Method for producing hexagonal boron nitride powder, and hexagonal boron nitride powder
The multi-step process of magnetic separation, oxidation treatment, acid washing, and firing significantly reduces foreign substances in hexagonal boron nitride powder, improving its insulation and thermal stability, addressing the limitations of conventional methods by achieving a high-purity product for advanced applications.
Patent Information
- Application Number
- PCT/JP2024/015665
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional methods for producing hexagonal boron nitride powder fail to adequately remove foreign substances, particularly colored particles containing carbon and metal elements, which can introduce electrical conductivity and reduce the material's insulation properties.
A multi-step process involving magnetic separation, oxidation treatment, acid washing, and firing, where the oxidation treatment and acid washing steps are performed before the firing step, to remove magnetizable foreign matter, organic components, and acid-soluble impurities, resulting in a hexagonal boron nitride powder with reduced foreign substances and improved crystallinity.
The process effectively reduces the number of colored foreign substances to 30 or less per kg, enhancing the electrical insulation properties and thermal stability of the hexagonal boron nitride powder, making it suitable for high-performance applications such as insulating sheets and resin compositions.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Method for producing hexagonal boron nitride powder and hexagonal boron nitride powder
[0001] The present invention relates to a method for producing hexagonal boron nitride powder and the hexagonal boron nitride powder.
[0002] Hexagonal boron nitride has excellent electrical insulation, thermal conductivity, and thermal stability, and is used as a material in a variety of fields. When using hexagonal boron nitride as a material, it is desirable to use hexagonal boron nitride powder with minimal foreign matter in order to ensure that the properties of hexagonal boron nitride are exhibited at a high level. In particular, colored foreign matter containing carbon and metal elements can be electrically conductive, so it is necessary to remove these to a high extent from the hexagonal boron nitride powder.
[0003] Under these circumstances, Patent Document 1 discloses hexagonal boron nitride in which the number of colored particles containing carbon is 50 or less per 10 g.
[0004] International Publication No. 2022 / 071245
[0005] The hexagonal boron nitride powder described in Patent Document 1 is examined for the number of colored particles on the order of 10 g. However, even a quantity of foreign matter that may be overlooked on the order of 10 g can be problematic. Therefore, there is a demand for a hexagonal boron nitride powder with even less foreign matter than that disclosed in Patent Document 1.
[0006] An object of one aspect of the present invention is to realize a hexagonal boron nitride powder containing less foreign matter than conventional powders.
[0007] In order to solve the above-mentioned problems, one embodiment of the present invention provides a method for producing a hexagonal boron nitride powder, which comprises subjecting a crude hexagonal boron nitride powder to the following treatments: (1) a magnetic separation step for removing magnetizable foreign matter by magnetic separation; (2) an oxidation treatment step for reducing the content of organic components by oxidation treatment under conditions of 300°C or higher and 700°C or lower; (3) an acid washing step for removing acid-soluble impurities by acid washing; and (4) a firing step for firing under conditions of 1800°C or higher and 2050°C or lower; wherein the oxidation treatment step (2) and the acid washing step (3) are performed before the firing step (4).
[0008] In order to solve the above problems, a hexagonal boron nitride powder according to one embodiment of the present invention is a hexagonal boron nitride powder that contains hexagonal boron nitride particles, has a brightness of 110 or less, and has 30 or less colored foreign matter particles with a particle size of 50 μm or more per kg.
[0009] According to one aspect of the present invention, it is possible to realize a hexagonal boron nitride powder containing less foreign matter than conventional powders.
[0010] Hereinafter, one embodiment of the present invention will be described in detail. In this specification, unless otherwise specified, the expression "A to B" representing a range of numerical values means "A or more and B or less."
[0011] [Method for producing hexagonal boron nitride powder] A method for producing hexagonal boron nitride powder according to one embodiment of the present invention will now be described in detail. The method for producing hexagonal boron nitride powder according to this embodiment is a method for producing hexagonal boron nitride powder from crude hexagonal boron nitride powder, and includes treatments using a magnetic separation step, an oxidation treatment step, an acid washing step, and a firing step. In one embodiment of the present invention, crude hexagonal boron nitride powder is used as the starting material, but in each of the above steps, the crude hexagonal boron nitride powder treated in the previous step may be further treated. For this reason, the hexagonal boron nitride powder treated in each of the above steps is sometimes referred to as the "treated hexagonal boron nitride powder."
[0012] (Coarse hexagonal boron nitride powder) Coarse hexagonal boron nitride powder is a powder of hexagonal boron nitride particles from which foreign matter has not been removed. The coarse hexagonal boron nitride powder is not particularly limited, and one obtained by any method may be used. In this specification, "foreign matter contained in the coarse hexagonal boron nitride powder" refers to objects such as particles different from hexagonal boron nitride particles, components different from hexagonal boron nitride particles attached to the surfaces of hexagonal boron nitride particles, or components or particles different from hexagonal boron nitride contained in hexagonal boron nitride aggregates. Examples of foreign matter contained in the coarse hexagonal boron nitride powder include colored foreign matter.
[0013] As used herein, "colored foreign matter" refers to a colored object having a particle size of 50 μm or more. A colored object refers to an object such as a particle colored by a component other than hexagonal boron nitride particles, or a particle itself other than hexagonal boron nitride particles. As used herein, "colored" refers to a brightness of 110 or less in 256-level grayscale image data, with black being 0 and white being 255. In other words, a colored foreign matter refers to an object having a brightness of 110 or less in 256-level grayscale image data containing coarse hexagonal boron nitride powder as the subject. Colored foreign matter includes, but is not limited to, magnetizable foreign matter, organic components, and acid-soluble impurities. Colored foreign matter may be determined by any method, for example, using a conventional foreign matter inspection machine that inspects for colored foreign matter in powders.
[0014] The magnetizable foreign matter refers to a foreign matter that has magnetism, and other characteristics are not particularly limited. For example, the magnetizable foreign matter may include foreign matter containing elements such as Co, Cr, Cu, Fe, Mg, Mn, Ni, Ti, Zn, and Al. These elements are often contained in coarse hexagonal boron nitride powder or in an apparatus for producing the same.
[0015] The organic component refers to a carbon-containing foreign substance, and other characteristics are not particularly limited. The organic component may be a component derived from carbon contained in the raw material of the crude hexagonal boron nitride powder, for example, a component derived from a carbon source or a boron carbon-containing compound.
[0016] Acid-soluble impurities refer to foreign substances that are soluble in acid, and other characteristics are not particularly limited. For example, acid-soluble impurities include impurities such as composite oxides of boron oxide and calcium oxide that are generated as by-products during the production of crude hexagonal boron nitride powder.
[0017] Many of the magnetic contaminants, organic components, and acid-soluble impurities are colored contaminants. Therefore, these colored contaminants are removed by the magnetic separation process, oxidation treatment process, and acid washing described below. Note that magnetic contaminants, organic components, and acid-soluble impurities that are not colored contaminants may also be removed in each process in the same way as colored contaminants. Because colored contaminants can be conductive, it is preferable that they be significantly reduced, especially when hexagonal boron nitride powder is used in insulating sheets.
[0018] (Magnetic Separation Process) In the magnetic separation process, magnetizable foreign matter is removed from the treated hexagonal boron nitride powder by magnetic separation. The magnetic separation process is preferably performed at a throughput of 50 kg / h or less, and particularly preferably at a throughput of 40 kg / h or less. By not exceeding the upper limit of the throughput of the magnetic separation process, magnetizable foreign matter can be removed to a high degree. The smaller the throughput value of the magnetic separation process, the higher the accuracy of removing magnetizable foreign matter. On the other hand, from the viewpoint of processing efficiency, the throughput of the magnetic separation process may be 0.5 kg / h or more, and particularly preferably 2 kg / h or more. The magnetic separation process may be performed using an electromagnetic sieve device having magnetic poles. By this magnetic separation process, hexagonal boron nitride powder from which magnetizable foreign matter has been removed can be obtained.
[0019] The magnetic separation treatment may be carried out before or after any step in the manufacturing method according to one embodiment of the present invention, but is preferably carried out as the first step.
[0020] The conditions for the magnetic poles of the electromagnetic sieve device may be as follows: The lower limits of the area of the magnetic poles and the magnetic force of the screen are shown below, but the larger the area of the magnetic poles and the magnetic force, the greater the effectiveness of magnetic separation in removing magnetized foreign matter, so there are no upper limits for the magnetic force and the area of the magnetic poles.
[0021] Mesh size: 5mm or less x 8mm or less Magnetic pole area: 30cm2 Screen magnetic force: 1.2 T or more Number of screens: 20 or more Screen shape: mesh-like flat plate Example of screen: electromagnet magnetized to 1.2 T or more by electric current The electromagnetic sieving device is a device that can be used by stacking 20 or more screens at specific intervals. The electromagnetic sieving device is, for example, a vertically long cylindrical device with protrusions on the inner side wall that hold the screens. After all the screens are set, powder is added from the top, and the entire device is vibrated, causing the powder to fall by gravity and pass through all the screens, thereby performing magnetic separation. The more screens there are, the more effective the magnetic separation in removing magnetized foreign matter. Therefore, there is no upper limit on the number of screens, but considering production efficiency, it is preferable that the number be 45 or less.
[0022] (Oxidation Treatment Step) In the oxidation treatment step, the content of organic components is reduced from the treated hexagonal boron nitride powder by oxidation treatment. By this oxidation treatment step, it is possible to obtain hexagonal boron nitride powder with reduced organic components. The oxidation treatment may be carried out at a temperature of 300°C or higher, and preferably at a temperature of 400°C or higher. By setting the temperature condition for the oxidation treatment not below the lower limit, it is possible to reduce the organic components to a high degree. Furthermore, the oxidation treatment step may be carried out at a temperature of 700°C or lower, and preferably at a temperature of 680°C or lower. By setting the temperature condition for the oxidation treatment not above the upper limit, it is possible to reduce the organic components without affecting the properties of the hexagonal boron nitride particles themselves, such as their structure and morphology.
[0023] The treatment time for the oxidation treatment is preferably 2 hours or more, more preferably 3 hours or more, from the viewpoint of suitably reducing the content of organic components. The upper limit of the treatment time for the oxidation treatment is not particularly limited, but in consideration of treatment efficiency, it is preferably 10 hours or less, more preferably 8 hours or less.
[0024] In the manufacturing method according to one embodiment of the present invention, the order of the oxidation treatment step is not particularly limited as long as it is performed before the firing step, but it is preferably performed after the magnetic separation step.
[0025] (Acid Washing Step) In the acid washing step, acid-soluble impurities are removed from the treated hexagonal boron nitride powder by acid washing. The method for acid washing the hexagonal boron nitride powder is not particularly limited, and any known method may be used without limitation. For example, there is a method in which the treated hexagonal boron nitride powder is placed in a container, and dilute hydrochloric acid (5 to 10 mass % HCl) is added in an amount 5 to 10 times the amount of the treated hexagonal boron nitride powder, and the mixture is allowed to come into contact for 4 to 8 hours. In addition to hydrochloric acid, the acid used in the acid washing may also be nitric acid, sulfuric acid, acetic acid, or the like.
[0026] After the acid washing, water washing using pure water may be performed to wash away any remaining acid. As a method of water washing, the acid used in the acid washing may be filtered, and then the pickled hexagonal boron nitride powder may be dispersed in pure water in the same amount as the acid used, followed by filtering again.
[0027] After pickling or water washing, the hydrous aggregate may be dried. Drying conditions may be, for example, in the atmosphere at 50 to 250°C, under reduced pressure, or in vacuum. There is no particular restriction on the drying time, but it is preferable to dry until the moisture content approaches 0%.
[0028] In the manufacturing method according to one embodiment of the present invention, the order of the acid washing step is not particularly limited as long as it is performed before the firing step, but it is preferably performed after the oxidation treatment step.
[0029] (Firing step) The firing step is a step of firing the treated hexagonal boron nitride powder. The heating temperature in the firing step may be 1800°C or higher and 2050°C or lower, and preferably 1900°C or higher and 2000°C or lower. By keeping the heating temperature in the firing step within this range, colored foreign matter with a boiling point of 1900°C or lower can be volatilized. This makes it possible to reduce the amount of colored foreign matter. Furthermore, by performing the firing step after the oxidation treatment step and the acid washing step, it is possible to improve the crystallinity of the hexagonal boron nitride powder whose surface crystallinity has been reduced by oxidation or acid washing.
[0030] The nitrogen-containing gas atmosphere in which the calcination is carried out may be, for example, an atmosphere containing nitrogen and oxygen. The nitrogen source can be supplied to the reaction system during the calcination by known means. The nitrogen source used is not limited to nitrogen gas, and is not particularly limited as long as it is a gas capable of nitriding. Specifically, ammonia gas can be used in addition to nitrogen gas. It is also possible to use a mixture of nitrogen gas or ammonia gas with a non-oxidizing gas such as hydrogen, argon, or helium.
[0031] The firing described above can be carried out using a known reaction apparatus capable of controlling the reaction atmosphere, such as an atmosphere-controlled high-temperature furnace that performs heat treatment by high-frequency induction heating or heater heating, or a batch furnace or a continuous heating furnace such as a pusher-type tunnel furnace or a vertical reactor.
[0032] As described above, the method for producing hexagonal boron nitride powder, which includes the magnetic separation step, oxidation treatment step, acid washing step, and firing step, can remove foreign matter, which has different properties depending on the step, from the crude hexagonal boron nitride powder with high precision. Therefore, this production method can produce hexagonal boron nitride powder with little colored foreign matter on the order of kilograms.
[0033] (Suction Removal Step) The suction removal step is a step of determining whether colored foreign matter is contained in the treated hexagonal boron nitride powder based on image data acquired by a camera, and removing the determined colored foreign matter by suction. The colored foreign matter may have a brightness of 110 or less and a particle size of 50 μm or more.
[0034] In the suction removal process, first, a camera is used to acquire grayscale image data of the hexagonal boron nitride powder in 256 gradations, with black being 0 and white being 255. Next, in the acquired grayscale image data, foreign matter with a brightness of 110 or less and a particle size of 50 μm or more is identified and determined to be colored foreign matter. The camera that acquires image data containing the hexagonal boron nitride powder as a subject is not particularly limited as long as it has a configuration that can achieve the above function. Furthermore, the configuration for determining colored foreign matter from the grayscale image data is also not particularly limited as long as it has a configuration that can achieve the above function. For example, colored foreign matter may be determined using any image processing device.
[0035] The colored foreign matter is removed from the hexagonal boron nitride powder by suction. The configuration for suction is not particularly limited. The hexagonal boron nitride powder subjected to the suction removal step preferably contains a small amount of foreign matter. For example, the hexagonal boron nitride powder subjected to the removal suction step may have 50 or fewer colored foreign matter particles with a particle size of 50 μm or more per kg, and more preferably 30 or fewer. Furthermore, for example, the hexagonal boron nitride powder subjected to the suction removal step preferably has a whiteness W calculated by the following formula (1) of 93 or more, and more preferably 95 or more.
[0036] W=100-[(100-L) 2 +a 2 +b 2 ] 1/2 ... (1) In formula (1), L, a, and b are L * a * b * L based on color system * Value, a * value, b * The value is L * a * b * Each value in the color system can be measured by a known method described in JIS Z8722 using, for example, a colorimeter / color difference meter.
[0037] In the suction removal step, the determined colored foreign matter is sucked in together with the surrounding hexagonal boron nitride powder. Therefore, for hexagonal boron nitride powder whose whiteness W is below the lower limit or whose number of colored foreign matter exceeds the upper limit, a large number of colored foreign matter is sucked in during the suction removal step, resulting in a large loss of hexagonal boron nitride powder due to suction removal. Therefore, by subjecting hexagonal boron nitride powder whose whiteness W is sufficiently high or whose number of colored foreign matter is sufficiently small, i.e., powder that has been treated at least through the magnetic separation step, oxidation treatment step, and acid washing step, to the suction removal step, it is possible to reduce the loss of hexagonal boron nitride powder.
[0038] The processing volume in the suction removal step is not particularly limited. For example, the processing volume in the suction removal step is 15 kg / h or less, and a processing volume of 10 kg / h or less is particularly preferred. By not exceeding the upper limit of the processing volume in the suction removal step, colored foreign matter can be removed to a high degree. The smaller the processing volume in the suction removal step, the higher the accuracy of removing colored foreign matter. On the other hand, from the viewpoint of processing efficiency, the processing volume in the suction removal step may be 0.1 kg / h or more, and a processing volume of 0.5 kg / h or more is particularly preferred. The magnetic separation process may be carried out using an electromagnetic sieve device having a magnetic pole section.
[0039] The hexagonal boron nitride powder subjected to the suction removal step may be in the form of a uniform layer having a thickness of any value between 50 μm and 300 μm. The method for achieving a uniform layer is not particularly limited, but for example, the hexagonal boron nitride powder may be leveled with a roller to achieve a uniform layer. By subjecting the hexagonal boron nitride powder in the form of a uniform layer to the suction removal step, highly accurate suction removal becomes possible.
[0040] The configuration for realizing the suction removal step is not particularly limited. For example, the suction removal step may be realized by an apparatus including all of the camera, the configuration for processing image data, the roller, and the configuration for suction removal.
[0041] The suction removal step can remove colored foreign matter that was not completely removed by the magnetic separation step, oxidation treatment step, acid washing step, and firing step. Therefore, a manufacturing method including the suction removal step can produce a high-purity hexagonal boron nitride powder.
[0042] (Other Treatments) In the manufacturing method according to this embodiment, crude hexagonal boron nitride powder may be prepared by a reduction-nitridation step. In the reduction-nitridation step, a raw material mixture of raw materials for the crude hexagonal boron nitride powder is heated to a temperature of 1600 to 1950°C in a nitrogen atmosphere to carry out a reduction-nitridation reaction. The nitrogen source may be supplied to the reaction system in the reduction-nitridation reaction in the same manner as in the firing step. The raw material mixture may contain an oxygen-containing boron compound, a carbon source, an oxygen-containing calcium compound, and a boron carbon-containing compound.
[0043] The oxygen-containing boron compound may be a compound containing boron and oxygen atoms. Examples of the oxygen-containing boron compound include boric acid, boric anhydride, metaboric acid, perboric acid, hypoboric acid, sodium tetraborate, and sodium perborate. Among these, boric acid or boron oxide, which are easily available, may be preferably used.
[0044] Examples of carbon sources include amorphous carbon such as carbon black, activated carbon, and carbon fiber, as well as crystalline carbon such as diamond, graphite, and nanocarbon, and pyrolytic carbon obtained by pyrolyzing a monomer or polymer. Among these, highly reactive amorphous carbon is preferred, and carbon black is particularly preferred because of its industrial quality control. Examples of carbon black include acetylene black, furnace black, and thermal black.
[0045] Examples of oxygen-containing calcium compounds include calcium carbonate, calcium bicarbonate, calcium hydroxide, calcium oxide, calcium nitrate, calcium sulfate, calcium phosphate, and calcium oxalate. These compounds can be used alone or in combination. Among these, calcium oxide or calcium carbonate is preferred.
[0046] The boron-carbon compound may be a compound containing carbon and boron (e.g., boron carbide). The particle size of the boron-carbon compound is preferably 1 to 500 μm, more preferably 10 to 400 μm, and even more preferably 20 to 300 μm.
[0047] The hexagonal boron nitride powder obtained after the reduction-nitridation reaction may be adjusted to a predetermined particle size distribution by crushing. Crushing is preferably carried out gently using a jet mill, ball mill, hammer mill, stone mill, or the like. The particle size of the crushed powder may also be appropriately adjusted by classification using air classification or sieving.
[0048] The particle size range to be adjusted is preferably set so as to remove particles larger than the mesh size of the screen of the electromagnetic sieving device used in the magnetic separation process. That is, if powder larger than the mesh size is present, it will not be able to pass through the screen, causing clogging and preventing the electromagnetic sieving device from functioning properly, and in the worst case, causing problems such as device breakdown.
[0049] [Hexagonal Boron Nitride Powder] A hexagonal boron nitride powder according to another embodiment of the present invention will be described below. The hexagonal boron nitride powder of this embodiment contains hexagonal boron nitride particles. The number of colored foreign matter having a brightness of 110 or less and a particle size of 50 μm or more in the hexagonal boron nitride powder is 30 or less per kg.
[0050] The number of colored foreign matter particles in the hexagonal boron nitride powder may be 30 or less per 1 kg, preferably 25 or less, more preferably 20 or less, and even more preferably 10 or less. Colored foreign matter may interfere with the properties of the hexagonal boron nitride powder, so the fewer colored foreign matter particles there are, the better; for example, there may be no colored foreign matter at all. The method for measuring the number of colored foreign matter particles is not particularly limited as long as it is capable of measuring 1 kg of hexagonal boron nitride powder. For example, this may be achieved by any powder foreign matter inspection and removal machine equipped with a camera.
[0051] Hexagonal boron nitride powder with colored inclusions falling within this range is hexagonal boron nitride powder with extremely little colored inclusions. Therefore, when filled into a sheet, it can stably exhibit a high withstand voltage. Furthermore, even when used for other applications, the properties of the hexagonal boron nitride powder can be stably exhibited at a high level.
[0052] Furthermore, the hexagonal boron nitride powder preferably has a whiteness W calculated by the following formula (1) of 93 or more, more preferably 95 or more. Such hexagonal boron nitride powder has less foreign matter. Therefore, when filled into a sheet, it can exhibit a higher withstand voltage. Furthermore, even when used for other applications, the properties of the hexagonal boron nitride powder can be stably exhibited at a high level.
[0053] The total content of Fe, Ca, Al, and Si elements contained in the hexagonal boron nitride powder is preferably 3 ppm or less, more preferably 2.5 ppm or less. When the total content of Fe, Ca, Al, and Si elements does not exceed the upper limit, the hexagonal boron nitride powder can have excellent electrical insulation properties.
[0054] The amount of Fe contained in the hexagonal boron nitride powder is preferably 1 ppm or less, more preferably 0.5 ppm or less. The amount of Ca contained in the hexagonal boron nitride powder is preferably 2.5 ppm or less, more preferably 2 ppm or less. The amount of Al contained in the hexagonal boron nitride powder is preferably 0.8 ppm or less, more preferably 0.5 ppm or less. The amount of Si contained in the hexagonal boron nitride powder is preferably 0.8 ppm or less, more preferably 0.5 ppm or less.
[0055] The amount of C contained in the hexagonal boron nitride powder is preferably 0.05% or less, and more preferably 0.035% or less. When the amount of C does not exceed the upper limit, the hexagonal boron nitride powder can have excellent electrical insulation properties.
[0056] The Fe, Ca, Al, and Si elements in the hexagonal boron nitride powder can be quantified by conventionally known ICP measurement. The amount of C present in the hexagonal boron nitride powder can be determined by burning the hexagonal boron nitride powder in an oxygen stream and measuring the CO gas and CO 2 It can be quantified from the amount of gas.
[0057] The average particle size of the hexagonal boron nitride powder may be 2 to 90 μm, and preferably 5 to 70 μm. If the average particle size is less than 2 μm, the particle size may be too small to handle, while if it exceeds 90 μm, the particle size may be too large to handle.
[0058] The graphite index (GI value), which indicates the crystallinity of the hexagonal boron nitride powder, is preferably 1.0 to 2.5, more preferably 1.3 to 2.0, more preferably 1.4 to 1.8, and even more preferably 1.5 to 1.7. The GI value is determined by dividing the sum of the peak areas originating from the (100) and (101) planes in the X-ray diffraction spectrum by the peak area originating from the (102) plane.
[0059] (Applications) The above-described hexagonal boron nitride powder can be filled into a resin as a filler. When filled into a resin as a filler, it is possible to impart extremely high insulating performance to the resulting resin composition. For example, when a resin sheet is produced from a resin filled with the above-described hexagonal boron nitride powder, the resin sheet can be imparted with insulating performance of 100 kv / mm or more. Here, if 70% or more of the produced resin sheet has an insulating performance of 100 kv / mm or more, it can be determined that insulating performance has been imparted. The applications of such resin sheets are not particularly limited, but they can be used, for example, for circuit board applications and insulating layer applications in multilayer printed wiring boards.
[0060] Hexagonal boron nitride powder can also be used as a raw material for boron nitride processed products such as cubic boron nitride or boron nitride molded products, a nucleating agent for engineering plastics, a phase change material, a solid or liquid thermal interface material, a release agent for molten metal or molten glass molds, cosmetics, and a raw material for composite ceramics.
[0061] Hexagonal boron nitride powder according to one aspect of the present invention is obtained, for example, by using the above-mentioned manufacturing method. The hexagonal boron nitride powder obtained by the above-mentioned manufacturing method is characterized by having a brightness of 110 or less and having 30 or less colored foreign particles with a particle size of 50 μm or more per kg. Furthermore, resin sheets made using the above-mentioned hexagonal boron nitride powder have high dielectric strength.
[0062] On the other hand, there are circumstances in which it is impossible or practical to directly identify the hexagonal boron nitride powder according to one aspect of the present invention based on other structures or characteristics. For example, although the above-described method for producing hexagonal boron nitride powder is characterized by including a step for removing colored impurities, the final product, hexagonal boron nitride powder, does not contain the removed colored impurities, and therefore the removed colored impurities cannot be considered as a defining feature of the hexagonal boron nitride powder. Therefore, it is impossible to generally identify the hexagonal boron nitride powder according to one aspect of the present invention based on anything other than the above-described characteristics. The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also within the technical scope of the present invention.
[0063] <Summary> As described above, the method for producing hexagonal boron nitride powder according to aspect 1 of the present invention involves subjecting crude hexagonal boron nitride powder to the following treatments: (1) a magnetic separation step of removing magnetizable foreign matter by magnetic separation; (2) an oxidation treatment step of reducing the content of organic components by oxidation treatment under conditions of 300°C or higher and 700°C or lower; (3) an acid washing step of removing acid-soluble impurities by acid washing; and (4) a firing step of firing under conditions of 1800°C or higher and 2050°C or lower; and the treatments by the oxidation treatment step (2) and the acid washing step (3) are performed before the treatment by the firing step (4).
[0064] The method for producing a hexagonal boron nitride powder according to Aspect 2 of the present invention may be the same as in Aspect 1, and may further include a suction removal step of determining, based on image data acquired by a camera, colored foreign matter contained in the hexagonal boron nitride powder that has a brightness of 110 or less and a particle size of 50 μm or more, and removing the determined colored foreign matter by suction.
[0065] The hexagonal boron nitride powder according to Aspect 3 of the present invention contains hexagonal boron nitride particles, has a brightness of 110 or less, and contains 30 or less colored foreign particles having a particle size of 50 μm or more per 1 kg.
[0066] The hexagonal boron nitride powder according to Aspect 4 of the present invention is the same as that of Aspect 3, except that the whiteness W calculated by the following formula (1) is 93 or more.
[0067] W=100-[(100-L) 2 +a 2 +b 2 ] 1/2 ...(1)
[0068] An embodiment of the present invention will be described below, but the present invention is not limited to each of the embodiments shown below.
[0069] <Production of Hexagonal Boron Nitride Powder> The hexagonal boron nitride powders according to the examples and comparative examples were each produced by the method described below.
[0070] Example 1 A crude hexagonal boron nitride powder according to Example 1 was prepared. 259 g of a mixture containing 141 g of boron oxide, 56 g of carbon black, 32 g of calcium oxide, and 30 g of boron carbide was mixed using a ball mill. The mixture was subjected to a reduction-nitriding treatment in a graphite Tammann furnace by holding it in a nitrogen gas atmosphere at a maximum temperature of 1750°C for 2 hours.
[0071] The obtained coarse hexagonal boron nitride was subjected to crushing, and the volumetric proportion of agglomerated particles of 10 μm or less in the particle size distribution was adjusted to 4%, and the volumetric proportion of agglomerated particles of more than 10 μm and 50 μm or less was adjusted to 48%. The coarse hexagonal boron nitride powder after particle size distribution adjustment was placed in a container, and a five-fold amount of hydrochloric acid (7 mass% HCl) was added. The mixture was stirred at a rotation speed of 700 rpm for 24 hours to perform an acid pickling treatment. After the acid pickling treatment, the acid was filtered, and the coarse hexagonal boron nitride powder obtained by filtration was dispersed in pure water in the same amount as the acid used, and then filtered again. This operation was repeated five times, and the mixture was then vacuum dried at 200°C for 6 hours.
[0072] Coarse hexagonal boron nitride powder was placed in a 54 cm diameter mold with a diameter of 145 mm, a thickness of 10 mm, and an opening of 5 mm x 8 mm. 2 Magnetic separation was carried out using an electromagnetic sieve device having a magnetic pole area of 1.6 T and 40 stacked screens magnetized to 1.6 T. The magnetic separation was carried out at a throughput of 15 kg / h (magnetic separation step).
[0073] The magnetically separated coarse cubic boron nitride powder was heated in an air atmosphere at an oxidation temperature of 600° C. for 5 hours to oxidize the organic components (oxidation treatment step).
[0074] The hexagonal boron nitride powder after the reduction-nitridation treatment was placed in a container, and a five-fold amount of hydrochloric acid (7 mass% HCl) was added. The mixture was stirred at 700 rpm for 5 hours to perform pickling (pickling step). After the pickling treatment, the acid was filtered, and the hexagonal boron nitride powder obtained by filtration was dispersed in pure water in the same amount as the acid used, and then filtered again. This procedure was repeated five times, and the mixture was then vacuum dried at 200°C for 6 hours.
[0075] The crude hexagonal boron nitride powder obtained after drying was subjected to a firing treatment in a graphite Tammann furnace by holding it at 1900°C for 6 hours under a nitrogen gas atmosphere (firing step). After the furnace was cooled, the hexagonal boron nitride powder according to Example 1 was recovered from the furnace.
[0076] The manufacturing conditions for the hexagonal boron nitride powder according to each example and comparative example are shown below, with the differences from the conditions of Example 1. Table 1 also shows a list of the conditions under which each step was carried out in Examples 1 to 6 and Comparative Examples 1 to 4.
[0077] (Example 2) Magnetic separation throughput: 25 kg / h, oxidation temperature: 500°C, firing temperature: 1850°C (Example 3) Magnetic separation throughput: 10 kg / h, oxidation temperature: 650°C, firing temperature: 1950°C (Example 4) Magnetic separation throughput: 15 kg / h, oxidation temperature: 550°C (Example 5) Magnetic separation throughput: 45 kg / h, oxidation temperature: 450°C, firing temperature: 1850°C (Example 6) Magnetic separation throughput: 15 kg / h, oxidation temperature: 600°C Furthermore, using a powder foreign matter inspection and removal machine (PGS-R2, manufactured by Nisshin Chemical Industry Co., Ltd.), colored foreign matter, which was particles with a brightness of 110 or less and a particle size of 50 μm or more, was removed by suction from the obtained hexagonal boron nitride powder (suction removal process).
[0078] (Comparative Example 1) Magnetic separation: not performed, oxidation temperature: 500°C (Comparative Example 2) Oxidation treatment: not performed (Comparative Example 3) Oxidation temperature: 500°C, acid cleaning: not performed (Comparative Example 4) Oxidation temperature: 500°C, baking after acid cleaning: not performed
[0079]
[0080] <Evaluation of Hexagonal Boron Nitride Powder> (Colored Foreign Matter Content) The number of colored foreign matter of 50 μm or larger contained in 1 kg of the hexagonal boron nitride powder prepared in each of Examples 1 to 6 and Comparative Examples 1 to 4 was measured. The number of colored foreign matter was measured using a foreign matter inspection machine (PGS-R2, manufactured by Nisshin Chemical Industry Co., Ltd.). The inspection section of the foreign matter inspection machine was equipped with an FA image processing device (IMAGECHECKAR PV200, manufactured by Panasonic Corporation).
[0081] (SEM-EDS Inspection) Of the detected colored foreign matter, five were sampled and subjected to an SEM-EDS inspection to perform elemental analysis of each colored foreign matter. The equipment used for the SEM-EDS inspection and the conditions for the SEM-EDS inspection are shown below.
[0082] (Apparatus) Scanning electron microscope (SEM): JEOL JSM-7000F Energy dispersive X-ray analyzer (EDS): EDXA GENESIS (Conditions) Qualitative analysis was performed under the following conditions to confirm element peaks: Acceleration voltage 10 kV, analysis target element 5B-92U As a result of SEM-EDS elemental analysis, the main component of the extracted colored foreign matter was either Fe, Ca, Al·Si, or C. The results of the SEM-EDS elemental analysis of the hexagonal boron nitride powders of Examples 1 to 6 and Comparative Examples 1 to 4 are shown in Table 2.
[0083] (Impurity Analysis) Ten samples of 0.5 g each were collected from any location of the hexagonal boron nitride powders according to Examples 1 to 6 and Comparative Examples 1 to 4. Each sample was placed in a pressure decomposition vessel together with 10 ml of hydrofluoric acid, 1.25 ml of sulfuric acid, and 0.25 ml of nitric acid. After leaving the sample in a dryer at 160°C for 20 hours, the solution was transferred to a platinum dish, heated to 220°C over 1 hour, and heated at 220°C for 5 hours until no more white smoke was emitted. After that, 1.25 ml of hydrochloric acid and 1.25 ml of ultrapure water were added and the solution was recovered. Ultrapure water was added to a 25 ml polypropylene measuring flask to make the volume constant, and the amount of Fe, Ca, Al, and Si present in the solution was measured using an ICP light emitting device (ICAP6500 manufactured by Thermo Fisher Scientific Co., Ltd.). The contents of each sample were calculated, and the average values for the 10 samples are shown in Table 2.
[0084] (Measurement of Total Carbon Content) The total carbon content in the hexagonal boron nitride powder was measured using a ceramic carbon analyzer EMIA-110 manufactured by Horiba Ltd. The powder was burned in an oxygen stream, and the generated CO gas and CO 2 The total carbon content was determined from the amount of gas. The measurement results of the total carbon content for the hexagonal boron nitride powders of Examples 1 to 6 and Comparative Examples 1 to 4 are shown in Table 2.
[0085] (Whiteness) L of hexagonal boron nitride powder * Value, a * value, b * The value was measured using a color difference meter ZE7700 (manufactured by Nippon Denshoku Industries Co., Ltd.) The whiteness W of the hexagonal boron nitride powder was calculated using the following formula (1).
[0086] W=100-[(100-L) 2 +a 2 +b 2 ] 1/2 ... (1) The calculation results of the whiteness W of the hexagonal boron nitride powders according to Examples 1 to 6 and Comparative Examples 1 to 4 are shown in Table 2.
[0087] (Average particle size) The average particle size of the hexagonal boron nitride powder was measured using a particle size distribution measuring device MT3000 manufactured by Nikkiso Co., Ltd. The measurement sample was prepared by the following method. First, 20 g of ethanol was added as a dispersion medium to a 50 mL screw tube bottle, and 1 g of hexagonal boron nitride powder was dispersed in the ethanol. Then, the particle size distribution of the measurement sample was measured without ultrasonic treatment. The average particle sizes of the hexagonal boron nitride powders according to Examples 1 to 6 and Comparative Examples 1 to 4 are shown in Table 2.
[0088] (Graphitization Index: GI Value) X-ray diffraction measurements were performed using a fully automated horizontal multipurpose X-ray diffractometer, SmartLab, manufactured by Rigaku Corporation. The measurement conditions were a scan speed of 20 degrees / min, a step width of 0.02 degrees, and a scan range of 10 to 90 degrees. The GI value was calculated from the integrated intensity ratio (area ratio) of the (100), (101), and (102) diffraction lines in the X-ray diffraction spectrum of the hexagonal boron nitride powder, using the formula: GI = [{(100) + (101)} / [(102)].
[0089]
[0090] (Insulating Performance) The hexagonal boron nitride powders of Examples 1 to 6 and Comparative Examples 1 to 4 were mixed with epoxy resin to prepare resin compositions, and their thermal conductivity was evaluated. A varnish-like mixture was prepared using 100 parts by mass of epoxy resin (JER828 manufactured by Mitsubishi Chemical Corporation) and 5 parts by mass of a curing agent (imidazole-based curing agent, Curesol 2E4MZ manufactured by Shikoku Kasei Co., Ltd.) and 210 parts by mass of methyl ethyl ketone as a solvent. Next, the varnish-like mixture and the hexagonal boron nitride powder were mixed in a rotation / revolution mixer (MAZERUSTAR manufactured by Kurabo Industries Co., Ltd.) to obtain a resin composition containing 65% by volume of epoxy resin and 35% by volume of hexagonal boron nitride powder.
[0091] The resin composition was coated onto a PET film to a thickness of approximately 250 to 300 μm using an automatic coater PI-1210 manufactured by Tester Sangyo Co., Ltd., dried, and cured under reduced pressure at a temperature of 200°C, a pressure of 5 MPa, and a holding time of 30 minutes to produce 10 sheets each having a thickness of 200 μm for each example or comparative example. The insulating performance of each sheet was measured using a withstand voltage tester (manufactured by Tama Densoku Co., Ltd.).
[0092] The results of the measurement are shown in Table 3. In Table 3, when there were 10 sheets with a dielectric strength of 100 kv / mm or more, the result was evaluated as "very good", when there were 7 or more sheets, the result was evaluated as "good", and when there were 3 or less sheets, the result was evaluated as "poor".
[0093]
[0094] The hexagonal boron nitride powder according to the present invention contains an extremely small number of colored inclusions, and can therefore be used as a raw material for a wide range of applications.
Claims
1. A method for producing a hexagonal boron nitride powder, comprising the steps of: (1) a magnetic separation process for removing magnetizable foreign matter by magnetic separation; (2) an oxidation process for reducing the content of organic components by oxidation treatment under conditions of 300°C or higher and 700°C or lower; (3) an acid washing process for removing acid-soluble impurities by acid washing; and (4) a firing process for firing under conditions of 1800°C or higher and 2050°C or lower, wherein the oxidation process in (2) and the acid washing process in (3) are performed before the firing process in (4).
2. The manufacturing method described in claim 1, further comprising a suction removal step of determining whether colored foreign matter contained in the hexagonal boron nitride powder has a brightness of 110 or less and a particle size of 50 μm or more based on image data acquired by a camera, and removing the determined colored foreign matter by suction.
3. Hexagonal boron nitride powder containing hexagonal boron nitride particles, having a brightness of 110 or less and containing 30 or less colored foreign matter particles having a particle size of 50 μm or more per 1 kg.
4. The hexagonal boron nitride powder according to claim 3, having a whiteness W of 93 or more as calculated by the following formula (1): W=100-[(100-L) 2 +a 2 +b 2 ] 1/2 ...(1)
Citation Information
Patent Citations
Hexagonal boron nitride powder and its manufacturing method
JP6955127B1
Boron nitride powder and method for producing boron nitride powder
WO2022071227A1
Boron nitride powder, and method for producing boron nitride powder
WO2022071246A1
Cited By
Hexagonal boron nitride powder, resin composition, resin sheet, and method for producing hexagonal boron nitride powder
JP2026166591A
Hexagonal boron nitride powder, resin composition, and method for producing hexagonal boron nitride powder
JP7871512B1
Boron nitride powder
JP7875395B1
Powder of hexagonal boron nitride, resin composition, and method for producing powder of hexagonal boron nitride
WO2026191360A1