes. The rest is the same as that of Example 1.

[0092] Example 16

[0093] This embodiment discloses a method for preparing a polyanion sulfate positive electrode material with a molecular formula of Na2Fe2(SO4)3@C. The preparation method is similar to that of Example 1, except that the material is heated to 400°C and kept warm for 1 minute. The rest is the same as that of Example 1.

[0094] Example 17

[0095] This embodiment discloses a method for preparing a polyanion sulfate positive electrode material, the molecular formula of which is Na 2.7 Fe 1.65 (SO4)3@C, in its preparation method, the molar ratio of sodium sulfate to ferrous sulfate is adjusted according to the chemical formula molar ratio, and the rest is the same as Example 1.

[0096] Example 18

[0097] This embodiment discloses a method for preparing a polyanion sulfate positive electrode material, the molecular formula of which is Na 1.5 Fe 2.25(SO4)3@C, in its preparation method, the molar ratio of sodium sulfate to ferrous sulfate is adjusted according to the chemical formula molar ratio, and the rest is the same as Example 1.

[0098] Comparative Example 1

[0099] This comparative example discloses a method for preparing a polyanionic sulfate cathode material having the molecular formula Na2Fe2(SO4)3@C. The preparation method differs from that of Example 1 in that S4 is replaced by heating to 350°C and holding for 20 minutes in a box-type furnace under a nitrogen atmosphere, followed by cooling to room temperature to obtain the Na2Fe2(SO4)3@C cathode material. The remainder of the preparation method is the same as that of Example 1.

[0100] Comparative Example 2

[0101] This comparative example discloses a method for preparing a polyanionic sulfate positive electrode material with a molecular formula of Na2Fe2(SO4)3@C. In its preparation method, the difference between this comparative example and Example 1 is that the mass of graphene used in S2 is 200.64g (accounting for 45wt% of the raw materials of the positive electrode material active material), and the rest is the same as Example 1.

[0102] Test Example 1

[0103] Test Example 1 is a sodium ion half-cell prepared using the positive electrode materials of Examples 1 to 18 and Comparative Examples 1 to 2. The preparation method includes the following steps:

[0104] A1: Add 1.8g of Na2Fe2(SO4)3@C cathode material powder and 0.2g of polyvinylidene fluoride to 2mL of nitrogen-methylpyrrolidone and grind thoroughly to obtain a uniform slurry. Apply the slurry evenly to the surface of aluminum foil (positive electrode current collector) and vacuum dry. Cut the dried electrode sheet into 10mm diameter discs, compact them, and use them as battery positive electrode sheets.

[0105] A2: Cut the glass fiber film into 16mm diameter discs and use them as diaphragms.

[0106] A3: Weigh 1.2244 g of sodium perchlorate and dissolve it in 9.5 mL of propylene carbonate. Add 0.5 mL of fluoroethylene carbonate as an additive. Mix thoroughly and use this as the electrolyte.

[0107] A4: Press the sodium metal into thin sheets and cut them into 12mm diameter discs to be used as the negative electrode of the battery.

[0108] A5: In an inert gas-protected glove box, stack the prepared positive electrode, separator, and negative electrode tightly in sequence, add electrolyte to completely soak the separator, and then encapsulate the stacked part into a button battery casing to complete the battery assembly.

[0109] Test Example 2

[0110] Test Example 2 is a sodium ion full battery prepared using the positive electrode materials of Examples 1, 3, 7, 8, 10, 11, 12, 15, 17 and Comparative Examples 1-2, and the negative electrode material is hard carbon. The preparation method includes the following steps:

[0111] A1: Add 1.8g of Na2Fe2(SO4)3@C cathode material powder and 0.2g of polyvinylidene fluoride to 2mL of nitrogen-methylpyrrolidone and grind thoroughly to obtain a uniform slurry. Apply the slurry evenly to the surface of aluminum foil (positive electrode current collector) and vacuum dry. Cut the dried electrode sheet into 10mm diameter discs, compact them, and use them as the battery positive electrode.

[0112] A2: Cut the glass fiber film into 16mm diameter discs and use them as diaphragms.

[0113] A3: Weigh 1.2244 g of sodium perchlorate and dissolve it in 9.5 mL of propylene carbonate. Add 0.5 mL of fluoroethylene carbonate as an additive. Mix thoroughly and use this as the electrolyte.

[0114] A4: Add 0.8g of hard carbon, 0.1g of carbon black, and 0.1g of polyvinylidene fluoride to 1mL of nitrogen-methyl pyrrolidone and grind thoroughly to obtain a uniform slurry. Apply the slurry evenly to the surface of aluminum foil (negative electrode current collector) and vacuum dry. Cut the dried electrode sheet into 12mm diameter discs, compact them, and use them as the battery negative electrode.

[0115] A5: In an inert gas-protected glove box, stack the prepared positive electrode, separator, and negative electrode tightly in sequence, add electrolyte to completely soak the separator, and then encapsulate the stacked part into a button battery casing to complete the battery assembly.

[0116] Performance testing: Sodium-ion batteries prepared from the above-mentioned cathode materials were tested. Constant current charge and discharge tests were conducted using a BTSDA test system from Shenzhen Xinwei Electronics Co., Ltd. in a constant temperature and humidity chamber (25°C, 35%). The cathode loading was 2-4 mg / cm3. 2, for the full battery, the N / P ratio of the positive and negative electrodes is 1.2, and the battery charge and discharge rate is 5C (1 C=120mAh / g). The voltage range of Test Example 1 is 2.0-4.5V, and the voltage range of Test Example 2 is 1.5-4.1V. The first-cycle capacity obtained by the sodium ion half-battery with Example 1-18 as the positive electrode in Test Example 1 is basically the same, about 82~86mAh / g, and other test results are shown in Table 1. The first-cycle capacity obtained by the sodium ion full battery with the material obtained in the embodiment of the present technical solution as the positive electrode in Test Example 2 is basically the same, about 78~82mAh / g, and other test parameters and results are shown in Table 2.

[0117] Table 1 Performance of sodium ion half-cell

[0118] Example Positive electrode active material First cycle discharge capacity (mAh / g) 1000th cycle median discharge voltage (V) 1000th cycle Coulombic efficiency (%) 3500th cycle capacity retention rate (%) 1Na2Fe2(SO4)3@C863.7899.780.512Na2Fe2(SO4)3@C833.7197.677.183Na2Fe2(SO4)3@C843.7798.479.354Na2Fe2(SO4)3@C85 3.7699.178.995Na2Fe2(SO4)3@C853.7498.879.396Na2Fe2(SO4)3@C843.7399.079.587Na2Fe2(SO4)3 @C823.7598.677.138Na2Fe2(SO4)3@C853.7799.478.789Na2Fe2(SO4)3@C843.7499.378.2210Na2Fe2(S O4)3@C853.7298.777.9811Na2Fe2(SO4)3@C823.5591.949.0912Na2Fe2(SO4)3@C833.7699.276.1313N a2Fe2(SO4)3@C833.7199.376.0614Na2Fe2(SO4)3@C843.7799.475.7115Na2Fe2(SO4)3@C833.7499.17 6.3116Na2Fe2(SO4)3@C853.7699.478.0617Na2.7Fe1.65(SO4)3@C863.7799.378.9818Na1.5Fe2.25(SO4)3@C833.7699.178.12Comparative Example 1Na2Fe2(SO4)3@C203.1086.754.46Comparative Example 2Na2Fe2(SO4)3@C503.0690.561.23

[0119] Table 2 Full battery positive and negative electrode materials and performance

[0120] Example Positive electrode active material First cycle discharge capacity (mAh / g) 100th discharge median voltage (V) 100th cycle Coulombic efficiency (%) 500th cycle capacity retention (%) 1Na2Fe2(SO4)3@C823.2199.681.653Na2Fe2(SO4)3@C803.1599.480.457Na2Fe2(SO4)3@C813.2099.179.968Na2Fe2(SO4)3@C813.2199.379.7510Na2Fe2(SO4)3@C793.16 99.578.7511Na2Fe2(SO4)3@C783.0491.259.7512Na2Fe2(SO4)3@C793.1899.280.0515Na2Fe2(SO4)3@C803.1799.578.3317Na2.7Fe1.65(SO4)3@C813.1999.480.48Comparative Example 1Na2Fe2(SO4)3@C182.3183.165.12Comparative Example 2Na2Fe2(SO4)3@C432.2584.868.47

[0121] As can be seen from Tables 1 and 2, the molecular formula of the solid phase microwave method prepared by the present invention is Na x Fe 3-0.5x (SO4)3@C (0<x<6) carbon-coated polyanion sulfate positive electrode active material has the advantages of high first cycle discharge capacity, high battery median voltage, high coulombic efficiency, and good cycle performance. Test Example 1 uses different raw material ratios and synthesis conditions to obtain Na x Fe 3-0.5x In a sodium-ion half-cell assembled with (SO4)3@C positive electrode material, it was found that the doping amount of the conductive carbon material had a significant impact on the electrochemical performance of the positive electrode material. When the conductive carbon material content was too low, the positive electrode conductivity dropped significantly, resulting in poor performance; when the conductive carbon material content was too high, the active material content was low, resulting in a decrease in battery performance. At the same time, the performance of the battery obtained in Comparative Example 1 using a traditional heat treatment method was significantly poorer. The reason is that the traditional heat treatment method has slow heat transfer and cannot fully react to obtain Na2Fe2(SO4)3@C material under short heating conditions. Other different raw material ratios and synthesis conditions have a certain impact on the electrochemical performance of the positive electrode, but the impact is not drastic.

[0122] As can be seen from Table 2, the Na x Fe 3-0.5xA sodium-ion full battery was assembled using (SO4)3@C cathode materials and cycled at a 5C rate. The amount of conductive carbon material doped in the examples significantly impacted battery performance, while capacity retention was high under all other conditions. However, the batteries produced in Comparative Example 1, which used a traditional heat treatment method, and Comparative Example 2, which used excess conductive carbon, exhibited poor performance, likely due to similar reasons as analyzed in Table 1.

[0123] The method provided by the invention has simple process, fast reaction and low cost, and can be widely used in industrial production.

[0124] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the scope of knowledge possessed by ordinary technicians in the relevant technical field without departing from the scope of the present invention.

Claims

1. A Na x Fe 3-0.5x The method for preparing a (SO4)3@C positive electrode material is characterized in that: The method comprises mixing the raw material of the active material and the conductive carbon material and then heating with microwave; The raw materials of the active material include sodium sulfate and ferrous sulfate; The conductive carbon material accounts for 1-40 wt% of the raw material of the active material; The mixing method includes ball milling.

2. Na according to claim 1 x Fe 3-0.5x The method for preparing a (SO4)3@C positive electrode material is characterized in that: The molar ratio of the sodium sulfate to the ferrous sulfate is 0.5x:(3-0.5x), wherein the value range of x is 0<x<6.

3. Na according to claim 1 x Fe 3-0.5x The method for preparing a (SO4)3@C positive electrode material is characterized in that: The ball milling includes wet ball milling and dry ball milling.

4. Na according to claim 3 x Fe 3-0.5x The method for preparing a (SO4)3@C positive electrode material is characterized in that: The solvent of the wet ball milling includes at least one of methanol, anhydrous ethanol, acetone, ethylene glycol and pyridine; preferably, the wet ball milling further includes drying; preferably, the drying temperature is 50-200°C.

5. Na according to claim 3 x Fe 3-0.5x The method for preparing a (SO4)3@C positive electrode material is characterized in that: The dry ball milling method comprises ball milling under an inert atmosphere; preferably, the inert atmosphere comprises at least one of nitrogen, argon and hydrogen.

6. Na according to claim 1 x Fe 3-0.5x The method for preparing a (SO4)3@C positive electrode material is characterized in that: The temperature of the microwave heating is 300-400° C.; the time of the microwave heating is 1-120 min.

7. Na according to claim 1 x Fe 3-0.5x The method for preparing a (SO4)3@C positive electrode material is characterized in that: The conductive carbon material includes at least one of carbon nanotubes, carbon fibers, activated carbon, Ketjen black, acetylene black, super P, hard carbon, soft carbon, graphite and graphene.

8. Na according to claim 1 x Fe 3-0.5x The method for preparing a (SO4)3@C positive electrode material is characterized in that: The method for preparing ferrous sulfate comprises drying the raw materials for preparing ferrous sulfate; preferably, the drying method comprises microwave drying; preferably, the temperature of the microwave drying is 100-400° C., and the time of the microwave drying is 1-120 min.

9. Use of a positive electrode material obtained by the preparation method according to any one of claims 1 to 8 in a positive electrode sheet.

10. Use of the positive electrode sheet as claimed in claim 9 in a sodium ion battery.

Citation Information

Patent Citations

  • Method for synthesizing sodium-ion battery positive-electrode material NaFePO4 through microwave method

    CN105006548A

  • Sodium ferrous sulfate / graphene composite positive electrode material for sodium ion battery, and preparation method thereof

    CN106848236A

  • Carbon composite sodion anode material and preparation method thereof

    CN108682827A

  • Battery positive electrode material as well as preparation method and application thereof

    CN111326715A

  • Carbon-coated sodium ferric sulfate positive electrode material and preparation method thereof

    CN115020681A