Method for high-value recovery and treatment of electrolytic manganese metal industrial waste salt
Through the 4-stage precipitation separation and 2-stage crystallization process, combined with low-temperature molten salt treatment, the problem of recycling waste salt in electrolytic manganese industry has been successfully solved, and the recycling and environmental protection effect of high-value resources is achieved, and it is suitable for large-scale industrial applications.
Patent Information
- Application Number
- CN202411276680.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-29
AI Technical Summary
The existing technology is difficult to effectively recycle and treat electrolytic manganese industrial waste salt, resulting in low pollution and industrial value, and cannot achieve large-scale application.
The 4-stage precipitation separation, 2-stage crystallization and low-temperature molten salt treatment process are used to separate and recover manganese, magnesium and ammonia nitrogen resources through chemical means such as ammonia water, oxygen, ammonium persulfate, magnesium precipitation reagents and phosphoric acid to form high-value products.
It realizes high-value recycling of electrolytic manganese industry waste salt, reduces energy consumption and costs, and reduces pollution. It is suitable for large-scale industrial applications. Its products include battery-grade manganese sulfate, industrial-grade ammonium sulfate and fertilizer-grade ammonium phosphate.
Smart Images

Figure CN119038609A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metallurgical solid waste treatment, and in particular relates to a method for high-value recovery and treatment of electrolytic manganese metal industrial waste salt. Background Art
[0002] As a traditional high-pollution industry, electrolytic manganese production generates a large amount of industrial solid waste during the manufacturing process. In addition to electrolytic manganese slag, it also generates a large amount of electrolytic manganese industrial waste salt. According to statistics, for every ton of electrolytic manganese produced, 1 to 2 tons of waste salt are generated.
[0003] The main disposal method for these industrial waste salts is to landfill them together with electrolytic manganese slag. Electrolytic manganese industrial waste salts are mainly produced in the static sedimentation and electrolysis process of electrolytic manganese production process. Its main components are Mg, Mn, NH4 + / NH3, Ca sulfate, and a small amount of sand. The mineral raw materials for electrolytic manganese production are mainly rhodochrosite and pyrolusite, which are accompanied by magnesite, orthorhombic zeolite, albite, white calcium silicate, hydromanganese calcium calcium, ferro-calcium rhodonite, calcium phosphate and other Mg and Ca minerals. When these minerals are leached with sulfuric acid, Mg and a small amount of Ca will enter the leachate along with Mn. As the electrolytic manganese anode liquid continues to circulate in the system, Mg in the solution is continuously enriched, and can even reach about 38g / L. When the leachate completes leaching and impurity removal, in the static sedimentation process and the electrolysis process, the Mg ions in the solution will cooperate with the Mn and NH4 in the solution. + / NH3 crystallizes and precipitates in the form of sulfate complex salt to form electrolytic manganese industrial waste salt. The physical phase of the waste salt is mainly ammonium sulfate, including hexahydrate magnesium sulfate, hexahydrate ammonium manganese sulfate, ammonium manganese sulfate, epsom salt and hemihydrate gypsum. The electrolytic manganese industrial waste salt, which is mainly soluble sulfate, is landfilled together with the electrolytic manganese slag, which not only increases the amount of electrolytic manganese slag, but also increases the soluble salt content in the electrolytic manganese slag, making it more difficult to treat it harmlessly. At the same time, it is washed into the slag field leachate with rainwater, increasing the amount of leachate and its salt concentration, and increasing the risk of pollution to the surrounding soil and water.
[0004] In this regard, many researchers have studied how to recycle and treat electrolytic manganese industrial waste salt. For example, patent application CN102154556A discloses a method for recovering manganese and magnesium from complex salt crystals produced in the electrolytic manganese process, including dissolving the complex salt in water and filtering it, adding ammonium persulfate to the resulting filtrate, precipitating to prepare manganese dioxide, adding oxalic acid to the filtrate after secondary filtration to precipitate magnesium, and obtaining magnesium oxalate and a filtrate containing ammonium sulfate after three filtrations. Although magnesium and manganese appear to be recovered, the separation of manganese and magnesium is not complete, the impurity content of the recovered product is high, the added value is low, and the required cost is high, so the industrial value is low and large-scale practical application cannot be achieved.
[0005] In addition, CN108396158A discloses a method for treating double salt crystals in an electrolytic manganese process, comprising dissolving the double salt crystals with 40°C water to a saturated solution, adjusting the pH value to 6.5-8.5 with ammonia water, filtering and introducing CO2 gas into the filtrate to generate manganese carbonate precipitation, filtering and adding magnesium oxide to the secondary filtrate to generate magnesium sulfate and ammonia water, sending the reaction product to a deamination tower for deamination, and crystallizing the solution after deamination to obtain a magnesium sulfate product. CN105154916A discloses a method for reducing the impurity magnesium content of an electrolytic manganese system by step-by-step precipitation, comprising adding liquid ammonia to the anolyte to adjust the pH, then adding a manganese precipitation additive, precipitating to obtain manganese precipitation slag and manganese precipitation liquid, returning the obtained manganese precipitation slag to the electrolytic manganese workshop to neutralize the residual acid, and adding a magnesium precipitation reagent to the manganese precipitation liquid. The industrial cost required for this method is high, and economic benefits cannot be obtained, so there is little hope for large-scale application. CN109321944A discloses a method for comprehensive utilization of by-product waste residue from electrolytic manganese, including removing manganese with ammonium bicarbonate, adding monoammonium phosphate and ammonia water to the filtered filtrate to obtain ammonium magnesium phosphate, and finally adjusting the pH value with sulfuric acid to prepare ammonium sulfate. However, these processes are difficult to achieve a more thorough separation of different resources, and the added value of the recovered products is low, so it is difficult to achieve high-value recovery of electrolytic manganese industrial waste salt, and thus difficult to achieve large-scale practical application. Summary of the invention
[0006] In response to the above technical problems, the present application provides a method for high-value recovery and treatment of electrolytic manganese industrial waste salt.
[0007] To achieve the above objectives, this application proposes the following technical solutions: A method for high-value recovery and treatment of electrolytic manganese metal industrial waste salt, comprising: (1) Dissolving electrolytic manganese metal industrial waste salt in water and filtering to obtain a waste salt solution; (2) adding ammonia water to the waste salt solution and introducing oxygen-containing gas to carry out a first reaction, and performing solid-liquid separation to obtain a first manganese oxide slag and a first precipitated liquid; adding ammonium persulfate to the first precipitated liquid, heating and keeping the temperature, and carrying out a second reaction. After the reaction is completed, performing solid-liquid separation to obtain a second manganese oxide slag and a second precipitated liquid; (3) adding a magnesium precipitation reagent to the second precipitated liquid, carrying out a third reaction, and performing solid-liquid separation to obtain a magnesium product and a third precipitated liquid; adding concentrated phosphoric acid to the third precipitated liquid, carrying out a fourth reaction, and performing solid-liquid separation to obtain magnesium ammonium phosphate and a magnesium-removed liquid; (4) adjusting the pH value of the solution after magnesium removal, and then evaporating and crystallizing to obtain ammonium sulfate; (5) The obtained manganese oxide slag is mixed with ammonium sulfate, subjected to a low-temperature molten salt reaction, and the molten salt reaction product is immersed in water to obtain a manganese sulfate solution, which is then evaporated and crystallized to obtain manganese sulfate.
[0008] Furthermore, in step (2), the temperature of the first reaction is 25 to 60° C.; and the time of the first reaction is 120 to 480 min.
[0009] Furthermore, in step (2), the concentration of the ammonia water is 4 to 25%; the amount of the ammonia water added is determined according to the molar ratio of nitrogen contained in the ammonia water to manganese in the waste salt solution being 3 to 8:1.
[0010] Furthermore, in step (2), the oxygen partial pressure of the oxygen-containing gas is 21 to 100%.
[0011] Furthermore, in step (2), the gas flow rate of the oxygen-containing gas is 5 to 20 L of oxygen-containing gas per liter of waste salt solution per minute.
[0012] Furthermore, in step (2), the temperature of the second reaction is 60 to 100° C.; and the time of the second reaction is 120 to 480 min.
[0013] Furthermore, in step (2), the amount of ammonium persulfate added is 1 to 2 times the molar amount of manganese ions in the first precipitation liquid.
[0014] Furthermore, in step (3), the temperature of the third reaction is 50-100° C.; and the time of the third reaction is 120-300 min.
[0015] Furthermore, in step (3), before adding the magnesium precipitation reagent, the pH of the second precipitation liquid is adjusted to 6.5-8.
[0016] Furthermore, in step (3), after adding the magnesium precipitation reagent, the initial reaction pH of the system is adjusted to 7.5-8.5.
[0017] Furthermore, in step (3), the magnesium precipitation reagent is ammonium carbonate or ammonium bicarbonate.
[0018] In step (3), the amount of ammonium bicarbonate or ammonium carbonate added is 2 to 5 times the molar amount of magnesium ions in the second precipitation liquid.
[0019] Furthermore, in step (3), the temperature of the fourth reaction is 25 to 60° C.; and the time of the fourth reaction is 30 to 180 min.
[0020] Furthermore, in step (3), the amount of phosphoric acid added is determined according to the molar amount of H3PO4 in phosphoric acid being 1.0 to 1.5 times the molar amount of magnesium ions in the third post-precipitation liquid. Furthermore, in step (3), the phosphoric acid is concentrated phosphoric acid.
[0021] Furthermore, in step (4), the pH value of the magnesium-removed liquid is adjusted to 5.0-6.8.
[0022] Furthermore, in step (4), sulfuric acid is used to adjust the pH value of the magnesium-removed liquid; preferably, in step (4), the sulfuric acid is concentrated sulfuric acid.
[0023] Furthermore, in step (5), the ammonium sulfate and the manganese oxide slag are determined according to a molar ratio of (NH4)2SO4 / Mn of 1.0 to 1.5.
[0024] Furthermore, in step (5), the mixing is ball milling mixing.
[0025] Furthermore, in step (5), the molten salt reaction temperature is 400-500° C.; and the molten salt reaction time is 60-180 min.
[0026] Furthermore, in step (5), the liquid-to-solid ratio of the water immersion is 10:1 to 2.5:1 mL / g; the temperature of the water immersion is 25 to 60° C.; and the time of the water immersion is 10 to 120 min.
[0027] Furthermore, step (5) also includes recovering the ammonia-containing flue gas generated by the low-temperature molten salt reaction.
[0028] Furthermore, in step (1), 50 to 300 g of electrolytic manganese industrial waste salt is dissolved in 1 L of water.
[0029] Furthermore, in step (1), the particle size of the electrolytic manganese industrial waste salt is less than 100 mesh.
[0030] Compared with the prior art, one or more of the above technical solutions can achieve at least one of the following beneficial effects: The method for recycling and treating electrolytic manganese metal industrial waste salt of the present application is simple in process, mild in process conditions, low in energy consumption, and low in cost, and can eliminate the environmental pressure of electrolytic manganese metal industrial waste salt storage, and realize the recovery of Mg, Mn, NH4 + / High-value recovery of NH3 resources and high returns from the recovery process.
[0031] The method for recycling and treating electrolytic manganese metal industrial waste salt can return all products except the product to the treatment system for reuse during the treatment process, does not generate secondary waste, is clean and environmentally friendly, reduces the environmental pressure of related enterprises while increasing economic benefits, and is suitable for large-scale industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 The present invention is a process flow chart of the high-value recovery and treatment method of electrolytic manganese metal industrial waste salt. DETAILED DESCRIPTION
[0034] In view of the technical problems of existing electrolytic manganese industrial waste salt treatment methods such as pollution, or high cost of benefits that make it difficult to apply on a large scale, the applicant has, after extensive research, innovatively proposed a method for recovering manganese, magnesium, and ammonia nitrogen resources from electrolytic manganese industrial waste salt with simple process, mild process conditions, and low processing cost. This method not only achieves the effective treatment of electrolytic manganese industrial waste salt, but also effectively and highly valuable recovers the manganese, ammonium, and magnesium resources therein. This not only reduces the soluble salt content in the electrolytic manganese slag, but also achieves high-value recovery of resources, which is suitable for large-scale application.
[0035] Specifically, innovative processes such as four-stage sedimentation separation, two-stage crystallization, molten salt treatment, and room-temperature water immersion are used to resource-process electrolytic manganese industrial waste salt. During the treatment process, all products except the final product can be returned to the treatment system, without generating secondary waste, which is clean and environmentally friendly.
[0036] Some embodiments of the present invention provide a method for high-value recovery and treatment of electrolytic manganese metal industrial waste salt, comprising: (1) Dissolving electrolytic manganese metal industrial waste salt in water and filtering to obtain a waste salt solution; (2) adding ammonia water to the waste salt solution and introducing oxygen-containing gas to carry out a first reaction, and performing solid-liquid separation to obtain a first manganese oxide slag and a first precipitated liquid; adding ammonium persulfate to the first precipitated liquid, heating and keeping the temperature, and carrying out a second reaction. After the reaction is completed, performing solid-liquid separation to obtain a second manganese oxide slag and a second precipitated liquid; (3) adding a magnesium precipitation reagent to the second precipitated liquid, carrying out a third reaction, and performing solid-liquid separation to obtain a magnesium product and a third precipitated liquid; adding phosphoric acid to the third precipitated liquid, carrying out a fourth reaction, and performing solid-liquid separation to obtain magnesium ammonium phosphate and a magnesium-removed liquid; (4) adjusting the pH value of the solution after magnesium removal, and then evaporating and crystallizing to obtain ammonium sulfate; (5) After mixing the obtained manganese oxide slag with ammonium sulfate, performing a low-temperature molten salt reaction, immersing the molten salt reaction product in water to obtain a manganese sulfate solution, and then obtaining manganese sulfate through evaporation and crystallization; in this step, the obtained manganese oxide slag includes a first manganese oxide slag and a second manganese oxide slag.
[0037] The method has the advantages of short process flow, low energy consumption, low cost and low pollution. The final products obtained through the process are battery-grade manganese sulfate, industrial-grade and fertilizer-grade ammonium sulfate, industrial-grade basic magnesium carbonate / magnesium carbonate and fertilizer-grade magnesium ammonium phosphate, which are all industrial best-sellers with high economic value.
[0038] In step (5), the ammonium sulfate required for the low-temperature molten salt reaction can be provided by the ammonium sulfate product recovered in step (4), thereby reducing the cost of chemical reagents.
[0039] In some preferred embodiments, in step (2), the temperature of the first reaction is 25-60°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, etc.; the time of the first reaction is 120-480 min, for example, 120 min, 150 min, 180 min, 200 min, 220 min, 250 min, 280 min, 300 min, 320 min, 350 min, 380 min, 400 min, 420 min, 450 min, 480 min, etc.
[0040] In some preferred embodiments, in step (2), the concentration of the ammonia water is 4-25%; the amount of the ammonia water added is determined according to the molar ratio of nitrogen contained in the ammonia water to manganese in the waste salt solution of 3-8:1, for example, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, etc.
[0041] In some preferred embodiments, in step (2), the oxygen partial pressure of the oxygen-containing gas is 21-100%; the oxygen-containing gas is one or both of air and oxygen.
[0042] In some preferred embodiments, in step (2), the gas flow rate of the oxygen-containing gas is 5 to 20 L of oxygen-containing gas per liter of waste salt solution per minute, for example 5 L, 6 L, 7 L, 8 L, 9 L, 10 L, 11 L, 12 L, 13 L, 14 L, 15 L, 16 L, 17 L, 18 L, 19 L, 20 L, etc.
[0043] In some preferred embodiments, in step (2), the temperature of the second reaction is 60-100°C, for example, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, etc.; the time of the second reaction is 120-480min, for example, 120min, 150min, 180min, 200min, 220min, 250min, 280min, 300min, 320min, 350min, 380min, 400min, 420min, 450min, 480min, etc.
[0044] In some preferred embodiments, in step (2), the amount of ammonium persulfate added is 1 to 2 times the molar amount of manganese ions in the first precipitation liquid, for example, 1 time, 1.1 times, 1.2 times, 1.3 times, 1.4 times, 1.5 times, 1.6 times, 1.7 times, 1.8 times, 1.9 times, 2 times, etc.
[0045] In some preferred embodiments, in step (3), the temperature of the third reaction is 50-100°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, etc.; the time of the third reaction is 120-300 min, for example, 120 min, 150 min, 180 min, 200 min, 220 min, 250 min, 280 min, 300 min, etc.
[0046] In some preferred embodiments, in step (3), before adding the magnesium precipitation reagent, the pH of the second precipitated liquid is further adjusted to 6.5-8, for example, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, etc.
[0047] In step (3), after adding the magnesium precipitation reagent, the initial reaction pH of the system is adjusted to 7.5-8.5, for example, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, etc.
[0048] In some preferred embodiments, in step (3), the magnesium precipitation reagent is ammonium carbonate or ammonium bicarbonate.
[0049] In step (3), the magnesium product is basic magnesium carbonate or magnesium carbonate.
[0050] In some preferred embodiments, in step (3), the amount of ammonium bicarbonate or ammonium carbonate added is 2 to 5 times the molar amount of magnesium ions in the second precipitation liquid, for example, 2 times, 2.2 times, 2.5 times, 2.8 times, 3 times, 3.2 times, 3.5 times, 3.8 times, 4 times, 4.2 times, 4.5 times, 4.8 times, 5 times, etc.
[0051] In some preferred embodiments, in step (4), the temperature of the fourth reaction is 25-60°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, etc.; the time of the fourth reaction is 30-180 min, for example, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min, 180 min, etc.
[0052] In some preferred embodiments, in step (4), the amount of phosphoric acid added is determined according to the molar amount of H3PO4 in phosphoric acid being 1.0 to 1.5 times the molar amount of magnesium ions in the third post-precipitation liquid, for example, 1 time, 1.1 times, 1.2 times, 1.3 times, 1.4 times, 1.5 times, etc. Preferably, the phosphoric acid is concentrated phosphoric acid, which has little effect on the volume of the solution. If dilute phosphoric acid with a low concentration is used, the amount of liquid increases too much, which will increase the subsequent crystallization cost.
[0053] In some preferred embodiments, in step (4), the pH value of the magnesium-removed liquid is adjusted to 5.0-6.8, for example, 5.0, 5.2, 5.5, 5.8, 6, 6.2, 6.5, 6.8, etc.
[0054] In some preferred embodiments, in step (4), sulfuric acid is used to adjust the pH value of the magnesium-removed liquid; preferably, the sulfuric acid is concentrated sulfuric acid.
[0055] In some preferred embodiments, in step (5), the ammonium sulfate and manganese oxide slag are determined according to a molar ratio of (NH4)2SO4 / Mn of 1.0 to 1.5, for example, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, etc.
[0056] In some preferred embodiments, in step (5), the mixing is ball milling mixing; the ball-to-material ratio and ball milling time of ball milling can be conventionally determined, for example, the ball-to-material ratio of ball milling is 3:1 to 20:1; and the ball milling time is 10 to 120 min.
[0057] In some preferred embodiments, in step (5), the molten salt reaction temperature is 400-500°C, for example, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, etc.; the molten salt reaction time is 60-180 min, for example, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min, 180 min, etc.
[0058] In some preferred embodiments, in step (5), the liquid-to-solid ratio of the water immersion is 10:1 to 2.5:1 mL / g, for example, 10:1, 9:1, 8:1, 7:1, 6:1, 5:1, 4:1, 3:1, 2.5:1, etc.; the temperature of the water immersion is 25 to 60°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, etc.; the time of the water immersion is 10 to 120 min, for example, 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, etc.
[0059] In some preferred embodiments, step (5) further includes recovering the ammonia-containing flue gas generated by the low-temperature molten salt reaction. Specifically, in step (5), the NH3-containing flue gas generated by the low-temperature molten salt reaction can be used to produce ammonia products, or can be returned to step (2) for use, which not only effectively utilizes the waste gas but also prevents pollution to the environment.
[0060] The chemical raw materials required for the process, air / oxygen, ammonia water, ammonium persulfate, ammonium bicarbonate / ammonium carbonate, concentrated phosphoric acid and concentrated sulfuric acid are all cheap, abundant and easy to obtain; an economic profit of 1,500 to 2,100 yuan can be obtained for each ton of electrolytic manganese industrial waste salt processed, which is suitable for large-scale industrial applications.
[0061] In some embodiments, in step (1), 50 to 300 g of electrolytic manganese industrial waste salt is dissolved in 1 L of water; for example, 50, 80 g, 100 g, 120 g, 150 g, 180 g, 200 g, 220 g, 250 g, 280 g, 300 g, etc. It is preferred to use a relatively high concentration so that a high-concentration waste salt solution can be obtained to improve the treatment efficiency. It is worth noting that the composition of electrolytic manganese industrial waste salt from different batches may vary to a certain extent, so the saturated concentration thereof dissolved in water may also vary to a certain extent.
[0062] In some preferred embodiments, in step (1), the particle size of the electrolytic manganese industrial waste salt is less than 100 mesh; the use of small particles of electrolytic manganese industrial waste salt is beneficial to improving the dissolution efficiency of the electrolytic manganese industrial waste salt and releasing the insoluble impurities inside it.
[0063] In order to facilitate the understanding of the present invention, the present invention will be described in more comprehensive and detailed manner below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.
[0064] The electrolytic manganese industrial waste salt in the following embodiments is taken from a conventional electrolytic manganese plant. The electrolytic manganese industrial waste salt is a composite sulfate mainly composed of hexahydrate ammonia magnesium sulfate, hexahydrate ammonium manganese sulfate, ammonium manganese sulfate, epsom salt and hemihydrate gypsum produced during the electrolytic manganese production process.
[0065] Example 1 A method for recovering manganese, magnesium and ammonia nitrogen resources from waste salt in electrolytic manganese industry, the process flow chart is as follows Figure 1 As shown, the following steps are included: (1) Dry the electrolytic manganese industrial waste salt, crush the dried electrolytic manganese industrial waste salt to less than 100 meshes with a pulverizer or a crusher, dissolve the electrolytic manganese industrial waste salt in deionized water at a concentration of about 250 g / L, filter out insoluble matter such as silt, and obtain a saturated waste salt solution.
[0066] (2) Place 1 L of the saturated waste salt molten salt solution obtained in step (1) in a water bath at 40°C and stir, introduce oxygen at a flow rate of 1 L / min, and use a peristaltic pump to add 20 wt.% ammonia solution at a flow rate of 2 mL / min. The amount of ammonia solution added is determined based on the molar ratio of nitrogen contained in ammonia water to manganese in the saturated waste salt molten salt solution of 5.5. The reaction is continued for 240 min, the precipitation rate of Mn is 95.3%, and the obtained manganese precipitation products are Mn3O4 and MnOOH. The Mg content in the manganese precipitation products is 0.43 wt.%.
[0067] (3) The precipitated solution obtained in step (2) was placed in a 90°C water bath with stirring, and ammonium persulfate was added in an amount according to a molar ratio of (NH4)2S2O8 / Mn = 1.7. The reaction was continued for 120 min. The residual Mn content in the solution was less than 0.3 mg / L. The obtained manganese precipitated product was manganese dioxide, in which the Mg content was 0.58 wt.%.
[0068] (4) The pH value of the solution obtained in step (3) was adjusted to about 7 using concentrated ammonia water, and solid ammonium bicarbonate was added according to the molar ratio of NH4HCO3 / Mg = 2.5, and the ammonium bicarbonate was completely dissolved by stirring, and the pH value of the solution was adjusted to 8.4 using concentrated ammonia water. The obtained solution was then placed in a water bath at 80°C and stirred, and reacted for 2 hours. After the reaction was completed, it was filtered to obtain basic magnesium carbonate and magnesium precipitation liquid, and the magnesium precipitation rate was 92.8%. The basic magnesium carbonate obtained by filtration was washed three times with deionized water to obtain a basic magnesium carbonate product that met the requirements of HG / T2959-2010 superior products. The component test results are shown in Table 1.
[0069] (5) Add concentrated phosphoric acid at a molar ratio of H3PO4 / Mg = 1.0 to the magnesium precipitation solution obtained in step (4), react at 25°C for 60 minutes, and filter after the reaction is complete to obtain magnesium ammonium phosphate and filtrate, wherein the residual Mg content in the filtrate is less than 12 mg / L. The filtered magnesium ammonium phosphate is washed three times with deionized water to obtain a fertilizer-grade magnesium ammonium phosphate product that meets the composition requirements of T / SXAS 005-2020 and has toxic and harmful element contents lower than the threshold of GB 38400-2019. The composition test results are shown in Table 2. The comprehensive recovery rate of magnesium exceeds 99.5%.
[0070] (6) The pH value of the filtrate obtained in step (5) was adjusted to 6.0 using concentrated sulfuric acid, and the ammonium sulfate product meeting the requirements of GB / T 535-2020 Class I and HG / T 5744-2020 was obtained by evaporation and crystallization. The component test results and the standard comparison are shown in Tables 3 and 4.
[0071] (7) The ammonium sulfate obtained in step (6) is uniformly mixed with the manganese oxide product obtained in step (2) of oxidative precipitation and step (3) of deep precipitation at a molar ratio of (NH4)2SO4 / Mn = 1:1, with a ball-to-material ratio of 8:1, and ball milled for 45 minutes. The mixed ball milled material is then placed in a muffle furnace at 450°C for reaction for 90 minutes to obtain a molten salt reaction product.
[0072] (8) The molten salt reaction product obtained in step (7) was slurried with deionized water at a liquid-solid ratio of 2.5:1 mL / g, and the obtained slurry was then placed in a water bath at 25°C for stirring and immersion, reacted for 20 minutes, and then filtered to obtain leached residue and manganese-containing leaching solution. The manganese-containing leaching solution was evaporated and crystallized to obtain a MnSO4·H2O product that meets the first-class requirements of HG / T 4823-2015. The product composition test results are shown in Table 5. The comprehensive recovery of manganese exceeds 99.9%.
[0073] The calculated cost and benefit of treating 1 ton of electrolytic manganese industrial waste salt by using this embodiment are shown in Table 7 (the material and energy consumption costs are calculated according to the prices on the treatment day). It can be seen from the table that the benefit of treating 1 ton of electrolytic manganese industrial waste salt is 2048 yuan.
[0074] Comparative Example 1 A method for recovering manganese, magnesium and ammonia nitrogen resources from electrolytic manganese metal industrial waste salt comprises the following steps: (1)~(2) are the same as step (1) and step (2) of Example 1.
[0075] (3) Use concentrated ammonia water to adjust the pH value of the precipitated solution obtained in step (2) to about 7, add ammonium bicarbonate solid according to the molar ratio of NH4HCO3 / Mg = 2.5, stir to completely dissolve the ammonium bicarbonate, and use concentrated ammonia water to adjust the pH value of the solution to 8.4. Then place the resulting solution in a water bath at 80°C and stir, react for 2 hours, and filter after the reaction is completed to obtain basic magnesium carbonate and magnesium precipitation solution. Wash the filtered basic magnesium carbonate three times with deionized water to obtain a basic magnesium carbonate product, and the component detection results are shown in Table 1. As can be seen from Table 1, the magnesium oxide in the obtained basic magnesium carbonate is significantly reduced, and the manganese content is significantly exceeded.
[0076] (4) Add concentrated phosphoric acid at a molar ratio of H3PO4 / Mg = 1.0 to the magnesium precipitation solution obtained in step (3), react at 25°C for 60 minutes, and filter after the reaction is complete to obtain magnesium ammonium phosphate and a filtrate, wherein the residual Mg content in the filtrate is less than 12 mg / L. Wash the filtered magnesium ammonium phosphate three times with deionized water to obtain a magnesium ammonium phosphate product, and the component detection results are shown in Table 2.
[0077] (5) The pH value of the filtrate obtained in step (4) was adjusted to 6.0 using concentrated sulfuric acid, and the ammonium sulfate product was obtained by evaporation and crystallization. The component detection results and the standard comparison are shown in Tables 3 and 4.
[0078] (6) The ammonium sulfate obtained in step (5) and the manganese oxide product obtained in step (2) were uniformly mixed at a molar ratio of (NH4)2SO4 / Mn = 1:1, with a ball-to-material ratio of 8:1, and ball milled for 45 minutes. The mixed ball milled material was then placed in a muffle furnace at 450°C for reaction for 90 minutes to obtain a molten salt reaction product.
[0079] (7) The molten salt reaction product obtained in step (6) was slurried with deionized water at a liquid-solid ratio of 2.5:1 mL / g, and the obtained slurry was then placed in a 25°C water bath for stirring and immersion, reacted for 20 minutes, and then filtered to obtain leaching residue and manganese-containing leaching solution. The composition test results of the evaporation crystallization manganese-containing leaching solution product are shown in Table 5.
[0080] Comparative Example 2 (1) Dry the electrolytic manganese industrial waste salt, crush the dried electrolytic manganese industrial waste salt to less than 100 meshes with a pulverizer or a crusher, dissolve the electrolytic manganese industrial waste salt in deionized water at a concentration of about 250 g / L, filter out insoluble matter such as silt, and obtain a saturated waste salt solution.
[0081] (2) The saturated waste salt solution obtained in step (1) was placed in a 90°C water bath and stirred, and the amount of ammonium persulfate added was in accordance with the molar ratio of (NH4)2S2O8 / Mn = 1.7. The reaction was carried out for 120 minutes. After testing, the residual Mn content in the solution exceeded 1g / L, and the obtained manganese precipitation product was manganese dioxide, in which the Mg content was 0.23%. After analysis, the precipitation rate of Mn was relatively low. This may be because for solutions with high manganese ion concentrations in the solution, due to the strong oxidation ability of ammonium persulfate and the fact that more hydrogen ions will be produced relative to oxygen oxidation, the excessive manganese ion concentration in the solution will produce excessive acid in the early stage, which will prevent the occurrence of manganese precipitation reaction.
[0082] (3) Use concentrated ammonia water to adjust the pH value of the manganese precipitation solution obtained in step (2) to about 7, add ammonium bicarbonate solid according to the molar ratio of NH4HCO3 / Mg = 2.5, stir to completely dissolve the ammonium bicarbonate, and use concentrated ammonia water to adjust the solution pH to 8.4. Then place the resulting solution in a water bath at 80°C and stir, react for 2 hours, and filter after the reaction is completed to obtain basic magnesium carbonate and magnesium precipitation solution. Use deionized water to wash the filtered basic magnesium carbonate three times to obtain a basic magnesium carbonate product, and the component detection results are shown in Table 1. As can be seen from Table 1, the magnesium oxide content in the obtained basic magnesium carbonate is significantly reduced, and the CaO, manganese content and sulfate content are significantly exceeded.
[0083] (4) Add concentrated phosphoric acid at a molar ratio of H3PO4 / Mg = 1.0 to the magnesium precipitation solution obtained in step (3), react at 25°C for 60 minutes, and filter after the reaction is complete to obtain magnesium ammonium phosphate and a filtrate, wherein the residual Mg content in the filtrate is less than 12 mg / L. Wash the filtered magnesium ammonium phosphate three times with deionized water to obtain a magnesium ammonium phosphate product, and the component detection results are shown in Table 2.
[0084] (5) The pH value of the filtrate obtained in step (4) was adjusted to 6.0 using concentrated sulfuric acid, and the ammonium sulfate product was obtained by evaporation and crystallization. The component detection results and the standard comparison are shown in Tables 3 and 4.
[0085] (6) The ammonium sulfate obtained in step (5) and the manganese oxide product obtained in step (2) were uniformly mixed at a molar ratio of (NH4)2SO4 / Mn = 1:1, with a ball-to-material ratio of 8:1, and ball milled for 45 minutes. The mixed ball milled material was then placed in a muffle furnace at 450°C for reaction for 90 minutes to obtain a molten salt reaction product.
[0086] (7) The molten salt reaction product obtained in step (6) was slurried with deionized water at a liquid-to-solid ratio of 2.5:1 mL / g, and the obtained slurry was then placed in a 25°C water bath for stirring and immersion, reacted for 20 minutes, and then filtered to obtain leached residue and manganese-containing leaching solution. The manganese-containing leaching solution was evaporated and crystallized to obtain a MnSO4·H2O product, and the product composition test results are shown in Table 5.
[0087] Comparative Example 3 A method for recovering manganese, magnesium and ammonia nitrogen resources from electrolytic manganese metal industrial waste salt comprises the following steps: (1) to (4) are the same as steps (1) to (4) of Example 1.
[0088] (5) The pH value of the filtrate obtained in step (4) was adjusted to 6.0 using concentrated sulfuric acid, and the ammonium sulfate product was obtained by evaporation and crystallization. The component detection results and the standard comparison are shown in Tables 3 and 4. It can be seen from Tables 3 and 4 that the N and S contents of the obtained ammonium sulfate product are significantly reduced, that is, the purity of the ammonium sulfate is reduced. After analysis, this may be because there is a limit to the precipitation of magnesium in step (4), resulting in the appearance of impurities in the ammonium sulfate product.
[0089] (6) The ammonium sulfate obtained in step (5) is uniformly mixed with the manganese oxide product obtained in step (2) of oxidative precipitation and step (3) of deep precipitation at a molar ratio of (NH4)2SO4 / Mn = 1:1, with a ball-to-material ratio of 8:1, and ball milled for 45 minutes. The mixed ball milled material is then placed in a muffle furnace at 450°C for reaction for 90 minutes to obtain a molten salt reaction product.
[0090] (7) The molten salt reaction product obtained in step (6) was slurried with deionized water at a liquid-solid ratio of 2.5:1 mL / g, and the obtained slurry was then placed in a water bath at 25°C and stirred for immersion, reacted for 20 minutes, and then filtered to obtain leached residue and manganese-containing leaching solution. The manganese-containing leaching solution was evaporated and crystallized to obtain the MnSO4·H2O product. The product component detection results are shown in Table 5. It can be seen from Table 5 that the purity of the obtained manganese sulfate is significantly reduced, and the impurity content of Na, Ca, Mg, etc. is significantly exceeded. After analysis, these impurities are introduced by the ammonium sulfate product prepared in step (5), indicating that the purity of the ammonium sulfate product obtained in step (5) is low.
[0091] Comparative Example 4 A method for recovering manganese, magnesium and ammonia nitrogen resources from electrolytic manganese metal industrial waste salt comprises the following steps: (1) to (3): the same as steps (1) to (3) of Example 1; (4) Concentrated phosphoric acid was added to the manganese precipitation solution obtained in step (3) at a molar ratio of H3PO4 / Mg = 1.0, and the reaction was carried out at 25°C for 60 minutes. After the reaction was complete, the solution was filtered to obtain magnesium ammonium phosphate and a filtrate, wherein the residual Mg in the filtrate exceeded 5 g / L. The magnesium ammonium phosphate obtained by filtration was washed three times with deionized water to obtain a magnesium ammonium phosphate product, and the component detection results are shown in Table 2.
[0092] (5) The pH value of the filtrate obtained in step (4) was adjusted to 6.0 using concentrated sulfuric acid, and the product was evaporated and crystallized to obtain an ammonium sulfate product. The component detection results and the standard comparison are shown in Table 3 and Table 4. It can be seen from the table that the N content in the ammonium sulfate is significantly reduced, that is, the purity of the ammonium sulfate product is reduced. Analysis shows that this may be due to the poor effect of the aforementioned magnesium precipitation.
[0093] (6) The ammonium sulfate obtained in step (5) is uniformly mixed with the manganese oxide product obtained in step (2) of oxidative precipitation and step (3) of deep precipitation at a molar ratio of (NH4)2SO4 / Mn = 1:1, with a ball-to-material ratio of 8:1, and ball milled for 45 minutes. The mixed ball milled material is then placed in a muffle furnace at 450°C for reaction for 90 minutes to obtain a molten salt reaction product.
[0094] (7) The molten salt reaction product obtained in step (6) was slurried with deionized water at a liquid-solid ratio of 2.5:1 mL / g, and the obtained slurry was then placed in a water bath at 25°C for stirring and immersion, reacted for 20 minutes, and then filtered to obtain leached residue and manganese-containing leaching solution. The manganese-containing leaching solution was evaporated and crystallized to obtain a MnSO4·H2O product. The product composition test results are shown in Table 5. It can be seen from Table 5 that the purity of the obtained manganese sulfate is significantly reduced, and the impurity content of Na, Ca, Mg, etc. is significantly exceeded.
[0095] Comparative Example 5 (1) Dry the electrolytic manganese industrial waste salt, crush the dried electrolytic manganese industrial waste salt to less than 100 meshes with a pulverizer or a crusher, dissolve the electrolytic manganese industrial waste salt in deionized water at a concentration of about 250 g / L, filter out insoluble matter such as silt, and obtain a saturated waste salt solution.
[0096] (2) 1 L of saturated waste salt solution obtained in step (1) was placed in a water bath at 40° C. and stirred, and the pH value of the solution was adjusted to 8 with aqueous ammonia. After neutralization, the solution was filtered, and carbon dioxide gas was introduced into the filtrate for precipitation to obtain manganese-containing slag and manganese precipitation liquid. The manganese-containing slag had a magnesium content of 5.43 wt.%. It can be seen that the removal effect of manganese by carbon dioxide precipitation was relatively poor, and magnesium was co-precipitated, resulting in excessive magnesium loss.
[0097] (3) The precipitated solution obtained in step (2) is placed in a 90° C. water bath and stirred, and ammonium persulfate is added in an amount according to a molar ratio of (NH4)2S2O8 / Mn=1.7. The reaction is carried out for 120 min. The residual Mn content in the solution is less than 0.3 mg / L, and the obtained manganese precipitation product is manganese dioxide.
[0098] (4) Use concentrated ammonia water to adjust the pH value of the solution obtained in step (3) to about 7, add ammonium bicarbonate solid according to the molar ratio of NH4HCO3 / Mg = 2.5, stir to completely dissolve the ammonium bicarbonate, and use concentrated ammonia water to adjust the pH value of the solution to 8.4. Then place the obtained solution in a water bath at 80°C and stir, react for 2 hours, and filter after the reaction is completed to obtain basic magnesium carbonate and magnesium precipitation liquid. Wash the filtered basic magnesium carbonate three times with deionized water to obtain a basic magnesium carbonate product, and the component detection results are shown in Table 1.
[0099] (5) Add concentrated phosphoric acid at a molar ratio of H3PO4 / Mg = 1.0 to the magnesium precipitation solution obtained in step (4), react at 25°C for 60 minutes, and filter after the reaction is complete to obtain magnesium ammonium phosphate and a filtrate, wherein the residual Mg content in the filtrate is less than 12 mg / L. Wash the filtered magnesium ammonium phosphate three times with deionized water to obtain a magnesium ammonium phosphate product, and the component detection results are shown in Table 2.
[0100] (6) The pH value of the filtrate obtained in step (5) was adjusted to 6.0 using concentrated sulfuric acid, and the ammonium sulfate product was obtained by evaporation and crystallization. The component detection results and the standard comparison are shown in Tables 3 and 4.
[0101] (7) The ammonium sulfate obtained in step (6) is uniformly mixed with the carbon dioxide precipitation product of step (2) and the manganese oxide product obtained by deep precipitation of manganese in step (3) at a molar ratio of (NH4)2SO4 / Mn = 1:1, with a ball-to-material ratio of 8:1, and ball milled for 45 minutes. The mixed ball milled material is then placed in a muffle furnace at 450°C for reaction for 90 minutes to obtain a molten salt reaction product.
[0102] (8) The molten salt reaction product obtained in step (7) was slurried with deionized water at a liquid-solid ratio of 2.5:1 mL / g, and the obtained slurry was then placed in a water bath at 25°C for stirring and immersion, reacted for 20 minutes, and then filtered to obtain leached residue and manganese-containing leaching solution. The manganese-containing leaching solution was evaporated and crystallized to obtain a MnSO4·H2O product. The product composition test results are shown in Table 5. It can be seen from Table 5 that the purity of the obtained product is insufficient, and the content of impurities Mg and Ca is significantly exceeded. After analysis, this is mainly because too many impurities were introduced into the manganese precipitation product in step (2).
[0103] Example 2 A method for recovering manganese, magnesium and ammonia nitrogen resources from electrolytic manganese metal industrial waste salt comprises the following steps: (1) Dry the obtained electrolytic manganese industrial waste salt, crush the dried electrolytic manganese industrial waste salt to less than 100 meshes with a pulverizer or a crusher, dissolve the electrolytic manganese industrial waste salt in deionized water at a concentration of about 250 g / L, filter out insoluble matter such as silt, and obtain a saturated waste salt solution.
[0104] (2) Place 1L of the saturated waste salt molten salt solution obtained in step (1) in a water bath at 30°C and stir, introduce air at a flow rate of 3L / min, and use a peristaltic pump to add 20wt.% ammonia solution at a flow rate of 2mL / min. The amount of ammonia solution added is determined according to the molar ratio of nitrogen contained in ammonia water to manganese in the saturated waste salt solution of 6. The reaction is continued for 300min, the precipitation rate of Mn is 92.8%, and the obtained manganese precipitation product is Mn3O4. The Mg content in the manganese precipitation product is 0.52wt.%.
[0105] (3) The precipitated solution obtained in step (2) was placed in a water bath at 80°C and stirred, and ammonium persulfate was added in a molar ratio of (NH4)2S2O8 / Mn = 1.5. The reaction was continued for 180 minutes, and the residual Mn content in the solution was less than 0.5 mg / L. The obtained manganese precipitation product was manganese dioxide, in which the Mg content was 0.36 wt.%.
[0106] (4) Use concentrated ammonia water to adjust the pH value of the solution obtained in step (3) to about 7, add ammonium bicarbonate solid according to the molar ratio of NH4HCO3 / Mg = 2.75, stir to completely dissolve the ammonium bicarbonate, and use concentrated ammonia water to adjust the pH value of the solution to 8.0. Then place the obtained solution in a 50°C water bath and stir, react for 4 hours, and filter after the reaction is completed to obtain magnesium carbonate and magnesium precipitation liquid, and the magnesium precipitation rate is 90.5%. Use deionized water to wash the filtered magnesium carbonate three times to obtain a magnesium carbonate product. The component detection results are shown in Table 6.
[0107] (5) Add concentrated phosphoric acid at a molar ratio of H3PO4 / Mg = 1.2 to the magnesium precipitation solution obtained in step (4), react at 25°C for 30 minutes, and filter after the reaction is complete to obtain magnesium ammonium phosphate and filtrate, wherein the residual Mg content in the filtrate is less than 1 mg / L. Wash the filtered magnesium ammonium phosphate three times with deionized water to obtain a fertilizer-grade magnesium ammonium phosphate product that meets the composition requirements of T / SXAS 005-2020 and has toxic and harmful element contents lower than the threshold of GB 38400-2019. The composition test results are shown in Table 2.
[0108] (6) The pH value of the filtrate obtained in step (5) was adjusted to 5.8 using concentrated sulfuric acid, and the ammonium sulfate product meeting the requirements of GB / T 535-2020 Class I and HG / T 5744-2020 was obtained by evaporation and crystallization. The component test results and the standard comparison are shown in Tables 3 and 4.
[0109] (7) The ammonium sulfate obtained in step (6) and the manganese oxide products obtained in steps (2) and (3) were uniformly mixed at a molar ratio of (NH4)2SO4 / Mn = 1.1:1, with a ball-to-material ratio of 5:1, and ball milled for 60 minutes. The mixed ball milled material was then placed in a muffle furnace at 500°C for reaction for 60 minutes to obtain a molten salt reaction product.
[0110] (8) The molten salt reaction product obtained in step (7) was slurried with deionized water at a liquid-solid ratio of 2.5:1 mL / g, and the obtained slurry was then placed in a water bath at 25°C for stirring and immersion, reacted for 20 minutes, and then filtered to obtain leached residue and manganese-containing leaching solution. The manganese-containing leaching solution was evaporated and crystallized to obtain a MnSO4·H2O product that met the first-class requirements of HG / T 4823-2015. The composition test results are shown in Table 5.
[0111] The cost and benefit of treating 1 ton of electrolytic manganese industrial waste salt by using this embodiment is 2023 yuan.
[0112] Example 3 A method for recovering manganese, magnesium and ammonia nitrogen resources from electrolytic manganese metal industrial waste salt comprises the following steps: (1) Dry the obtained electrolytic manganese industrial waste salt, crush the dried electrolytic manganese industrial waste salt to less than 100 meshes with a pulverizer or a crusher, dissolve the electrolytic manganese industrial waste salt in deionized water at a concentration of about 250 g / L, filter out insoluble matter such as silt, and obtain a saturated waste salt solution.
[0113] (2) Place 1 L of the saturated waste salt molten salt solution obtained in step (1) in a water bath at 60°C and stir, introduce air at a flow rate of 6 L / min, and use a peristaltic pump to add 20 wt.% ammonia solution at a flow rate of 1 mL / min. The amount of ammonia solution added is determined based on the molar ratio of nitrogen contained in ammonia water to manganese in the saturated waste salt solution of 8. The reaction is continued for 240 min, the precipitation rate of Mn is 89.3%, and the obtained manganese precipitation product is Mn3O4. The Mg content in the manganese precipitation product is 0.26 wt.%.
[0114] (3) The precipitated solution obtained in step (2) was placed in a 60°C water bath and stirred, and ammonium persulfate was added in a molar ratio of (NH4)2S2O8 / Mn = 1.2. The reaction was continued for 300 min, and the residual Mn content in the solution was less than 0.7 mg / L. The obtained manganese precipitation product was manganese dioxide, in which the Mg content was 0.74 wt.%.
[0115] (4) Use concentrated ammonia water to adjust the pH value of the solution obtained in step (3) to about 7, add ammonium bicarbonate solid according to the molar ratio of NH4HCO3 / Mg = 4, stir to completely dissolve the ammonium bicarbonate, and use concentrated ammonia water to adjust the pH value of the solution to 8.0. Then place the obtained solution in a 70°C water bath and stir, react for 3 hours, and filter after the reaction is completed to obtain basic magnesium carbonate and magnesium precipitation liquid, and the magnesium precipitation rate is 93.5%. Wash the filtered basic magnesium carbonate three times with deionized water to obtain a basic magnesium carbonate product, and the component detection results are shown in Table 1.
[0116] (5) Add concentrated phosphoric acid at a molar ratio of H3PO4 / Mg = 1.5 to the magnesium precipitation solution obtained in step (4), react at 60°C for 90 minutes, and filter after the reaction is complete to obtain magnesium ammonium phosphate and a filtrate, wherein the residual Mg content in the filtrate is less than 1 mg / L. Wash the filtered magnesium ammonium phosphate three times with deionized water to obtain a fertilizer-grade magnesium ammonium phosphate product that meets the composition requirements of T / SXAS 005-2020 and has toxic and harmful element contents lower than the threshold of GB 38400-2019. The composition test results are shown in Table 2.
[0117] (6) The pH value of the filtrate obtained in step (5) was adjusted to 6.2 using concentrated sulfuric acid, and the ammonium sulfate product meeting the requirements of GB / T 535-2020 Class I and HG / T 5744-2020 was obtained by evaporation and crystallization. The component test results and the standard comparison are shown in Tables 3 and 4.
[0118] (7) The ammonium sulfate obtained in step (6) and the manganese oxide product obtained by oxidative precipitation of manganese in step (2) and step (3) were uniformly mixed at a molar ratio of (NH4)2SO4 / Mn = 1.5:1, with a ball-to-material ratio of 5:1, and ball milled for 60 minutes. The mixed ball milled material was then placed in a muffle furnace at 400°C for reaction for 180 minutes to obtain a molten salt reaction product.
[0119] (8) The molten salt reaction product obtained in step (7) was slurried with deionized water at a liquid-solid ratio of 5:1 mL / g, and the obtained slurry was then placed in a 60°C water bath for stirring and immersion, reacted for 10 min, and then filtered to obtain leached residue and manganese-containing leaching solution. The manganese-containing leaching solution was evaporated and crystallized to obtain a MnSO4·H2O product that met the first-class requirements of HG / T 4823-2015. The composition test results are shown in Table 5.
[0120] The cost and benefit of treating 1 ton of electrolytic manganese industrial waste salt by using this embodiment is 1,769 yuan.
[0121] Table 1 Comparison of basic magnesium carbonate products prepared in various examples and comparative examples with HG / T 2959-2010 (wt. %) Table 2 Comparison of magnesium ammonium phosphate products prepared in various embodiments and comparative examples with T / SXAS 005-2020 / GB 38400-2019 (wt. %) Table 3 Comparison of ammonium sulfate products prepared in each embodiment and comparative example with GB / T 535-2020 (wt. %) Table 4 Comparison of ammonium sulfate products prepared in various examples and comparative examples with HG / T 5744-2020 (wt. %) Table 5 Comparison of manganese sulfate products prepared in each embodiment and comparative example with HG / T 4823-2015 (wt. %) Table 6 Composition detection of magnesium carbonate product prepared in Example 2 Table 7 Economic benefit calculation of treating 1 ton of waste salt in Example 1 (unit: yuan) The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for high-value recovery and treatment of electrolytic manganese metal industrial waste salt, characterized in that: include: (1) Dissolving electrolytic manganese metal industrial waste salt in water and filtering to obtain a waste salt solution; (2) adding ammonia water to the waste salt solution and continuously introducing oxygen-containing gas to carry out a first reaction, and performing solid-liquid separation to obtain a first manganese oxide slag and a first precipitated liquid; adding ammonium persulfate to the first precipitated liquid, heating and keeping the temperature, and carrying out a second reaction. After the reaction is completed, performing solid-liquid separation to obtain a second manganese oxide slag and a second precipitated liquid; (3) adding a magnesium precipitation reagent to the second precipitated liquid, carrying out a third reaction, and performing solid-liquid separation to obtain a magnesium product and a third precipitated liquid; adding phosphoric acid to the third precipitated liquid, carrying out a fourth reaction, and performing solid-liquid separation to obtain magnesium ammonium phosphate and a magnesium-removed liquid; (4) adjusting the pH value of the solution after magnesium removal, evaporating and crystallizing to obtain ammonium sulfate; (5) The obtained manganese oxide slag is mixed with ammonium sulfate, subjected to a low-temperature molten salt reaction, and the molten salt reaction product is immersed in water to obtain a manganese sulfate solution, which is then evaporated and crystallized to obtain manganese sulfate.
2. The method for high-value recovery and treatment of electrolytic manganese industrial waste salt according to claim 1, characterized in that: In step (2), the temperature of the first reaction is 25 to 60° C.; the time of the first reaction is 120 to 480 min; In step (2), the concentration of the ammonia water is 4 to 25%; the amount of the ammonia water added is determined according to the molar ratio of nitrogen contained in the ammonia water to manganese in the waste salt solution of 3 to 8:1; In step (2), the oxygen partial pressure of the oxygen-containing gas is 21 to 100%; In step (2), the gas flow rate of the oxygen-containing gas is 5 to 20 liters of oxygen-containing gas per minute per liter of waste salt solution.
3. The method for high-value recovery and treatment of electrolytic manganese industrial waste salt according to claim 1, characterized in that: In step (2), the temperature of the second reaction is 60 to 100° C.; the time of the second reaction is 120 to 480 min; In step (2), the amount of ammonium persulfate added is 1 to 2 times the molar amount of manganese ions in the first precipitation solution.
4. The method for high-value recovery and treatment of electrolytic manganese industrial waste salt according to claim 1, characterized in that: In step (3), the temperature of the third reaction is 50-100° C.; the time of the third reaction is 120-300 min; In step (3), before adding the magnesium precipitation reagent, the pH of the second precipitation liquid is adjusted to 6.5-8; In step (3), after adding the magnesium precipitation reagent, the initial reaction pH of the system is adjusted to 7.5-8.
5.
5. The method for high-value recovery and treatment of electrolytic manganese industrial waste salt according to claim 1, characterized in that: In step (3), the magnesium precipitation reagent is ammonium carbonate or ammonium bicarbonate; In step (3), the amount of ammonium bicarbonate or ammonium carbonate added is 2 to 5 times the molar amount of magnesium ions in the second precipitation liquid.
6. The method for high-value recovery and treatment of electrolytic manganese industrial waste salt according to claim 1, characterized in that: In step (3), the temperature of the fourth reaction is 25 to 60° C.; the time of the fourth reaction is 30 to 180 min; In step (3), the amount of phosphoric acid added is determined according to the molar amount of H3PO4 in phosphoric acid being 1.0 to 1.5 times the molar amount of magnesium ions in the third precipitation liquid; In step (3), the phosphoric acid is concentrated phosphoric acid.
7. The method for high-value recovery and treatment of electrolytic manganese industrial waste salt according to claim 1, characterized in that: In step (4), the pH value of the magnesium-removed liquid is adjusted to 5.0-6.8; Preferably, in step (4), sulfuric acid is used to adjust the pH value of the magnesium-removed liquid; preferably, in step (4), the sulfuric acid is concentrated sulfuric acid.
8. The method for high-value recovery and treatment of electrolytic manganese industrial waste salt according to claim 1, characterized in that: In step (5), the ammonium sulfate and the manganese oxide slag are determined according to a molar ratio of (NH4)2SO4 / Mn of 1.0 to 1.5; Preferably, in step (5), the mixing is ball milling mixing; Preferably, in step (5), the molten salt reaction temperature is 400-500° C.; and the molten salt reaction time is 60-180 min.
9. The method for high-value recovery and treatment of electrolytic manganese industrial waste salt according to claim 1, characterized in that: In step (5), the liquid-to-solid ratio of the water immersion is 10:1 to 2.5:1 mL / g; the temperature of the water immersion is 25 to 60° C.; and the time of the water immersion is 10 to 120 min. Preferably, step (5) further includes recovering the ammonia-containing flue gas generated by the low-temperature molten salt reaction.
10. The method for high-value recovery and treatment of electrolytic manganese industrial waste salt according to claim 1, characterized in that: In step (1), 50-300 g of electrolytic manganese industrial waste salt is dissolved in 1 L of water; Preferably, in step (1), the particle size of the electrolytic manganese industrial waste salt is less than 100 mesh.
Citation Information
Cited By
Method for recovering electrolytic manganese industrial waste salt
CN119797435A
Eutectic molten salt-based low-temperature thermal deconstruction ternary battery positive electrode material recovery method
CN121922750A