Method for producing low-molecular-weight fluorine compound
By controlling temperature differences in the microwave-assisted fluororesin decomposition process, the method enhances the selectivity of low molecular weight fluorine compounds, addressing the limitations of conventional recycling methods and achieving higher purity and efficiency in fluororesin recycling.
Patent Information
- Application Number
- PCT/JP2024/016553
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional chemical recycling methods for fluororesins lack control over the temperature environment for low-molecular-weight fluorine compounds, resulting in suboptimal selectivity of constituent monomers during thermal decomposition.
The method involves controlling temperature differences in a microwave-assisted fluororesin decomposition process by setting the temperature difference between the microwave absorber and the carrier gas inlet to exceed 500°C, and the temperature difference between the microwave absorber and the generated gas outlet to 300°C or more, using a microwave absorber with specific properties and configurations to enhance the selectivity of low molecular weight fluorine compounds.
This approach significantly improves the selectivity of constituent monomers among the produced low molecular weight fluorine compounds, achieving higher purity and efficiency in the decomposition process.
Smart Images

Figure JP2024016553_31102024_PF_FP_ABST
Abstract
Description
Method for producing low molecular weight fluorine compounds
[0001] The present invention relates to a technology for decomposing fluororesins. More specifically, the present invention relates to a method for producing low-molecular-weight fluorine compounds by thermal decomposition of fluororesins using microwave irradiation heating.
[0002] Fluorine resins, taking advantage of their excellent properties such as lubricity, heat resistance, and chemical resistance, are widely used in applications such as heat-resistant wire coatings, semiconductor manufacturing materials, and electronic components. In recent years, decomposition and reuse of synthetic resins containing fluororesins has been actively studied. For example, Patent Document 1 proposes a chemical recycling method for extracting low-molecular-weight tetrafluoroethylene monomers and dimers generated by thermal decomposition of PTFE from a material containing PTFE, the chemical recycling method including the steps of: heating a fluidized-bed reactor having a fluidized bed formed of an inert granular material therein and into which the material is supplied; introducing an inert gas as a fluidizing gas into the fluidized-bed reactor; and extracting from the fluidized-bed reactor the low-molecular-weight tetrafluoroethylene monomers and dimers generated by thermal decomposition of PTFE together with the inert gas.
[0003] Japanese Patent Application Laid-Open No. 2004-346000
[0004] The present inventors noticed that in the conventional chemical recycling technology for fluororesin, no consideration has been given to controlling the temperature environment to which low molecular weight fluorine compounds such as fluorine-based monomers generated from fluororesin are exposed, and discovered a method of intentionally controlling the temperature of the product gas discharged from a reaction vessel to be lower than the temperature in the decomposition reaction system. However, further investigations have led to the problem that such a method leaves room for improvement in the selectivity of the constituent monomers of the fluororesin among the low molecular weight fluorine compounds generated.
[0005] Therefore, the present invention aims to improve the selectivity of constituent monomers of the fluororesin from among the low-molecular-weight fluorine compounds produced in a fluororesin decomposition method in which a temperature difference (hereinafter also referred to as "temperature TE") is provided so as to control the temperature of the product gas discharged from a reaction vessel to be lower than the temperature in the decomposition reaction system, i.e., the temperature of a heated microwave absorber (hereinafter also referred to as "temperature TR").
[0006] As a result of extensive investigation, the present inventors have found that the selectivity of constituent monomers of fluororesin from the produced low-molecular-weight fluorine compounds can be improved by setting the temperature difference Δ1 (TR - TI) obtained by subtracting the carrier gas temperature TI (°C) at the reactor inlet from the temperature TR (°C) of the microwave absorber heated in the reactor to more than 500°C, and / or by setting the temperature difference Δ2 (TR - TE) obtained by subtracting the decomposition gas outlet TE (°C) of the produced gas discharged from the reactor from the temperature TR (°C) of the microwave absorber heated in the reactor to more than 300°C. The present invention was completed based on this finding and through further investigation.
[0007] That is, the present invention provides the following aspects: Item 1. A method for producing a low molecular weight fluorine compound, comprising a decomposition step of heating a microwave absorber by microwave irradiation in a reaction vessel provided with a carrier gas inlet and a decomposition gas outlet, and bringing the heated microwave absorber into contact with a material containing a fluororesin to decompose the fluororesin into a low molecular weight fluorine compound, wherein (i) a temperature difference Δ1 (TR - TI) obtained by subtracting the carrier gas temperature TI (°C) at the inlet from the temperature TR (°C) of the heated microwave absorber is set to exceed 500°C. Item 2. A method for producing a low molecular weight fluorine compound, comprising: a decomposition step of heating a microwave absorber by microwave irradiation in a reaction vessel provided with a carrier gas inlet and a decomposition gas outlet, and bringing the heated microwave absorber into contact with a material containing a fluororesin to decompose the fluororesin into a low molecular weight fluorine compound, wherein (ii) a temperature difference Δ2(TR - TE) obtained by subtracting a temperature TE (°C) of a product gas at the outlet discharged from the reaction vessel from a temperature TR (°C) of the heated microwave absorber is set to be 300°C or more. Item 3. The production method according to Item 1 or 2, wherein an introduction speed R of the carrier gas from the inlet is 0.005 to 20 m / s. Item 4. The production method according to any one of Items 1 to 3, wherein a temperature TE (°C) of the product gas discharged from the reaction vessel at the outlet is 20°C or more but less than 250°C. Item 5. Item 6. The manufacturing method according to any one of Items 1 to 4, wherein the microwave absorber is prepared in the form of a microwave absorber-containing layer containing particles of a material containing the microwave absorber and the fluororesin and arranged to allow an airflow to pass from the carrier gas inlet to the decomposition gas outlet, wherein, when the center of the opening of the outlet is defined as point Pe and the intersection point between the central axis of the microwave absorber-containing layer and the surface of the microwave absorber-containing layer opposite to the outlet is defined as point Pl, a ratio h / H of a height h of the microwave absorber-containing layer to a height H from point Pl to point Pe is 0.01 to 0.8. Item 7. The manufacturing method according to any one of Items 1 to 5, wherein a particle diameter d of the microwave absorber is 0.1 to 25 mm. Item 8. The manufacturing method according to Items 5 or 6, wherein the height h of the microwave absorber-containing layer is 0.1 to 200 mm.Item 8. The manufacturing method according to any one of Items 2 to 7, wherein a temperature difference Δ1 (TR - TI) obtained by subtracting a carrier gas temperature TI (°C) at the inlet from a temperature TR (°C) of the heated microwave absorber is set to exceed 250°C.
[0008] According to the present invention, in a fluororesin decomposition method in which a temperature difference Δ2 (TR - TE) is provided so as to control the temperature TE of the product gas discharged from a reaction vessel to be lower than the temperature in the decomposition reaction system, i.e., the temperature TR of the heated microwave absorber, the selectivity of the constituent monomers of the fluororesin can be improved from among the low-molecular-weight fluorine compounds produced.
[0009] 1 shows a schematic diagram of an example of an apparatus (upward parallel flow cylindrical reactor) used in the production method of the present invention; 2 shows a schematic diagram of an example of an apparatus (downward parallel flow cylindrical reactor) used in the production method of the present invention; 3 shows a schematic diagram of an example of an apparatus (continuous tank reactor) used in the production method of the present invention; 4 shows a schematic diagram of an example of an apparatus (continuous tank reactor) used in the production method of the present invention.
[0010] The method for producing a low molecular weight fluorine compound of the present invention includes a decomposition step of heating a microwave absorber by microwave irradiation in a reaction vessel provided with a carrier gas inlet and a decomposition gas outlet, and bringing the heated microwave absorber into contact with a material containing a fluororesin to decompose the fluororesin into a low molecular weight fluorine compound, and is characterized by setting the following (i) and / or (ii): (i) setting the temperature difference Δ1 (TR - TI) obtained by subtracting the carrier gas temperature TI (°C) at the inlet from the temperature TR (°C) of the heated microwave absorber to be greater than 500°C, (ii) setting the temperature difference Δ2 (TR - TE) obtained by subtracting the temperature TE (°C) at the outlet of the generated gas discharged from the reaction vessel from the temperature TR (°C) of the heated microwave absorber to be 300°C or greater. The method for producing a low molecular weight fluorine compound of the present invention will now be described in detail.
[0011] [1. Fluororesin] In the present invention, a fluororesin is used as a raw material for a low molecular weight fluorine compound. The fluororesin is a fluorine compound having a molecular weight of 500 or more and a fluorine content (by weight) of 57% or more.
[0012] Examples of the fluororesin include fluorinated polyolefin and fluorinated polyether.
[0013] Fluorinated polyolefins are polymers or oligomers having repeating units derived from a fluorinated olefin.
[0014] Examples of the fluorinated olefin include tetrafluoroethylene (TFE), hexafluoropropylene (HFP), vinylidene fluoride (VDF), chlorotrifluoroethylene (CTFE), partially fluorinated or perfluorovinyl ether, partially fluorinated or perfluoroallyl ether, and the like.
[0015] The perfluorovinyl ethers include those represented by the general formula CF2=CF-O-R f A compound represented by the formula f represents a perfluorinated linear, cyclic, or branched aliphatic group which may contain one or more oxygen atoms. f When R contains one or more oxygen atoms, f As for -(R a f O) n (R b f O) m R c f [wherein R a f and R b f are different linear or branched or cyclic perfluoroalkylene groups having 1 to 6 carbon atoms, in particular 2 to 6 carbon atoms, m and n are independently integers from 0 to 10, R c f is a perfluoroalkyl group having 1 to 6 carbon atoms. f When does not contain an oxygen atom, specific examples of the perfluorovinyl ether include perfluoromethyl vinyl ether (PMVE), perfluoropropyl vinyl ether, and perfluoroisopropyl vinyl ether.
[0016] Specific examples of the perfluorovinyl ether include perfluoro(methyl vinyl) ether (PMVE), perfluoro(ethyl vinyl) ether (PEVE), perfluoro(n-propyl vinyl) ether (PPVE-1), perfluoro-2-propoxypropyl vinyl ether (PPVE-2), perfluoro-3-methoxy-n-propyl vinyl ether, perfluoro-2-methoxy-ethyl vinyl ether, CF3-(CF2)2-O-CF(CF3)-CF2-O-CF(CF3)-CF2-O-CF=CF2, CF2=CF-O-(CF2)3OCF3, CF2=CFO(CF2)2OCF3, and the like.
[0017] The perfluoroallyl ethers include those represented by the general formula CF2=CF-CF2-O-R f A compound represented by the formula f is the R described above for the perfluorovinyl ether. f is the same as above.]
[0018] The fluorinated polyolefin may be a polymer or oligomer comprising repeating units derived from a fluorinated olefin, or may be a polymer or oligomer comprising repeating units derived from a non-fluorinated olefin in addition to repeating units derived from a fluorinated olefin. The non-fluorinated olefin is not particularly limited, but examples thereof include C2 to C8 olefins, and more preferably ethylene (E) and propylene (P). Among these fluorinated polyolefins, preferred are polymers or oligomers comprising repeating units derived from a fluorinated olefin (i.e., fluorinated polyolefins in which the molar ratio of repeating units derived from a non-fluorinated olefin is 0%).
[0019] Suitable examples of the fluorinated polyolefin include a homopolymer of TFE and the following copolymers: TFE and HFP; TFE, HFP and VDF; TFE and CTFE; TFE, CTFE and E or P; TFE and PMVE, PEVE, PPVE-1 or PPVE-2; TFE, E and HFP; and polymers containing repeating units derived from CTFE and E or P. Among these fluorinated polyolefins, a homopolymer of TFE is preferable.
[0020] Fluorinated polyethers are polymers or oligomers having fluorinated oxyalkylene repeating units.
[0021] The fluorinated oxyalkylene repeat unit is —C l X 2l O-, l is an integer of 1 or more, X is hydrogen or fluorine, is linear or branched, and l and X may be different in each occurrence.
[0022] The fluororesin may be a fluorinated non-ionomer or a fluorinated ionomer (multiple -SO3 - and / or -COO - The fluorinated ionomer may be a fluoropolymer having a group as a pendant group or a terminal group. Any fluorinated ionomer used in the preparation of membranes in fuel cells or electrochemical reactions can be used without any particular limitation.
[0023] The fluororesin may have a functional group containing a hydrogen atom or an atom other than fluorine at its terminal. The functional group containing an atom other than fluorine is not particularly limited, but examples thereof include an iodine group, a bromine group, a chlorine group, a hydroxyl group and its esters, and a vinyl group.
[0024] The above fluororesins may be used alone or in combination of two or more.
[0025] [2. Material containing fluororesin] The fluororesin is subjected to the decomposition step in the form of a material containing the fluororesin. The material may consist of the fluororesin alone, or may contain other components in addition to the fluororesin. Examples of other components include resin additives to be blended into the fluororesin composition, and more specifically, examples include fillers, pigments, lubricants, curing agents, curing accelerators, thermal conductive agents, and electrical conductive agents.
[0026] The properties of the fluororesin-containing material in the decomposition step are determined depending on the conditions in the decomposition step and are not particularly limited. When the fluororesin-containing material is solid, it is used in a particulate form. The particles are obtained by processing the fluororesin material into particles by any means. Examples of such means include a milling device and a pulverizing device.
[0027] The particle size is not particularly limited, but may be, for example, 20 μm to 100 mm, preferably 100 μm to 10 mm, and more preferably 250 μm to 5 mm.
[0028] The fluororesin-containing material may be obtained by a pretreatment that can be carried out prior to the decomposition step. Such pretreatment is not particularly limited as long as it can obtain a fluororesin-containing material, and examples include a treatment for separating and removing components that do not contain fluororesin and / or materials other than fluororesin from the material to be recycled, a treatment for removing oil and / or dust, and a fluorination treatment of a polymer material (a treatment for converting C—H bonds into C—F bonds by treating a polymer material with F gas).
[0029] The method for feeding the fluororesin-containing material into the reaction vessel is not particularly limited, and may be appropriately selected by a person skilled in the art. For example, when the fluororesin-containing material is in the form of particles, it is preferable to feed it into the reaction vessel by gravity, and when the fluororesin-containing material is in the form of a liquid, it can be fed into the reaction vessel by spraying, for example.
[0030] [3. Reaction Vessel] The reaction vessel is provided with a carrier gas inlet and a decomposition gas outlet for introducing and discharging a gas flow. Examples of the reaction vessel used in the present invention include a parallel-flow cylindrical reaction vessel and a continuous tank reaction vessel.
[0031] Specific examples of parallel flow cylindrical reactors are shown in Figures 1 and 2. The parallel flow cylindrical reactor 1 shown in Figure 1 is provided with a carrier gas inlet 1I and a decomposition gas outlet 1E, and is configured so that the flow pattern of the carrier gas 3 is an upward parallel flow type. The parallel flow cylindrical reactor 1a shown in Figure 2 is provided with a carrier gas inlet 1I and a decomposition gas outlet 1E, and is configured so that the flow pattern of the carrier gas 3 is a downward parallel flow type.
[0032] Specific examples of continuous-tank reaction vessels are shown in Figures 3 and 4. The continuous-tank reaction vessel 1b shown in Figure 3 is provided with a carrier gas inlet 1I and a decomposition gas outlet 1E, and is preferably used for small-scale reactions. The continuous-tank reaction vessel 1c shown in Figure 4 is provided with a carrier gas inlet 1I and a decomposition gas outlet 1E, and is preferably used for large-scale reactions. The continuous-tank reaction vessels 1b and 1c shown in Figures 3 and 4 can also be equipped with a stirrer (not shown).
[0033] More specifically, the reaction vessel of the present invention can be incorporated into an apparatus similar to a general catalytic reactor, and in this apparatus, a microwave absorber is used instead of the catalyst in the general catalytic reactor.
[0034] Furthermore, since microwaves are used as the heating means in the present invention, the device may be equipped with a microwave generator. The microwave generator may be appropriately selected from known devices, examples of which include a diode, a magnetron, a gyrotron, a traveling wave tube, a klystron, a ubitron, and an amplitron.
[0035] [4. Microwave Absorber] [4-1. Examples of Microwave Absorber] The microwave absorber is not particularly limited as long as it absorbs irradiated microwaves, generates heat to a temperature at which the fluororesin can be decomposed, and has the properties of being in a solid state and chemically inactive under the decomposition reaction conditions of the fluororesin. The temperature TR of the microwave absorber heated in the decomposition step establishes temperature conditions for progressing the decomposition reaction of the fluororesin, and corresponds to the temperature in the reaction system of the decomposition reaction of the fluororesin.
[0036] Specific examples of microwave absorbers include metals, metal salts, intermetallic compounds, carbon, carbides, etc., which have the above-mentioned properties. Preferably, the microwave absorber has a density of, for example, 1 to 10 g / cm. 3 , preferably 1.5 to 7 g / cm 3 Preferably, the microwave absorber may be a material having microwave absorption capability with a dielectric loss of, for example, 0.01 to 30, preferably 0.1 to 11.
[0037] More specific examples of microwave absorbers include metals such as single metals like Ni, Pt, Co, and Pt, and alloys like Pt / Cu and Pt / Re. Metal salts include metal oxides, metal hydroxides, metal halides, and silicides. Intermetallic compounds include molybdenum silicide and titanium boride. Carbons include graphite such as expanded graphite, activated carbon, carbon fiber, carbon nanotubes, and carbon black. Carbides include silicon carbide, boron carbide, titanium carbide, and zirconium carbide. These microwave absorbers may be used alone or in combination. Of these microwave absorbers, carbides are preferred, and silicon carbide is more preferred.
[0038] [4-2. Particle size d of microwave absorber] In the present invention, the microwave absorber is preferably used in the form of particles. The particle size of the microwave absorber particles (hereinafter also referred to as "particle size d") is not particularly limited, but may be, for example, 0.1 to 25 mm. Furthermore, when the microwave absorber-containing layer described below is in the form of a fixed bed, the particle size d is preferably 0.1 to 25 mm, more preferably 1 to 25 mm, even more preferably 2.8 to 25 mm, and even more preferably 4.8 to 25 mm, from the viewpoint of further increasing the temperature difference Δ2 (TR-TE) and further improving the selectivity of the constituent monomer of the fluororesin. Furthermore, the upper limit of the range of the particle size d may be 10 mm or less, or 8 mm or less. When the microwave absorber-containing layer described below is in the form of a fluidized bed, the particle size d is preferably 0.5 to 25 mm, more preferably 1 to 25 mm, even more preferably 2 to 10 mm, still more preferably 2.8 to 25 mm, and even more preferably 4.8 to 25 mm, from the viewpoint of further increasing the temperature difference Δ2 (TR-TE) and further improving the selectivity of the constituent monomer of the fluororesin. Furthermore, the upper limit of the range of these particle size d may be 15 mm or less, 10 mm or less, 5 mm or less, 2.5 mm or less, 2 mm or less, or 1.5 mm or less. In the present invention, the particle size d is the average of the measured values obtained by measuring the maximum diameter in a certain direction of 20 randomly selected particles with a gauge. For the gauge measurement, visual observation, an optical microscope, or an electron microscope is used depending on the size of the particles.
[0039] In order to control (i) above, the upper limit of the particle size d of the microwave absorber can be set to preferably 2.5 mm or less, more preferably 2 mm or less, and even more preferably 1.5 mm or less.
[0040] [4-3. Mode of Microwave Absorber-Containing Layer] A more specific mode of the microwave absorber during the decomposition reaction may be either a fixed bed or a fluidized bed.
[0041] The microwave absorber can be prepared in the reaction vessel before the decomposition step in the form of a microwave absorber-containing layer of a mixture containing the microwave absorber and particles of the material containing the fluororesin.
[0042] The microwave absorber-containing layer is provided in the reaction vessel so as to allow passage of the gas flow from the carrier gas inlet to the decomposition gas outlet. Specifically, in the parallel flow type cylindrical reaction vessels 1 and 1a shown in Figures 1 and 2, the microwave absorber-containing layer 2 is provided between the carrier gas inlet and the decomposition gas outlet, and in the continuous tank type reaction vessels 1b and 1c shown in Figures 3 and 4, the microwave absorber-containing layer 2 is provided at the bottom of the reaction vessel.
[0043] The amount of microwave absorber used relative to the amount of particles of the material containing fluororesin is not particularly limited, but may be, for example, 0.1 to 1000 parts by weight, preferably 1 to 100 parts by weight, more preferably 10 to 50 parts by weight, and even more preferably 15 to 45 parts by weight relative to 1 part by weight of particles of the material containing fluororesin.
[0044] The microwave absorber-containing layer 2 has a height h when the contact surface with the gas phase is horizontally leveled in the initial stage (before the decomposition step is started). The height h refers to the height at the central axis CI of the microwave absorber-containing layer 2 (in the embodiments of FIGS. 1 to 4, the central axis CI of the microwave absorber-containing layer 2 coincides with the central axis of the reaction vessels 1, 1a, 1b, and 1c).
[0045] Specific examples of the height h of the microwave absorber-containing layer 2 include, for example, 0.1 to 200 mm, and from the viewpoint of further increasing the temperature difference Δ2 (TR-TE) and further improving the selectivity of the constituent monomer of the fluororesin, the height h is preferably 1 to 100 mm, more preferably 3 to 50 mm, and even more preferably 5 to 30 mm. When the microwave absorber-containing layer 2 is in the form of a fixed bed, the height h is preferably 3 to 50 mm, more preferably 5 to 30 mm, and when it is in the form of a fluidized bed, the height h is preferably 5 to 30 mm.
[0046] Furthermore, when the center of the opening of the outlet 1E of each of the reaction vessels 1, 1a, 1b, and 1c is defined as point Pe, and the intersection point between the central axis CI of the microwave absorber-containing layer 2 and the surface of the microwave absorber-containing layer 2 on the opposite side to the outlet 1E is defined as point Pl, and the height H from point Pl to point Pe is defined as 1, the ratio (h / H) of the height h of the microwave absorber-containing layer 2 to the height H of the microwave absorber-containing layer 2 is, for example, 0.01 to 0.8, and from the viewpoint of further increasing the temperature difference Δ2 (TR-TE) and further improving the selectivity of the constituent monomer of the fluororesin, is preferably 0.01 to 0.5, more preferably 0.05 to 0.4, even more preferably 0.1 to 0.3, and still more preferably 0.15 to 0.25.
[0047] [5. Carrier Gas] [5-1. Examples of Carrier Gas] The carrier gas introduced from the carrier gas inlet of the reaction vessel is not particularly limited as long as it has chemically inert properties under the decomposition reaction conditions of the fluororesin, and examples thereof include water vapor, nitrogen, and rare gases (Xe, Ar, Ne, He, etc.). These carrier gases may be used alone or in combination of two or more. Among these carrier gases, water vapor and nitrogen are preferred.
[0048] [5-2. Carrier Gas Temperature TI at Inlet and Its Setting] In the present invention, the carrier gas temperature TI at the inlet is the temperature at the center of the opening of the inlet 1I (hereinafter also referred to as "point Pi").
[0049] In the present invention, in order to improve the selectivity of the constituent monomer of the fluororesin among the low-molecular-weight fluorine compounds produced, the temperature TI of the carrier gas at the inlet can be set so as to achieve the temperature difference Δ1 (TR-TI) shown in (i) above.
[0050] The temperature difference Δ1(TR-TI) is not particularly limited as long as it is greater than 500°C, but from the viewpoint of further improving the selectivity of the constituent monomers of the fluororesin, it is preferably 530°C or higher, 540°C or higher, 550°C or higher, 570°C or higher, 590°C or higher, or 600°C or higher, more preferably 620°C or higher, 640°C or higher, 660°C or higher, 680°C or higher, 700°C or higher, 720°C or higher, and even more preferably 740°C or higher, 760°C or higher, or 780°C or higher. The upper limit of the temperature difference Δ1(TR-TI) is also not particularly limited, but examples include 1000°C or lower, 900°C or lower, or 800°C or lower.
[0051] In the present invention, when setting (ii), the temperature difference Δ1 (TR-TI) is allowed to be more than 250°C (preferably 300°C or more, more preferably 350°C or more, even more preferably 400°C or more, and even more preferably 450°C or more).
[0052] In the present invention, the value obtained by dividing the temperature difference Δ1(TR-TI) by the temperature TR (°C) is, for example, 0.5 or more, preferably 0.85 or more, more preferably 0.9 or more, even more preferably 0.93 or more, still more preferably 0.94 or more, and even more preferably more than 0.97, and from the viewpoint of further improving the selectivity of the constituent monomer of the fluororesin, is preferably 0.965 or more, more preferably 0.972 or more, and even more preferably 0.976 or more. The upper limit of the value obtained by dividing the temperature difference Δ1(TR-TI) by the temperature TR is not particularly limited, and examples thereof include 0.990 or less, 0.985 or less, and 0.980 or less.
[0053] In order to perform the control of (i) above, the value obtained by dividing the temperature difference Δ1(TR-TI) by the temperature TR (°C) can be set to preferably more than 0.97, more preferably 0.965 or more, even more preferably 0.972 or more, and even more preferably 0.976 or more. In order to control Δ1(TR-TI) to a larger value, this value can be set higher.
[0054] To achieve the control of (ii) above, the temperature difference Δ1 (TR-TI) divided by the temperature TR (°C) can be set to, for example, 0.5 or more, preferably 0.85 or more, more preferably 0.9 or more, even more preferably 0.93 or more, and even more preferably 0.94 or more. Furthermore, it can also be controlled to be greater than 0.97, more preferably 0.965 or more, even more preferably 0.972 or more, and even more preferably 0.976 or more. In order to control Δ2 (TR-TE) to a larger value, this value can be set higher.
[0055] In the present invention, the carrier gas at the inlet may or may not be preheated. That is, in the present invention, a step of preheating the carrier gas may or may not be included. Specific examples of the temperature TI include, for example, 10 to 400°C, preferably 15 to 300°C, and more preferably 20 to 200°C. More specifically, preferred examples of the temperature TI when not preheating include, for example, 10 to 30°C, preferably 13 to 25°C, and even more preferably 15 to 23°C, and preferred examples of the temperature TI when preheating is performed include, for example, 80 to 400°C, preferably 90 to 200°C, and more preferably 100 to 150°C.
[0056] [5-3. Carrier Gas Introduction Rate R] The introduction rate of the carrier gas from the carrier gas inlet (hereinafter also referred to as "introduction rate R") is not particularly limited and may be, for example, 0.005 to 20 m / s. From the viewpoint of further increasing the temperature difference Δ2 (TR-TE) and further improving the selectivity of the constituent monomer of the fluororesin, the introduction rate is preferably 0.007 to 2 m / s, more preferably 0.009 to 0.2 m / s, even more preferably 0.011 to 0.08 m / s, and still more preferably 0.013 to 0.02 m / s.
[0057] [6. Decomposition Reaction] In the decomposition reaction, a microwave absorber is heated by microwave irradiation in a reaction vessel, and the heated microwave absorber is brought into contact with particles of a material containing a fluororesin, thereby decomposing the fluororesin into low-molecular-weight fluorine compounds.
[0058] [6-1. Reaction temperature TR] The temperature TR of the heated microwave absorber may be any temperature at which the fluororesin is decomposed. Specific examples of the temperature TR include 280 to 1500°C, preferably 490 to 1400°C or 530 to 1300°C, more preferably 640 to 1100°C, even more preferably 680 to 1000°C, and even more preferably 760 to 900°C. The microwave irradiation conditions (wavelength and frequency) for heating the microwave absorber may be appropriately set according to the above-mentioned temperature TR.
[0059] In order to perform the control of (i) above, the temperature TR of the heated microwave absorber can be set preferably to 490 to 1400°C, or 530 to 1300°C, more preferably to 640 to 1100°C, even more preferably to 680 to 1000°C, and still more preferably to 760 to 900°C, and further, in order to control Δ1(TR-TI) to be larger, the temperature TR can be set higher.
[0060] The temperature TR is the temperature measured at the center position in the height h direction of the microwave absorber-containing layer from the side of the reaction vessel in an insulated state. The reaction vessel is insulated when measuring the temperature TR by surrounding the reaction vessel with ceramic wool to a thickness of 20% of the maximum outer periphery width of the reaction vessel. An optical fiber thermometer or a non-contact thermometer can be used for temperature measurement. Note that the insulation method constitutes the measurement conditions for the temperature TR specified in the present invention, and the manufacturing method of the present invention is not limited to a form in which the insulation method is used.
[0061] [6-2. Temperature TE of the produced gas at the outlet and its setting] The low-molecular-weight fluorine compound produced by the decomposition reaction of the fluororesin is discharged as a gas (produced gas) to the outside of the reaction vessel through the outlet 1E. In the present invention, the temperature TE of the produced gas at the outlet is the temperature at the center of the opening of the outlet 1E (hereinafter also referred to as "point Pe"). Furthermore, the temperature TE in the present invention is the temperature at the time when the decomposition gas (produced gas) that has passed through the microwave absorber-containing layer reaches point Pe of the decomposition gas outlet of the reaction vessel without being cooled using a quenching method. Here, the quenching method refers to a method of cooling the decomposition gas to a temperature lower than that in the case of natural cooling (i.e., the temperature at the time when the decomposition gas that has passed through the microwave absorber-containing layer is naturally cooled before reaching the decomposition gas outlet of the reaction vessel and reaches the decomposition gas outlet). Specific methods are known in the technical field, and examples thereof include a method of expanding the decomposition gas (produced gas), a method of cooling using a separately prepared cooling gas, and a method of cooling using a cooling liquid.
[0062] In the present invention, in order to improve the selectivity of the constituent monomer of the fluororesin from among the low-molecular-weight fluorine compounds produced, the temperature TE of the produced gas at the outlet can be set so as to achieve the temperature difference Δ2 (TR-TE) shown in (ii) above.
[0063] The temperature difference Δ2(TR-TE) is not particularly limited as long as it is 300°C or higher, but from the viewpoint of further improving the selectivity of the constituent monomers of the fluororesin, it is preferably 400°C or higher, more preferably 460°C or higher, 480°C or higher, 500°C or higher, 520°C or higher, 540°C or higher, 560°C or higher, 580°C or higher, or 600°C or higher, even more preferably 610°C or higher, 630°C or higher, 650°C or higher, 670°C or higher, 690°C or higher, or 710°C or higher, and even more preferably 730°C or higher, 750°C or higher, or 770°C or higher. The upper limit of the temperature difference Δ2(TR-TE) is not particularly limited either, and examples include 1000°C or lower, 900°C or lower, or 850°C or lower.
[0064] In order to perform the control of (i) above, Δ2(TR-TE) can be set to preferably 460°C or higher, 480°C or higher, 500°C or higher, 520°C or higher, 540°C or higher, 560°C or higher, 580°C or higher, or 600°C or higher, more preferably 610°C or higher, 630°C or higher, 650°C or higher, 670°C or higher, 690°C or higher, or 710°C or higher, and even more preferably 730°C or higher, 750°C or higher, or 770°C or higher. In addition, in order to control Δ1(TR-TI) to a larger value, Δ2(TR-TE) can be set to a larger value.
[0065] Specific examples of the temperature TE include, for example, 20° C. or higher and lower than 250° C. The upper limit of the temperature range (20° C. or higher and lower than 250° C.) is preferably 200° C. or lower, more preferably 150° C. or lower, even more preferably 100° C. or lower, and even more preferably 90° C. or lower, 85° C. or lower, or 80° C. or lower, and the lower limit can be 30° C. or higher, 40° C. or higher, 50° C. or higher, 55° C. or higher, 60° C. or higher, 65° C. or higher, 70° C. or higher, or 75° C. or higher.
[0066] In order to perform the control (i) above, the temperature TE can be set preferably to 50°C or higher, 55°C or higher, 60°C or higher, 65°C or higher, 70°C or higher, or 75°C or higher, and the temperature TE can be set higher in order to control Δ1(TR-TI) to a larger value.
[0067] [6-3. Decomposition Products] The low molecular weight fluorine compounds that are products of the decomposition reaction are compounds that are generated from the raw material fluororesin and have lower molecular weights than the fluororesin, and usually contain a plurality of compounds. According to the present invention, the selectivity of the constituent monomers of the fluororesin among the low molecular weight fluorine compounds generated is high (i.e., the proportion of the constituent monomers of the fluororesin in the low molecular weight fluorine compounds generated is high).
[0068] Among the low molecular weight fluorine compounds produced, the constituent monomers of the target fluorine resin are determined depending on the polymer structure of the raw material fluorine resin. Specifically, the constituent monomers of the fluorine resin are those represented by the general formula CF2=CF-R d f [In the formula, R df represents F or a perfluoroalkyl group having 1 to 10, preferably 1 to 5, carbon atoms. Preferred examples include tetrafluoroethylene (TFE) and hexafluoropropylene (HFP). Other specific examples of fluoroolefins include vinylidene fluoride (VDF), chlorotrifluoroethylene (CTFE), perfluorovinyl ether, and perfluoroallyl ether.
[0069] Of the low-molecular-weight fluorine compounds produced, compounds other than the constituent monomers of the fluororesin include polymers with a low degree of polymerization that have not decomposed to the constituent monomers of the above-mentioned fluororesin (dimers, trimers, or oligomers with a higher degree of polymerization that are gaseous at temperature TE), and by-products (e.g., octafluorocyclobutane) and other by-products that are produced by further side reactions of the constituent monomers of the above-mentioned fluororesin.
[0070] The product, low molecular weight fluorine compound (product gas), is discharged by the airflow from the outlet of the reaction vessel and recovered by appropriately cooling and / or concentrating the product gas.
[0071] During the decomposition step, the material containing the fluororesin may not be additionally supplied (i.e., it may be a batch process), or the fluororesin may be additionally supplied continuously or intermittently.
[0072] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0073] A continuous-tank type reactor 1b shown in Figure 3 was prepared. A microwave absorber-containing layer 2 containing a microwave absorber having a predetermined particle size d and particles of a material containing a fluororesin (PTFE, i.e., a homopolymer of tetrafluoroethylene) was provided in the cylindrical reactor 1b at a predetermined height h (cm). The size of the particles of the fluororesin-containing material was 20 µm, and the amount of microwave absorber used per part by weight of the particles of the fluororesin-containing material was 20 to 40 parts by weight.
[0074] Carrier gas (nitrogen) 3 was introduced from inlet 1I at a predetermined carrier gas temperature TI and a predetermined introduction rate R. While stirring with a stirrer (not shown), the microwave absorber in microwave absorber-containing layer 2 was heated to a predetermined temperature TR using a microwave generator (not shown). The temperature TE at outlet 1E (specifically, point Pe, the center of the opening of outlet 1E) of the generated gas was measured. The temperature TR was measured using a non-contact thermometer at the center of the height h of microwave absorber-containing layer 2 from the side of the reactor, with the reactor insulated by surrounding the outer periphery of the reactor with ceramic wool to a thickness of 20% of the outer diameter of the reactor. The generated gas was recovered from outlet 1E, and the mass fractions of the three main components were calculated from the composition analysis results. The set conditions and the composition analysis results of the generated gas are shown in Table 1.
[0075]
[0076] As shown in Table 1, in Examples 1 to 3, it was confirmed that the ratio of by-products (HFP, C318) among the low-molecular-weight fluorine compounds produced was extremely low, and the selectivity of the constituent monomer (TFE) of the fluororesin (TFE homopolymer) was extremely high. The constituent components of the produced gas consisted of TFE, HFP, C138, and other products, and in all of Examples 1 to 3, TFE, HFP, and C138 accounted for approximately 95% or more of the area value of the gas chromatograph (detector FID: Flame Ionization Detector). It was also confirmed that the proportion of the remaining products in the produced gas was similar between Examples 1 to 3.
[0077] 1, 1a, 1b, 1c Reaction vessel 1I Carrier gas inlet TI Carrier gas temperature at inlet 1I Pi Opening center of inlet 1I 1E Carrier gas outlet TE Temperature of generated gas at outlet 1E Pe Opening center of outlet 1E 2 Microwave absorber-containing layer CI Central axis of microwave absorber-containing layer 2 Pl Intersection point between central axis CI and the surface of microwave absorber-containing layer 2 opposite to outlet 1E TR Temperature of heated microwave absorber 3 Carrier gas H Height from point Pl to point Pe h Height of microwave absorber-containing layer 2
Claims
1. A method for producing a low molecular weight fluorine compound, comprising a decomposition step of heating a microwave absorber by microwave irradiation in a reaction vessel provided with a carrier gas inlet and a decomposition gas outlet, and decomposing the fluororesin into a low molecular weight fluorine compound by contacting the heated microwave absorber with a material containing a fluororesin, wherein (i) a temperature difference Δ1 (TR-TI) obtained by subtracting the carrier gas temperature TI (°C) at the inlet from the temperature TR (°C) of the heated microwave absorber is set to exceed 500°C.
2. A method for producing a low molecular weight fluorine compound, comprising: a decomposition step of heating a microwave absorber by microwave irradiation in a reaction vessel provided with a carrier gas inlet and a decomposition gas outlet, and decomposing the fluororesin into a low molecular weight fluorine compound by contacting the heated microwave absorber with a material containing a fluororesin; (ii) setting a temperature difference Δ2 (TR-TE) obtained by subtracting the temperature TE (°C) of the generated gas at the outlet discharged from the reaction vessel from the temperature TR (°C) of the heated microwave absorber so as to be 300°C or more.
3. The method according to claim 1 or 2, wherein the introduction speed R of the carrier gas from the inlet is 0.005 to 20 m / s.
4. The method according to claim 1 or 2, wherein the temperature TE (°C) of the generated gas discharged from the reaction vessel at the outlet is 20°C or higher and lower than 250°C.
5. The method according to claim 1 or 2, wherein the microwave absorber is prepared in the form of a microwave absorber-containing layer which contains particles of a material containing the microwave absorber and the fluororesin and is provided so as to pass an airflow from the carrier gas inlet to the decomposition gas outlet, and wherein, when the center of the opening of the outlet is defined as point Pe and the intersection point between the central axis of the microwave absorber-containing layer and a surface of the microwave absorber-containing layer opposite to the outlet is defined as point Pl, a ratio h / H of a height h of the microwave absorber-containing layer to a height H from point Pl to point Pe is 0.01 to 0.
8.
6. The method according to claim 1 or 2, wherein the particle diameter d of the microwave absorber is 0.1 to 25 mm.
7. The method according to claim 5, wherein the height h of the microwave absorber-containing layer is 0.1 to 200 mm.
8. The manufacturing method according to claim 2, wherein a temperature difference Δ1 (TR-TI) obtained by subtracting a carrier gas temperature TI (°C) at the inlet from a temperature TR (°C) of the heated microwave absorber is set to be greater than 250°C.
Citation Information
Patent Citations
Chemically recycling method
JP2004346000A
Production process of fluoroolefins by thermal decomposition of fluorinated materials
JP2012504633A
Method and apparatus for decomposing organic halogen compound
JP2013202314A
Chemical reaction device and chemical reaction method
JP2015142904A
Method for producing fluoroolefins by pyrolysis of fluorinated ionomers