Electrode membrane processing method and electrode membrane processing device

By extruding and extending the fibrous powder to increase the contact area between PTFE particles and active material powder, the problem of insufficient strength of the dry electrode diaphragm is solved, and the performance of the electrode diaphragm and the energy density of the battery are improved.

WO2024222449A1PCT designated stage expired Publication Date: 2024-10-31EVE ENERGY CO LTD

Patent Information

Application Number
PCT/CN2024/086764
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-12-29
Filing Date
2024-04-09
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The strength and toughness of the dry electrode diaphragm are insufficient, resulting in low production efficiency and affecting battery performance. Adding PTFE particles to improve strength will reduce the content of active material powder and conductive agent, affecting battery energy density.

Method used

By extruding the initial PTFE particles, active material powder and conductive agent in the fibrous powder into a calendered embryo body, the contact area between the initial pressed PTFE particles and the active material powder and conductive agent is increased, and the shear during the extrusion and extension process is utilized. Cutting and stretching effects fully fiberize the PTFE particles to improve the coating effect.

Benefits of technology

It improves the strength and toughness of the electrode diaphragm, enhances liquid absorption, and maintains the energy density and performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024086764_31102024_PF_FP_ABST
    Figure CN2024086764_31102024_PF_FP_ABST
Patent Text Reader

Abstract

An electrode membrane processing method and an electrode membrane processing device. The electrode membrane processing method comprises the following steps: providing a fiberized powder, wherein the fiberized powder contains initial PTFE particles, an active substance powder and a conductive agent, with the contact area between the initial PTFE particles and the active substance powder and between the initial PTFE particles and the conductive agent being set as S1 (S01); placing the fiberized powder in a blank-forming module, and performing extrusion molding on the fiberized powder to form a calendered blank body, wherein the state of the PTFE particles in the calendered blank body is initially pressed PTFE particles, with the contact area between the initially pressed PTFE particles and the active substance powder and between the initially pressed PTFE particles and the conductive agent being set as S2, and S2 being larger than S1 (S02); and calendaring and molding the calendered blank body into a finished product membrane (S03).
Need to check novelty before this filing date? Find Prior Art

Description

Electrode membrane processing method and electrode membrane processing equipment

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on December 29, 2023, with application number 202311873521.3. The entire contents of the above application are incorporated by reference into this application. Technical Field

[0002] The present application relates to the technical field of battery electrode preparation, for example, to an electrode membrane processing method and an electrode membrane processing device. Background Art

[0003] With the continuous strengthening of people's environmental awareness and the continuous development of new energy technologies, lithium-ion batteries have received widespread attention. The electrode membrane preparation process of lithium-ion batteries is generally divided into dry electrode process and wet coating process. In process research and development, dry electrodes have advantages over wet electrodes in material cost, equipment space, energy consumption, environmental protection and investment cost. At the same time, the dry electrode process can produce thicker electrodes, so that the electrode is no longer limited to the coating crack thickness of 160μm. At the same time, it can ensure that the performance of batteries made with dry electrodes is comparable to that of batteries made with wet coating process. Therefore, lithium-ion batteries made with dry electrodes have gradually become the mainstream of the market.

[0004] In related technologies, the preparation process for dry-process electrode membranes involves first fiberizing a mixed powder containing added polytetrafluoroethylene (PTFE) particles, and then directly rolling the fiberized powder through a roller pressing device to achieve dry-process electrode membrane preparation. However, this method of directly rolling the fiberized powder into a membrane results in a large amount of unfiberized parts in the PTFE particles, resulting in insufficient strength and toughness of the roll-formed membrane. Furthermore, due to the insufficient strength and toughness of the membrane, the quality of the produced dry-process electrode membrane is poor. Furthermore, the insufficient strength and toughness of the dry-process electrode membrane also restricts the actual production efficiency of the dry-process electrode membrane, resulting in low actual production efficiency of the dry-process electrode membrane.

[0005] The strength and toughness of dry-process electrode membranes depend on the amount of PTFE particles added and the processing technology used. However, increasing the PTFE particle content will affect battery energy density and performance. Since the total mass of a dry-process electrode membrane is constant, and the electrochemical reaction of the dry-process electrode membrane relies on active material powder and conductive agent, PTFE particles do not participate in the electrochemical reaction. Increasing the amount of PTFE particles in the dry-process electrode membrane will lead to a decrease in the content of active material powder and conductive agent in the dry-process electrode membrane, thereby reducing the energy density of the dry-process electrode membrane. Furthermore, as the PTFE particle content in the dry-process electrode membrane increases, the side reactions of the PTFE particles also increase. These side reactions primarily arise from the carbon-fluorine (CF) bond breaking during battery discharge with reduced anions and reduced lithium, generating byproducts. This results in active lithium loss in the battery cell, electrolyte consumption, and byproduct deposition, which in turn affects battery performance. In order to meet the needs of rapid production of dry-process membranes with high strength, high toughness and fast liquid absorption rate, the processing technology of dry-process electrode membranes is improved without changing the amount of PTFE particles added, so as to improve the performance of battery membranes without affecting the battery energy density and battery performance.

[0006] Therefore, there is an urgent need to invent an electrode membrane processing method and an electrode membrane processing equipment to solve the above problems. Summary of the Invention

[0007] The present application provides an electrode diaphragm processing method and an electrode diaphragm processing device to improve the fiberization degree of PTFE particles in the fiberized powder and improve the strength and toughness of the electrode diaphragm.

[0008] In a first aspect, the present application provides a method for processing an electrode membrane, comprising:

[0009] Providing a fibrous powder, wherein the fibrous powder contains initial PTFE particles, active material powder and a conductive agent, wherein the contact area between the initial PTFE particles, the active material and the conductive agent is set to S1;

[0010] The fibrous powder is placed in an embryo forming module and extruded into a calendered embryo body, wherein the PTFE particles in the calendered embryo body are in the form of initially compressed PTFE particles, and the contact area between the initially compressed PTFE particles, the active material powder, and the conductive agent is set to S2, wherein S2 is greater than S1;

[0011] The calendered embryo body is calendered to form a finished film.

[0012] In one embodiment, the steps of providing a fiberized powder, placing the fiberized powder in an embryo forming module, and extruding the powder into a calendered embryo body include:

[0013] The initial PTFE particles, the active material powder and the conductive agent are mixed according to a preset ratio to form the fiberized powder;

[0014] placing the fiberized powder in the embryo forming module;

[0015] Scraping the upper end surface of the fibrous powder in the embryo forming module flat;

[0016] The fibrous powder in the flattened embryo module is extruded and molded, and the fibrous powder is heated while being extruded to form the calendered embryo body.

[0017] In one embodiment, before placing the fibrosis powder in the embryo forming module, the method further comprises: weighing the fibrosis powder to obtain a preset weight of the fibrosis powder;

[0018] The step of placing the fibrosis powder in the embryo forming module includes placing the fibrosis powder of a preset weight into the embryo forming module.

[0019] In one embodiment, the method further comprises: in the process of extruding the fibrotic powder into the calendered embryo, adding the fibrotic powder to the embryo forming module so that the weight of the extruded calendered embryo is a preset weight.

[0020] In one embodiment, during the process of extruding the fibrous powder into the calendered embryo, the pressure range of the calendered embryo is 50N to 2000N, and the heating temperature range is 0°C to 200°C.

[0021] In one embodiment, after the calendering embryo is formed by extrusion, a pre-film forming process is further included;

[0022] The pre-filming process includes: pressing the calendered embryo body into a pre-processed film sheet through a pre-filming mold;

[0023] The step of calendering the calendered blank into a finished film sheet includes: calendering the pre-processed film sheet into the finished film sheet.

[0024] In one embodiment, the pre-film forming process includes: a first thinning process and a second thinning process;

[0025] The first thinning process includes thinning the calendered embryo body to a first calendered film with a thickness of H1;

[0026] The second thinning process includes thinning the first calendered film into a second calendered film with a thickness of H2.

[0027] In one embodiment, in the second thinning process, the feeding speed of the first calendered film is in the range of 0.1 m / s to 2 m / s.

[0028] In one embodiment, the electrode membrane processing method further includes:

[0029] The storage process includes: storing and placing the finished film.

[0030] In one embodiment, the electrode membrane processing method further includes: a deviation correction process and an edge trimming process;

[0031] The trimming process is located before the storage process, and the trimming process includes cutting the width of the finished film sheet into a preset width so that the storage process can store and place the finished film sheet of the preset width;

[0032] The deflection correction process is located before the edge trimming process, and the deflection correction process includes aligning the finished film with a cutting tool used in the edge trimming process.

[0033] In one embodiment, in the receiving process, the feeding speed of the finished film is in the range of 0.1 m / s to 2 m / s.

[0034] In a second aspect, an embodiment of the present application provides an electrode membrane processing device, including an embryonic forming module and a finished product calendering module;

[0035] The embryo forming module is configured to extrude the provided fibrous powder into a calendered embryo body, wherein the fibrous powder contains initial polytetrafluoroethylene (PTFE) particles, active material powder, and a conductive agent, and the contact area between the initial PTFE particles and the active material powder and the conductive agent is set to S1; the PTFE particles in the calendered embryo body are in the form of initially compressed PTFE particles, and the contact area between the initially compressed PTFE particles and the active material powder and the conductive agent is set to S2, and S2 is greater than S1;

[0036] The finished product calendering module is configured to calender the calendered blank into the finished film.

[0037] In one embodiment, the embryo forming module includes an embryo forming mold, a scraping member and an embryo forming roller, the embryo forming mold has a forming groove, the groove opening of the forming groove faces the top of the embryo forming mold, the scraping member and the embryo forming roller are both arranged in the forming groove, and the scraping member and the embryo forming roller are respectively connected to the first driving member and the second driving member, the first driving member is configured to drive the scraping member to move horizontally so as to scrape the upper end surface of the fibrotic powder arranged in the forming groove along the horizontal plane, and the second driving member is configured to drive the embryo forming roller to move horizontally so as to extrude the fibrotic powder in the forming groove to form the calendered embryo body.

[0038] In one embodiment, a heating element is provided on the embryo forming mold and / or the embryo forming pressing roller.

[0039] In one embodiment, the electrode membrane processing equipment further includes:

[0040] The calendering module is arranged between the embryo forming module and the finished product calendering module, and the calendering module is configured to calender the calendered embryo body into a pre-processed membrane sheet.

[0041] In one embodiment, the calendering module comprises: a first calendering module and a second calendering module;

[0042] The first calendering module is disposed between the embryo forming module and the second calendering module, and is configured to calender the calendered embryo body into a first calendered membrane. The PTFE particles in the first calendered membrane are in the form of initially calendered PTFE particles. The contact area between the initially calendered PTFE particles and the active material powder and the conductive agent is set to S3, and S2 is greater than S2;

[0043] The second calendering module is arranged between the first calendering module and the finished product calendering module. The second calendering module is configured to calender the first calendered membrane into a second calendered membrane. The PTFE particles in the second calendered membrane are in the state of two-extended PTFE particles. The contact area between the two-extended PTFE particles and the active material powder and the conductive agent is set to S4, and the S4 is greater than the S3. The second calendered membrane is the pre-processed membrane.

[0044] In one embodiment, the electrode membrane processing equipment further includes:

[0045] A receiving module is located downstream of the finished product calendering module, and the receiving module includes a winding roller, which is configured to wind up the finished film.

[0046] In one embodiment, the electrode membrane processing equipment further includes:

[0047] A conveying module, which sequentially connects the embryo module, the first calendering module, the second calendering module, the finished product calendering module and the storage module. The conveying module is configured to transfer the calendered embryo to the first calendering module, transfer the first calendered film to the second calendering module, transfer the second calendered film to the finished product calendering module, and transfer the finished product film to the storage module.

[0048] In one embodiment, the first calendering module comprises:

[0049] a first pressing roller;

[0050] a limiter, disposed below the first pressing roller, with a gap between the first pressing roller and the limiter, and the limiter being configured to limit a width of the first rolled film;

[0051] A driving member is provided at one end of the first pressing roller close to the embryo forming module, and the driving member is configured to drive the calendered embryo body to move in a direction close to the first pressing roller.

[0052] In one embodiment, the second calendering module comprises:

[0053] A thinning roller pressing structure, comprising two second pressing rollers arranged opposite to each other in an up-and-down direction, with a gap between the two second pressing rollers;

[0054] a first speed detecting member, the first speed detecting member being located at one end of the second pressing roller close to the first calendering module, the first speed detecting member being configured to detect a speed at which the conveying module drives the first calendered film to enter the gap between the two second pressing rollers, the first speed detecting member being signal-connected to the conveying module;

[0055] The conveying module is further configured to control the speed at which it drives the first calendered film to enter the gap between the two second pressing rollers according to the detection information of the first speed detecting member.

[0056] In one embodiment, the finished product calendering module includes:

[0057] A finished product rolling structure, comprising two third pressing rollers arranged opposite to each other in an up-and-down direction, with a gap between the two third pressing rollers;

[0058] a second speed detecting member, the second speed detecting member being located at one end of the third pressing roller close to the second calendering module, the second speed detecting member being configured to detect the speed at which the conveying module drives the second calendered film to enter the gap between the two third pressing rollers, the second speed detecting member being signal-connected to the conveying module;

[0059] The conveying module is further configured to control the speed at which it drives the second calendered film to enter the gap between the two third pressing rollers according to the detection information of the second speed detecting member.

[0060] In one embodiment, the electrode membrane processing equipment further includes:

[0061] A first cutting module is provided between the finished product calendering module and the storage module, and the first cutting module is configured to cut the width of the finished film into a first preset width.

[0062] In one embodiment, the electrode membrane processing equipment further includes:

[0063] A deviation correction module is provided between the finished product calendering module and the first cutting module, and the deviation correction module is configured to drive the finished product film to face the first cutting module.

[0064] Beneficial effects of this application:

[0065] The electrode diaphragm processing method provided by the present application is to extrude the fibrotic powder into a calendered embryo, so that the initial PTFE particles in the fibrotic powder are pressed into initial compressed PTFE particles, and the contact area S2 of the initial compressed PTFE particles in the calendered embryo with the active material powder and the conductive agent is ensured to be greater than the contact area S1 of the initial PTFE particles in the fibrotic powder with the active material powder and the conductive agent, and the calendered embryo is calendered into a finished diaphragm, so as to achieve the effect of squeezing the initial PTFE particles in the fibrotic powder together to form a calendered embryo, and fully expanding the initial compressed PTFE particles squeezed together in the calendered embryo. , utilizing the shearing and stretching effects generated during the extrusion and extension of the fiberized powder, the initially pressed PTFE particles in the calendered embryo are fully fiberized, so as to ensure the full fiberization of the PTFE particles without changing the content of each component in the fiberized powder, and improve the coating effect of the PTFE particles on the active material powder and the conductive agent in the fiberized powder, so that the fiberized PTFE particles can more fully wrap and connect the active material powder and the conductive agent in the fiberized powder, thereby achieving the effect of improving the strength and toughness of the electrode diaphragm, improving the liquid absorption of the electrode diaphragm, and ensuring the energy density and battery performance of the battery.

[0066] The present application also provides an electrode diaphragm processing device, which realizes that the initial PTFE particles in the fibrotic powder are squeezed together to form a calendered embryo, so that the contact area S2 of the initial PTFE particles in the calendered embryo with the active material powder and the conductive agent is greater than the contact area S1 of the initial PTFE particles in the fibrotic powder with the active material powder and the conductive agent, and the initial PTFE particles squeezed together in the calendered embryo are calendered and expanded, and the similar shearing and stretching effects generated in the process of extruding and stretching the fibrotic powder are utilized to make the PTFE particles The initially pressed PTFE particles in the calendered embryo are fully fiberized, so as to ensure the full fiberization of the PTFE particles without changing the content of each component in the fiberized powder, further increase the contact area between the PTFE particles and the active material powder and the conductive agent, and improve the coating effect of the PTFE particles on the active material powder and the conductive agent in the fiberized powder, so that the fiberized PTFE particles can more fully wrap and connect the active material powder and the conductive agent in the fiberized powder, thereby achieving the effect of improving the strength and toughness of the electrode diaphragm, improving the liquid absorption of the electrode diaphragm, and ensuring the energy density and battery performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] FIG1 is a flow chart of an electrode membrane processing method provided in Example 1 of the present application;

[0068] FIG2A is a schematic structural diagram of an electrode membrane processing device provided in Example 2 of the present application;

[0069] FIG2B is a schematic structural diagram of another electrode membrane processing device provided in Example 2 of the present application.

[0070] In the picture:

[0071] 1. Calendered embryo; 2. First calendered film; 3. Second calendered film; 4. Finished film;

[0072] 1000. Electrode membrane processing equipment;

[0073] 100, embryo forming module; 110, embryo forming mold; 120, embryo forming roller; 130, scraping member; 140, forming groove;

[0074] 200, first calendering module; 210, auxiliary driving member; 220, limiting member; 230, first pressing roller;

[0075] 300, second calendering module; 310, first speed detection component; 320, second pressing roller;

[0076] 400, finished product calendering module; 410, second speed detection component; 420, third pressing roller;

[0077] 500, storage module;

[0078] 600, conveying module;

[0079] 700, first cutting module;

[0080] 800, correction module;

[0081] 900. Second cutting module. DETAILED DESCRIPTION

[0082] In the description of this application, unless otherwise specified or limited, the terms "connected," "connect," and "fixed" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integration; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; and can refer to internal communication between two components or interaction between two components. Those skilled in the art will understand the specific meanings of the above terms in this application based on the specific circumstances.

[0083] In this application, unless otherwise expressly specified or limited, a first feature being "above" or "below" a second feature may include the first feature being in direct contact with the second feature, or may include the first feature being in contact with the second feature through another feature between them instead of being in direct contact. Moreover, a first feature being "above," "above," and "above" a second feature may include the first feature being directly above or obliquely above the second feature, or may simply mean that the first feature is higher in level than the second feature. A first feature being "below," "below," and "below" a second feature may include the first feature being directly below or obliquely below the second feature, or may simply mean that the first feature is lower in level than the second feature.

[0084] In the description of this embodiment, the terms "upper," "lower," "left," and "right," etc., regarding orientations or positions, are based on the orientations or positions shown in the accompanying drawings and are intended solely for ease of description and simplified operation. They do not indicate or imply that the devices or components referred to must have, be constructed, or operate in a specific orientation. Therefore, they should not be construed as limitations on this application. Furthermore, the terms "first" and "second" are used solely for descriptive purposes and have no special meanings. Example 1

[0085] This embodiment provides a method for processing an electrode membrane. As shown in FIG1 and FIG2A , the method for processing an electrode membrane provided by this embodiment includes the following steps:

[0086] S01, providing a fibrous powder, wherein the fibrous powder contains initial PTFE particles, active material powder and a conductive agent, and the contact area between the initial PTFE particles, the active material powder and the conductive agent is set to S1;

[0087] S02, placing the fibrotic powder in the embryo forming module 100, and the embryo forming module 100 extruding the fibrotic powder to form a calendered embryo body 1, wherein the PTFE particles in the calendered embryo body 1 are in the state of initially compressed PTFE particles, and the contact area between the initially compressed PTFE particles and the active material powder and the conductive agent is set to S2, where S1 is smaller than S2;

[0088] S03, calendering the calendered embryonic body 1 into a finished film 4.

[0089] The electrode diaphragm processing method extrudes the fibrous powder into a calendered embryo 1, so that the initial PTFE particles in the fibrous powder are pressed into initial pressed PTFE particles, ensuring that the contact area S2 of the initial pressed PTFE particles in the calendered embryo 1 with the active material powder and the conductive agent is greater than the contact area S1 of the initial PTFE particles in the fibrous powder with the active material powder and the conductive agent, and calendering the calendered embryo 1 into a finished diaphragm 4, achieving the effect of squeezing the initial PTFE particles in the fibrous powder together to form the calendered embryo 1, and fully expanding the initial pressed PTFE particles squeezed together in the calendered embryo 1, and utilizing the fibrous powder to extrude and extend The shearing and stretching effects generated during the process fully fiberize the initially pressed PTFE particles in the calendered embryo 1, so as to ensure the full fiberization of the PTFE particles without changing the content of each component in the fiberized powder, further increase the contact area between the PTFE particles and the active substance powder and the conductive agent, and improve the coating effect of the PTFE particles on the active substance powder and the conductive agent in the fiberized powder, so that the fiberized PTFE particles can more fully wrap and connect the active substance powder and the conductive agent in the fiberized powder, thereby achieving the effect of improving the strength and toughness of the electrode diaphragm, improving the liquid absorption of the electrode diaphragm, and ensuring the energy density and battery performance of the battery.

[0090] In the related art, the preparation method of dry electrode membrane is to directly press the fiberized powder into a dry electrode membrane. The fiberization effect of PTFE particles is poor, resulting in poor coating effect between PTFE particles and active material powder and conductive agent, which in turn affects the strength and toughness of the dry electrode membrane.

[0091] In this embodiment, when the fibrotic powder is extruded into a calendered embryo 1, the fibrotic powder is compressed, and the active material, conductive agent and PTFE particles in the fibrotic powder are all forced to gather together, thereby increasing the contact area between the PTFE particles and the active material powder and the conductive agent. When the calendered embryo 1 is calendered into shape, the calendered embryo 1 extends outward, and the PTFE particles gathered together in the calendered embryo 1 are subjected to tensile force and / or shear force, so that the PTFE particles in the calendered embryo 1 are fully fibrotic, further increasing the contact area between the PTFE particles and the active material powder and the conductive agent, thereby improving the coating effect of the PTFE particles on the active material and the conductive agent, and improving the strength and toughness of the finished diaphragm 4 after calendering.

[0092] During the process of extruding the fiberized powder into the calendered body 1, the steps of forming the calendered body 1 include:

[0093] The initial PTFE particles, active material powder and conductive agent are mixed according to a preset ratio to form a fiberized powder;

[0094] Placing the fiberized powder in the embryo forming module 100;

[0095] Scrape the upper end surface of the fiberized powder in the embryo forming module 100 flat;

[0096] The fibrous powder in the flattened embryo forming module 100 is extruded and formed, and the fibrous powder is heated while being extruded to obtain a calendered embryo body 1 .

[0097] The initial PTFE particles, active material powder and conductive agent are first mixed according to a preset ratio to form a fiberized powder, and then the fiberized powder is placed in the embryo forming module 100, the upper end surface of the fiberized powder in the embryo forming module 100 is scraped flat, and finally the scraped fiberized powder is extruded and molded, and the fiberized powder is heated during the extrusion molding. This can improve the extrusion molding efficiency of the fiberized powder and ensure the molding quality of the calendered embryo 1, thereby ensuring the processing quality of the subsequent finished product diaphragm 4.

[0098] For example, the preset ratio of initial PTFE particles: active material powder: conductive agent is 1-10:98-85:0.5-3. In this embodiment, the preset ratio of initial PTFE particles: active material powder: conductive agent is 2:97:1. In other embodiments, the preset ratio of initial PTFE particles: active material powder: conductive agent can also be adjusted within the range of 1-10:98-85:0.5-3.

[0099] In other embodiments, the preset ratio of initial PTFE particles: active material powder: conductive agent can be 1:98:1, 3:96:1, 4:95:1, 5:94:1, 5:93:1, 7:92:1, 8:91:1, 9:90:1, 10:89:1, 1:97:2, 2:96:2, 3:95:2, 4:94:2, 5:93:2, 6:92:2, 7:91:2, 8:90:2, 9:989:2, 10:88:2, 1:96:3, 2:95:3, 3:94:3, 4:93:3, 5:92:3, 6:91:3, 7:90:3, 8:89:3, 9:88:3 or 10:97:3. It is understood that the aforementioned preset ratio of initial PTFE particles: active material powder: conductive agent is merely illustrative and is not intended to be a specific limitation. Furthermore, this preset ratio is not a primary innovation of this solution; in actual applications, the ratio can be adjusted based on actual needs.

[0100] During the process of extruding the fibrous powder into the calendered embryo 1, the pressure range of the calendered embryo is 50N to 2000N, and the heating temperature range is 0°C to 200°C. In this embodiment, the pressure of the calendered embryo is 500N and the heating temperature is 100°C. In other embodiments, the rolling pressure of the embryo pressing roller 120 can be adjusted within the range of 50N to 1000N and the heating temperature can be adjusted within the range of 0°C to 200°C according to actual needs. This embodiment is not specifically limited. In other embodiments, the pressure of the calendered embryo can be 50N, 100N, 200N, 300N, 400N, 600N, 700N, 800N, 900N, 1000, 1100N, 1200N, 1300N, 1400N, 1500N, 1600N, 1700N, 1800N, 1900N or 2000N. In other embodiments, the heating temperature may be 0°C, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, or 200°C. It is understood that the above-mentioned pressing pressure and heating temperature for pressing the embryo can be arbitrarily combined to ensure the pressing effect of the calendered embryo 1. The above-mentioned pressing pressure and heating temperature are merely exemplary. Any heating temperature and pressing pressure within the range of 0°C to 200°C and the range of 50N to 2000N can also be selected to press the calendered embryo 1.

[0101] Optionally, before the fibrotic powder is placed in the embryo forming module 100, the fibrotic powder is weighed, and after a preset weight of the fibrotic powder is weighed, it is placed in the embryo forming module 100. By weighing the fibrotic powder before extrusion molding and placing the preset weight of the fibrotic powder in the embryo forming module 100, the consistency of the product specifications of the subsequent calendered embryo 1 and the finished membrane 4 can be ensured.

[0102] During the actual extrusion process of the fibrotic powder, the fibrotic powder may fall from the embryo forming module 100. Therefore, during the extrusion process of the fibrotic powder into the calendered embryo 1, the electrode diaphragm processing method also includes a feeding step to ensure that the extruded calendered embryo 1 maintains a preset weight, further ensuring the consistency of the product specifications of the subsequent calendered embryo 1 and the finished diaphragm 4. The "feed" added in the feeding step is the fibrotic powder formed by mixing the initial PTFE particles, the active material powder, and the conductive agent according to a preset ratio.

[0103] The feeding steps include:

[0104] Weighing the pressed calendered embryo body 1 to obtain the actual weight of the pressed calendered embryo body 1;

[0105] If the actual weight is the same as the preset weight, there is no need to add fiberized powder;

[0106] If the actual weight is less than the preset weight, the weight of the fibrous powder to be added is calculated based on the difference between the actual weight of the pressed calendered embryo 1 and the preset weight of the fibrous powder placed in the embryo forming module 100;

[0107] The pressed calendered embryo body 1 is placed back into the embryo forming module 100, and the fibrous powder of the feed weight is placed into the embryo forming module 100;

[0108] Scrape the upper end surface of the fiberized powder in the embryo forming module 100 flat;

[0109] Extruding the fibrous powder in the flattened embryo forming module 100 and the calendered embryo body 1, and heating the fibrous powder while extruding the fibrous powder;

[0110] The pressed calendered embryo body 1 is weighed again to obtain the actual weight of the calendered embryo body 1;

[0111] If the actual weight is the same as the preset weight, the feeding operation is stopped. If the actual weight is still less than the preset weight, the feeding operation is continued until the actual weight is the same as the preset weight.

[0112] Optionally, after the calendered embryo 1 is formed, the electrode diaphragm processing method further includes a pre-filming step, wherein the calendered embryo 1 is calendered through a pre-filming mold to form a pre-processed diaphragm, and then the pre-processed diaphragm is calendered into a finished diaphragm 4. By first calendering the calendered embryo 1 into a pre-processed diaphragm after the calendered embryo 1 is extruded, and then calendering the pre-processed diaphragm into the finished diaphragm 4, the calendered embryo 1 is thinned before being calendered into the finished diaphragm 4. This can improve the fiberization effect of the PTFE particles in the calendered embryo 1, thereby improving the coating effect of the PTFE particles on the active material powder and the conductive agent, and improving the strength and toughness of the finished diaphragm 4.

[0113] The pre-filming process includes a first thinning process and a second thinning process. The first thinning process is used to thin the calendered body 1 to a first calendered film sheet 2 with a thickness of H1, and the second thinning process is used to thin the first calendered film sheet 2 to a second calendered film sheet 3 with a thickness of H2. The first thinning process thins the calendered body 1 to a first calendered film sheet 2 with a thickness of H1, and the second thinning process thins the first calendered film sheet 2 to a second calendered film sheet 3 with a thickness of H2. This achieves step-by-step thinning of the calendered body 1, further improving the fiberization effect of the PTFE particles in the calendered body 1.

[0114] For example, the thickness H1 of the first rolled film 2 ranges from 0.5 mm to 5 mm, and the thickness H2 of the second rolled film 3 ranges from 0.1 mm to 1 mm. In this embodiment, the thickness of the first rolled film 2 can be 2 mm, and the thickness of the second rolled film 3 can be 0.5 mm. In other embodiments, the thickness H1 of the first rolled film 2 can be adjusted within the range of 0.5 mm to 5 mm, and the thickness H2 of the second rolled film 3 can be adjusted within the range of 0.1 mm to 1 mm according to actual needs. This embodiment does not impose specific limitations.

[0115] In other embodiments, H1 may be 0.5 mm, 1.0 mm, 1.5 mm, 2.5 mm, 3.0 mm, 3.5 mm, 4.0 mm, 4.5 mm, or 5.0 mm, and H2 may be 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, or 1.0 mm. It is understood that the specific values ​​of the thickness H1 of the first rolled film 2 and the thickness H2 of the second rolled film 3 are merely illustrative and are not intended to be limiting.

[0116] To improve the thinning effect of the calendered body 1 during the first and second thinning steps, the feed speed of the first calendered film 2 in the second thinning step is set within a range of 0.1 m / s to 2 m / s to ensure sufficient thinning of the first calendered film 2 during the second thinning step. In this embodiment, the feed speed of the first calendered film 2 is 1 m / s. In other embodiments, the feed speed of the first calendered film 2 can be adjusted within the range of 0.1 m / s to 2 m / s based on actual needs, and this embodiment does not impose any specific limitations. In other embodiments, the feed speed of the first calendered film 2 may be 0.1 m / s, 0.2 m / s, 0.3 m / s, 0.4 m / s, 0.5 m / s, 0.6 m / s, 0.7 m / s, 0.8 m / s, 0.9 m / s, 1.1 m / s, 1.2 m / s, 1.3 m / s, 1.4 m / s, 1.5 m / s, 1.6 m / s, 1.7 m / s, 1.8 m / s, 1.9 m / s or 2.0 m / s. It will be understood that the feed speed of the first calendered film 2 is only for illustrative purposes and is not specifically limited herein.

[0117] Optionally, the electrode membrane processing method further includes a storage step for storing and placing the finished membrane 4. By providing the storage step for storing and placing the finished membrane 4, the processed finished membrane 4 can be stored, thereby avoiding unnecessary damage to the finished membrane 4 due to accumulation after processing, and improving the protection of the finished membrane 4.

[0118] In the storage process, the feeding speed of the finished diaphragm 4 ranges from 0.1m / s to 2m / s. In this embodiment, the feeding speed of the finished diaphragm 4 can be selected as 1m / s. In other embodiments, the feeding speed of the finished diaphragm 4 can be adjusted within the range of 0.1m / s to 2m / s according to actual needs, and this embodiment does not make specific limitations. In other embodiments, the feeding speed of the finished diaphragm 4 can be 0.1m / s, 0.2m / s, 0.3m / s, 0.4m / s, 0.5m / s, 0.6m / s, 0.7m / s, 0.8m / s, 0.9m / s, 0.1m / s, 1.1m / s, 1.2m / s, 1.3m / s, 1.4m / s, 1.5m / s, 1.6m / s, 1.7m / s, 1.8m / s, 1.9m / s or 2.0m / s. It can be understood that the feeding speed of the finished film 4 is merely an example and is not specifically limited here.

[0119] The electrode membrane processing method also includes a deflection correction process and a trimming process, wherein the trimming process is located before the storage process, and the trimming process is used to cut the width of the finished membrane 4 to a preset width so that the storage process can store and place the finished membrane 4 of the preset width. The deflection correction process is located before the trimming process, and the deflection correction process is used to align the finished membrane 4 with the cutting tool. By providing the trimming process before the storage process to cut the width of the finished membrane 4 to the preset width, the product specification consistency of the stored and placed finished membrane 4 can be further ensured. By providing the deflection correction process before the trimming process to align the finished membrane 4 with the cutting tool, the cutting effect of the finished membrane 4 can be further improved, thereby improving the product specification consistency of the finished membrane 4. Example 2

[0120] As shown in FIG2A , this embodiment provides an electrode membrane processing device 1000. The electrode membrane processing method described above is applied to the electrode membrane processing device 1000. The electrode membrane processing device 1000 includes a finished product calendering module 400 and an embryo module 100. The embryo module 100 is configured to extrude fibrous powder into a calendered embryo 1, and the finished product calendering module 400 is configured to calender the calendered embryo 1 into a finished membrane 4. The embryo module 100 is positioned upstream of the finished product calendering module 400 along the processing direction of the finished membrane 4.

[0121] By applying the above-mentioned electrode diaphragm processing method to the electrode diaphragm processing equipment 1000, the initial PTFE particles in the fibrotic powder are squeezed together to form a calendered embryo 1, so that the contact area S2 of the initial PTFE particles in the calendered embryo 1 with the active material powder and the conductive agent is greater than the contact area S1 of the initial PTFE particles in the fibrotic powder with the active material powder and the conductive agent, and the initial PTFE particles squeezed together in the calendered embryo 1 are fully expanded, and the similar shearing and stretching effects generated in the process of extruding and stretching the fibrotic powder are utilized to make the calendered embryo 1 The initial pressure PTFE particles in 1 are fully fiberized, so as to ensure the full fiberization of the PTFE particles on the basis of not changing the content of each component in the fiberized powder, further increase the contact area between the PTFE particles and the active material powder and the conductive agent, improve the coating effect of the PTFE particles on the active material powder and the conductive agent in the fiberized powder, so that the fiberized PTFE particles can more fully wrap and connect the active material powder and the conductive agent in the fiberized powder, thereby achieving the effect of improving the strength and toughness of the electrode diaphragm, improving the liquid absorption of the electrode diaphragm, and ensuring the energy density and battery performance of the battery.

[0122] As shown in Figure 2B, the embryo forming module 100 includes an embryo forming mold 110, a scraping member 130 and an embryo forming roller 120. The embryo forming mold 110 has a forming groove 140, and the notch of the forming groove 140 faces the top of the embryo forming mold 110. The scraping member 130 and the embryo forming roller 120 are both arranged in the forming groove 140, and the scraping member 130 and the embryo forming roller 120 are respectively connected to the first driving member and the second driving member. The first driving member drives the scraping member 130 to move horizontally to scrape the upper end surface of the fiberized powder arranged in the forming groove 140 along the horizontal plane. The second driving member drives the embryo forming roller 120 to move horizontally to extrude the fiberized powder in the forming groove 140 to form a calendered embryo body 1.

[0123] When the fiberized powder is extruded into a calendered embryo 1, the fiberized powder that has been weighed and has a preset weight is placed into the forming groove along the notch of the forming groove, and then the first driving member is started to drive the scraping member 130 to move horizontally to scrape the upper end surface of the fiberized powder in the forming groove along the horizontal plane, and then the first driving member is closed and the second driving member is started to drive the embryo pressing roller 120 to move horizontally to extrude the fiberized powder in the forming groove into a calendered embryo 1. The structure is simple and the forming effect is good.

[0124] The embryo forming mold 110 and / or the embryo forming roller 120 are provided with a heating element, and the heating temperature range of the heating element is 0°C to 200°C. In this embodiment, the embryo forming mold 110 is provided with a heating element, which is capable of heating the fiberized powder in the forming tank, and the heating temperature of the heating element can be selected to be 100°C. In other embodiments, the heating temperature of the heating element can be adjusted within the range of 0°C to 200°C according to actual needs, and this embodiment does not specifically limit this.

[0125] In other embodiments, the heating temperature of the heating element in the finished product mold 110 and / or the embryo forming press roller 120 may be 0° C., 10° C., 20° C., 30° C., 40° C., 50° C., 60° C., 70° C., 80° C., 90° C., 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., 180° C., 190° C., or 200° C. It will be understood that the above heating temperatures are merely exemplary and are not intended to be limiting.

[0126] In addition, the diameter of the embryo pressing roller 120 ranges from 20 mm to 200 mm, and the rolling pressure of the embryo pressing roller 120 ranges from 50 N to 1000 N. In this embodiment, the diameter of the embryo pressing roller 120 can be selected to be 50 mm, and the rolling pressure of the embryo pressing roller 120 can be selected to be 500 N. In other embodiments, the diameter of the embryo pressing roller 120 can be adjusted within the range of 20 mm to 200 mm, and the rolling pressure of the embryo pressing roller 120 can be adjusted within the range of 50 N to 1000 N according to actual needs, and this embodiment does not specifically limit this.

[0127] In other embodiments, the rolling pressure of the embryo forming press roller 120 may be 50 N, 100 N, 200 N, 300 N, 400 N, 600 N, 700 N, 800 N, 900 N, 1000 N, 1100 N, 1200 N, 1300 N, 1400 N, 1500 N, 1600 N, 1700 N, 1800 N, 1900 N, or 2000 N. In other embodiments, the diameter of the embryo forming press roller 120 may also be 20 mm, 40 mm, 60 mm, 80 mm, 100 mm, 120 mm, 140 mm, 160 mm, 180 mm, or 200 mm. It will be understood that the rolling pressure and diameter of the embryo forming press roller 120 are merely exemplary and are not specifically limited herein.

[0128] The rolled body 1 is a rectangular block. The roll forming die 110 includes two mutually perpendicular fixed baffles and two mutually perpendicular movable baffles. The two mutually perpendicular fixed baffles and the two mutually perpendicular movable baffles together form a forming groove. The two mutually perpendicular movable baffles can move independently. One of the two mutually perpendicular movable baffles is used to adjust the length of the rolled body 1, and the other is used to adjust the width of the rolled body 1. When the formed length of the rolled body 1 needs to be adjusted, the movable baffle of the two movable baffles responsible for adjusting the length of the rolled body 1 can be adjusted; when the formed width of the rolled body 1 needs to be adjusted, the movable baffle of the two movable baffles responsible for adjusting the width of the rolled body 1 can be adjusted; when the length and width of the rolled body 1 need to be adjusted simultaneously, both movable baffles can be adjusted. In addition, the two movable baffles can be removed from the roll forming die 110 to facilitate the removal of the roll-formed rolled body 1 from the forming groove along the side where the movable baffles are provided.

[0129] The length of the forming groove ranges from 400 mm to 2000 mm, the width ranges from 100 mm to 200 mm, and the depth ranges from 5 mm to 20 mm. In this embodiment, the length of the forming groove can be selected to be 500 mm, the width can be selected to be 100 mm, and the depth can be selected to be 20 mm. The length of the calendered embryo 1 formed by the embryo pressing roller 120 is 500 mm, the width of the calendered embryo 1 is 100 mm, and the height of the calendered embryo 1 is 15 mm. In other embodiments, the length of the forming groove can be adjusted within the range of 400 mm to 2000 mm, the width of the forming groove can be adjusted within the range of 100 mm to 200 mm, and the depth of the forming groove can be adjusted within the range of 5 mm to 20 mm according to actual needs. This embodiment does not impose specific limitations.

[0130] In other embodiments, the length of the forming groove may be 400 mm, 500 mm, 600 mm, 700 mm, 800 mm, 900 mm, 1000 mm, 1100 mm, 1200 mm, 1300 mm, 1400 mm, 1500 mm, 1600 mm, 1700 mm, 1800 mm, 1900 mm, or 2000 mm. The width of the forming groove may be 100 mm, 110 mm, 120 mm, 130 mm, 140 mm, 150 mm, 160 mm, 170 mm, 180 mm, 190 mm, or 200 mm. The depth of the forming groove may be 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, 16 mm, 17 mm, 18 mm, 19 mm, or 20 mm. It can be understood that the length, width and depth of the above-mentioned forming groove are only exemplary descriptions, and any value in the range of 400mm to 2000mm can be taken as the length of the forming groove, any value in the range of 100mm to 200mm can be taken as the width of the forming groove, and any value in the range of 5mm to 20mm can be taken as the depth of the forming groove, and the three can be combined at will, and no specific restrictions are given here.

[0131] Optionally, the electrode membrane processing equipment 1000 further includes a calendering module, wherein the calendering module is arranged between the embryo module 100 and the finished product calendering module 400, and the calendering module can calender the calendered embryo body 1 into a pre-processed membrane.

[0132] The calendering module includes a first calendering module 200 and a second calendering module 300, wherein the first calendering module 200 is arranged between the embryo module 100 and the second calendering module 300, and the first calendering module 200 can calender the calendered embryo 1 into a first calendered membrane 2, and the PTFE particles in the first calendered membrane 2 are in the state of primary calendered PTFE particles, and the contact area between the primary calendered PTFE particles and the active material powder and the conductive agent is set to S3, and S3 is greater than S2. The second calendering module 300 is arranged between the first calendering module 200 and the finished product calendering module 400, and the second calendering module 300 can calender the first calendered membrane 2 into a second calendered membrane 3, and the PTFE particles in the second calendered membrane 3 are in the state of secondary calendered PTFE particles, and the contact area between the secondary calendered PTFE particles and the active material powder and the conductive agent is S4, and S4 is greater than S3. The second calendered membrane 3 is a pre-processed membrane. By arranging the first calendering module 200 and the second calendering module 300 in the calendering film group, the first calendering module 200 is located upstream of the second calendering module 300, ensuring that the contact area S3 between the primary PTFE particles and the active material powder and the conductive agent in the first calendered film 2 calendered by the first calendering module 200 is greater than the contact area S2 between the primary PTFE particles and the active material powder and the conductive agent in the calendered embryo 1, and ensuring that the contact area S4 between the secondary PTFE particles and the active material powder and the conductive agent in the second calendered film 3 calendered by the second calendering module 300 is greater than the contact area S3 between the primary PTFE particles and the active material powder and the conductive agent in the first calendered film 2, thereby gradually improving the coating effect of the PTFE particles on the active material powder and the conductive agent, and thereby gradually improving the strength and toughness of the finished film 4.

[0133] In addition, the electrode membrane processing equipment 1000 also includes a storage module 500, wherein the storage module 500 is located downstream of the finished product calendering module 400 and includes a winding roller configured to wind up the finished membrane 4. By providing the storage module 500 for winding up the finished membrane 4 downstream of the finished product calendering module 400, it is possible to prevent the finished membrane 4 from accumulating downstream of the finished product calendering module 400, thereby improving the protection of the finished membrane 4.

[0134] To further improve the processing efficiency of the electrode membrane, the electrode membrane processing equipment 1000 also includes a conveying module 600, wherein the conveying module 600 sequentially connects the embryo module 100, the first calendering module 200, the second calendering module 300, the finished product calendering module 400, and the storage module 500. The conveying module 600 can transfer the calendered embryo 1 to the first calendering module 200, transfer the first calendered membrane 2 to the second calendering module 300, transfer the second calendered membrane 3 to the finished product calendering module 400, and transfer the finished membrane 4 to the storage module 500. By providing the conveying module 600, the automated circulation processing of the fiberized powder within the electrode membrane processing equipment 1000 can be achieved, thereby improving the processing efficiency of the electrode membrane.

[0135] Optionally, the electrode membrane processing equipment 1000 further includes a first cutting module 700, wherein the first cutting module 700 is arranged between the finished product calendering module 400 and the storage module 500, and the first cutting module 700 is capable of cutting the width of the finished membrane 4 into a first preset width. By arranging the first cutting module 700 between the finished product calendering module 400 and the storage module 500, the first cutting module 700 cuts the width of the finished membrane 4 calendered by the finished product calendering module 400 into the first preset width, thereby ensuring that the width of the finished membrane 4 rolled up by the storage module 500 is consistent, and ensuring the consistency of the specifications of the finished membrane 4. In this application, the transport direction of the finished membrane 4 is the length direction on the horizontal plane, and the direction on the same horizontal plane that is horizontally perpendicular to the transport direction of the finished membrane 4 is the width direction.

[0136] In this embodiment, the first cutting module 700 includes two cutters, which are respectively arranged at two ends perpendicular to the transfer direction of the conveying module 600. The distance between the two cutters is a first preset width. When the conveying module 600 drives the finished film sheet 4 to move toward the storage module 500, the conveying module 600 will drive the finished film sheet 4 through the two cutters. At this time, the two cutters will cut the two ends of the finished film sheet 4 that exceed the first preset width to ensure that the width of the finished film sheet 4 rolled up by the storage module 500 is consistent.

[0137] The electrode membrane processing equipment 1000 further includes a deflection correction module 800, wherein the deflection correction module 800 is disposed between the finished product calendering module 400 and the first cutting module 700. The deflection correction module 800 is capable of driving the finished membrane 4 to face the first cutting module 700. By disposing the deflection correction module 800 between the finished product calendering module 400 and the first cutting module 700 and utilizing the deflection correction module 800 to drive the finished membrane 4 to face the first cutting module 700, not only can the cutting effect of the finished membrane 4 by the first cutting module 700 be improved, but also the subsequent winding effect of the finished membrane 4 cut to the first preset width by the storage module 500 can be ensured.

[0138] The correction module 800 includes a detection part, a supporting part, a control part and a linear motor, wherein the finished film sheet 4 is overlapped on the supporting part, and the detection part is configured to detect the relative position of the finished film sheet 4 overlapped on the supporting part and the two cutters in the first cutting module 700. The linear motor can drive the supporting part to move along the transportation direction of the finished film sheet 4. The control part is connected to the detection part signal, and the control part can control the start and stop of the linear motor and the driving direction and driving distance of the supporting part according to the detection information of the detection part. When the detection part detects that the finished film 4 is offset to the left relative to the two cutters in the first cutting module 700, the detection part sends the detection information to the control part. The control part controls the linear motor to drive according to the detection information of the detection part and controls the linear motor to drive the supporting part to move to the right relative to the two cutters in the first cutting module 700 until the detection part detects that the finished film 4 overlapped on the supporting part is facing the two cutters in the first cutting module 700. At this time, the detection part sends the detection information to the control part. The control part controls the linear motor to stop according to the detection information to ensure that the finished film 4 is facing the cutting edges of the two cutters in the first cutting module 700.

[0139] In addition, the electrode membrane processing equipment 1000 also includes a second cutting module 900, wherein the second cutting module 900 is arranged between the second calendering module 300 and the finished product calendering module 400, and the second cutting module 900 can cut the width of the second calendered membrane 3 into a second preset width. Since the calendered blank 1 undergoes significant expansion in its length and width directions after being calendered into the first calendered film 2 by the first calendering module 200 and into the second calendered film 3 by the second calendering module 300, the second calendered film 3 can be cut to a second preset width before the calendering process is performed by the finished product calendering module 400 by providing a second cutting module 900 between the second calendering module 300 and the finished product calendering module 400. This prevents the second calendered film 3 from extending in the width direction and exceeding the processing range of the finished product calendering module 400 due to force during the calendering process of the second calendered film 3 by the finished product calendering module 400, thereby ensuring normal calendering and thinning of the second calendered film 3 by the finished product calendering module 400. The specific structure of the second cutting module 900 is the same as that of the first cutting module 700 and will not be repeated here.

[0140] The width of the finished film sheet 4 after cutting is in the range of 100mm to 300mm, the width of the second calendered film sheet 3 after cutting is in the range of 100mm to 300mm, the width of the first preset width is in the range of 100mm to 300mm, and the width of the second preset width is in the range of 100mm to 300mm. In this embodiment, optionally, the first preset width is equal to the second preset width, so the width of the second calendered film sheet 3 after cutting by the second cutting module 900 is equal to the width of the finished film sheet 4 after cutting by the first cutting module 700, and the width of the uncut second calendered film sheet 3 is greater than the first preset width, thereby ensuring that the first cutting module 700 can cut the finished film sheet 4 and the second cutting module 900 can cut the second calendered film sheet 3. In this embodiment, the width of the uncut finished film sheet 4 and the second calendered film sheet 3 can both be selected to be 250mm, and the first preset width and the second preset width can both be selected to be 240mm. In other embodiments, the thickness of the finished film 4 and the second rolled film 3 can be adjusted within the range of 100 mm to 300 mm according to actual needs, and the first preset width and the second preset width can also be adjusted within the range of 100 mm to 300 mm according to actual needs. It is only necessary to ensure that the widths of the uncut finished film 4 and the second rolled film 3 are both greater than the first preset width and the second preset width. This embodiment does not make specific limitations.

[0141] In other embodiments, the width of the second calendered film 3 and the width of the finished film 4 may also be 110mm, 120mm, 130mm, 140mm, 150mm, 160mm, 170mm, 180mm, 190mm, 200mm, 210mm, 220mm, 230mm, 240mm, 260mm, 270mm, 280mm, 290mm or 300mm. The first preset width and the second preset width may also be 100mm, 110mm, 120mm, 130mm, 140mm, 150mm, 160mm, 170mm, 180mm, 190mm, 200mm, 210mm, 220mm, 230mm, 250mm, 260mm, 270mm, 280mm, 290mm or 300mm. It is sufficient to ensure that the widths of the uncut finished film sheet 4 and the second rolled film sheet 3 are both greater than the first predetermined width and the second predetermined width. It is understood that the widths of the second rolled film sheet 3, the finished film sheet 4, the first predetermined width, and the second predetermined width are merely exemplary and will not be further elaborated upon herein.

[0142] Optionally, the first calendering module 200 includes a first pressing roller 230, a limiter 220 and an auxiliary drive member 210, wherein the limiter 220 is arranged below the first pressing roller 230, and there is a gap between the first pressing roller 230 and the limiter 220, and the limiter 220 is arranged to limit the width of the first calendering film 2, and the auxiliary drive member 210 is arranged at one end of the first pressing roller 230 close to the embryo module 100, and the auxiliary drive member 210 can drive the calendered embryo body 1 to move toward the direction close to the first pressing roller 230. By arranging the first pressing roller 230 and the limiting member 220 relative to each other in the up and down directions, a gap is ensured between the first pressing roller 230 and the limiting member 220, and the gap between the first pressing roller 230 and the limiting member 220 is used to achieve the thinning of the calendered embryo 1. After the calendered embryo 1 is calendered, the thickness of the first calendered film 2 is the distance of the gap between the first pressing roller 230 and the limiting member 220. In addition, the width of the first calendered film 2 is limited by the limiting member 220, which can ensure that the extension along the width direction is limited when the calendered embryo 1 is calendered, thereby improving the calendering yield of the calendered embryo 1. In addition, since the thickness of the calendered embryo 1 is usually large, an auxiliary driving member 210 is provided to drive the calendered embryo 1 to move toward the direction close to the first pressing roller 230, thereby driving the calendered embryo 1 to abut against the gap between the first pressing roller 230 and the limiting member 220, thereby improving the rolling effect of the first pressing roller 230 and the limiting member 220 on the calendered embryo 1.

[0143] In this embodiment, the auxiliary driving member 210 is a mechanical pusher that moves the rolled blank 1 toward the gap between the first pressing roller 230 and the limiting member 220. The limiting member 220 has limiting portions extending upward along both ends of its width. The first rolled film 2 is accommodated between the two limiting portions, thereby limiting the width of the first rolled film 2.

[0144] The rolling pressure of the first pressing roller 230 ranges from 50N to 5000N, the diameter of the first pressing roller 230 ranges from 20mm to 150mm, the distance between the first pressing roller 230 and the limiting member 220, that is, the thickness H1 of the first rolled film 2 ranges from 0.5mm to 5mm, and the distance between the two limiting portions of the limiting member 220, that is, the width of the first rolled film 2 ranges from 100mm to 200mm. In this embodiment, the rolling pressure of the first pressing roller 230 can be selected to be 800N, the diameter of the first pressing roller 230 can be selected to be 50mm, the gap between the first pressing roller 230 and the limiting member 220, that is, the thickness H1 of the first rolled film 2 can be selected to be 2mm, and the distance between the two limiting portions of the limiting member 220, that is, the width of the first rolled film 2 can be selected to be 100mm. In other embodiments, the rolling pressure of the first pressing roller 230 can be adjusted within the range of 50N to 5000N according to actual needs; the diameter of the first pressing roller 230 can be adjusted within the range of 20mm to 150mm, the distance between the first pressing roller 230 and the limiter 220 can be adjusted within the range of 0.5mm to 5mm, and the distance between the two limit parts in the limiter 220 can be adjusted within the range of 100mm to 200mm. This embodiment does not make specific limitations.

[0145] In other embodiments, the diameter of the first pressing roller 230 may be 20 mm, 40 mm, 60 mm, 80 mm, 100 mm, 120 mm, 140 mm, 160 mm, 180 mm, or 200 mm. Furthermore, the pressing pressure of the first pressing roller 230 may be 50 N, 100 N, 500 N, 1000 N, 1500 N, 2000 N, 2500 N, 3000 N, 3500 N, 4000 N, 4500 N, or 5000 N. Moreover, the distance between the first pressing roller 230 and the limit member 220, that is, the thickness H1 of the first rolled film 2 can also be 0.5mm, 1.0mm, 1.5mm, 2.5mm, 3.0mm, 3.5mm, 4.0mm, 4.5mm or 5.0mm. It can be understood that the diameter and rolling pressure of the above-mentioned first pressing roller 230 and the distance between the first pressing roller 230 and the limit member 220 are only exemplary descriptions and are not specifically limited here.

[0146] The first pressing roller 230 has a heating function. When the first pressing roller 230 rolls the calendered embryo 1 into the first calendered membrane 2, the first pressing roller 230 can heat the calendered embryo 1 to ensure that the PTFE particles in the calendered embryo 1 are fully fiberized, so as to improve the rolling effect of the calendered embryo 1 while improving the structural strength of the first calendered membrane 2.

[0147] The heating range of the first pressing roller 230 is 0° C. to 200° C. In this embodiment, the heating temperature of the first pressing roller 230 can be selected to be 100° C. In other embodiments, the heating temperature of the first pressing roller 230 can also be adjusted within the range of 0° C. to 200° C. according to actual needs, and this embodiment does not specifically limit this.

[0148] In other embodiments, the heating temperature of the first pressing roller 230 may be 0° C., 10° C., 20° C., 30° C., 40° C., 50° C., 60° C., 70° C., 80° C., 90° C., 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., 180° C., 190° C., or 200° C. It will be understood that the above heating temperatures are merely exemplary and are not specifically limited herein.

[0149] In addition, the limiting member 220 may also have the same heating function as the embryo forming mold 110 to further improve the calendering effect on the calendered embryo body 1.

[0150] Optionally, the second calendering module 300 includes a thinning roller structure and a first speed detection member 310, wherein the thinning roller structure includes two second pressing rollers 320 arranged opposite to each other in the up and down directions, and there is a gap between the two second pressing rollers 320, and the first speed detection member 310 is located at one end of the second pressing roller 320 close to the first pressing roller 230. The first speed detection member 310 is configured to detect the speed at which the conveying module 600 drives the first calendered film 2 to enter the gap between the two second pressing rollers 320. The first speed detection member 310 is connected to the conveying module 600 by signal, and the conveying module 600 can control the speed at which it drives the first calendered film 2 to enter the gap between the two second pressing rollers 320 according to the detection information of the first speed detection member 310. By setting two second pressing rollers 320 arranged opposite to each other in the up and down directions and ensuring that there is a gap between the two second pressing rollers 320, the gap is used to roll and thin the first calendered film 2 to thin the first calendered film 2 into a second calendered film 3, and by setting a first speed detection component 310 to detect the speed at which the first calendered film 2 enters the gap between the two second pressing rollers 320, and the conveying module 600 controls its driving speed of the first calendered film 2 according to the detection information of the first speed detection component 310 to ensure that the second pressing roller 320 can fully calender and thin the first calendered film 2.

[0151] In other embodiments, in order to further improve the calendering forming effect of the second calendering module 300 on the first calendered film 2, multiple groups of thinning roller pressing structures can also be arranged in the second calendering module 300. The multiple groups of thinning roller pressing structures are arranged in sequence along the transmission direction of the conveying module 600, and each group of thinning roller pressing structures includes two second pressing rollers 320 arranged opposite to each other in the up and down directions.

[0152] When the first speed detector 310 detects that the speed at which the first rolled film 2 enters the gap between the two second rollers 320 exceeds a preset speed, the conveying module 600 can reduce the speed at which the first rolled film 2 enters the gap between the two second rollers 320 according to the detection information of the first speed detector 310 until the speed at which the first rolled film 2 enters the gap between the two second rollers 320 decreases to the preset speed. When the first speed detector 310 detects that the speed at which the first rolled film 2 enters the gap between the two second rollers 320 decreases to the preset speed, the conveying module 600 can increase the speed at which the first rolled film 2 enters the gap between the two second rollers 320 according to the detection information of the first speed detector 310 until the speed at which the first rolled film 2 enters the gap between the two second rollers 320 increases to the preset speed, thereby ensuring that the second rollers 320 fully thin the first rolled film 2. The preset speed range set in the first speed detector 310 is 0.1 m / s to 2 m / s. In this embodiment, the preset speed can be selected as 1 m / s. In other embodiments, the preset speed set in the first speed detection component 310 can be adjusted within the range of 0.1 m / s to 2 m / s according to actual needs, and this embodiment does not make any specific limitation.

[0153] In other embodiments, the preset speed set in the first speed detection member 310 can be 0.1m / s, 0.2m / s, 0.3m / s, 0.4m / s, 0.5m / s, 0.6m / s, 0.7m / s, 0.8m / s, 0.9m / s, 1.1m / s, 1.2m / s, 1.3m / s, 1.4m / s, 1.5m / s, 1.6m / s, 1.7m / s, 1.8m / s, 1.9m / s or 2.0m / s. It can be understood that the preset speed set in the first speed detection member 310 is only for illustrative purposes and is not specifically limited herein.

[0154] The rolling pressure of each second pressing roller 320 ranges from 50N to 30,000N, the diameter of each second pressing roller 320 ranges from 30mm to 200mm, and the gap between the two second pressing rollers 320, i.e., the thickness H2 of the second rolled film 3, ranges from 0.1mm to 1mm. In this embodiment, the rolling pressure of each second pressing roller 320 can be selected to be 10,000N, the diameter of each second pressing roller 320 can be selected to be 100mm, and the gap between the two second pressing rollers 320, i.e., the thickness H2 of the second rolled film 3, can be selected to be 0.5mm. In other embodiments, the rolling pressure of each second pressing roller 320 can be adjusted within the range of 50N to 30,000N, the diameter of each second pressing roller 320 can be adjusted within the range of 30mm to 200mm, and the gap between the two second pressing rollers 320 can be adjusted within the range of 0.1mm to 1mm according to actual needs. This embodiment does not impose any specific limitations.

[0155] In other embodiments, the diameter of each second pressing roller 320 may also be 30 mm, 40 mm, 60 mm, 80 mm, 120 mm, 140 mm, 160 mm, 180 mm or 200 mm. The rolling pressure of each second pressing roller 320 can also be 50N, 100N, 500N, 1000N, 1500N, 2000N, 2500N, 3000N, 3500N, 4000N, 4500N, 5000N, 10000N, 11000N, 12000N, 13000N, 14000N, 15000N, 16000N, 17000N, 18000N, 19000N, 20000N, 21000N, 22000N, 23000N, 24000N, 25000N, 26000N, 27000N, 28000N, 29000N or 30000N. Furthermore, the gap between the two second pressing rollers 320, i.e., the thickness H1 of the second rolled film 3, can also be 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, or 1.0 mm. It is understood that the diameter and rolling pressure of the second pressing rollers 320, as well as the distance between the two second pressing rollers 320, are merely exemplary and are not specifically limited herein.

[0156] Similarly, each second pressing roller 320 has a heating function, so that the first calendered membrane 2 is heated while the two second pressing rollers 320 are rolling the first calendered membrane 2, thereby improving the fiberization effect of the PTFE particles in the first calendered membrane 2, and further improving the coating effect of the PTFE particles in the first calendered membrane 2 on the active material powder and the conductive agent, thereby improving the structural strength of the second calendered membrane 3 processed by calendering.

[0157] The heating temperature of each second pressing roller 320 ranges from 0°C to 200°C. In this embodiment, the heating temperature of each second pressing roller 320 can be selected to be 100°C. In other embodiments, the heating temperature of each second pressing roller 320 can also be adjusted within the range of 0°C to 200°C according to actual needs, and this embodiment does not specifically limit this.

[0158] In other embodiments, the heating temperature of each second pressing roller 320 may be 0° C., 10° C., 20° C., 30° C., 40° C., 50° C., 60° C., 70° C., 80° C., 90° C., 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., 180° C., 190° C., or 200° C. It will be understood that the above heating temperatures are merely exemplary and are not specifically limited herein.

[0159] Optionally, the finished product calendering module 400 includes a finished product rolling structure and a second speed detection member 410, wherein the finished product rolling structure includes two third pressing rollers 420 arranged opposite to each other in the up and down directions, and there is a gap between the two third pressing rollers 420, and the second speed detection member 410 is located at one end of the third pressing roller 420 close to the second pressing roller 320. The second speed detection member 410 is configured to detect the speed at which the conveying module 600 drives the second calendered film 3 to enter the gap between the two third pressing rollers 420. The second speed detection member 410 is connected to the conveying module 600 signal, and the conveying module 600 can control the speed at which it drives the second calendered film 3 to enter the gap between the two third pressing rollers 420 according to the detection information of the second speed detection member 410. By setting two third pressing rollers 420 arranged opposite to each other in the up and down directions and ensuring that there is a gap between the two third pressing rollers 420, the gap is used to roll and thin the second calendered film 3 to form the second calendered film 3 into a finished film 4, and by setting a second speed detection component 410 to detect the speed at which the second calendered film 3 enters the gap between the two third pressing rollers 420, and the conveying module 600 controls its driving speed of the second calendered film 3 according to the detection information of the second speed detection component 410 to ensure that the third pressing roller 420 can fully calender and thin the second calendered film 3.

[0160] When the second speed detector 410 detects that the speed at which the second rolled film 3 enters the gap between the two third rollers 420 exceeds a preset speed, the conveying module 600 can reduce the speed at which the second rolled film 3 enters the gap between the two third rollers 420 according to the detection information of the second speed detector 410 until the speed at which the second rolled film 3 enters the gap between the two third rollers 420 decreases to the preset speed. When the second speed detector 410 detects that the speed at which the second rolled film 3 enters the gap between the two third rollers 420 decreases to the preset speed, the conveying module 600 can increase the speed at which the second rolled film 3 enters the gap between the two third rollers 420 according to the detection information of the second speed detector 410 until the speed at which the second rolled film 3 enters the gap between the two third rollers 420 increases to the preset speed, thereby ensuring that the third rollers 420 fully thin the second rolled film 3. The preset speed range set in the second speed detector 410 is 0.1 m / s to 2 m / s. In this embodiment, the preset speed can be selected as 1 m / s. In other embodiments, the preset speed set in the second speed detection component 410 can be adjusted within the range of 0.1 m / s to 2 m / s according to actual needs, and this embodiment does not make any specific limitation.

[0161] In other embodiments, the preset speed set in the second speed detection member 410 can be 0.1m / s, 0.2m / s, 0.3m / s, 0.4m / s, 0.5m / s, 0.6m / s, 0.7m / s, 0.8m / s, 0.9m / s, 1.1m / s, 1.2m / s, 1.3m / s, 1.4m / s, 1.5m / s, 1.6m / s, 1.7m / s, 1.8m / s, 1.9m / s or 2.0m / s. It can be understood that the preset speed set in the second speed detection member 410 is only for exemplary purposes and is not specifically limited herein.

[0162] The finished product calendering module 400 includes multiple sets of finished product rolling structures, each set of which includes two third pressing rollers 420 arranged in a vertically opposed relationship. These multiple sets of finished product rolling structures are sequentially arranged along the transport direction of the conveyor module 600. By providing multiple sets of finished product rolling structures along the transport direction of the conveyor module 600, the calendering effect of the second calendered film 3 by the finished product calendering module 400 can be improved. In this embodiment, the finished product calendering module 400 is provided with four sets of finished product rolling structures sequentially arranged along the transport direction of the conveyor module 600. In other embodiments, any number of finished product rolling structures may be provided according to actual needs, and this embodiment is not specifically limited thereto.

[0163] The rolling pressure of each third roller 420 ranges from 50 N to 50,000 N, the diameter of each third roller 420 ranges from 100 mm to 500 mm, and the gap between two third rollers 420 positioned vertically opposite each other, i.e., the thickness of the finished membrane 4, ranges from 50 μm to 200 μm. In this embodiment, the rolling pressure of each third roller 420 can be 25,000 N, the diameter of each third roller 420 can be 300 mm, and the gap between two third rollers 420 positioned vertically opposite each other can be 100 μm. In other embodiments, the rolling pressure of each third roller 420 can be adjusted within the range of 50 N to 50,000 N, the diameter of each third roller 420 can be adjusted within the range of 100 mm to 500 mm, and the gap between two third rollers 420 positioned vertically opposite each other can be adjusted within the range of 50 μm to 200 μm, depending on actual needs. This embodiment does not impose any specific limitations.

[0164] In other embodiments, the diameter of each third pressing roller 420 may also be 100 mm, 150 mm, 200 mm, 250 mm, 350 mm, 400 mm, 450 mm, or 500 mm. The rolling pressure of each second pressing roller 320 may also be 50 N, 100 N, 500 N, 1000 N, 1500 N, 2000 N, 2500 N, 3000 N, 3500 N, 4000 N, 4500 N, 5000 N, 10000 N, 15000 N, 20000 N, 25000 N, 30000 N, 35000 N, 40000 N, 45000 N, or 50000 N. Furthermore, the gap between the two third pressing rollers 420 disposed opposite to each other in the vertical direction, i.e., the thickness H1 of the second rolled film 3, can also be 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 12 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, or 200 μm. It will be understood that the diameter and rolling pressure of the third pressing rollers 420, as well as the distance between the two third pressing rollers 420, are merely exemplary and are not specifically limited herein.

[0165] In addition, each third pressing roller 420 has a heating function, so that the second calendered diaphragm 3 is heated while the third pressing roller 420 rolls the second calendered diaphragm 3, thereby improving the fiberization effect of the PTFE particles in the second calendered diaphragm 3, and further improving the coating effect of the PTFE particles in the second calendered diaphragm 3 on the active material powder and the conductive agent, thereby improving the structural strength of the finished diaphragm 4 after calendering and thinning.

[0166] The heating temperature of each third pressing roller 420 ranges from 0° C. to 200° C. In this embodiment, the heating temperature of each third pressing roller 420 can be selected to be 100° C. In other embodiments, the heating temperature of each third pressing roller 420 can also be adjusted within the range of 0° C. to 200° C. according to actual needs, and this embodiment does not specifically limit this.

[0167] In other embodiments, the heating temperature of each third pressing roller 420 may be 0° C., 10° C., 20° C., 30° C., 40° C., 50° C., 60° C., 70° C., 80° C., 90° C., 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., 180° C., 190° C., or 200° C. It will be understood that the above heating temperatures are merely exemplary and are not specifically limited herein.

[0168] Optionally, the storage module 500 includes a winding roller and a rotary motor, wherein the free end of the finished film sheet 4 cut into the first preset width by the first cutting module 700 is fixed to the winding roller, and the winding roller is connected to the output end of the rotary motor. The rotary motor drives the winding roller to rotate along its central axis, thereby winding the finished film sheet 4 cut into the first preset width onto the winding roller. The structure is simple and the winding effect is good. The speed at which the rotary motor drives the winding roller to rotate needs to be compatible with the transportation speed of the finished film sheet 4 cut into the first preset width by the conveying module 600, so as to avoid the problem of the finished film sheet 4 piling up due to the winding roller winding speed being too slow, or the finished film sheet 4 being pulled apart by the winding roller due to the winding speed being too fast, thereby improving the winding effect of the finished film sheet 4.

[0169] The conveying module 600 includes but is not limited to guide rollers and conveyor belts. It only needs to be able to realize the transfer function, and the specific structure of the conveying module 600 is not specifically limited.

Claims

1. A method for processing an electrode membrane, comprising: Providing a fibrous powder, wherein the fibrous powder contains initial polytetrafluoroethylene (PTFE) particles, active material powder and a conductive agent, wherein the contact area between the initial PTFE particles, the active material powder and the conductive agent is set to S1; The fibrous powder is placed in an embryo forming module (100) and extruded to form a calendered embryo (1), wherein the PTFE particles in the calendered embryo (1) are in the form of initially compressed PTFE particles, and the contact area between the initially compressed PTFE particles and the active material powder and the conductive agent is set to S2, wherein S2 is greater than S1; The calendered embryonic body (1) is calendered to form a finished membrane sheet (4).

2. The electrode membrane processing method according to claim 1, wherein: The process of providing fibrous powder, placing the fibrous powder in an embryo forming module (100), and extruding the fibrous powder into a calendered embryo body (1) comprises: The initial PTFE particles, the active material powder and the conductive agent are mixed according to a preset ratio to form the fibrous powder; and the fibrous powder is placed in the embryo forming module (100); Scraping the upper end surface of the fiberized powder in the embryo forming module (100) flat; The fibrous powder in the flattened embryo forming module (100) is extruded and molded, and the fibrous powder is heated while being extruded and molded, so as to form the calendered embryo body (1).

3. The electrode membrane processing method according to claim 1, before placing the fiberized powder in the embryo forming module (100), further comprising: Weighing the fibrous powder to obtain a preset weight of the fibrous powder; The step of placing the fibrosis powder in the embryo forming module (100) comprises: placing the fibrosis powder of a preset weight in the embryo forming module (100).

4. The electrode membrane processing method according to claim 1, further comprising: During the process of extruding the fibrous powder into the calendered embryo (1), the fibrous powder is added to the embryo forming module (100) so that the weight of the extruded calendered embryo (1) is a preset weight.

5. The electrode membrane processing method according to claim 1, wherein: In the process of extruding the fibrous powder into the calendered embryo (1), the pressure range of calendering embryo is 50N to 2000N, and the heating temperature range is 0°C to 200°C.

6. The electrode membrane processing method according to claim 1, further comprising a pre-film forming step after extrusion forming the calendered embryo body (1); The pre-film forming process comprises: The calendered embryo body (1) is calendered into a pre-processed film sheet through a pre-filming mold; Wherein, calendering the calendered embryo (1) into a finished film (4) comprises: calendering the pre-processed film into the finished film (4).

7. The electrode membrane processing method according to claim 6, wherein: The pre-film forming process includes: a first thinning process and a second thinning process; The first thinning step comprises thinning the calendered embryo (1) to a first calendered film (2) with a thickness of H1; The second thinning step comprises thinning the first calendered film (2) by calendering to obtain a second calendered film (3) with a thickness of H2.

8. The electrode membrane processing method according to claim 7, wherein: In the second thinning step, the feeding speed of the first calendered film (2) is in the range of 0.1 m / s to 2 m / s.

9. The electrode membrane processing method according to claim 1, further comprising: A storage process, the storage process comprising: storing and placing the finished film (4).

10. The electrode membrane processing method according to claim 9, further comprising: Deviation correction process and edge trimming process; The trimming process is located before the storage process, and the trimming process includes cutting the width of the finished film sheet (4) into a preset width, so that the storage process can store and place the finished film sheet (4) of the preset width; The deflection correction process is located before the edge trimming process, and the deflection correction process includes aligning the finished film (4) with the cutting tool used in the edge trimming process.

11. The electrode membrane processing method according to claim 9, wherein: In the storage process, the feeding speed of the finished film (4) is in the range of 0.1 m / s to 2 m / s.

12. An electrode membrane processing device, comprising: Embryo forming module (100) and finished product calendering module (400); The embryo forming module (100) is configured to extrude the provided fibrous powder into a calendered embryo body (1), wherein the fibrous powder contains initial polytetrafluoroethylene (PTFE) particles, active substance powder and a conductive agent, the contact area between the initial PTFE particles and the active substance powder and the conductive agent is set to S1, the PTFE particles in the calendered embryo body (1) are in the state of initially compressed PTFE particles, the contact area between the initially compressed PTFE particles and the active substance powder and the conductive agent is set to S2, and S2 is greater than S1; The finished product calendering module (400) is configured to calender the calendered embryo (1) into a finished product membrane (4).

13. The electrode film processing equipment according to claim 12, wherein: The embryo forming module (100) comprises an embryo forming mold (110), a flattening member (130) and an embryo forming roller (120), wherein the embryo forming mold (110) has a forming groove (140), the notch of the forming groove (140) faces the top of the embryo forming mold (110), the flattening member (130) and the embryo forming roller (120) are both arranged in the forming groove (140), and the flattening member (130) and the embryo forming roller (120) are respectively connected to a first driving member and a second driving member in a transmission manner, wherein the first driving member is arranged to drive the flattening member (130) to move horizontally so as to flatten the upper end surface of the fibrous powder arranged in the forming groove (140) along a horizontal plane, and the second driving member is arranged to drive the embryo forming roller (120) to move horizontally so as to extrude the fibrous powder in the forming groove (140) to form the calendered embryo body (1).

14. The electrode film processing equipment according to claim 13, wherein: A heating element is provided on at least one of the embryo forming mold (110) and the embryo forming pressing roller (120).

15. The electrode film processing equipment according to claim 12, further comprising: A calendering module is arranged between the embryo forming module (100) and the finished product calendering module (400), and the calendering module is arranged to calender the calendered embryo body (1) into a pre-processed membrane sheet.

16. The electrode film processing equipment according to claim 15, wherein: The calendering module comprises: a first calendering module (200) and a second calendering module (300); The first calendering module (200) is arranged between the embryo forming module (100) and the second calendering module (300), and the first calendering module (200) is arranged to calender the calendered embryo body (1) into a first calendered film (2), the PTFE particles in the first calendered film (2) are in the state of initially calendered PTFE particles, and the contact area between the initially calendered PTFE particles and the active material powder and the conductive agent is set to S3, and S3 is greater than S2; The second calendering module (300) is arranged between the first calendering module (200) and the finished product calendering module (400), and the second calendering module (300) is configured to calender the first calendered membrane (2) into a second calendered membrane (3). The PTFE particles in the second calendered membrane (3) are in a state of double-extended PTFE particles. The contact area between the double-extended PTFE particles and the active material powder and the conductive agent is S4, and the S4 is greater than the S3. The second calendered membrane (3) is the pre-processed membrane.

17. The electrode film processing equipment according to claim 16, further comprising: A storage module (500), the storage module (500) is located downstream of the finished product calendering module (400), the storage module (500) comprises a winding roller, and the winding roller is configured to wind up the finished film (4).

18. The electrode film processing equipment according to claim 17, further comprising: A conveying module (600), wherein the conveying module (600) sequentially connects the embryo module (100), the first calendering module (200), the second calendering module (300), the finished product calendering module (400) and the storage module (500), and the conveying module (600) is configured to transfer the calendered embryo (1) to the first calendering module (200), transfer the first calendered film (2) to the second calendering module (300), transfer the second calendered film (3) to the finished product calendering module (400), and transfer the finished product film (4) to the storage module (500).

19. The electrode film processing equipment according to claim 16, wherein: The first calendering module (200) comprises: A first pressing roller (230); a limiter (220) disposed below the first pressing roller (230), wherein a gap exists between the first pressing roller (230) and the limiter (220), and wherein the limiter (220) is configured to limit the width of the first calendered film (2); A driving member (210) is arranged at one end of the first pressing roller (230) close to the embryo forming module (100), and the driving member (210) is configured to drive the calendered embryo body (1) to move in a direction close to the first pressing roller (230).

20. The electrode film processing equipment according to claim 18, wherein: The second calendering module (300) comprises: A thinning roller pressing structure, the thinning roller pressing structure comprising two second pressing rollers (320) arranged opposite to each other in an up-and-down direction, with a gap between the two second pressing rollers (320); a first speed detection member (310), the first speed detection member (310) being located at one end of the second pressing roller (320) close to the first calendering module (200), the first speed detection member (310) being configured to detect a speed at which the conveying module (600) drives the first calendered film (2) to enter a gap between the two second pressing rollers (320), the first speed detection member (310) being connected to the conveying module (600) by signal; The conveying module (600) is further configured to control the speed at which it drives the first calendered film (2) to enter the gap between the two second pressing rollers (320) according to the detection information of the first speed detection member (310).

21. The electrode film processing equipment according to claim 18, wherein: The finished product calendering module (400) comprises: A finished product rolling structure, the finished product rolling structure comprising two third pressing rollers (420) arranged opposite to each other in an up-and-down direction, with a gap between the two third pressing rollers (420); a second speed detection member (410), the second speed detection member (410) being located at one end of the third pressing roller (420) close to the second calendering module (300), the second speed detection member (410) being configured to detect a speed at which the conveying module (600) drives the second calendered film (3) to enter a gap between the two third pressing rollers (420), the second speed detection member (410) being connected to the conveying module (600) by signal; The conveying module (600) is further configured to control the speed at which it drives the second calendered film (3) to enter the gap between the two third pressing rollers (420) according to the detection information of the second speed detection member (410).

22. The electrode film processing equipment according to claim 12, further comprising: A first cutting module (700), the first cutting module (700) being arranged between the finished product calendering module (400) and the storage module (500), the first cutting module (700) being arranged to cut the width of the finished product film (4) into a first preset width.

23. The electrode film processing equipment according to claim 22, further comprising: A deviation correction module (800), the deviation correction module (800) being arranged between the finished product calendering module (400) and the first cutting module (700), the deviation correction module (800) being arranged to drive the finished product film (4) to face the first cutting module (700).

Citation Information

Patent Citations

  • Dry-method electrode preparation method and battery production line

    CN114122309A

  • Electrode film forming method and device and pole piece manufacturing method and device

    CN115101721A

  • Dry-method electrode plate of sodium ion battery and preparation method of dry-method electrode plate

    CN116525770A

  • Dry-method pole piece, preparation method thereof and secondary battery

    CN117199261A

  • Electrode diaphragm processing method and electrode diaphragm processing equipment

    CN117810376A

Cited By

  • Method and device for manufacturing double-sided electrode plate and double-sided electrode plate

    CN119725401A