Carbon dioxide fixation method
The method of forming and peeling a carbon dioxide film on minerals enhances carbonation efficiency and productivity, addressing the limitations of conventional methods by using specific conditions and avoiding expensive chemicals, thus providing a cost-effective carbon sequestration solution.
Patent Information
- Application Number
- PCT/JP2024/010418
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional carbon dioxide fixation methods using mineral carbonation are limited by slow reaction rates with silicate minerals and require expensive chelating agents, leading to incomplete carbonation and reduced industrial viability.
A method involving the formation and peeling of a carbon dioxide film on minerals containing calcium and/or magnesium in the presence of water, with alternating or simultaneous immobilization and peeling steps, utilizing specific conditions such as particle size, water ratio, partial pressure, and additives to enhance carbonation efficiency without expensive chemicals.
This method effectively immobilizes carbon dioxide on minerals, increasing reaction rates and productivity while reducing the risk of carbon dioxide emission, offering a cost-effective and industrially viable solution for carbon sequestration.
Smart Images

Figure JP2024010418_31102024_PF_FP_ABST
Abstract
Description
Carbon dioxide fixation method
[0001] The present invention relates to a method for immobilizing carbon dioxide, and more particularly to a method for immobilizing carbon dioxide in the atmosphere or exhaust gases, thereby enabling sequestration underground or in the sea.
[0002] In recent years, global warming has become a major issue, and there is a worldwide demand for a reduction in emissions of carbon dioxide, a greenhouse gas. To reduce carbon dioxide emissions, technology to reduce emissions itself and technology to capture and capture carbon dioxide and sequester it underground or in the sea are required. With regard to the latter, a method called mineral carbonation, which fixes carbon dioxide in minerals, has attracted attention.
[0003] Mineral carbonation is a method of artificially reacting metal elements such as calcium and magnesium in minerals with carbon dioxide to produce carbon dioxide. 3 ) and magnesium carbonate (MgCO 3 Carbonates such as ) are stable at room temperature and pressure, and are less likely to emit carbon dioxide after immobilization than geological storage. Furthermore, compared to geological storage, there are fewer geological constraints and it can be applied to low concentrations of carbon dioxide, so mineral carbonation can be said to be one of the most effective methods for furnaces and boilers with carbon dioxide concentrations of 10 to 20% and generating amounts of tens of thousands to hundreds of thousands of tons.
[0004] Minerals used in mineral carbonation include silicate minerals (CaSiO 3 , Mg 3 Si 2 O 5 (OH) 4 ), quicklime (CaO) in steelmaking slag, quicklime (CaO) in fly ash, etc. are known.
[0005] Patent Document 1 describes a method for producing carbonated slag from steelmaking slag by immersing steelmaking slag in water in a reaction tank and injecting carbon dioxide-containing gas into the water. 2By washing while blowing gas, the Ca content is converted to Ca(HCO 3 ) 2 [2] a step of dissolving the slurry obtained in the washing step as Ca(HCO 3 ) 2 Patent Document 3 describes a method for treating fly ash that also fixes carbon dioxide, comprising a step of recovering the solid content in a post-washing solution and recovering the solid content as a washing residue. Patent Document 3 describes a method for fixating carbon dioxide and a method for recovering carbon dioxide, in which an alkaline aqueous solution is formed containing a raw material containing a metal element capable of forming a carbonate mineral by combining with carbonate ions and a chelating agent in an aqueous solution formation step, the metal element is reacted with the chelating agent in the aqueous solution to separate the metal element from the raw material as metal ions in a separation step, and a method for forming a carbonate mineral by adding a compound capable of generating carbonate ions to the aqueous solution and reacting the carbonate ions generated from the compound with the metal ions in a mineral formation step.
[0006] It is known that calcium in steelmaking slag and fly ash, which contain a few percent of free lime, reacts with carbon dioxide and easily becomes carbonated. However, silicate minerals in natural ores react slower than free lime (CaO) in slag, making it unrealistic to directly apply the prior art techniques described in Patent Documents 1 and 2 to mineral carbonation. Furthermore, Patent Document 3 improves the reaction rate by using a chelating agent, but these chelating agents are generally expensive and therefore unrealistic from an economic standpoint.
[0007] Furthermore, in each of the above-mentioned conventional techniques, silicate minerals are prone to react with carbon dioxide on the particle surface to form a carbonate film or a metal oxide film (e.g., FeOOH), which can cause the reaction to stop with the calcium and magnesium inside the particles remaining unreacted, resulting in a problem of a slower reaction rate.
[0008] JP 2013-147370 A JP 2005-246225 A JP 2022-102786 A
[0009] In view of the above circumstances, an object of the present invention is to provide a method for immobilizing carbon dioxide in a mineral containing calcium and / or magnesium without using expensive chemicals.
[0010] A carbon dioxide immobilization method according to a first invention comprises a fixation step of immobilizing a coating formed by reacting carbon dioxide with a calcium and / or magnesium-containing solid in the presence of water, and a peeling step of applying an external force to the solid to which the coating is fixed, thereby peeling off the coating and restoring the carbon dioxide immobilization capacity. A carbon dioxide immobilization method according to a second invention is characterized in that the fixation step and the peeling step are alternately repeated. A carbon dioxide immobilization method according to a third invention is characterized in that the fixation step and the peeling step are simultaneously performed. A carbon dioxide immobilization method according to a fourth invention is characterized in that the solid to be immobilized comprises one or more of minerals containing calcium silicate and / or magnesium silicate obtained by mining, and slag, clinker, dust, and incineration ash generated during the smelting of the minerals. A carbon dioxide immobilization method according to a fifth invention is characterized in that the solid to be immobilized is crushed to a size of 64 μm or less and supplied to the fixation step. A sixth aspect of the present invention is a method for immobilizing carbon dioxide according to the first aspect of the present invention, characterized in that the weight ratio of the water to the solid to be treated in the immobilization step is 0.01 to 10. A seventh aspect of the present invention is a method for immobilizing carbon dioxide according to the first aspect of the present invention, characterized in that in the immobilization step, the solid to be treated and the carbon dioxide are reacted while adjusting the partial pressure of carbon dioxide to 0.1 atm to 5 atm. A eighth aspect of the present invention is a method for immobilizing carbon dioxide according to the first aspect of the present invention, characterized in that in the immobilization step, when the solid to be treated is a mineral containing calcium silicate and / or magnesium silicate obtained by mining, sodium bicarbonate and / or potassium bicarbonate are further added. A ninth aspect of the present invention is a method for immobilizing carbon dioxide according to the first aspect of the present invention, characterized in that in the immobilization step, when the solid to be treated is a mineral containing calcium silicate and / or magnesium silicate obtained by mining, one or more of sulfide, sulfur, sulfate, and sulfite are further added.A carbon dioxide fixation method of a tenth invention is the first invention, characterized in that in the fixation step, the reaction with carbon dioxide is carried out while maintaining a reaction temperature of 5°C to 90°C. A carbon dioxide fixation method of an eleventh invention is the first invention, characterized in that in the fixation step, the iron content in the solid to be treated is 25% by weight or less. A carbon dioxide fixation method of a twelfth invention is the first invention, characterized in that in the fixation step, the solid to be treated is a mineral containing calcium silicate and / or magnesium silicate obtained by mining, and further characterized in that a preheating step of heating the solid to 600°C or higher is provided prior to the fixation step.
[0011] According to the first invention, in the immobilization process, a coating is formed on the surface of the treated solid, which contains calcium and / or magnesium coexisting with water, by reacting carbon dioxide with the treated solid. The coating is then peeled off in the peeling process, separating the treated solid from the coating. This allows carbon dioxide to be immobilized in the coating without the use of expensive chemicals, making the process extremely valuable industrially. According to the second invention, the immobilization process and the peeling process are alternately repeated, allowing the coating to be sufficiently formed before peeling off, thereby increasing the productivity of the entire immobilization method. According to the third invention, the immobilization process and the peeling process are carried out simultaneously, allowing the immobilization process to be carried out even in short operations. According to the fourth invention, calcium and / or magnesium contained in the treated solid, which is a mineral obtained by mining, dissolves in water and reacts with carbon dioxide to form a coating made of carbonates, etc., thereby allowing carbon dioxide to be immobilized in the coating. Furthermore, if the coating is made of carbonate, it is stable at room temperature and atmospheric pressure, reducing the risk of carbon dioxide emissions. According to the fifth invention, the solid to be treated is crushed to 64 μm or less, thereby increasing the specific surface area of the solid, and thereby enabling the immobilization of more carbon dioxide. According to the sixth invention, the amount of water coexisting with the solid to be treated is set to a range of 0.01 to 10 by weight, in terms of the weight of water to the solid to be treated, thereby enabling the dissolution reaction to proceed sufficiently. According to the seventh invention, the partial pressure of carbon dioxide is set to a range of 0.1 atm to 5 atm, thereby enabling the reaction to proceed sufficiently quickly and requiring simple carbon dioxide introduction equipment. According to the eighth invention, the addition of sodium bicarbonate and / or potassium bicarbonate promotes the carbonation of silicates. According to the ninth invention, the addition of one or more of sulfide, sulfur, sulfate, and sulfite promotes the dissolution of calcium and / or magnesium into water by sulfate ions and / or sulfite ions. According to the tenth invention, the reaction temperature is set to a range of 5°C to 90°C, thereby enabling the reaction to proceed smoothly and eliminating the need for excessive heating. According to the eleventh aspect of the present invention, the iron content in the treated solid is 25% by weight or less, so that the carbonation of calcium and / or magnesium is less likely to be inhibited, and the fixation of carbon dioxide proceeds efficiently.According to the twelfth invention, by preheating the treated solid to 600°C or higher, the crystalline structure of the mineral can be partially rendered amorphous, allowing more calcium and / or magnesium in the treated solid to be dissolved into water.
[0012] Fig. 3 is a process diagram of a carbon dioxide fixation method according to a first embodiment of the present invention. Fig. 4 is an explanatory diagram of implementation equipment used in the process shown in Fig. 1. Fig. 5 is a process diagram of a carbon dioxide fixation method according to a second embodiment of the present invention. Fig. 6 is an explanatory diagram of implementation equipment used in the process shown in Fig. 3.
[0013] (Basic principle of the present invention) As shown in Figure 1, the carbon dioxide fixation method of the present invention comprises an immobilization step I in which carbon dioxide is reacted with a treated solid 1 containing calcium and / or magnesium in the presence of water to produce a coating 2, which is fixed to the surface of the treated solid 1, and a peeling step II in which an external force is applied to the treated solid 1 with the fixed coating 2 to peel off the coating 2 and regenerate the carbon dioxide fixation capacity. The immobilization method of the present invention includes a method in which the immobilization step I and the peeling step II are repeated alternately, and a method in which the immobilization step I and the peeling step II are performed simultaneously.
[0014] According to the carbon dioxide fixation method of the present invention, in fixation step I, a coating 2 containing carbon dioxide can be formed on the surface of a treated solid 1 containing calcium and / or magnesium coexisting with water, and in peeling step II, the coating 2 is peeled off to separate the treated solid 1 from the coating 2 containing carbon dioxide. When the coating 2 is separated, the surface of the treated solid 1 is exposed, and the carbon dioxide fixation capacity is restored.
[0015] The immobilization method of the present invention allows carbon dioxide to be immobilized in a film without using expensive chemicals. Carbonates are a typical example of the film that can be formed. Carbonates are stable at room temperature and pressure, and have the advantage of lowering the risk of releasing carbon dioxide after immobilization compared to conventional methods such as underground storage. Therefore, their industrial value is extremely high.
[0016] The solid to be treated 1 in the present invention refers to one or more of minerals containing calcium silicate and / or magnesium silicate obtained by mining, and slag, clinker, dust, and incineration ash produced in the process of smelting the minerals. These are fixatives suitable for carbon dioxide fixation.
[0017] First Embodiment Hereinafter, a fixation method of a first embodiment will be described with reference to the process diagram of Fig. 1 and the equipment explanatory diagram of Fig. 2. The fixation method of the first embodiment is a method in which a fixation step I and a peeling step II are alternately repeated.
[0018] 1 , the treated solid 1 is allowed to coexist with water, thereby dissolving the calcium and / or magnesium contained therein in the water. Then, when carbon dioxide (specifically, carbonate ions) is reacted with the calcium and / or magnesium dissolved in the water, carbonates (i.e., calcium carbonate and / or magnesium carbonate), iron oxide (FeOOH), and the like are produced.
[0019] Representative reactions for producing carbonate include the following formulas 1, 2, and 3: CaO + CO 2 → CaCO 3 ...(Formula 1) MgO + CO 2 → MgCO 3 ...(Formula 2) Mg 3 Si 2 O 5 (OH) 4 + 3CO 2 → 3MgCO 3 + 2SiO 2 +2H 2 O (Equation 3) These reactions produce carbon dioxide (CO 2 ) are these carbonates (CaCO 3 , MgCO 3 , 3MgCO 3 The produced carbonates, iron oxides, etc. are formed as a film 2 on the surface of the treated object 1.
[0020] The immobilization step I can be carried out using equipment such as that shown in Figure 2. Reference numeral 10 denotes a reaction tank, which is composed of a tank body 11 and a lid 12 and is sealable. The reaction tank 10 is configured so that the solids to be treated 1 can be supplied through a supply device 13 (for example, a chute), water can be supplied through a water conduit 14, and carbon dioxide gas can be introduced through an inlet pipe 15. When water 4 is stored in the tank body 11 of the reaction tank 10 and the solids to be treated 1 are present in the water, and carbon dioxide is also dissolved in the water, a reaction to produce carbonates and the like can be carried out.
[0021] However, the equipment used in the immobilization step I is not limited to that shown in Figure 2, and any equipment may be used as long as it is possible to cause the treated solids 1 to react with carbon dioxide in water. Although not shown, the reaction tank 10 in Figure 2 may be provided with an agitation device that agitates the treated solids 1 and water within the tank body 11, in which case carbonates are produced efficiently.
[0022] In the immobilization step I, the solid 1 to be treated is preferably pulverized to a fine particle size. This increases the specific surface area, making it possible to immobilize a larger amount of carbon dioxide. A general ball mill or vibration mill can be used for pulverization. The particle size after pulverization is preferably 64 μm or less, and more preferably 32 μm or less. The lower limit of pulverization is 1 μm, and it is preferable to set it to 1 μm or more. If the particle size is less than 1 μm, an extremely large amount of energy is required for pulverization, and the pulverization equipment must be enlarged.
[0023] The reaction tank 10 shown in Figure 2 may be provided with a stirring device as needed to stir the treated individuals 1 and the water so that all of the treated individuals 1 come into contact with the water 4. Note that the treated individuals 1 in Figure 2 are shown as spherical and the coating 2 is shown to have a uniform thickness, but in reality the treated individuals 1 are irregular in shape and the coating 2 is also non-uniform in thickness, with some coatings partially covering the treated individuals 1.
[0024] The weight ratio of water 4 to the treated solids 1 in the tank body 11 during the immobilization step I is preferably 0.01 to 10. In other words, a water content small enough to wet the surface of the treated solids 1, as well as a slurry with a high water content, are acceptable. In the immobilization step I, the lower limit of the amount of water coexisting with the treated solids 1 is a weight ratio of 0.01 or more. This amount of water allows the dissolution reaction of the treated solids 1 to occur. Adding less than 1% by weight of water may result in an insufficient reaction, and handling may be difficult due to the increased likelihood of dust generation. The upper limit of the amount of water coexisting with the treated solids 1 is adjusted so that the weight ratio of water to the treated solids 1 is 10 or less, more preferably 5 or less. Adding an excessive amount of water requires an increase in the size of the treatment equipment and is undesirable from the perspective of conserving water resources.
[0025] The carbon dioxide introduced in fixation step I is contained in the atmosphere and exhaust gases, and by using this carbon dioxide, the CO 2 This can contribute to reducing emissions. The method of introducing carbon dioxide (gas) is not particularly limited. For example, any method can be used as long as the object 1 to be treated is placed in a sealed container together with water and carbon dioxide is introduced therein. The reaction tank 10 in Figure 2 uses an introduction pipe 15, but this is just one example.
[0026] When carbon dioxide is introduced into the reaction vessel 10, the introduction pressure is preferably adjusted so that the carbon dioxide partial pressure is 0.1 atm to 5 atm. Within this pressure range, simple introduction equipment is sufficient. If the carbon dioxide partial pressure is lower than 0.1 atm, the reaction tends to be slow, and if it is higher than 5 atm, the introduction equipment tends to be expensive.
[0027] In the immobilization step I, when the treated solid 1 is a mineral containing calcium silicate and / or magnesium silicate, sodium bicarbonate and / or potassium bicarbonate can be further added. This can promote the carbonation of silicate. That is, potassium bicarbonate can carbonate magnesium silicate by the reaction shown in the following formula 4. Mg 3 Si 2 O5 (OH) 4 + 6KHCO 3 → 3MgCO 3 + 2SiO 2 +5H 2 O+3K 2 CO 3 ...(Formula 4)
[0028] When magnesium silicate is carbonated, potassium carbonate is produced, but the produced potassium carbonate is regenerated as potassium bicarbonate by the reaction shown in the following formula 5, so after a predetermined amount of potassium bicarbonate has been added, there is no need to add new potassium bicarbonate. 2 CO 3 +CO 2 +H 2 O → 2KHCO 3 (CO 2 (playback) ... (Equation 5)
[0029] In the immobilization step I, if the treated solid 1 is a mineral containing calcium silicate and / or magnesium silicate, one or more of sulfide, sulfur, sulfate, and sulfite can be further added. This can promote the elution of calcium and / or magnesium into water by the sulfate ions and / or sulfite ions generated. Note that a gas containing sulfur oxide (SOx) may be introduced instead of sulfide, sulfur, sulfate, and sulfite.
[0030] In the immobilization step I, the reaction between calcium and / or magnesium and carbon dioxide proceeds more efficiently at higher temperatures. For example, the reaction can be carried out in a temperature range of 5°C to 90°C. In particular, the reaction is preferably carried out in a temperature range of 20°C or higher, and more preferably in a temperature range of 50°C or higher. In this case, the reaction proceeds smoothly and the amount of heat required is not excessive. However, temperatures above 90°C tend to be uneconomical because more heat is required.
[0031] The iron content in the treated solid 1 is preferably 25% by weight or less, and more preferably 10% by weight or less. In other words, a lower iron content in the treated solid 1 is advantageous because it allows for more efficient fixation of carbon dioxide. The reason for this is that, in the presence of water, the iron in the treated solid 1 dissolves into the water and deposits as hydroxide on the particle surface of the treated solid 1, forming a coating of iron hydroxide that tends to inhibit the carbonation of calcium and / or magnesium.
[0032] (Peeling Step II) As shown in Fig. 1, in peeling step II, an external force F is applied to the coating 2 made of carbonate or the like obtained in the immobilization step I, to peel off the coating 2. As shown in Fig. 2, the applied external force F need only be such that it can crack or peel off the coating 2. Therefore, it is not necessary to apply a large external force F that would destroy the particles of the individual 1 to be treated, and the peeling step can be carried out by applying a relatively small external force.
[0033] The application of the external force can be carried out using, for example, a device such as a homogenizer (atomizer), an agitator (mixer), or a wet scrubber (wet dust collector), or it can also be carried out by lightly mixing using a pestle and mortar. Therefore, the device is not limited to the various devices exemplified above, and an ultrasonic vibration device that applies a smaller external force F may also be used. Furthermore, the peeling treatment may be carried out by applying an external force using thermal stress.
[0034] Although the treated individual 1 and the coating 2 separated in the peeling step II are separated, they remain mixed in the reaction tank 10. Therefore, the immobilization step I and the peeling step II may be repeated several times (for example, three times), after which the treated individual 1 and the coating 2 may be recovered together.
[0035] If the coating 2 obtained as described above is a carbonate, it is stable at room temperature and pressure, and therefore, if the solid is sequestrated underground or in the sea after immobilization, it has the advantage of lowering the risk of carbon dioxide emissions compared to conventional methods such as underground sequestration. Furthermore, a new surface of the treated solid 1 from which carbon dioxide has been separated will be exposed, as shown in Figure 2. Therefore, even if the carbon dioxide immobilization reaches saturation, the immobilization capacity can be easily regenerated, and the treated solid 1 can be supplied again to the immobilization step I, as shown in Figure 1.
[0036] In the first embodiment described above, the immobilization step I and the peeling step II are separated and alternately repeated, so that the coating 2 is sufficiently formed before the process moves on to peeling off the coating 2, thereby increasing the productivity of the entire immobilization method.
[0037] Second Embodiment An immobilization method of a second embodiment will be described with reference to the process diagram of Fig. 3 and the equipment explanatory diagram of Fig. 4. The immobilization method of the second embodiment is a method in which the immobilization step I and the peeling step II are carried out simultaneously.
[0038] In the immobilization method of the second embodiment, the immobilization step I and the peeling step II are carried out simultaneously, as shown in Fig. 3. To carry out this second embodiment, a stirring device 20 is provided in a reaction vessel 10, and an external force F is applied to peel off the coating 2 while the coating 2 made of carbonate or the like is being formed, as shown in Fig. 4.
[0039] There are no particular limitations on the structure or function of the agitator 20 used, and an example is one in which the agitator blades 21 are rotated by a motor or the like 22. Agitation causes the treated individuals 1 to collide with each other in the water, or the treated individuals 1 to collide with the agitator blades 21, applying an external force F and causing the coating 2 to peel off from the treated individuals 1. By simultaneously producing and peeling off the coating 2 made of carbonate or the like in this way, the coating 2 is produced while exposing a new surface on the surface of the treated individuals 1, and carbon dioxide can be fixed in this coating 2, allowing for efficient carbon dioxide fixation. Furthermore, the carbon dioxide fixation ability of the treated individuals 1 can be regenerated.
[0040] In the second embodiment, the immobilization step I and the peeling step II are carried out simultaneously, so that the immobilization process can be carried out in a short period of time. Furthermore, the regenerated solids 1 can be supplied to the immobilization step I again, as shown in FIG.
[0041] (Other Embodiments) In the carbon dioxide fixation method of the present invention, a preheating step may be provided prior to fixation step I. When the treated solid 1 is a mineral containing calcium silicate and / or magnesium silicate, providing such a preheating step can partially amorphize the crystalline structure of these minerals. This allows a larger amount of calcium and / or magnesium in the treated solid 1 to be eluted into water. Specifically, heating to 600°C or higher is preferable, which allows for good elution. This activates the reaction in fixation step I, enabling efficient fixation of carbon dioxide.
[0042] Example 1: The immobilization method shown in Figure 1 was tested as follows. (Immobilization Step I) Waste ore composed primarily of lizardite and containing 23% Fe, 13% Si, and 14% Mg was used as the treated solid 1. The entire waste ore was crushed to 64 μm or less using a pestle and mortar. 15 mL of pure water was added to 3 g of crushed waste ore to prepare a slurry. The prepared slurry was filled into a sample container (a jar-type sample container made of fluororesin (trade name "Teflon (registered trademark)")), stirred while supplying carbon dioxide so that the pressure inside the sealed container was 5 atm, and held for one week. The sample container was left at room temperature without heating for the test. The slurry removed from the sample container was subjected to solid-liquid separation, and the solid side was dried. The amount of carbon dioxide absorbed (weight) was calculated by total carbon measurement. The calculated amount of carbon dioxide absorbed was 0.85 wt% of the waste ore.
[0043] (Peeling Step II) Subsequently, the dried sample was lightly stirred in a mortar to perform a peeling treatment. Then, 1.5 g of the sample was taken out and 7.5 mL of water was added to prepare a slurry again. The prepared slurry was filled into a sample container in the same manner as the first time, and stirred while supplying carbon dioxide so that the pressure inside the sealed container was 5 atm, and the mixture was kept for one week.
[0044] According to the results of this experiment, the amount of carbon dioxide absorbed (weight) was 1.68% by weight relative to the mineral, and it was confirmed that the amount of carbon dioxide absorbed had increased even two weeks after the start of the test.
[0045] Comparative Example 1 Except for not carrying out the peeling treatment II, the same procedure as in Example 1 was carried out. According to the experimental results, the amount of carbon dioxide absorbed by the mineral after 4 weeks from the start of the test was 0.8% by weight, and no increase in the amount of carbon dioxide absorbed was observed.
[0046] (Summary) As described above, it has been confirmed that by carrying out the carbon dioxide fixation method of the present invention, carbon dioxide can be absorbed into a coating formed on the surface of a mineral containing calcium and / or magnesium without adding expensive chemicals.
[0047] According to the present invention, carbon dioxide can be fixed in a film made of carbonate or the like, and then isolated underground or in the sea, thereby reducing carbon dioxide in the atmosphere.
[0048] REFERENCE SIGNS LIST 1 object to be treated 2 coating 4 water 10 reaction tank 11 tank body 20 stirring device 21 stirring blade
Claims
1. A method for fixating carbon dioxide, comprising: a fixation step of reacting a calcium and / or magnesium-containing solid body with carbon dioxide in the presence of water to produce a coating on the solid body; and a peeling step of applying an external force to the solid body with the coating fixed thereto to peel off the coating and regenerate the carbon dioxide fixation ability.
2. The method for fixation of carbon dioxide according to claim 1, characterized in that the fixation step and the peeling step are repeated alternately.
3. The method for fixation of carbon dioxide according to claim 1, characterized in that the fixation step and the peeling step are carried out simultaneously.
4. The method for fixation of carbon dioxide as described in claim 1, characterized in that the solid to be treated is one or more of minerals containing calcium silicate and / or magnesium silicate obtained by mining, and slag, clinker, dust, and incineration ash generated in the process of smelting the minerals.
5. The method for fixation of carbon dioxide according to claim 1, characterized in that the solid to be treated is pulverized to 64 μm or less and supplied to the fixation step.
6. The method for fixation of carbon dioxide according to claim 1, characterized in that the weight ratio of the water to the solid to be treated in the fixation step is 0.01 to 10.
7. A method for immobilizing carbon dioxide according to claim 1, characterized in that in the immobilization step, the solid to be treated is reacted with the carbon dioxide while adjusting the partial pressure of the carbon dioxide to 0.1 atm to 5 atm.
8. A method for fixing carbon dioxide as described in claim 1, characterized in that in the fixation step, when the treated solid is a mineral containing calcium silicate and / or magnesium silicate obtained by mining, sodium hydrogen carbonate and / or potassium hydrogen carbonate is further added.
9. A method for fixing carbon dioxide as described in claim 1, characterized in that in the fixation step, when the treated solid is a mineral containing calcium silicate and / or magnesium silicate obtained by mining, one or more of sulfide, sulfur, sulfate, and sulfite are further added.
10. The method for fixation of carbon dioxide according to claim 1, characterized in that in the fixation step, the reaction with carbon dioxide is carried out while maintaining a reaction temperature of 5°C to 90°C.
11. The method for fixation of carbon dioxide according to claim 1, characterized in that the iron content in the solid to be treated in the fixation step is 25% by weight or less.
12. A method for fixation of carbon dioxide as described in claim 1, characterized in that in the fixation process, the treated solid is a mineral containing calcium silicate and / or magnesium silicate obtained by mining, and a preheating process is provided prior to the fixation process in which the treated solid is heated to 600°C or higher.
Citation Information
Patent Citations
Treating method for fly ash combined with fixation of carbon dioxide
JP2005246225A
Method for manufacturing carbonated slag
JP2013147370A
Carbon dioxide fixing method, recovery method of carbon dioxide, carbon dioxide fixation apparatus, and environment-oriented industrial apparatus
JP2022102786A
Integrated Chemical Method
JP2010510161A
Improved integrated chemical method
JP2012500718A