Reflection adjustment film, optical member, and lens unit
The reflection adjustment film with a multilayer structure addresses light reflection issues in hydrophilic lenses by suppressing reflectance and maintaining hydrophilicity, enhancing visibility and durability for outdoor optical components.
Patent Information
- Application Number
- PCT/JP2024/015033
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-31
AI Technical Summary
Hydrophilic lenses with photocatalytic silicate materials struggle with light reflection, leading to reduced visibility due to adherence of organic stains and water droplets, which affects the performance of optical components used outdoors.
A reflection adjustment film with a multilayer structure of low and high refractive index layers, placed between a hydrophilic layer and a light-transmitting member, suppresses light reflection and maintains hydrophilicity, enhancing visibility by reducing ghost and flare phenomena.
The solution effectively reduces light reflectance to 3% or less, minimizing image defects and maintaining hydrophilicity through photocatalytic restoration, while ensuring sufficient transmittance and durability.
Smart Images

Figure JP2024015033_31102024_PF_FP_ABST
Abstract
Description
Reflection adjustment film, optical component and lens unit
[0001] The present disclosure relates to a reflection control film, an optical member, and a lens unit.
[0002] Visibility is impaired by water droplets on window glass of buildings or automobiles exposed to outdoor wind and rain. One solution to this problem is to make the surface of the window glass hydrophilic. This turns the adhering water into a film, preventing the adhesion of water droplets and ensuring visibility on the window glass.
[0003] However, the surface of hydrophilic materials is prone to the adhesion of organic contaminants, such as those from automobile exhaust fumes or factory smoke. When organic contaminants adhere to the surface, water droplets adhere to the surface, significantly reducing visibility.
[0004] Therefore, a hydrophilic lens including a glass substrate and a hydrophilic layer formed on the glass substrate has been disclosed (for example, Patent Document 1). In the hydrophilic lens of Patent Document 1, the hydrophilic layer contains a silicate material in which fine particles having photocatalytic activity are dispersed, the film thickness of the hydrophilic layer is 30 nm or less, the average particle diameter of the fine particles is 30 nm or less, and the arithmetic mean roughness Ra of the surface of the hydrophilic layer is 0.7 to 1.9 nm.
[0005] Japanese Patent Publication No. 2018-77260
[0006] However, in the hydrophilic lens of Patent Document 1, a portion of incident light is reflected without being transmitted by optical members such as the hydrophilic layer and the glass substrate.
[0007] The present disclosure has been made in consideration of the above-mentioned problems, and its purpose is to provide a reflection adjustment film, an optical element, and a lens unit that can suppress reflection of incident light by a hydrophilic layer and an optical element.
[0008] An exemplary reflection adjustment film according to the present disclosure is used in an optical element having a hydrophilic layer containing a plurality of photocatalytic particles. The reflection adjustment film is disposed below the hydrophilic layer. The thickness of the reflection adjustment film is at least five times the thickness of the hydrophilic layer.
[0009] An exemplary optical member according to the present disclosure includes the reflection adjustment film, the translucent member, and the hydrophilic layer. The translucent member transmits light having a wavelength of 400 nm or more and 700 nm or less. The reflection adjustment film is disposed between the hydrophilic layer and the translucent member.
[0010] An exemplary lens unit according to the present disclosure includes the optical element described above and an optical lens that transmits light having a wavelength of 400 nm or more and 700 nm or less, and the optical element is disposed on the opposite side of the optical lens in the traveling direction of the light.
[0011] According to the exemplary embodiment of the present disclosure, for example, the hydrophilic layer and the optical member can suppress reflection of incident light.
[0012] Fig. 1 is a schematic diagram showing an example of an optical unit according to the present embodiment. Fig. 2 is a schematic diagram showing an example of an optical member according to the present embodiment. Fig. 3 shows measurement results of the optical member according to Example 1 and the optical member according to Comparative Example 1. Fig. 4 shows measurement results of the optical member according to Example 1, the optical member according to Example 5, and the optical member according to Comparative Example 4.
[0013] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference numerals, and the description will not be repeated. The dimensions, shapes, and dimensional relationships between components in the drawings are not necessarily the same as the actual dimensions, shapes, and dimensional relationships between components. In particular, the thickness ratios and curvatures of the reflection adjustment film, hydrophilic layer, and translucent member in the drawings may differ significantly from the actual products.
[0014] In this specification, "thickness" refers to the length of an optical member in the optical axis direction. The "outside" of an optical member refers to the direction from the light-transmitting member toward the hydrophilic layer. The "inside" of an optical member refers to the direction from the hydrophilic layer toward the light-transmitting member.
[0015] The optical member according to this embodiment is suitable, for example, as an optical member used in an optical unit including one or more optical members (particularly an optical unit used outdoors). The optical member according to this embodiment is particularly suitable as a lens for a lens unit of an in-vehicle camera for monitoring the surroundings of a vehicle. FIG. 1 is a schematic diagram showing an example of an optical unit according to this embodiment. As shown in FIG. 1, an optical unit 1000 includes an optical member 100. The optical unit is an example of a "lens unit."
[0016] The optical element according to this embodiment may be used in an optical unit (particularly an optical unit for use outdoors) including the optical element 100 and an optical lens. The optical lens transmits light with a wavelength of 400 nm or more and 700 nm or less. The optical element 100 is disposed on the opposite side of the optical lens in the light traveling direction.
[0017] The static contact angle of the surface of the optical element 100 with pure water is preferably 30.0° or less, more preferably 20.0° or less, and particularly preferably 10.0° or less. Hereinafter, the static contact angle with pure water may be simply referred to as the "contact angle." Note that the contact angle of the surface of the optical element according to this embodiment is a value measured in an environment at a temperature of 23°C ± 3°C and a relative humidity of 50% ± 3%.
[0018] Furthermore, the reflectance for light with a wavelength of 400 nm or more and 700 nm or less is 3% or less. The maximum reflectance of the optical element 100 for light with a wavelength of 400 nm or more and 700 nm or less is preferably 1.5% or less, and more preferably 1.0% or less. The optical element 100 according to this embodiment can suppress the occurrence of image defects known as ghost phenomena and flare phenomena as the maximum reflectance described above decreases. In particular, the lower the maximum reflectance described above, the more effectively the occurrence of ghost phenomena can be suppressed. When the maximum reflectance described above is 3.0% or less, the occurrence of ghost phenomena can be suppressed. When the maximum reflectance described above is 1.0% or less, the occurrence of ghost phenomena can be more effectively suppressed. Note that light with a wavelength of 400 nm or more and 700 nm or less corresponds to light in the visible light region.
[0019] An example of the optical member 100 according to this embodiment will be described below with reference to Fig. 2. Fig. 2 is a schematic diagram showing an example of the optical member 100 according to this embodiment. The optical member 100 includes a light-transmitting member 10, a hydrophilic layer 20, and a reflection adjustment film 30.
[0020] <Light-Transmitting Member> The light-transmitting member 10 has light-transmitting properties. That is, the light-transmitting member 10 transmits visible light. The light-transmitting member 10 may be transparent or translucent. The light-transmitting member 10 contains, for example, glass or synthetic resin as a main component.
[0021] The light-transmitting member 10 functions as, for example, a lens (specifically, for example, a biconvex lens, a biconcave lens, a plano-convex lens, a plano-concave lens, a convex meniscus lens, or a concave meniscus lens). In this specification, when the light-transmitting member 10 is a lens, the lens surface of the light-transmitting member 10 may be spherical or aspherical. The radius of curvature of the lens surface of the light-transmitting member 10 is preferably 9 mm or more and 16 mm or less.
[0022] <Hydrophilic Layer> The hydrophilic layer 20 covers the light-transmitting member 10. Specifically, the hydrophilic layer 20 is disposed on the reflection adjustment film 30. The hydrophilic layer 20 has hydrophilic properties.
[0023] The thickness of the hydrophilic layer 20 is preferably 20 nm to 200 nm, more preferably 30 nm to 100 nm. If the thickness of the hydrophilic layer 20 is less than 20 nm, the hydrophilicity recovery function tends to be insufficient. If the thickness of the hydrophilic layer 20 is more than 200 nm, the transmittance to visible light tends to be insufficient.
[0024] In the present specification, "thickness" may be determined using a stylus-type step gauge. Specifically, a sharp needle is traced across the surface to measure the step between areas with and without a layer (film). Steps are measured at three arbitrary locations, and the average value of the step differences at the three locations is taken as the "thickness."
[0025] The hydrophilic layer 20 contains a plurality of photocatalytic particles. The photocatalytic particles have a photocatalytic function. For example, when the optical element 100 is used for a long period of time, dirt adheres to the optical element 100, reducing the hydrophilic function. When the optical element 100 is irradiated with ultraviolet light (sunlight), the dirt is decomposed and the hydrophilic function can be restored. The optical element 100 according to this embodiment exhibits a high hydrophilicity when exposed to ultraviolet light at a dose of 1 mW / cm when the contact angle exceeds 30.0°. 2 It is preferable that the contact angle be 30.0° or less when the hydrophilic layer 20 is irradiated with light at 1000 W for 6 hours. Examples of photocatalyst particles include particles of titanium oxide, strontium titanate, zinc oxide, silicon carbide, gallium phosphate, cadmium sulfide, cadmium selenide, and molybdenum trisulfide, but titanium oxide particles are preferable in terms of photocatalytic function. Specifically, the photocatalyst particles are, for example, primary or secondary particles of titanium dioxide. In particular, the hydrophilic layer 20 preferably contains secondary particles formed by agglomeration of multiple titanium dioxide primary particles.
[0026] Examples of titanium dioxide include anatase type titanium dioxide, rutile type titanium dioxide, and brookite type titanium dioxide. From the viewpoint of photocatalytic activity, anatase type titanium dioxide is preferred.
[0027] The hydrophilic layer 20 preferably further contains tetraethoxysilane and silicon dioxide, which results in further improved abrasion resistance of the optical member 100.
[0028] <Reflection Adjustment Film> The reflection adjustment film 30 is disposed below the hydrophilic layer 20. The reflection adjustment film 30 covers the light-transmitting member 10. The reflection adjustment film 30 is disposed between the light-transmitting member 10 and the hydrophilic layer 20. The reflection adjustment film 30 suppresses reflection of light.
[0029] The reflection adjustment film 30 has a multilayer structure. Specifically, the reflection adjustment film 30 includes low-refractive index layers and high-refractive index layers alternately stacked along the thickness direction (optical axis direction). The refractive indices of the low-refractive index layers and the high-refractive index layers are not limited as long as the combination allows the reflection adjustment film 30 to exhibit an anti-reflection effect. The refractive index of the low-refractive index layers is, for example, 1.80 or less. The refractive index of the high-refractive index layers is, for example, greater than 1.80.
[0030] The refractive index of the low-refractive index layer may be less than the refractive index of the high-refractive index layer. For example, the refractive index of the low-refractive index layer is preferably 1.30 or more and 1.80 or less, and more preferably 1.40 or more and 1.60 or less. When the refractive index of the low-refractive index layer is 1.30 or more and 1.80 or less, the reflectance of the optical member 100 is further reduced. The low-refractive index layer preferably contains, for example, SiO2, Al2O3, or MgF2, and more preferably contains SiO2.
[0031] The refractive index of the high-refractive index layer may be higher than that of the low-refractive index layer. For example, the refractive index of the high-refractive index layer is preferably 1.80 or more and 3.00 or less, and more preferably 2.00 or more and 2.80 or less. When the refractive index of the high-refractive index layer is 1.80 or more and 3.00 or less, the reflectance of the optical element 100 is further reduced. The high-refractive index layer preferably contains, for example, Si3N4, ZrO2, TiO2, Ti3O5, Ta2O5, In2O3, CeO2, and Nb2O5, and more preferably contains Si3N4.
[0032] The refractive indices of the low-refractive-index layer and the high-refractive-index layer described above are merely examples and are not limited to these. The refractive indices of the low-refractive-index layer and the high-refractive-index layer may be set to values that are optimal for the refractive index of the light-transmitting member 10.
[0033] The thickness of the reflection adjustment film 30 is at least 5 times the thickness of the hydrophilic layer 20. From the viewpoint of productivity, the thickness of the reflection adjustment film 30 is preferably 100 times or less the thickness of the hydrophilic layer 20. That is, the thickness of the reflection adjustment film 30 is preferably 5 times or more and 100 times or less the thickness of the hydrophilic layer 20. The total film thickness of the reflection adjustment film 30 is preferably 20 nm or more and 2000 nm or less, and more preferably 200 nm or more and 750 nm or less. If the total film thickness of the reflection adjustment film 30 is less than 20 nm, a sufficient anti-reflection effect tends to be insufficient. If the total film thickness of the reflection adjustment film 30 exceeds 2000 nm, film formation takes a long time, and the productivity of the optical element 100 tends to decrease. Furthermore, if the total film thickness exceeds 2000 nm, the production cost of the optical element 100 tends to increase.
[0034] The thickness of one low refractive index layer is, for example, 5.0 nm or more and 200.0 nm or less, and the thickness of one high refractive index layer is, for example, 5.0 nm or more and 200.0 nm or less.
[0035] The total number of low refractive index layers and high refractive index layers is usually an odd number, but may be an even number.
[0036] 1 and 2 , in this embodiment, the thickness of the reflection adjustment film 30 is five times or more the thickness of the hydrophilic layer 20, and therefore it is possible to suppress reflection of incident light by the hydrophilic layer 20 and the translucent member 10. Specifically, by including the reflection adjustment film 30, the optical member 100 suppresses reflection of light attempting to enter the translucent member 10 from the reflection adjustment film 30 on the surface on the reflection adjustment film 30 side.
[0037] Furthermore, the reflection adjustment film 30 has low refractive index layers and high refractive index layers alternately stacked along the thickness direction (optical axis direction), so that the effect of multilayer film interference can be obtained.
[0038] Furthermore, it is preferable that the Vickers hardness of the reflection adjustment film 30 is 400 HV or more. As a result, the durability of the reflection adjustment film 30 can be improved. As a result, the durability of the optical element 100 can be improved. A coating layer may be disposed on the reflection adjustment film 30. The coating layer may contain titanium oxide particles.
[0039] <Method for Manufacturing Optical Member> An example of a method for manufacturing the optical member 100 according to this embodiment will be described below. The method for manufacturing the optical member 100 includes a preparation step, a reflection adjustment film formation step, a coating step, and a drying step.
[0040] <Preparation Step> Prepare the light-transmitting member 10. The light-transmitting member 10 contains, for example, glass or synthetic resin as a main component.
[0041] <Reflection Adjustment Film Formation Step> A low refractive index material is prepared. The low refractive index material preferably contains, for example, SiO2, Al2O3, or MgF2, and more preferably contains SiO2. The SiO2 content in the low refractive index material is preferably 95 mass% or more. The low refractive index material is preferably formed by vapor deposition or sputtering.
[0042] A high refractive index material is prepared. The high refractive index material preferably contains, for example, Si3N4, ZrO2, TiO2, Ti3O5, Ta2O5, In2O3, CeO2, and Nb2O5, and more preferably contains Si3N4. The content of Si3N4 in the high refractive index material is preferably 95 mass% or more. The high refractive index material is preferably formed by vapor deposition or sputtering.
[0043] The low refractive index layers and the high refractive index layers are alternately laminated. The total number of low refractive index layers and high refractive index layers is usually an odd number, although the total number of low refractive index layers and high refractive index layers may be an even number.
[0044] <Coating Step> A hydrophilic material is coated. The hydrophilic material contains a plurality of primary particles of photocatalyst particles. The average particle size of the primary particles of the photocatalyst particles is preferably 5 nm or more and 20 nm or less.
[0045] The hydrophilic material preferably further contains a solvent. The solvent is preferably an aqueous solvent. The aqueous solvent contains water and an additive. Examples of the additive include an organic acid, an alcohol compound, or ammonia. Examples of the organic acid include nitric acid, formic acid, acetic acid, propionic acid, succinic acid, citric acid, or malic acid. Examples of the alcohol compound include methanol, ethanol, isopropyl alcohol, n-propyl alcohol, or butanol.
[0046] The content of the solvent in the hydrophilic material is preferably 50.0% by mass or more and 99.9% by mass or less. By having the content of the solvent be 50.0% by mass or more and 99.9% by mass or less, coating can be easily performed.
[0047] The method for applying the hydrophilic material is preferably a wet process. Examples of the wet process include spin coating, roll coating, bar coating, dip coating, spray coating, and a combination of two or more of these (e.g., dip spin coating). Preferred wet processes are spin coating, dip coating, and dip spin coating.
[0048] <Drying Step> The hydrophilic material is dried to form the hydrophilic layer 20. The hydrophilic layer 20 preferably contains secondary particles formed by agglomeration of a plurality of primary particles of photocatalyst particles.
[0049] It is preferable to heat-treat the coated hydrophilic material. Heat treatment promotes the removal of the solvent in the hydrophilic material. Heating conditions can be, for example, a treatment temperature of 60°C to 200°C and a treatment time of 10 minutes to 2 hours.
[0050] Preferably, the method for manufacturing the optical element 100 further includes a coating material application step.
[0051] The above describes embodiments of the present disclosure with reference to the drawings. However, the above embodiments are merely examples of the present disclosure, and the present disclosure is not limited to the above embodiments and can be implemented in various forms without departing from the spirit and scope of the present disclosure. The drawings mainly show each component in a schematic manner for ease of understanding, and the thickness, length, number, etc. of each component shown in the drawings may differ from the actual components due to the convenience of creating the drawings. Furthermore, the materials, shapes, dimensions, etc. of each component shown in the above embodiments are merely examples and are not particularly limited. Various modifications are possible within a scope that does not substantially deviate from the effects of the present disclosure. The configuration of the embodiments may be appropriately modified within a scope that does not deviate from the technical concept of the present disclosure. Furthermore, the embodiments may be implemented in combination within the scope of possibility.
[0052] The present technology can also employ the following configuration.
[0053] (1) A reflection adjustment film used in an optical element having a hydrophilic layer containing a plurality of photocatalytic particles, the reflection adjustment film being disposed below the hydrophilic layer, wherein the thickness of the reflection adjustment film is 5 times or more the thickness of the hydrophilic layer.
[0054] (2) The reflection adjustment film according to (1), wherein the thickness of the reflection adjustment film is 20 nm or more and 2000 nm or less.
[0055] (3) The reflection adjustment film according to (1) or (2), wherein the reflection adjustment film includes a low refractive index layer and a high refractive index layer.
[0056] (4) An optical element comprising: the reflection adjustment film according to any one of (1) to (3); a translucent member that transmits light having a wavelength of 400 nm or more and 700 nm or less; and the hydrophilic layer, wherein the reflection adjustment film is disposed between the hydrophilic layer and the translucent member.
[0057] (5) The optical element according to (4), wherein the photocatalyst particles are titanium oxide particles.
[0058] (6) The optical element according to (4) or (5), wherein the reflection adjustment film has a Vickers hardness of 400 HV or more.
[0059] (7) A lens unit comprising: the optical element according to any one of (4) to (6); and an optical lens that transmits light having a wavelength of 400 nm or more and 700 nm or less, wherein the optical element is disposed on the opposite side of the optical lens in the traveling direction of the light.
[0060] The present invention will be described in more detail below using examples, but the present invention is not limited to the scope of the examples.
[0061] <Production of Optical Members> Optical members according to Examples 1 to 10 and optical members according to Comparative Examples 1 to 6 were produced.
[0062] Example 1 Preparation Steps A lens (manufactured by HOYA Corporation, "TAFD-5G", composition: glass, diameter: 12.9 mm, refractive index: 1.835) was prepared as a light-transmitting member. One surface of the lens was convex (radius of curvature: 12 mm) and the other surface was concave (radius of curvature: 3.07 mm).
[0063] <Reflection adjustment film formation step> A low refractive index material containing SiO2 and a high refractive index material containing Si3N4 were alternately laminated to form a reflection adjustment film according to Example 1 having a total of 11 low refractive index layers and 11 high refractive index layers, with a thickness of 579 nm.
[0064] <Coating Step> A hydrophilic material according to Example 1 containing titanium dioxide particles and silicon dioxide was prepared.
[0065] A hydrophilic material was applied onto the reflection adjustment film. Specifically, 60 μL of the hydrophilic material was dropped onto the optical axis of the light-transmitting member. Next, using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.), the light-transmitting member was rotated at a rotation speed of 5000 rpm. At this time, the rotation axis was aligned with the optical axis of the light-transmitting member.
[0066] <Drying Step> A hydrophilic layer having a thickness of 30 nm was formed by heat treatment at 90° C. for 30 minutes. The thickness of the reflection adjustment film was 19 times the thickness of the hydrophilic layer.
[0067] <Example 2> In the <Reflection adjustment film formation step> of Example 1, the total number of low-refractive index layers and high-refractive index layers was 11, and a reflection adjustment film with a thickness of 579 nm was formed, but instead, the total number of low-refractive index layers and high-refractive index layers was 13, and a reflection adjustment film with a thickness of 415 nm was formed according to Example 2. The thickness of the reflection adjustment film was 14 times the thickness of the hydrophilic layer.
[0068] <Example 3> In the <Reflection adjustment film formation step> of Example 1, the total number of low-refractive index layers and high-refractive index layers was 11, and a reflection adjustment film with a thickness of 579 nm was formed, but instead, the total number of low-refractive index layers and high-refractive index layers was 9, and a reflection adjustment film with a thickness of 388 nm was formed. The thickness of the reflection adjustment film was 13 times the thickness of the hydrophilic layer.
[0069] <Example 4> In the <Reflection adjustment film formation step> of Example 1, the total number of low-refractive index layers and high-refractive index layers was 11, and a reflection adjustment film with a thickness of 579 nm was formed, but instead, the total number of low-refractive index layers and high-refractive index layers was 7, and a reflection adjustment film with a thickness of 324 nm was formed according to Example 4. The thickness of the reflection adjustment film was 11 times the thickness of the hydrophilic layer.
[0070] <Example 5> In the <Reflection adjustment film formation step> of Example 1, the total number of low-refractive index layers and high-refractive index layers was 11, and a reflection adjustment film with a thickness of 579 nm was formed, but instead, the total number of low-refractive index layers and high-refractive index layers was 5, and a reflection adjustment film with a thickness of 196 nm according to Example 5 was formed. The thickness of the reflection adjustment film was 7 times the thickness of the hydrophilic layer.
[0071] <Example 6> In the <Reflection adjustment film formation step> of Example 1, the total number of low-refractive index layers and high-refractive index layers was 11, and a reflection adjustment film with a thickness of 579 nm was formed, but instead, the total number of low-refractive index layers and high-refractive index layers was 17, and a reflection adjustment film with a thickness of 749 nm according to Example 6 was formed. The thickness of the reflection adjustment film was 25 times the thickness of the hydrophilic layer.
[0072] <Comparative Example 1> In the <Reflection adjustment film formation step> of Example 1, the total number of low refractive index layers and high refractive index layers was 11, and instead of forming a reflection adjustment film with a thickness of 579 nm, no reflection adjustment film was formed.
[0073] <Comparative Example 2> In the <Reflection adjustment film formation step> of Example 1, instead of forming a reflection adjustment film with a total number of low-refractive index layers and high-refractive index layers of 11 and a thickness of 579 nm, a reflection adjustment film with a total number of low-refractive index layers and high-refractive index layers of 5 and a thickness of 115 nm was formed according to Comparative Example 2. The thickness of the reflection adjustment film was four times the thickness of the hydrophilic layer.
[0074] Comparative Example 3 In Example 1, a hydrophilic layer having a thickness of 30 nm was formed in the <Coating Step>, the total number of low-refractive-index layers and high-refractive-index layers was 11 in the <Reflection Adjustment Film Forming Step>, and a reflection adjustment film having a thickness of 579 nm was formed. However, in the <Coating Step>, a hydrophilic layer having a thickness of 40 nm was formed, and the total number of low-refractive-index layers and high-refractive-index layers was 5 in the <Reflection Adjustment Film Forming Step>, and a reflection adjustment film having a thickness of 108 nm was formed. The thickness of the reflection adjustment film was three times the thickness of the hydrophilic layer.
[0075] Example 7 Instead of forming a 30 nm thick hydrophilic layer in the <Coating Step> of Example 1, forming a 579 nm thick reflection adjustment film with a total of 11 low and high refractive index layers in the <Reflection Adjustment Film Forming Step>, a 50 nm thick hydrophilic layer was formed in the <Coating Step>, forming a 745 nm thick reflection adjustment film with a total of 17 low and high refractive index layers in the <Reflection Adjustment Film Forming Step> according to Example 7. The thickness of the reflection adjustment film was 15 times the thickness of the hydrophilic layer.
[0076] Example 8 Instead of forming a 30 nm thick hydrophilic layer in the <Coating Step> of Example 1, forming a 579 nm thick reflection adjustment film with a total of 11 low and high refractive index layers in the <Reflection Adjustment Film Forming Step>, a 50 nm thick hydrophilic layer was formed in the <Coating Step>, and forming a 558 nm thick reflection adjustment film with a total of 11 low and high refractive index layers in the <Reflection Adjustment Film Forming Step> according to Example 8. The thickness of the reflection adjustment film was 11 times the thickness of the hydrophilic layer.
[0077] Example 9 Instead of forming a 30 nm thick hydrophilic layer in the <Coating Step> of Example 1, forming a 579 nm thick reflection adjustment film with a total of 11 low and high refractive index layers in the <Reflection Adjustment Film Forming Step>, a 50 nm thick hydrophilic layer was formed in the <Coating Step>, forming a 289 nm thick reflection adjustment film with a total of 7 low and high refractive index layers in the <Reflection Adjustment Film Forming Step> according to Example 9. The thickness of the reflection adjustment film was 6 times the thickness of the hydrophilic layer.
[0078] Comparative Example 4 In Example 1, a hydrophilic layer having a thickness of 30 nm was formed in the <Coating Step>, the total number of low-refractive-index layers and high-refractive-index layers was 11 in the <Reflection Adjustment Film Forming Step>, and a reflection adjustment film having a thickness of 579 nm was formed. Instead, a hydrophilic layer having a thickness of 50 nm was formed in the <Coating Step>, and the total number of low-refractive-index layers and high-refractive-index layers was 5 in the <Reflection Adjustment Film Forming Step>, and a reflection adjustment film having a thickness of 100 nm was formed according to Comparative Example 4. The thickness of the reflection adjustment film was twice as thick as the hydrophilic layer.
[0079] Comparative Example 5 In Example 1, a hydrophilic layer having a thickness of 30 nm was formed in the <Coating Step>, the total number of low-refractive-index layers and high-refractive-index layers was 11 in the <Reflection Adjustment Film Forming Step>, and a reflection adjustment film having a thickness of 579 nm was formed. Instead, a hydrophilic layer having a thickness of 50 nm was formed in the <Coating Step>, and the total number of low-refractive-index layers and high-refractive-index layers was 5 in the <Reflection Adjustment Film Forming Step>, and a reflection adjustment film having a thickness of 181 nm was formed according to Comparative Example 5. The thickness of the reflection adjustment film was four times the thickness of the hydrophilic layer.
[0080] Example 10 Instead of forming a 30 nm thick hydrophilic layer in the <Coating Step> of Example 1, forming a 579 nm thick reflection adjustment film with a total of 11 low and high refractive index layers in the <Reflection Adjustment Film Forming Step>, a 100 nm thick hydrophilic layer was formed in the <Coating Step>, forming a 656 nm thick reflection adjustment film with a total of 17 low and high refractive index layers in the <Reflection Adjustment Film Forming Step>, in which the thickness of the reflection adjustment film according to Example 10 was 7 times the thickness of the hydrophilic layer.
[0081] Comparative Example 6 In Example 1, instead of forming a 30 nm thick hydrophilic layer in the <Coating Step>, forming a 579 nm thick reflection adjustment film with a total of 11 low and high refractive index layers in the <Reflection Adjustment Film Forming Step>, a 100 nm thick hydrophilic layer was formed in the <Coating Step>, forming a 70 nm thick reflection adjustment film with a total of 5 low and high refractive index layers in the <Reflection Adjustment Film Forming Step>, according to Comparative Example 6. The thickness of the reflection adjustment film was 0.7 times the thickness of the hydrophilic layer.
[0082] <Evaluation> The reflectance and productivity of the optical members according to Examples 1 to 10 and Comparative Examples 1 to 6 were evaluated by the following methods. The measurement results are shown in Tables 1 to 4 below. All measurements were carried out in an environment of a temperature of 23°C ± 3°C and a relative humidity of 50% ± 3%.
[0083] <Reflectance> Using a reflectance measuring device ("USPM-RU" manufactured by Olympus Corporation), the maximum reflectance of the optical members was measured for light with a wavelength of 400 nm or more and 700 nm or less. The angle of incidence of the incident light was set to 0 degrees. The maximum reflectance of the optical members was evaluated according to the following criteria. The evaluation results are shown in Tables 1 to 4. The measurement results of the optical members according to Example 1 and Comparative Example 1 are shown in FIG. 3. The measurement results of the optical members according to Example 1, Example 5, and Comparative Example 4 are shown in FIG. 4.
[0084] 〇: 1.0% or less △: More than 1.0% and 3.0% or less ×: More than 3.0%
[0085] <Productivity> The working time for the <reflection adjustment film formation step> was measured. The evaluation results are shown in Tables 1 to 4.
[0086] 〇: Less than 1 hour △: More than 1 hour and less than 2 hours ×: More than 2 hours
[0087]
[0088]
[0089]
[0090]
[0091] The optical members according to Comparative Examples 1 to 6 had reflectances exceeding 3% for light with wavelengths of 400 nm or more and 700 nm or less. In contrast, the optical members according to Examples 1 to 10 had reflectances within 3% for light with wavelengths of 400 nm or more and 700 nm or less. In particular, the optical members according to Examples 1 to 5 and Examples 7 to 10 also had good productivity.
[0092] 10... Transparent member 20... Hydrophilic layer 30... Reflection adjusting film 60... Coating layer 100... Optical member
Claims
1. A reflection adjustment film used in an optical component having a hydrophilic layer containing a plurality of photocatalytic particles, the reflection adjustment film being disposed under the hydrophilic layer, the thickness of the reflection adjustment film being 5 times or more the thickness of the hydrophilic layer.
2. The reflection adjustment film according to claim 1, wherein the thickness of the reflection adjustment film is 20 nm or more and 2000 nm or less.
3. The reflection adjustment film according to claim 1, comprising a low refractive index layer and a high refractive index layer.
4. An optical component comprising: the reflection adjustment film according to claim 1; a translucent member that transmits light having a wavelength of 400 nm or more and 700 nm or less; and the hydrophilic layer, wherein the reflection adjustment film is disposed between the hydrophilic layer and the translucent member.
5. The optical member according to claim 4, wherein the photocatalyst particles are particles of titanium oxide.
6. The optical member according to claim 4, wherein the reflection adjustment film has a Vickers hardness of 400 HV or more.
7. A lens unit comprising: the optical element according to claim 4; and an optical lens that transmits light having a wavelength of 400 nm or more and 700 nm or less, the optical element being positioned on the opposite side of the optical lens in the traveling direction of the light.
8. An optical component comprising: a translucent member that transmits light having a wavelength of 400 nm or more and 700 nm or less; a hydrophilic layer containing a plurality of photocatalyst particles; and a reflection adjustment film disposed between the hydrophilic layer and the translucent member, wherein the reflectance of light having a wavelength of 400 nm or more and 700 nm or less is 3% or less.
Citation Information
Patent Citations
Defogging antireflection optical product
JP1999052104A
Hydrophilic lens
JP2018077260A
Lens with hydrophilic antireflection film and manufacturing method therefor
JP2018197171A