Preparation method for titanium-based amorphous spherical powder

By combining the plasma rotating electrode atomization method with the protective gases of argon and helium, the problem of the inability to prepare titanium-based amorphous spherical powder with the existing technology has been solved, and the preparation of titanium-based amorphous powder with high success rate and high purity has been achieved, improving Improve the welding effect and application performance of titanium alloy.

WO2024222053A1PCT designated stage expired Publication Date: 2024-10-31ZHENGZHOU RES INST OF MECHANICAL ENG CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/071756
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-01-11
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing technology cannot effectively prepare titanium-based amorphous spherical powder, resulting in poor welding effects and difficulty in achieving precise connections of titanium alloy components.

Method used

The plasma rotating electrode atomization method (PREP) is used combined with argon and helium as protective gases to increase the cooling rate to form amorphous powder, ensuring the preparation of titanium-based solder with high purity and sphericity.

Benefits of technology

It significantly improves the preparation success rate and purity of titanium-based amorphous powder, avoids component segregation and crystallization defects, and meets the high-performance requirements of titanium alloy welding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024071756_31102024_PF_FP_ABST
    Figure CN2024071756_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of amorphous alloy preparation methods. Disclosed is a preparation method for titanium-based amorphous spherical powder, comprising treating a titanium-based brazing filler metal by means of plasma rotating electrode process (PREP) atomization, wherein argon and helium are used as protective gas in the PREP atomization. According to this solution, PREP atomization is used, and argon and helium are used in combination as protective gas, thereby effectively increasing the cooling speed required by titanium-based amorphous powder that can be achieved in this process and thus significantly improving the preparation success rate and purity of the titanium-based amorphous powder. By means of long-term experiments, the applicant finds that when argon and helium are used in combination as protective gas, the thermal conductivity coefficient of the mixed gas is effectively improved, so that the cooling rate is increased, and the success rate of preparing the titanium-based amorphous spherical powder by means of PREP atomization is fully improved.
Need to check novelty before this filing date? Find Prior Art

Description

A method for preparing titanium-based amorphous spherical powder Technical Field

[0001] The invention relates to the technical field of amorphous alloy preparation methods, and in particular to a preparation method of titanium-based amorphous spherical powder. Background Art

[0002] Titanium and its alloys' excellent heat resistance, corrosion resistance, and fatigue resistance have led to their widespread use in aerospace and marine equipment. To ensure reliable, corrosion-resistant, and precise connections between titanium and titanium alloy components, titanium-based brazing filler metals are typically used for welding. The main components of titanium-based brazing filler metals are Ti and Zr. Ti and Zr have similar properties and are infinitely soluble in each other, but Ti and Zr have higher melting points. To lower their melting points, other elements are added to the alloy to produce titanium-based brazing filler metals. The elements in titanium-based brazing filler metals easily form large amounts of intermetallic compounds, resulting in hard and brittle properties and difficulty in processing into strips or ribbons. Furthermore, Ti and Zr elements easily segregate in the brazing filler metal, affecting the welding effect.

[0003] In order to avoid the influence of composition segregation in the brazing filler metal on the welding effect, and based on the characteristics of titanium-based amorphous alloys such as single phase, uniform composition, and no dislocation and crystal defects, the use of titanium-based amorphous alloys in the brazing process of titanium and titanium alloys can effectively avoid composition segregation, reduce dissolution, and obtain reliable welded joints; therefore, titanium-based brazing filler metals can be welded in the amorphous alloy state. In addition, for the precision connection of complex and thin-walled components of titanium and titanium alloys, the requirements for titanium-based brazing filler metals are higher, and titanium-based brazing filler metals need to be assembled in powder or paste form. Among them, spherical powder has obvious advantages over strip crystalline brazing filler metals due to its high bulk density, weak overlap effect during use, and small impact on welding.

[0004] In order to solve the above problems, the conventional technologies for preparing titanium-based powders (not titanium-based amorphous powders) are electrode induction melting gas atomization (EIGA) and plasma rotating electrode atomization (PREP). However, the following technical problems still exist when preparing titanium-based powders using existing technologies: (1) EIGA powder preparation uses an inert gas (argon) pressure of 3 to 6 MPa, and the air flow velocity is relatively low, which has low efficiency in removing heat, and the cooling rate generally does not exceed 10 2 K / s, which does not have the cooling rate to form amorphous powder. (2) The low speed of PREP powder making leads to large powder particle size, low relative speed of powder flying, and weak ability of alloy powder to form amorphous. The thermal conductivity and cooling rate of argon as the protection and cooling medium do not meet the critical cooling conditions for amorphous formation.

[0005] In summary, the existing technologies are unable to prepare titanium-based amorphous spherical powder; therefore, there is an urgent need to develop a method for preparing titanium-based amorphous spherical powder with a high success rate and high performance, and to prepare titanium-based brazing filler metal into titanium-based amorphous spherical powder, which not only effectively makes up for the shortcomings of the existing technology for preparing amorphous alloy powder, but also has important significance for the wide application of titanium-based amorphous powder.

[0006] Summary of the Invention

[0007] The present invention aims to provide a method for preparing titanium-based amorphous spherical powder, so as to solve the technical problem that the prior art cannot prepare titanium-based amorphous spherical powder.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: a method for preparing titanium-based amorphous spherical powder, comprising treating titanium-based solder using a plasma rotating electrode atomization method (PREP), wherein argon and helium are used as protective gases in the PREP.

[0009] The principles of this program are:

[0010] Plasma Rotating Electrode Atomization (PREP) is a centrifugal atomization technology commonly used to produce high-purity spherical titanium powder. Its basic principle is shown in Figure 1. In a protective gas environment, the end surface of the consumable electrode is melted into a liquid film by the plasma arc. Under the action of the rotating centrifugal force, it is thrown out at high speed to form droplets. The droplets then spheroidize and condense into spherical powder under the action of surface tension. However, the formation of amorphous powder directly depends on the critical cooling rate of the alloy melt. When the external cooling rate is higher than the critical cooling rate of the alloy, when the alloy melt reaches the solidification temperature, its internal atoms are frozen near the position they were in the liquid state before they have time to crystallize, thus forming an amorphous solid with an amorphous structure. In other words, when the external cooling rate is fast enough, the alloy can form amorphous powder.

[0011] The advantages of this solution are:

[0012] 1. Compared with the existing gas atomization technology that cannot produce titanium-based amorphous powder, this solution adopts the plasma rotating electrode atomization method and uses argon and helium as protective gases to effectively improve the process to achieve the required cooling rate of titanium-based amorphous powder, thereby significantly improving the success rate and purity of the preparation of titanium-based amorphous powder. The applicant found through long-term experiments that the combination of argon and helium as protective gases effectively improves the thermal conductivity of the mixed gas, thereby making the cooling rate reach 6.35×10 4 K / s, meeting the critical cooling rate of titanium-based bulk amorphous 10 3 ~10 4 K / s, fully improving the success rate of preparing titanium-based amorphous spherical powders using plasma rotating electrode atomization method.

[0013] 2. Compared with the existing technology that uses electrode induction melting gas atomization technology to prepare titanium-based powder, which is prone to non-spherical powder and satellite powder, this scheme uses plasma rotating electrode atomization (PREP) to prepare amorphous spherical powder. By using consumable electrode rotation, the prepared powder has high purity and will not form hollow powder and satellite powder particles due to the "umbrella effect" caused by different powder particle sizes similar to the existing gas atomization method. This significantly improves the quality of the prepared titanium-based amorphous powder and ensures the application performance of the titanium-based amorphous spherical powder in related fields.

[0014] Preferably, the concentration of argon in the protective gas is 10-50%.

[0015] Beneficial effect: This method fully improves the cooling rate of the environment of the consumable electrode made of titanium-based solder by mixing argon and helium, thereby ensuring the external requirements of the titanium-based solder being atomized into amorphous spherical powder, thereby improving the success rate. In addition, the applicant found through long-term experiments that when the argon concentration in the shielding gas is 10-50%, titanium-based amorphous powder can be successfully prepared, and the obtained amorphous spherical powder has high purity and concentrated particle size; when the argon concentration is lower than 10%, the helium concentration in the shielding gas is too high, resulting in difficulty in plasma arcing and failure to prepare titanium-based amorphous powder; when the argon concentration is higher than 50%, the success rate is reduced because the cooling rate cannot meet the cooling rate requirements of the titanium-based amorphous powder. Specifically, the prepared powder has a high content of crystalline powder, and the particle size range of the amorphous powder is too wide, resulting in the formation of hollow powder and satellite powder particles, which in turn affects the application of titanium-based amorphous powder.

[0016] Preferably, the atomization of the titanium-based solder is completed in a box, and the argon and helium are mixed before being filled into the box.

[0017] Beneficial effects: This solution effectively improves the uniformity of the mixed gas by mixing argon and helium in advance to form a mixed gas, thereby ensuring uniform thermal conductivity of the mixed gas in various spaces within the box, thereby improving the particle size uniformity of the prepared titanium-based amorphous spherical powder, and further ensuring the performance and quality of the amorphous spherical powder.

[0018] Preferably, the titanium-based brazing filler metal is a rod with a diameter of 60 to 90 mm.

[0019] Preferably, the rotation speed of the rod in the plasma rotating electrode atomization method is greater than 25500 rpm.

[0020] Beneficial effect: This solution can effectively increase the initial speed of powder thrown out of the rod by increasing the rotation speed of the rod, thereby reducing the particle size of the prepared titanium-based amorphous powder.

[0021] Preferably, the linear velocity of the rod in the plasma rotating electrode atomization method is greater than 80 m / s.

[0022] Beneficial effects: In the plasma rotating electrode atomization method (PREP), the faster the plasma rotating electrode atomization rotation speed, the smaller the droplet diameter d. However, excessively high rotation speeds not only pose certain safety risks, but also significantly increase the operating energy consumption of the equipment, thereby reducing production efficiency. This solution, by limiting the diameter of the titanium-based brazing filler metal, can effectively reduce the rotation speed of the rod to form amorphous spherical powder, thereby effectively lowering the conditions for preparing the titanium-based brazing filler metal into titanium-based amorphous spherical powder and reducing energy consumption, thereby improving production efficiency. At the same time, it can also effectively reduce the potential safety hazards of high-speed rotation and improve production safety.

[0023] Preferably, the titanium-based brazing filler metal comprises Ti, Zr and M, wherein M is a combination of two or three of Cu, Ni, Be, Ag, Sn, Si, Hf and Al, and the relative melting point offset J of the titanium-based alloy is ≥0.2.

[0024] Beneficial effect: The glass-forming ability of the alloy can be expressed by J, that is, the relative shift of the melting point, and the calculation formula is Where T m is the melting point of the alloy, is the mixed melting point; The calculation formula is Where n i is the mole fraction of the i-th element in the multi-component alloy system; The applicant has experimentally found that when the relative melting point offset J of the titanium-based alloy is greater than or equal to 0.2, the alloy is likely to form an amorphous alloy.

[0025] Preferably, the total mass percentage of Ti and Zr in the titanium-based solder exceeds 50%.

[0026] Beneficial effect: The applicant has experimentally found that when the total mass percentage of titanium Ti and zirconium Zr in the titanium-based brazing filler metal exceeds 50%, the relative shift of the melting point of the titanium-based alloy is always greater than or equal to 0.2, which makes it easier to obtain a titanium-based alloy that is easy to form amorphous powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] FIG1 is a schematic diagram showing the principle of the plasma rotating electrode atomization method of the present invention.

[0028] FIG2 is a scanning electron microscope image of the titanium-based amorphous powder prepared in Example 1 of the present invention.

[0029] FIG3 is an XRD pattern of the titanium-based amorphous powder prepared in Example 1 of the present invention.

[0030] FIG4 is an XRD pattern of the titanium-based powder prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0031] The following is further described in detail through specific embodiments, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the technical means used in the following embodiments are conventional means well known to those skilled in the art; the experimental methods used are all conventional methods; and the materials, reagents, etc. used are all commercially available.

[0032] Example 1

[0033] A method for preparing titanium-based amorphous spherical powder. In this solution, the titanium-based solder includes Ti, Zr and M, wherein M is a combination of two or three of Cu, Ni, Be, Ag, Sn, Si, Hf, and Al, and the total mass percentage of Ti and Zr in the titanium-based solder exceeds 50%. In this embodiment 1, Ti and Zr are specifically combined with Cu and Ni, and the mass percentage of each element is Ti 37.5%, Zr 37.5%, Cu 15%, and Ni 10%. The relative melting point offset J of the titanium-based alloy is ≥0.2.

[0034] Specifically, the calculation formula for the relative shift of melting point is as follows:

[0035] Where T m is the melting point of the alloy, is the mixed melting point, and The calculation formula is Where n i is the mole fraction of the i-th element in the multi-component alloy system; is the melting point of the i-th element in the multi-component alloy system.

[0036] In this embodiment 1, Ti-Zr-Cu-Ni is taken as an example. The composition is Ti37.5Zr37.5Cu15Ni10 (mass percentage), the molar fraction is Ti48.93Zr25.68Cu14.75Ni10.64, and the liquidus of the alloy is 848°C. The calculation formula is:

[0037] Therefore, the raw material composition of the titanium-based brazing filler metal in this scheme can meet the raw material requirements for preparing amorphous spherical powder from the alloy.

[0038] In this solution, when preparing amorphous spherical powder of titanium-based solder, the titanium-based solder is treated by plasma rotating electrode atomization (PREP). Argon and helium are used as protective gases in PREP. The argon concentration in the protective gas is 10-50%, specifically 10% in this embodiment 1.

[0039] In this solution, the titanium-based brazing filler metal is a rod with a diameter of 60 to 90 mm. The rotational speed of the rod in the plasma rotating electrode atomization method is greater than 25,500 rpm, and the linear velocity of the rod in the plasma rotating electrode atomization method is greater than 80 m / s. Furthermore, the titanium-based brazing filler metal is atomized within a chamber, with argon and helium mixed before being introduced into the chamber. The rod is atomized at a plasma power of 80 kW and a feed rate of 0.8 mm / s.

[0040] Among them, plasma rotating electrode atomization (PREP) is a more commonly used centrifugal atomization technology for producing high-purity spherical titanium powder. Its basic principle is: in a protective gas environment, the end surface of the consumable electrode is melted into a liquid film by the plasma arc, and is thrown out at high speed under the action of rotating centrifugal force to form droplets. The droplets are then spheroidized and condensed into spherical powder under the action of surface tension.

[0041] However, the formation of amorphous powder directly depends on the critical cooling rate R when the alloy melt is cooled. c When the external cooling rate R is higher than the critical cooling rate R of the alloy c When the alloy melt reaches the solidification temperature, the atoms inside it are frozen near the position where they were in the liquid state before they have time to crystallize, thus forming an amorphous solid with an amorphous structure; that is, when the external cooling speed is fast enough, the alloy can form an amorphous powder. c The model is:

[0042] Where Z is the thermodynamic factor parameter, Z = 2 × 10 -6 ;

[0043] Tm is the set temperature, calculated as follows;

[0044] n i is the content of component i, is the melting point of component i;

[0045] a is the average atomic diameter;

[0046] η represents the viscosity of metallic glass;

[0047] ΔG is the free energy difference between the solid and liquid states obtained ΔG = ΔH - TΔS

[0048] ΔH and ΔS represent the mixing enthalpy and mixing entropy, respectively.

[0049] In the titanium-based alloy Ti37.5Zr37.5Cu15Ni10 (mass percentage) used in this scheme, Cu and Ni are adjacent transition elements in the fourth period, and Ti and Zr are adjacent transition elements in the same family. Cu and Ni are regarded as one element, and the atomic diameters are taken as the average of the two; Ti and Zr are regarded as one atom, and the atomic diameters are taken as the average of the two. Change the quaternary alloy system into a binary alloy system, take N as 4, calculate ΔH and ΔS of the quaternary alloy system, and calculate R c The theoretical value is 1.66×10 4 K / s; therefore, theoretically, the cooling rate R of the alloy powder must be higher than 1.66×10 4 K / s is required to prepare the amorphous spherical powder of titanium-based alloy Ti37.5Zr37.5Cu15Ni10.

[0050] Specifically, the thermal equilibrium condition of the molten droplet (specifically, the droplet formed after the titanium-based alloy is melted) is: during the solidification process, the molten droplet releases heat to the surrounding environment, and the thermal equilibrium equation is as follows:

[0051] Where: V is the droplet volume (m 3 ), ρ is the density (kg / m 3 ), C p is the specific heat (J / (kg·K)), h is the heat transfer coefficient (w / (m·K)), and A is the surface area of ​​the droplet (m 2 ), T d is the droplet temperature, T f is the gas temperature. When the cooling rate of the droplet The larger it is, the easier it is for the titanium-based alloy to form amorphous.

[0052] The powder prepared by plasma rotating electrode atomization method has good sphericity, and formula (1) can be expressed as:

[0053] From formula (2), it can be seen that the greater the heat transfer h, the smaller the droplet diameter d, the faster the cooling rate, and the stronger the amorphous forming ability of the titanium-based powder. The faster the plasma rotating electrode atomization rotation speed, the smaller the droplet diameter d.

[0054] Heat transfer h is the mutual heat transfer between the high-temperature molten droplet and the gas, and the calculation formula is as follows:

[0055] Where λ m is the thermal conductivity of the gas (W / m·K), P r is the Planck constant of the gas (Kg·m 2 / S;R e is the Reynolds number. It can be seen that the thermal conductivity of the protective gas in the box significantly affects the heat transfer h.

[0056] In the prior art, the method of using a certain gas alone as a shielding gas has certain defects. For example, when the applicant uses nitrogen or hydrogen alone, the titanium-based brazing filler metal will react with nitrogen, hydrogen and other gases to form TiH or TiN, which will cause the titanium-based alloy to fail to prepare titanium-based amorphous powder; when the applicant uses argon alone, the thermal conductivity of argon is low (the thermal conductivity of argon is 1.62×10 -2 W / (m·K)) and could not meet the cooling rate requirement for preparing titanium-based amorphous powder; and when the applicant tried to use helium alone as the shielding gas, the plasma could not start an arc, resulting in abnormal production.

[0057] Therefore, this solution selects argon and helium as the shielding gas; and calculates the thermal conductivity of the mixed gas according to the following calculation formula:

[0058] Where: m is the thermal conductivity of the gas mixture (W / m·K);

[0059] λ i is the thermal conductivity of component i in the gas mixture;

[0060] y i is the mole fraction of component i in the gas mixture;

[0061] M i 1 / 3 is the molar mass of component i in the gas mixture (kg / kmol).

[0062] In this embodiment 1, the concentration of argon in the protective gas is specifically 10%, that is, Ar:He=1:9; at this time, the thermal conductivity of the mixed gas is calculated as follows (specifically, the thermal conductivity of argon is 1.62×10 -2 W / (m·K), the thermal conductivity of helium (He) is 5.79×10 -2 W / (m·K) and the mixing ratio of the two are substituted into formula (4) for calculation):

[0063] In this way, λ m =3.53×10 -2 Substitute W / (m·K) into formula (3) to calculate the heat transfer h.

[0064] In addition, the Reynolds number Re in formula (3) can be calculated using the following formula:

[0065] In formula (5), ρ g is the density of the gas, μ g is the dynamic viscosity, d is the droplet diameter, and U is the relative velocity between the droplet and the gas.

[0066] According to formula (3) and formula (5), we can get:

[0067] According to formula (2) and formula (6), we can get:

[0068] In this solution, the titanium-based brazing filler metal is a rod of 60 to 90 mm in diameter, with a rotation speed greater than 25,500 rpm and a linear speed greater than 80 m / s.

[0069] The values ​​of each data in the formula are as follows after testing:

[0070] Substituting the above values ​​into formula (7) yields a cooling rate R of 6.35×10 4 K / s, R c The theoretical value is 1.66×10 4 K / s, and the actual cooling rate R is calculated to be greater than the critical cooling rate Rc for amorphous formation. Therefore, this scheme adopts the plasma rotating electrode atomization method (using argon and helium 1:9 as the shielding gas, titanium-based brazing material as a rod with a diameter of 60-90 mm, and a rod linear speed greater than 80 m / s) to produce a powder with a particle size of 70×10 -6 m (ie 70μm) titanium-based amorphous spherical powder.

[0071] Comparative Example 1

[0072] This comparative example is basically the same as Example 1, except that argon is used as the protective gas when the titanium-based amorphous powder is prepared by the existing plasma rotating electrode atomization method (PREP).

[0073] In this comparative example, 100% argon is used as the protective gas, and the thermal conductivity λ m Take 1.62×10 -2 W / (m·K), substituting into the above formula, the cooling rate of TiZrCuNi is 1.03×10 4 K / s, the actual cooling rate R is less than the critical cooling rate Rc for amorphous formation, the conditions for forming amorphous are not met, and titanium-based amorphous powder cannot be prepared.

[0074] Experimental Example 1: Scanning electron microscope to detect the morphology of the prepared titanium-based amorphous powder

[0075] The alloy powders prepared in Example 1 and Comparative Example 1 were scanned using a scanning electron microscope (for reference, the electron microscope scanner used in this solution was purchased from Phenom, Inc., USA, model PHENOM XL). The electron microscope scanning results of the alloy powder obtained in Example 1 are shown in FIG2 .

[0076] Experimental data show that the alloy powder prepared by the applicant using the parameter settings in Example 1 is basically titanium-based amorphous spherical powder, and its diameter is distributed around 70 μm (as shown in FIG2 ).

[0077] The alloy powder obtained in Comparative Example 1 is a crystalline powder.

[0078] Experimental Example 2: Powder Phase Analysis Using a Bruker Diffractometer

[0079] The phase compositions of the alloy powders obtained in Example 1 and Comparative Example 1 were analyzed using a Bruker diffractometer. Screenshots of the obtained XRD patterns are shown in Figures 3 and 4 .

[0080] The XRD spectrum of the TiZrCuNi solder in Example 1 is shown in FIG3 . Obvious steamed-bun peaks can be observed in the XRD spectrum of the titanium-based amorphous powder prepared in Example 1 of this scheme, proving that the powder has become amorphous during the cooling process, and the degree of amorphism is high.

[0081] The XRD spectrum of the TiZrCuNi solder in Comparative Example 1 is shown in Figure 4. There are multiple sharp crystalline diffraction peaks in the figure. The diffraction peaks are broadened in the range of 2θ=30°~45°. There is interference between the crystalline diffraction peaks, and the correspondence between the crystalline phase and the diffraction peak is affected. This shows that the alloy powder obtained in Comparative Example 1 is crystalline and contains an intermetallic compound phase. The Ti-Zr-Cu-Ni crystalline solder prepared in Comparative Example 1 includes Ti, Zr matrix phase, (Zr, Cu) solid solution phase and complex crystalline phase. The crystalline phase includes Cu 10 Zr7, CuTi2, Ni 10 Zr7、Cu 51 Zr 14 , CuTi3, Ti2Ni, CuTi, Zr2Ni7 and NiZr2, etc.

[0082] In summary, this solution, through the combined use of argon and helium as shielding gases, effectively increases the cooling rate required for titanium-based amorphous powders, thereby significantly improving the success rate and purity of the preparation of titanium-based amorphous powders. Furthermore, through long-term experimental optimization, the applicant has limited the argon concentration in the shielding gas to 10-50%. This not only ensures that the titanium-based brazing filler metal forms titanium-based amorphous spherical powders, but also significantly reduces the cost of shielding gas, thereby improving production efficiency.

[0083] In addition, by limiting the diameter and rotation speed of the rods prepared from titanium-based brazing filler metal, this solution can effectively reduce the equipment requirements and energy consumption conditions for preparing titanium-based amorphous spherical powder using the ion rotating electrode atomization method (PREP), thereby not only improving production safety but also further reducing production costs and improving overall production efficiency.

[0084] The above is only Example 1 of the present invention, and the common knowledge such as the specific technical solutions and / or characteristics in the solution are not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several variations and improvements can be made, which should also be regarded as the scope of protection of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for preparing titanium-based amorphous spherical powder, characterized in that: The invention comprises adopting a plasma rotating electrode atomization method (PREP) to treat titanium-based solder, wherein argon and helium are used as protective gases in the PREP.

2. The method for preparing a titanium-based amorphous spherical powder according to claim 1, characterized in that: The concentration of argon in the protective gas is 10-50%.

3. The method for preparing a titanium-based amorphous spherical powder according to claim 2, characterized in that: The atomization of the titanium-based solder is specifically completed in the box, and the argon gas and the helium gas are mixed before being filled into the box.

4. The method for preparing a titanium-based amorphous spherical powder according to claim 3, characterized in that: The titanium-based brazing filler metal is a rod with a diameter of 60 to 90 mm.

5. The method for preparing a titanium-based amorphous spherical powder according to claim 4, characterized in that: The rotation speed of the rod in the plasma rotating electrode atomization method is greater than 25500 rpm.

6. The method for preparing a titanium-based amorphous spherical powder according to claim 4, characterized in that: In the plasma rotating electrode atomization method, the linear speed of the rod material is greater than 80 m / s.

7. A method for preparing a titanium-based amorphous spherical powder according to any one of claims 5 to 6, characterized in that: The titanium-based solder comprises Ti, Zr and M, wherein M is a combination of two or three of Cu, Ni, Be, Ag, Sn, Si, Hf and Al, and the relative melting point offset of the titanium-based alloy is J≥0.

2.

8. The method for preparing a titanium-based amorphous spherical powder according to claim 7, characterized in that: The total mass percentage of Ti and Zr in the titanium-based solder exceeds 50%.

Citation Information

Patent Citations

  • Method for preparing copper alloy powder based on plasma rotating electrode

    CN109014228A

  • Titanium-based brazing filler metal as well as preparation method and application thereof

    CN111872594A

  • Preparation method of spherical powder of high-strength titanium alloy for additive manufacturing

    CN112548109A

  • Method and system for preparing titanium or titanium alloy powder with high sphericity degree and low oxygen increment

    CN115283683A

  • Preparation method of titanium-based amorphous spherical powder

    CN116441530A