Rare earth-containing additive
By optimizing the density and melting point of rare earth and iron, and designing a reasonable shape structure, the problem of limited application of rare earth additives in the steel industry is solved, the efficient, uniform addition and high yield of rare earth elements are achieved, and the window of applicable ingredients is expanded. .
Patent Information
- Application Number
- PCT/CN2024/083565
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-31
AI Technical Summary
The application of existing rare earth additives in the steel industry is limited, mainly because the oxygen content of rare earth master alloys is difficult to control, and the melting point and density are greatly different from that of molten steel, which leads to problems such as nozzle blockage, slag layer influence and low yield.
By optimizing the density, melting point and shape design of rare earth and iron, a rare earth-containing additive is prepared, including rare earth metal and iron, with a density of 6.3g/cm3~8.4g/cm3, a melting point of 850℃~1450℃, and an oxygen content of ≤ 150ppm, small inclusions, reasonable appearance structure and shell design, reducing viscous resistance and the influence of slag layer, and improving the input depth and uniformity of additives.
It effectively reduces the inclusion of foreign rare earth oxides in steel, improves the uniformity of rare earth yield and distribution, expands the applicable composition window of the master alloy, and promotes the uniform addition and high yield of rare earth elements.
Smart Images

Figure CN2024083565_31102024_PF_FP_ABST
Abstract
Description
An additive containing rare earth
[0001] Cross-references
[0002] This application is based on the Chinese patent application with application number 2023104784055 and application date April 28, 2023, and claims the priority of the Chinese patent application. The entire content of the Chinese patent application is hereby introduced into this application as a reference. Technical Field
[0003] The present invention relates to the technical field of metal material alloy preparation, in particular to an additive containing rare earth. Background Art
[0004] Rare earths have the functions of purifying molten steel, refining grains, modifying inclusions and microalloying in steel. Adding rare earths to steel is an effective way to improve the quality of steel. However, because existing rare earth additives cannot meet the application requirements, rare earths have not yet been widely used in the steel industry. The main reasons are as follows: (1) The active chemical properties of rare earths make it difficult to control the oxygen content in rare earth master alloy additives. Oxygen exists in the rare earth additives in the form of large-sized rare earth oxides. The above rare earth oxide inclusions will cause nozzle blockage during the casting process of rare earth steel, affecting the industrial continuous production of rare earth steel; (2) The melting point and density of the rare earth master alloy additives themselves are very different from those of the molten steel. The rare earth master alloy can only be added to the upper part of the molten steel. After melting, the slag-metal reaction occurs, which greatly reduces the rare earth yield; (3) The rare earth master alloy additives are mostly regular rectangular or irregular blocks. Due to their own buoyancy and the viscous resistance of the molten steel, they cannot be added to the effective depth of the ladle away from the slag layer, affecting the uniformity of rare earth distribution and yield.
[0005] In order to reduce the rare earth activity in rare earth additives and the difference between the melting point and density of rare earth additives and molten steel, the commonly used method at present is to increase the iron content in rare earth iron intermediate alloy additives. However, since its density and melting point cannot exceed those of molten steel, although the yield and position depth of rare earth additives in molten steel have improved, the effect is still not ideal, and there is a problem of too narrow applicable composition window. At the same time, a large increase in iron content will also lead to an increase in the amount of rare earth additives required, which will have an adverse effect on the temperature of molten steel and the compactness of various metallurgical links.
[0006] To improve the placement of rare earth elements, the ladle press method was invented. This method uses steel plates welded together to create an iron box. The rare earth alloy additive is placed inside the box and then pressed into the molten steel using a crane. While this method avoids the effects of the slag layer and allows for controllable addition locations, it also presents challenges such as complex equipment, a cumbersome addition process, a short iron box lifespan, and potential contamination of the molten steel.
[0007] Summary of the Invention
[0008] The purpose of the embodiments of the present invention is to provide a rare earth-containing additive. By regulating the density, melting point, and shape of the rare earth and iron-containing additive, the applicable composition window of the additive is increased, the speed at which the additive is added to the molten steel through the upper slag layer is increased, the viscous resistance of the molten steel to the additive is effectively reduced, the influence of the slag layer is eliminated, the depth of insertion of the rare earth-containing additive is increased, the depth of addition of the additive is effectively increased, and thereby the rare earth yield and distribution uniformity are improved.
[0009] To solve the above technical problems, a first aspect of an embodiment of the present invention provides a rare earth-containing additive, comprising: a rare earth metal and iron, wherein the content of the rare earth metal is 5wt% to 90wt%, and the content of the iron is 10wt% to 95wt%;
[0010] The density of the additive is 6.3 g / cm 3 ~8.4g / cm 3 , melting point is 850℃~1450℃, oxygen content is ≤150ppm, maximum size of inclusions is ≤35μm, and total amount of inclusions is ≤0.5wt%.
[0011] Furthermore, the additive comprises: a first part and a second part formed integrally;
[0012] One end of the first part away from the second part is a hemispherical, cylindrical or parabolic structure;
[0013] The cross section of the connecting end of the second part and the first part is circular or elliptical;
[0014] The maximum dimension of any cross section of the second portion is smaller than the maximum dimension of the cross section of the connecting end of the first portion and the second portion.
[0015] Furthermore, the end of the first part away from the second part is a hemispherical or parabolic structure;
[0016] The edge point coordinates of the axial cross section of the first part satisfy the following formula:
[0017] Wherein, x is the X-axis coordinate value of the first part along the axial direction, y is the Y-axis coordinate value perpendicular to the axial direction, the coordinate origin is the vertex of the first part away from the second part, n is the taper control factor of the first part of the additive, when n=0, the first part is a cylinder, when n=1, the first part is a cone, the value range of n is 0<n<1, and L is the length value of the additive along the axial direction.
[0018] Furthermore, the value range of n is 0.7<n<1.
[0019] Furthermore, the ratio of the length L1 of the first portion along the axial direction of the cross section to the total length L of the additive is: 0.5≤L1 / L≤1;
[0020] The cross-sectional radius R of the first portion at one end close to the second portion has a value range of 1.5 cm to 24 cm, and the cross-sectional radius L has a value range of 3 cm to 48 cm.
[0021] Furthermore, a shell is provided outside the additive, and the shape of the shell matches the shape of the additive;
[0022] The iron content of the shell is greater than 95wt% and less than 99.9wt%, the thickness of the shell is 0.5cm to 4cm, the melting point is 1500℃ to 1538℃, and the density is 7.6g / cm 3 ~8.6g / cm 3 .
[0023] Furthermore, the additive further comprises: a transition metal, wherein the transition metal comprises: at least one of nickel, chromium, tungsten, molybdenum, cobalt, manganese, vanadium, niobium, and titanium;
[0024] The content of the transition metal is 0.1 wt% to 15 wt%, the content of the rare earth metal is 15 wt% to 70 wt%, and the content of iron is 20 wt% to 70 wt%;
[0025] The density of the additive is 7.2 g / cm 3 ~8.2g / cm 3 , melting point is 1000℃~1300℃, oxygen content ≤100ppm, carbon content ≤300ppm, maximum size of inclusions ≤25μm, total inclusion amount ≤0.1wt%.
[0026] Furthermore, the transition metal includes at least one of chromium, tungsten, molybdenum, vanadium, niobium and titanium.
[0027] Furthermore, the rare earth metal includes at least one of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, and yttrium;
[0028] Preferably, the rare earth metal includes at least one of lanthanum, cerium and yttrium.
[0029] The above technical solutions of the embodiments of the present invention have the following beneficial technical effects:
[0030] 1. The additive prepared by this patent has the advantages of low oxygen, small total amount and size of inclusions, etc., which can effectively reduce the introduction of foreign rare earth oxide inclusions in steel and alleviate nozzle blockage;
[0031] 2. By optimizing the composition of rare earth, iron, and transition metal microalloying elements in the additive, the rare earth additive has an appropriate density and melting point, achieving simultaneous addition of rare earth and the main transition metal microalloying elements in steel and effectively increasing the depth of additive addition, thereby improving rare earth yield and distribution uniformity;
[0032] 3. According to the melting point, density and other inherent characteristics of rare earth additives, a reasonable rare earth additive shape is designed, which can effectively reduce the viscous resistance of molten steel to the additive, get rid of the influence of the slag layer, increase the input depth of rare earth additives, promote a significant improvement in rare earth yield and uniformity indicators, and also increase the applicable composition window range of the master alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] FIG1 is a cross-sectional view of a rare earth-containing additive provided in an embodiment of the present invention.
[0034] Figure numerals: 1, first part, 2, second part. DETAILED DESCRIPTION
[0035] To make the objectives, technical solutions, and advantages of the present invention more clearly understood, the present invention will be further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are merely exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, descriptions of well-known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present invention.
[0036] Referring to FIG. 1 , a first aspect of an embodiment of the present invention provides a rare earth-containing additive, comprising: a rare earth metal and iron, wherein the rare earth metal content is 5 wt% to 90 wt% and the iron content is 10 wt% to 95 wt%; the density of the additive is 6.3 g / cm 3 ~8.4g / cm 3 , melting point is 850℃~1450℃, oxygen content is ≤150ppm, maximum size of inclusions is ≤35μm, and total amount of inclusions is ≤0.5wt%.
[0037] The above-mentioned additives are used to replace existing rare earth iron additives, ladle blowing powder, ladle pressing method, and rare earth wire feeding method as additives used in steelmaking. By regulating the density, melting point, and shape of the additives containing rare earth and iron, the speed at which the additives are added to the molten steel and pass through the upper slag layer is increased, the viscous resistance of the molten steel to the additives is effectively reduced, the influence of the slag layer is eliminated, the depth of insertion of the rare earth-containing additives is increased, the depth of addition of the additives is effectively increased, and the rare earth yield and distribution uniformity are thereby improved.
[0038] Specifically, the rare earth metal in the additive includes at least one of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, and yttrium. Preferably, the rare earth metal includes at least one of lanthanum, cerium, and yttrium. Lanthanum, cerium, and yttrium have the best advantages for modifying inclusions in steel, refining grain size, and improving mechanical properties and corrosion resistance.
[0039] Furthermore, the additive further comprises: a transition metal. The transition metal comprises: at least one of nickel, chromium, tungsten, molybdenum, cobalt, manganese, vanadium, niobium, and titanium; the content of the transition metal is 0.1 wt% to 15 wt%, the content of the rare earth metal is 15 wt% to 70 wt%, and the content of iron is 20 wt% to 70 wt%; the density of the additive is 7.2 g / cm 3 ~8.2g / cm 3 , melting point is 1000℃~1300℃, oxygen content ≤100ppm, carbon content ≤300ppm, maximum size of inclusions ≤25μm, total inclusion amount ≤0.1wt%.
[0040] The technical solution of the present invention optimizes the composition design of rare earth, iron and transition group microalloying elements in the additive, so that the rare earth additive has a suitable density and melting point, and realizes the simultaneous addition of rare earth and main transition group microalloying elements in steel.
[0041] Preferably, the transition metal includes at least one of chromium, tungsten, molybdenum, vanadium, niobium, and titanium. Chromium, tungsten, molybdenum, vanadium, niobium, and titanium have optimal solid solution strengthening and precipitation strengthening effects on steel materials, effectively improving the room temperature and high temperature mechanical properties of steel materials.
[0042] In a specific embodiment of an embodiment of the present invention, the additive includes: a first part and a second part formed as one piece; the end of the first part away from the second part is a hemispherical, cylindrical or parabolic structure; the cross-section of the connecting end of the second part and the first part is circular or elliptical; the maximum dimension D of any cross-section of the second part is smaller than the maximum dimension 2R of the cross-section of the connecting end of the first part and the second part.
[0043] According to the melting point, density and other inherent characteristics of rare earth additives, by adopting a hemispherical, cylindrical or parabolic structure, the shape of the additive is made more reasonable, effectively reducing the viscous resistance of the molten steel to the additive, getting rid of the influence of the slag layer, increasing the input depth of the rare earth additive, promoting a significant improvement in the rare earth yield and uniformity indicators, and also increasing the applicable composition window range of the intermediate alloy.
[0044] It fundamentally solves the problem of effective addition of rare earths in the steelmaking process.
[0045] Furthermore, the end of the first part away from the second part is a hemispherical or parabolic structure; the coordinates of the edge points of the axial cross section of the first part satisfy the following formula:
[0046] Among them, x is the X-axis coordinate value of the first part along the axial direction, y is the Y-axis coordinate value perpendicular to the axial direction, the coordinate origin is the vertex of the first part away from the end of the second part, n ranges from 0<n<1, and L is the length value of the additive along the axial direction.
[0047] Furthermore, n is in the range of 0.7<n<1. The ratio of the length L1 of the first portion along the axial direction of the cross section to the total length L of the additive is 0.5≤L1 / L≤1. The cross-sectional radius R of the first portion at the end close to the second portion is in the range of 1.5 cm to 24 cm, and the value of L is in the range of 3 cm to 48 cm.
[0048] Under these proportions, the first portion of the additive becomes sharper and accounts for a larger proportion by weight. When added to molten steel, this additive, due to its superior hydrodynamic design, exhibits minimal viscous drag and flotation, allowing it to quickly reach the middle and lower parts of the ladle, ensuring uniform addition of rare earth elements and a higher yield.
[0049] Furthermore, a shell is provided outside the additive, and the shape of the shell matches the shape of the additive; the iron content of the shell is greater than 95wt% and less than 99.9wt%, the thickness of the shell is 0.5cm to 4cm, the melting point is 1500℃ to 1538℃, and the density is 7.6g / cm 3 ~8.6g / cm 3 .
[0050] First, the outer iron alloy layer has a higher melting point and density than the inner rare earth and iron additives, which better protects the rare earth additives and facilitates their storage and transportation. Furthermore, the outer iron alloy prevents rare earth loss caused by reactions between the inner rare earth additives and the slag layer on the surface of the molten steel. Secondly, by adopting a suitable outer shell shape based on the melting point, density, and other characteristics of the inner rare earth additives, the viscous resistance of the molten steel to the additives can be effectively reduced, increasing the depth of rare earth additive injection, significantly improving rare earth yield and uniformity, and expanding the applicable composition window of the master alloy.
[0051] The following describes the test values obtained by the additive under different rare earth contents, different iron contents, different transition metal element contents, different shapes, and with or without a shell in several examples to determine the physical properties of the rare earth-containing additive, as shown in Table 1.
[0052] Table 1
[0053] Table 2 shows two comparative examples of commercially available ferrocerium alloy (Ce: 5wt%, Fe: 95wt%) and ferroydtria alloy (Y: 5wt%, Fe: 95wt%), and their physical properties are shown in Table 2 below:
[0054] Table 2
[0055] Accordingly, an embodiment of the present invention further provides a method for preparing a rare earth-containing additive, which is used to prepare the above-mentioned rare earth-containing additive. Specifically, the additive can be prepared by the following three methods.
[0056] (1) Molten salt electrolysis
[0057] Iron and transition metal elements are made into alloy rods, which serve as high-melting-point iron alloy consumable cathodes.
[0058] Rare earth fluoride and lithium fluoride are placed inside the electrolytic cell as molten salt. The high melting point iron alloy consumable cathode and graphite anode are used to conduct electricity through the molten salt. During electrolysis, direct current is connected through the cathode and anode, and the electrolysis raw material rare earth oxide is added to the electrolysis molten salt through the upper opening of the electrolytic cell. The electrolysis temperature is (T m +50)℃~(T m +100)℃,T m The melting point of rare earth-containing additives. The cathode current density is less than 8A / cm 2 Under the action of direct current, an electrochemical reaction occurs, and the formed rare earth additive alloy drips from the cathode surface to the crucible at the bottom of the electrolytic cell.
[0059] (2) Thermal reduction method
[0060] The raw materials are rare earth fluoride, iron block, transition metal and reducing agent calcium particles, wherein the reducing agent dosage is 105% to 120% of the theoretical value. The raw materials are vacuum dehydrated at 400°C for 2 hours. The dehydrated raw materials are mixed in a mixer and then loaded into a heating furnace. Vacuum the furnace and purge it with argon gas, then pass argon gas to 20000Pa-80000Pa to reduce the volatilization of volatile elements. Heat to (T m +50)℃~(T m +150)℃,T m The melting point of the rare earth-containing additive is obtained by removing the slag after constant temperature for 2 to 10 hours, turning off the power and casting, and cooling the furnace to room temperature to obtain the rare earth-containing additive.
[0061] (3) Melt-matching method
[0062] The raw materials are pure rare earth metals, iron blocks and transition metals, which are proportioned according to the target content of each element in the rare earth additive. The iron blocks and transition elements are placed in the crucible of the medium frequency furnace, and the pure rare earth metals are placed in the charge trough of the medium frequency furnace. The medium frequency furnace is powered on and heated to the melting temperature (T m +50)~(T m +150)℃,T m The furnace atmosphere can be vacuum or atmosphere protection. The pressure in the furnace during vacuum melting is 10 - 8 The furnace pressure is between 10,000 and 110,000 Pa during atmosphere melting. After the iron and transition metal raw materials in the crucible are completely melted, the rare earth metals in the trough are added. After heat preservation and refining, a rare earth-containing additive alloy melt is obtained. The alloy solution is cast into a mold and cooled in the furnace to obtain the rare earth-containing additive.
[0063] The following describes the preparation process of the above additives in detail with reference to several embodiments:
[0064] Example 1:
[0065] Prepare rare earth metal yttrium and pure iron in proportions of 5% and 95% by mass, respectively. Place the pure iron raw material into a crucible in a vacuum induction melting furnace, and place the rare earth metal yttrium into a feed trough in the vacuum induction melting furnace; fill with high-purity argon gas, and when the vacuum in the furnace is maintained at 70,000 Pa, raise the temperature to 1,600°C. After the metal in the crucible is completely melted, add rare earth metal cerium to the molten iron through the feed trough, and refine for 10 minutes after it is completely melted. Finally, pour the alloy solution into a spherical mold with a radius of 10 cm and cool it in the furnace under the protection of an argon atmosphere. The ferrocerium additive in this embodiment has a spherical shape with a radius of 10 cm, a density of 7.7 g / cm3, and a melting point of 1,450°C.
[0066] Comparative Example 1:
[0067] Comparative Example 1 is a commercially available ferrocerium alloy (Ce: 5wt%, Fe: 95wt), which is in the form of a small square block with a side length of 10 cm, a density of 7.8 g / cm3, and a melting point of 1500°C.
[0068] Comparative Example 2:
[0069] Comparative Example 2 is a commercially available yttrium-iron alloy (Y: 5wt%, Fe: 95wt), which has an irregular shape with an equivalent diameter of 10 cm, a density of 7.7 g / cm3, and a melting point of 1450°C.
[0070] The yttrium-iron alloy of Example 1 and the commercially available ferrocerium and yttrium-iron additives of Comparative Examples 1-2 were added as rare earth additives to a ladle with a molten steel depth of 3 m to smelt rare earth steel. The yttrium-iron alloy of Example 1 had significantly better rare earth yield in the ladle, rare earth distribution uniformity, and inclusion modification effect in the steel than those of Comparative Examples 1-2. The comparison results are shown in Table 3.
[0071] Example 2:
[0072] The raw material ratios and preparation methods for the rare earth metal yttrium and pure iron were the same as in Example 1. After refining, the alloy solution was poured into a cylindrical mold with a radius R of 10 cm and a height L of 20 cm and then cooled in a furnace under an argon atmosphere. The yttrium iron additive in this example was cylindrical with a radius of 10 cm and a height of 20 cm, a density of 7.7 g / cm³, and a melting point of 1450°C.
[0073] The yttrium-iron alloy of Example 2 and the commercially available ferrocerium and yttrium-iron additives of Comparative Examples 1-2 were used as rare earth additives and added to a ladle with a molten steel depth of 3 m to smelt rare earth steel. The rare earth yield, rare earth distribution uniformity and inclusion modification effect of the yttrium-iron alloy of Example 2 in the ladle were significantly better than those of Comparative Examples 1-2. The comparison results are shown in Table 3.
[0074] Example 3:
[0075] The raw material ratios and preparation methods for the rare earth metal yttrium and pure iron were the same as those in Example 1. After refining, the alloy solution was poured into a parabolic mold with a radius R of 10 cm, L1 of 10 cm, a height L of 20 cm, and n of 0.4, and then cooled in a furnace under an argon atmosphere. The yttrium iron additive in this example had a parabolic shape with a radius R of 10 cm, L1 of 10 cm, a height L of 20 cm, and n of 0.4, a density of 7.7 g / cm3, and a melting point of 1450°C.
[0076] The yttrium-iron alloy of Example 3 and the commercially available ferrocerium and yttrium-iron additives of Comparative Examples 1-2 were used as rare earth additives and added to a ladle with a molten steel depth of 3 m to smelt rare earth steel. The rare earth yield, rare earth distribution uniformity and inclusion modification effect of the ferrocerium alloy of Example 3 in the ladle were significantly better than those of Comparative Examples 1-2. The comparison results are shown in Table 3.
[0077] Table 3
[0078] Tables 1, 2, and 3 demonstrate that the present invention, through controlled rare earth, iron, and transition metal composition and optimized shape, offers a wide window for additive compatibility. The alloy additives of the present invention effectively reduce the viscous resistance of the molten steel to the additives, eliminate the effects of the slag layer, and allow for optimal addition to the molten steel. Compared to Comparative Examples 1-2, inclusions are smaller, the rare earth element yield is higher, and the distribution is more uniform.
[0079] The embodiment of the present invention is intended to protect a rare earth-containing additive, the additive comprising: rare earth metal and iron, the rare earth metal content is 5wt% to 90wt%, the iron content is 10wt% to 95wt%; the density of the additive is 6.3g / cm 3 ~8.4g / cm 3 , melting point 850℃~1450℃, oxygen content ≤150ppm, maximum inclusion size ≤35μm, total inclusion amount ≤0.5wt%. The above technical solution has the following effects:
[0080] 1. The additive prepared by this patent has the advantages of low oxygen, small total amount and size of inclusions, etc., which can effectively reduce the introduction of foreign rare earth oxide inclusions in steel and alleviate nozzle blockage;
[0081] 2. By optimizing the composition of rare earth, iron, and transition metal microalloying elements in the additive, the rare earth additive has an appropriate density and melting point, achieving simultaneous addition of rare earth and the main transition metal microalloying elements in steel and effectively increasing the depth of additive addition, thereby improving rare earth yield and distribution uniformity;
[0082] 3. According to the melting point, density and other inherent characteristics of rare earth additives, a reasonable rare earth additive shape is designed, which can effectively reduce the viscous resistance of molten steel to the additive, get rid of the influence of the slag layer, increase the input depth of rare earth additives, promote a significant improvement in rare earth yield and uniformity indicators, and also increase the applicable composition window range of the master alloy.
[0083] It should be understood that the above-described specific embodiments of the present invention are merely illustrative or illustrative of the principles of the present invention and do not constitute limitations of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included within the scope of protection of the present invention. In addition, the appended claims are intended to cover all variations and modifications that fall within the scope and metes and bounds of the appended claims, or equivalents thereof.
Claims
1. A rare earth-containing additive, characterized in that: include: Rare earth metal and iron, wherein the rare earth metal content is 5wt% to 90wt%, and the iron content is 10wt% to 95wt%; The density of the additive is 6.3 g / cm 3 ~8.4g / cm 3 , melting point is 850℃~1450℃, oxygen content is ≤150ppm, maximum size of inclusions is ≤35μm, and total amount of inclusions is ≤0.5wt%.
2. The rare earth-containing additive according to claim 1, characterized in that: The additive comprises: a first part and a second part formed in one piece; One end of the first part away from the second part is a hemispherical, cylindrical or parabolic structure; The cross section of the connecting end of the second part and the first part is circular or elliptical; The maximum dimension of any cross section of the second portion is smaller than the maximum dimension of the cross section of the connecting end of the first portion and the second portion.
3. The rare earth-containing additive according to claim 2, characterized in that: One end of the first part away from the second part is a hemispherical or parabolic structure; The edge point coordinates of the axial cross section of the first part satisfy the following formula: Among them, x is the X-axis coordinate value of the first part along the axial direction, y is the Y-axis coordinate value perpendicular to the axial direction, the coordinate origin is the vertex of the first part away from the second part, n is the taper control factor of the first part of the additive, when n=0, the first part is a cylinder, when n=1, the first part is a cone, the value range of n is 0<n<1, and L is the length value of the additive along the axial direction.
4. The rare earth-containing additive according to claim 3, characterized in that: The value range of n is 0.7<n<1.
5. The rare earth-containing additive according to claim 3, characterized in that: The ratio of the length L1 of the first portion along the axial direction of the cross section to the total length L of the additive is: 0.5≤L1 / L≤1; The value range of the cross-sectional radius R of the end of the first part close to the second part is 1.5 cm~24cm, L value range is 3cm~48cm.
6. The rare earth-containing additive according to claim 1, characterized in that: A shell is also provided outside the additive, and the shape of the shell matches the shape of the additive; The iron content of the shell is greater than 95wt% and less than 99.9wt%, the thickness of the shell is 0.5cm to 4cm, the melting point is 1500℃ to 1538℃, and the density is 7.6g / cm 3 ~8.6g / cm 3 .
7. The rare earth-containing additive according to claim 1, characterized in that: The additive further comprises: a transition metal, wherein the transition metal comprises: at least one of nickel, chromium, tungsten, molybdenum, cobalt, manganese, vanadium, niobium and titanium; The content of the transition metal is 0.1wt% to 15wt%, the content of the rare earth metal is 15wt% to 70wt%, and the content of iron is 20wt% to 70wt%; The density of the additive is 7.2-8.2 g / cm 3 , melting point is 1000-1300℃, oxygen content ≤100ppm, carbon content ≤300ppm, maximum size of inclusions ≤25μm, total amount of inclusions ≤0.1wt%.
8. The rare earth-containing additive according to claim 7, characterized in that: The transition metal includes at least one of chromium, tungsten, molybdenum, vanadium, niobium and titanium.
9. The rare earth-containing additive according to any one of claims 1 to 8, characterized in that: The rare earth metal includes at least one of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium; Preferably, the rare earth metal includes at least one of lanthanum, cerium and yttrium.
Citation Information
Patent Citations
Preparation method of rare earth ferroalloy
CN111411372A
Iron-niobium-rare earth intermediate alloy and preparation method thereof
CN112981223A
Rare earth-containing additive
CN116516106A
Deoxidization body easy to settle
CN202913013U
Metallic lead deoxidier
CN206109447U
Cited By
Powder spraying refining process for production of rare earth oxide dispersion strengthened alloy
CN119571010A