Preparation method for active layer containing volatile solid additive and use thereof in organic photovoltaics

By using 1,3,5-tribromobenzene (TBr) to form an active layer with electron donor and acceptor powder, the problem of limited application of existing volatile solid additives in organic solar cells is solved, and the structure is simple and cost-effective Low-cost additives with good volatile properties significantly improve device performance and stability.

WO2024227303A1PCT designated stage expired Publication Date: 2024-11-07CHANGZHOU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/093565
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-30
Filing Date
2023-05-11
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

The existing volatile solid additives are used in organic solar cells due to their complex structure, high cost, poor volatile characteristics and weak intermolecular forces, resulting in unstable and unpredictable device performance, which limits their polymer/small molecules. Application in blended systems.

Method used

1,3,5-tribromobenzene (TBr) is used as a process additive solution, combined with electron donor and acceptor powder, and the active layer is formed by spin coating and annealing treatment, morphology of the photoactive layer is regulated, and the intermolecular action force is improved. and universality.

Benefits of technology

It realizes volatile solid additives with simple structure, low cost and good volatile characteristics, significantly improves the performance and stability of organic solar cells, has the advantages of economical and efficient, and can significantly improve the overall stability and universality of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023093565_07112024_PF_FP_ABST
    Figure CN2023093565_07112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a preparation method for an active layer containing a volatile solid additive and the use thereof in organic photovoltaics. The preparation method comprises the following steps: preparing a process additive solution; adding electron donor powder and electron acceptor powder to the process additive solution to form an active layer solution; and spin-coating an anode interface layer with the active layer solution to form a film, and then performing annealing treatment on same for 10min to obtain an active layer, the process additive being selected from 1,3,5-tribromobenzene (TBr). The process additive used by the present invention has a low price and easily adjustable and controllable morphology, can achieve performance improvement of solar cells, and has the advantages of economy and high efficiency. The obtained product can be used for organic photovoltaic materials and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

A method for preparing an active layer of a volatile solid additive and its organic photovoltaic application Technical Field

[0001] The present invention relates to the field of solar cells, in particular to a preparation method of a volatile solid additive active layer and application thereof. Background Art

[0002] Organic solar cells (OSCs) have become an attractive energy technology due to their simple structure, lightweight, and ability to be fabricated into flexible devices through layer-by-layer solution processing. In recent years, efforts have focused on designing narrow-bandgap non-fullerene acceptors to overcome the inherent limitations of fullerene acceptors. These efforts, along with the development of polymer donors, have boosted the power conversion efficiency (PCE) of organic solar cells to as high as 20% of single-junction devices, demonstrating their promising potential for practical applications. Most highly efficient non-fullerene OSCs are achieved with the aid of solvent additives, such as 1-chloronaphthalene (CN) or 1,8-diiodooctane (DIO). Due to their high boiling points, these additives are difficult to remove from the active layer, resulting in poor device performance reproducibility and stability, hindering the industrial application of organic solar cells. In recent years, researchers have developed volatile solid additives to circumvent these issues. However, these reported volatile solid additives are generally only applicable to polymer donor:small molecule acceptor systems and are not applicable to other polymer / small molecule blends, limiting their application. Analysis revealed that the primary reason for this is the weak interaction between solid additives and donors / acceptors, resulting in the reported solid additive materials being non-universal. Furthermore, the majority of currently developed volatile solids are large, conjugated, fused-ring molecules with complex structures, resulting in high preparation costs and poor volatility properties.

[0003] Therefore, there is a need for a volatile solid material with a simple structure, good volatility characteristics, strong intermolecular forces, and universal performance to make up for the defects of existing volatile solid additive technology.

[0004] Summary of the Invention

[0005] The purpose of this section is to summarize some aspects of the embodiments of the present application and to briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the abstract of the specification and the application title of this application to avoid blurring the purpose of this section, the abstract of the specification and the application title, and such simplifications or omissions cannot be used to limit the scope of this application.

[0006] In view of the above problems and / or the problems existing in the prior art, this application is proposed.

[0007] Therefore, the technical problem to be solved by this application is to screen a class of volatile solid additives with simple structure, low cost, good volatility characteristics, and strong intermolecular forces to significantly improve device performance and universality.

[0008] To solve the above technical problems, the present application provides the following technical solution: a method for regulating the morphology of a photoactive layer, comprising the following steps:

[0009] Prepare process additive solution;

[0010] adding electron donor powder and electron acceptor powder into a process additive solution to form an active layer solution;

[0011] The active layer solution was spin-coated on the anode interface layer to form a film, and then annealed for 10 minutes to obtain the active layer;

[0012] The process aid solution is 1,3,5-tribromobenzene (TBr) solution, and the molecular structure is:

[0013] As a preferred solution of the method for regulating the morphology of the photoactive layer described in the present application, the concentration of TBr in the process aid solution is 10-30 mg / ml.

[0014] As a preferred solution of the method for regulating the morphology of the photoactive layer described in this application, the temperature of the annealing treatment in step S3 is 75-120°C.

[0015] As a preferred embodiment of the method for regulating the morphology of the photoactive layer described in the present application, the electron acceptor is a small molecule or polymer having a dithienothiophene[3.2-b]pyrrolothiadiazole (BTP) core:

[0016] The electron donor is a PM6 polymer donor or a BTR-Cl small molecule donor. The structural formulas of PM6 and BTR-Cl are as follows:

[0017] Another object of the present invention is to provide a face-up polymer solar cell, which includes an anode conductive layer, an anode interface layer, an active layer, an electron transport layer, an anode and interface layer, a cathode interface layer and a metal electrode, and the active layer is prepared by the above method.

[0018] As a preferred solution of the face-up polymer solar cell described in the present application, wherein: the thickness of the anode interface layer is 20-30 nm; and the material of the anode interface layer is PEDOT:PSS.

[0019] As a preferred solution of the face-up polymer solar cell described in the present application, the thickness of the cathode interface layer is 5-20 nm, and the material of the cathode interface layer is PDINN.

[0020] As a preferred solution of the face-up polymer solar cell described in the present application, the metal electrode is Ag, and the thickness of the metal electrode is 100 nm.

[0021] Another object of the present invention is to provide a method for preparing a face-up polymer solar cell, comprising the following steps:

[0022] Step 1: Spin-coating a dispersion of an anode interface layer material on the surface of an anode ITO substrate to form an anode interface layer;

[0023] Step 2, spin-coating an active layer solution composed of TBr, an electron donor and an electron acceptor on the surface of the anode interface layer away from the anode ITO substrate to form a photoactive layer;

[0024] Step 3, spin coating a dispersion of a cathode interface layer material on a surface of the photoactive layer away from the anode interface layer to form a cathode interface layer;

[0025] Step 4: Under vacuum conditions, evaporate Ag on the surface of the cathode interface layer away from the photoactive layer to form a metal electrode.

[0026] As a preferred solution of the method for preparing a face-up polymer solar cell described in the present application, wherein: in the step 1, the anode ITO substrate is pretreated, and the pretreatment includes: cleaning, drying and UVO treatment.

[0027] The beneficial effects of the present application are as follows: the process additives used in the present invention are inexpensive, easy to control the morphology, can achieve performance improvement of solar cells, have the advantages of economy, high efficiency and stable performance, can significantly improve the stability of the overall device, and can be stored longer than devices not doped with TBr. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] To more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present application. Those skilled in the art can also derive other drawings based on these drawings without inventive effort. Among them:

[0029] FIG1 is a characteristic curve of current density and voltage of a solar cell prepared by doping with an electron donor PM6, an electron acceptor Y6 and a volatile solid additive TBr in Example 1 of the present application;

[0030] FIG2 is a characteristic curve of current density and voltage of a solar cell prepared by doping with an electron donor PM6, an electron acceptor L8-BO and a volatile solid additive TBr in Example 5 of the present application;

[0031] FIG3 is a characteristic curve of current density and voltage of a solar cell prepared by doping with an electron donor PM6, an electron acceptor PY-IT and a volatile solid additive TBr in Example 6 of the present application;

[0032] FIG4 is a characteristic curve of current density and voltage of a solar cell prepared by doping with an electron donor BTR-Cl, an electron acceptor Y6, and a volatile solid additive TBr in Example 1 of the present application;

[0033] 5 is a characteristic curve of current density and voltage of a solar cell prepared by doping with an electron donor BTR-Cl, an electron acceptor PY-IT, and a volatile solid additive TBr in Example 1 of the present application;

[0034] FIG6 is a Y6 absorption curve before and after TBr incorporation;

[0035] FIG7 is a PY-IT absorption curve before and after TBr incorporation;

[0036] FIG8 is a thermogravimetric curve of TBr;

[0037] FIG9 is an absorption spectrum curve of TBr. DETAILED DESCRIPTION

[0038] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the drawings in the specification.

[0039] In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application may also be implemented in other ways different from those described herein. Those skilled in the art may make similar generalizations without violating the connotation of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.

[0040] Secondly, this application is described in detail with reference to schematic diagrams. When describing the embodiments of this application, for ease of explanation, cross-sectional views of device structures may be partially enlarged and not to scale. Furthermore, these schematic diagrams are merely illustrative and should not limit the scope of protection of this application. Furthermore, in actual production, three-dimensional dimensions, including length, width, and depth, should be included.

[0041] Furthermore, the term "one embodiment" or "embodiment" herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present application. The phrase "in one embodiment" appearing in various places throughout this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0042] Example 1

[0043] The present invention provides a front-mounted polymer solar cell, which is manufactured by the following steps:

[0044] The glass substrate with the ITO conductive layer was ultrasonically treated with detergent water, deionized water, acetone, and isopropyl alcohol for 15 minutes each, then dried in an 80°C oven, and then subjected to ozone plasma surface treatment for 15 minutes;

[0045] The PEDOT:PSS solution was spin-coated on the treated surface of the ITO conductive layer at a spin-coating speed of 4800 rpm for 30 seconds, and then annealed at 150°C for 30 minutes to form an anode interface layer with a thickness of 20 to 30 nm.

[0046] Dissolve TBr in chloroform to prepare a TBr solution with a concentration of 10 mg / ml;

[0047] A PM6:Y6 mixed powder with a mass ratio of 1:1 was added to the TBr solution to form a blended active layer solution with a PM6:Y6 mixed powder concentration of 18 mg / ml;

[0048] The blended active layer solution was spin-coated on the surface of the ITO / PEDOT:PSS anode interface layer at a speed of 3000 rpm and annealed at room temperature for 10 min to obtain the target organic solar cell active layer;

[0049] PDINN was dissolved in methanol to obtain a 1 mg / ml PDINN solution. The PDINN solution was spin-coated on the surface of the active layer. Then, a layer of silver was evaporated on the PDINN surface by vacuum evaporation with a thickness of 100 nm and an evaporation area of ​​0.06 cm. 2 , and obtain the finished product upright polymer solar cell.

[0050] Among them, the molecular structures of TBr, PM6 and Y6 are:

[0051] Example 2

[0052] The difference between Example 2 and Example 1 is that in Example 2, the concentration of the TBr solution is adjusted to 15 mg / ml, and the other steps are the same as those in Example 1.

[0053] Example 3

[0054] The difference between Example 2 and Example 1 is that in Example 2, the concentration of the TBr solution is adjusted to 20 mg / ml, and the other steps are the same as those in Example 1.

[0055] Example 4

[0056] The difference between Example 4 and Example 1 is that in Example 5, Y6 is replaced by L8-BO, and the other steps are the same as in Example 1.

[0057] Among them, the molecular structures of TBr, PM6 and L8-BO are:

[0058] Example 5

[0059] The difference between Example 5 and Example 2 is that in Example 5, the electron acceptor is changed from Y6 to PY-IT, and the other steps are the same as those in Example 2.

[0060] Among them, the molecular structures of TBr, PM6 and PY-IT are:

[0061] Example 6

[0062] The difference between Example 6 and Example 2 is that in Example 6, the electron donor is changed from PM6 to BTR-Cl, and the other steps are the same as in Example 2.

[0063] Among them, the molecular structures of TBr, BTR-Cl and Y6 are:

[0064] Example 7

[0065] The difference between Example 7 and Example 2 is that in Example 7, the electron donor is changed from PM6 to BTR-Cl, and the electron acceptor is changed from Y6 to PY-IT. The other steps are the same as in Example 2.

[0066] Comparative Example 1

[0067] Comparative Example 1 provides a front-mounted polymer solar cell. The difference between Comparative Example 1 and Example 2 is that TBr is not added in Comparative Example 1.

[0068] Comparative Example 2

[0069] Comparative Example 2 provides a front-mounted polymer solar cell. The difference between Comparative Example 1 and Example 4 is that TBr is not added in Comparative Example 2.

[0070] Comparative Example 3

[0071] Comparative Example 3 provides a front-mounted polymer solar cell. The difference between Comparative Example 1 and Example 5 is that TBr is not added in Comparative Example 3.

[0072] Comparative Example 4

[0073] Comparative Example 4 provides a front-mounted polymer solar cell. The difference between Comparative Example 2 and Example 6 is that TBr is not added in Comparative Example 4.

[0074] Comparative Example 5

[0075] Comparative Example 5 provides a front-mounted polymer solar cell. The difference between Comparative Example 3 and Example 7 is that TBr is not added in Comparative Example 5.

[0076] Battery performance parameter test

[0077] (1) The performance of the upright polymer solar cells adjusted with different TBr solution concentrations was tested using the Oriel-300 solar simulator from Newport, USA. The test results are shown in Table 1:

[0078] Table 1 Battery performance test results

[0079] Results Analysis: Comparing the data reveals that changes in TBr concentration correlate with changes in the battery's performance parameters, demonstrating that TBr doping in the active layer affects battery performance. While each parameter exhibits advantages and disadvantages at different TBr concentrations, the battery exhibits optimal overall performance at a TBr concentration of 15 mg / ml, making Example 2 the preferred choice.

[0080] (2) The performance of the upright polymer solar cells prepared in Examples 2, 4, 5, 6, 7 and Comparative Examples 1-5 was tested using an Oriel-300 solar simulator from Newport, USA. The test results are shown below:

[0081] Results Analysis: Comparing the test results of Examples 2, 4, and 5, the battery performance improved to varying degrees when using Y6, L8-BO, and PY-IT as the electron acceptor, respectively. The best performance was achieved when using Y6 as the electron acceptor. This demonstrates the wide applicability of TBr and suggests its potential application in future developments of novel electron acceptors to enhance overall device performance.

[0082] In addition, Example 5 is compared with Comparative Example 3, Example 6 is compared with Comparative Example 4, and Example 7 is compared with Comparative Example 5. It can be demonstrated that when TBr is added to the active layer, the overall performance of the battery can be improved.

[0083] 1-3 , when the battery is doped with TBr, its current density and fill factor are significantly higher than those of the battery without TBr doping, further proving that doping the active layer with TBr improves battery performance.

[0084] As can be seen from Figures 8 and 9, the solar cell active layer treated with 1,3,5-tribromobenzene (TBr) has a higher thermal decomposition temperature and better thermal stability.

[0085] In the field of organic solar cells, the majority of currently used acceptors are based on thiophene[3.2-b]pyrrolothiadiazole (BTP) cores, with Y6 being a representative example of the BTP family. Research has revealed that the unique three-dimensional π-π molecular stacking of Y6, particularly the densely packed central BTP core, significantly promotes strong intermolecular electron and exciton coupling and delocalization, improving exciton dissociation efficiency and reducing non-radiative energy loss. This property suggests that the BTP core plays a crucial role in regulating the aggregate structure and subsequent carrier transport of BTP-based molecules. Halogen bonds, a strong non-covalent force, can form significant electron push-pull and orbital coupling interactions with adjacent lone-pair N, S, and O atoms, enabling precise control of the chemical and physical properties of materials and molecules. Halogen bonding has been widely applied in perovskite optoelectronics, successfully regulating perovskite nucleation, crystal growth, and other film formation dynamics.

[0086] Inspired by this, the BTP-series small molecule derivatives currently used all contain atoms such as N, O, and S. If this intermolecular force is used to achieve fine control of the molecular aggregation state within the active layer and the corresponding cross-scale evolution of the morphology, the device performance of organic solar cells will be greatly improved.

[0087] This application utilizes the strong halogen bond interaction between TBr and BTP core. The relevant interaction can be confirmed in the FT-IR spectrum (Figure 6). The -CH2- peak of the BTP core is from 2930.1cm -1 Move to 2929.3cm -1

[0088] The volatile solid additive used in the present invention is cheap (1 gram: 10-20 RMB), easy to control the morphology, can achieve the performance improvement of solar cells, and has the advantages of economy and high efficiency.

[0089] As shown in Figure 4, the volatile solid additive provided by the present invention is universally applicable to the Y6 small molecule donor-acceptor system. Therefore, the method provided by the present invention has good practicality and is compatible with the actual solar cell industry.

[0090] As shown in Figures 8 and 9, the solar cell provided by the present invention can significantly improve the stability of the entire device and can be stored for a longer time than a device not doped with TBr.

[0091] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present application and are not intended to limit the present application. Although the present application has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present application, and all of these should be included in the scope of the claims of the present application.

Claims

1. A method for preparing an active layer of a volatile solid additive, characterized in that: The following steps are involved: Prepare process additive solution; adding electron donor powder and electron acceptor powder into a process additive solution to form an active layer solution; After the active layer solution is spin-coated on the anode interface layer to form a film, an annealing treatment is performed to obtain an active layer; The process aid is 1,3,5-tribromobenzene, and the molecular structure is:

2. The preparation method according to claim 1, characterized in that: The concentration of 1,3,5-tribromobenzene in the process aid solution is 10-30 mg / ml.

3. The preparation method according to claim 1 or 2, characterized in that: The annealing treatment temperature is 75-120° C., and the treatment time is 5 minutes.

4. The preparation method according to claim 3, characterized in that: The electron acceptor is a small molecule or polymer having a dithienothiophene [3.2-b] pyrrolothiadiazole core, including one of Y6, L8-BO, and PY-IT. The structural formulas of Y6, L8-BO, and PY-IT are as follows: The electron donor is a PM6 polymer donor or a BTR-Cl small molecule donor. The structural formulas of PM6 and BTR-Cl are as follows:

5. An application of an active layer prepared by the preparation method according to claim 1 in organic photovoltaics, characterized in that: The active layer can be used to prepare a front-mounted polymer solar cell, which comprises an anode conductive layer, an anode interface layer, an active layer, a cathode interface layer and a metal electrode.

6. The use according to claim 5, characterized in that: The thickness of the anode interface layer is 20-30 nm; the material of the anode interface layer is PEDOT:PSS.

7. The use according to claim 5 or 6, characterized in that: The thickness of the cathode interface layer is 5-20 nm, and the material of the cathode interface layer is PDINN.

8. The use according to claim 7, characterized in that: The metal electrode is Ag, and the thickness of the metal electrode is 100 nm.

9. The use according to claim 8, characterized in that: The method for preparing the metal electrode comprises the following steps: Pre-treating the anode ITO substrate and spin-coating a dispersion of the anode interface layer material to form an anode interface layer; Spin coating an active layer solution composed of TBr, an electron donor and an electron acceptor on the surface of the anode interface layer away from the anode ITO substrate to form a photoactive layer; Spin coating a dispersion of a cathode interface layer material on a surface of the photoactive layer away from the anode interface layer to form a cathode interface layer; Under vacuum conditions, Ag is evaporated on a surface of the cathode interface layer away from the photoactive layer to form a metal electrode.

10. The use according to claim 9, characterized in that: The pretreatment of the anode ITO substrate includes cleaning, drying and UVO treatment.

Citation Information

Patent Citations

  • Method for regulating and controlling morphology of optical active layer and solar cell applying method

    CN114497386A

  • Photovoltaic element

    JP2013191794A

  • Electroluminescent device

    US20060051611A1