Sodium ferric phosphate pyrophosphate-modified carbon composite material as well as preparation method and application thereof
By using boron-phosphorus double-doped modified carbon coating in sodium ferric pyrophosphate material, the problem of low conductivity of Na3Fe2(PO4)(P2O7) material is solved, and higher conductivity and cyclic stability are achieved , expanding the application scenarios of sodium ion batteries.
Patent Information
- Application Number
- CN202410970781.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The conductivity of Na3Fe2(PO4)(P2O7) material is low, resulting in poor cycling stability and rate performance in sodium ion batteries. The existing carbon coating methods have problems of insufficient agglomeration and affinity.
Boron-phosphorus double-doped modified carbon cladding layer is used to double-doplate in the form of coupling agent by adding boron and phosphorus sources to sodium ferric pyrophosphate material, thereby improving the binding force and conduction of the cladding layer to the core layer. , forming a B/P pair to enhance electron conduction.
The conductive and rate-based properties of the composite material are significantly improved, and cycle stability is enhanced, allowing it to show better electrochemical properties in sodium ion batteries.
Smart Images

Figure CN118943320A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sodium ion batteries, and in particular to a sodium iron phosphate pyrophosphate-modified carbon composite material and a preparation method and application thereof. Background Art
[0002] Na 3 Fe 2 (PO 4 )(P 2 O 7 ) crystal framework is a typical orthorhombic structure, consisting of [Fe 3 P 2 O 13 ] and [P 2 O 7 ] groups, forming a large tunnel along the b axis. 4 -P 2 O 7 The open framework constructed by the mixed polyanion units has a small lattice distortion during the sodium ion insertion and extraction process, so the electrochemical properties of the material show excellent cycle stability and thermal stability. At the same time, the material has low preparation cost, is safe and non-toxic, and has good cycle performance, which has attracted the attention of many researchers.
[0003] However, the theoretical specific capacity of this material is not high and its electronic conductivity is poor. It must be coated with a material with good conductivity to improve its conductivity and charge-discharge specific capacity. 3 Fe 2 (PO 4 )(P 2 O 7 ) materials to improve their electrical conductivity, organic carbon is usually used as a carbon source to coat Na 3 Fe 2 (PO 4 )(P 2 O 7 ) materials, such as glucose, sucrose, starch, phenolic resin, etc. These carbon sources are relatively cheap and have a better effect on improving conductivity, which can help improve the low electronic conductivity problem that is common in polyanion cathode materials.
[0004] However, carbon layer coating inevitably has carbon source agglomeration during the early processing and sintering process, which affects the coating effect. If the carbon source and raw materials are not fully mixed during the early processing, the unmixed carbon source will spontaneously agglomerate, making the coating effect worse. 3 Fe 2 (PO 4 )(P 2 O 7) and the structural stability of carbon materials will also affect the carbon layer and Na 3 Fe 2 (PO 4 )(P 2 O 7 ) is not sufficiently affinity to the main body, and is easily detached during the subsequent gas-powder process, resulting in a decrease in the coating effect and poor electrochemical performance. 3 Fe 2 (PO 4 )(P 2 O 7 ) As a mixed polyanion material, its sintering temperature is generally not high, and there are still some functional groups in the carbon material that affect the conductivity, thereby affecting the Na 3 Fe 2 (PO 4 )(P 2 O 7 ) rate performance.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] One of the objects of the present invention is to provide a composite material of sodium iron pyrophosphate-modified carbon to solve at least one of the above-mentioned technical problems.
[0007] The second object of the present invention is to provide a method for preparing a composite material of sodium iron pyrophosphate-modified carbon.
[0008] The third object of the present invention is to provide an application of a composite material of sodium iron pyrophosphate-modified carbon.
[0009] In order to solve the above technical problems, the present invention particularly adopts the following technical solutions:
[0010] A first aspect of the present invention provides a sodium ferric phosphate pyrophosphate-modified carbon composite material, the composite material comprising a core layer and a coating layer, the core layer is made of sodium ferric phosphate pyrophosphate, and the coating layer is a modified carbon coating layer.
[0011] The chemical formula of the sodium ferric phosphate pyrophosphate is Na 3 Fe 2 (PO 4 )(P 2 O 7 ).
[0012] The material of the modified carbon coating layer is boron-phosphorus dual-doped modified carbon.
[0013] Furthermore, the coating layer has a thickness of 2nm to 50nm.
[0014] Furthermore, the content of boron in the composite material is 0.1 wt.% to 5 wt.%.
[0015] The content of phosphorus in the composite material is 0.1wt.% to 5wt.%.
[0016] The second aspect of the present invention provides a method for preparing the composite material, which comprises adding a carbon source, a boron source and a phosphorus source to a raw material aqueous solution for preparing sodium ferric phosphate pyrophosphate, mixing them evenly, and then sand-milling, spray-drying, pre-burning and calcining to obtain the composite material;
[0017] At least one of the boron source and the phosphorus source is in the form of a coupling agent.
[0018] Further, the boron-containing coupling agent includes a borate coupling agent.
[0019] or,
[0020] The boron-containing non-coupling agent includes at least one of boric acid, borax and boron trioxide.
[0021] Furthermore, the phosphorus-containing coupling agent includes a phosphate coupling agent.
[0022] or,
[0023] Phosphorus-containing non-couplers include sodium phytate.
[0024] The carbon source comprises at least one of sucrose, glucose, starch, cyclodextrin, ascorbic acid, polyethylene glycol and citric acid.
[0025] The added amount of the carbon source is 3wt.%-20wt.% of the total mass of the sodium ferric pyrophosphate, the carbon source, the boron source and the phosphorus source.
[0026] The added amount of the boron source is 0.1wt.%-5wt.% of the total mass of the sodium ferric pyrophosphate, the carbon source, the boron source and the phosphorus source.
[0027] The added amount of the phosphorus source is 0.1wt.%-5wt.% of the total mass of the sodium ferric pyrophosphate, the carbon source, the boron source and the phosphorus source.
[0028] Furthermore, the sand grinding is performed using a sand grinder.
[0029] The rotation speed of the sand mill is 1500 rpm to 3500 rpm, and the time is 0.5 h to 2 h.
[0030] Furthermore, the pre-burning temperature is 150-350°C and the time is 1h-4h.
[0031] The calcination temperature is 400-600°C, and the calcination time is 3h-8h.
[0032] The third aspect of the present invention provides the use of the above-mentioned sodium iron pyrophosphate-modified carbon composite material in the positive electrode material of a sodium ion battery.
[0033] Compared with the prior art, the present invention has at least the following beneficial effects:
[0034] The composite material of sodium iron phosphate pyrophosphate-modified carbon provided by the present invention is subjected to boron-phosphorus dual doping modification in the coating layer, and the added P element is combined with the oxygen atoms in the coating layer on the surface and / or the composite body to play a bridging role, thereby enhancing the structural stability between the coating layer and the composite body, and making the coating layer more tightly wrapped on the surface of the core layer. At the same time, the B in the coating layer produces a hole effect as an electron acceptor, turning the composite material into a p-type semiconductor; on the other hand, P forms a carrier effect in the coating layer as an electron donor, turning the composite material into an n-type semiconductor. Therefore, after B / P dual doping modification, a B / P pair is formed in the coating layer, making it easier for electrons to escape and embed, thereby greatly enhancing the conductivity of the composite material, and thus having better rate performance and cycle stability.
[0035] The preparation method provided by the present invention realizes the dual doping of boron and phosphorus by using a coupling agent, improves the crosslinking between sodium ferric pyrophosphate and the carbon source, improves the coating effect of the carbon source, and increases the bonding force between the coating layer and the core layer. The preparation method has a simple process, a high degree of mechanization, a large batch processing volume, and is suitable for large-scale industrial production.
[0036] The application of the composite material provided by the present invention, in view of the advantages of the above-mentioned composite material, enables it to have better conductivity, stability and rate performance as a positive electrode material for sodium ion batteries, promotes the development of sodium ion batteries, and expands the application scenarios of sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0038] Figure 1 is the Na obtained in Example 10 3 Fe 2 (PO 4 )(P 2 O 7 )@B / PC scanning electron microscope image;
[0039] Figure 2 is the Na obtained in Example 10 3 Fe2 (PO 4 )(P 2 O 7 )@B / PC SEM image at another magnification;
[0040] Figure 3 For Example 10, Na 3 Fe 2 (PO 4 )(P 2 O 7 )@B / PC transmission electron microscope image;
[0041] Figure 4 The Raman spectra of the materials prepared in Example 10 and Comparative Example 1;
[0042] Figure 5 XRD patterns of the materials prepared in Example 10 and Comparative Example 1;
[0043] Figure 6 The charge and discharge curves of Example 10 and Comparative Example 1 are shown;
[0044] Figure 7 The graphs are the data changes of the number of cycles and the cycle retention rate of Example 10 and Comparative Example 1;
[0045] Figure 8 The graph showing the change in the number of cycles and capacity data for Example 10 and Comparative Example 1. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. The components of the embodiments of the present invention described and shown herein can be arranged and designed in various different configurations.
[0047] A first aspect of the present invention provides a sodium ferric phosphate pyrophosphate-modified carbon composite material, the composite material comprising a core layer and a coating layer, the core layer is made of sodium ferric phosphate pyrophosphate, and the coating layer is a modified carbon coating layer.
[0048] The chemical formula of the sodium ferric phosphate pyrophosphate is Na 3 Fe 2 (PO 4 )(P 2 O 7 ).
[0049] The material of the modified carbon coating layer is boron-phosphorus dual-doped modified carbon.
[0050] The composite material of sodium iron phosphate pyrophosphate-modified carbon provided by the present invention is subjected to boron-phosphorus dual doping modification in the coating layer, and the added P element is combined with the oxygen atoms in the coating layer on the surface and / or the composite body to play a bridging role, thereby enhancing the structural stability between the coating layer and the composite body, and making the coating layer more tightly wrapped on the surface of the core layer. In the subsequent heat treatment process, boron acts as a catalyst to promote the graphitization degree of the carbon source and improve the conductivity of the coating layer. At the same time, B in the coating layer produces a hole effect as an electron acceptor, turning the composite material into a p-type semiconductor; on the other hand, P, as an electron donor, forms a carrier effect in the coating layer, turning the composite material into an n-type semiconductor. Therefore, after B / P dual doping modification, a B / P pair is formed in the coating layer, making it easier for electrons to escape and embed, thereby greatly enhancing the conductivity of the composite material, and thus having better rate performance and cycle stability.
[0051] Furthermore, the coating layer has a thickness of 2nm to 50nm.
[0052] When the thickness of the coating layer is less than 2nm, it cannot effectively form a stable and complete coating layer when deposited on the surface of the core layer, resulting in the instability of sodium iron pyrophosphate to air, and also reducing the stability of the material to water, causing gas production and pole piece peeling when the electrode slurry is made; when the thickness of the coating layer is greater than 50nm, the carbon layer will hinder the rapid transmission of sodium ions, causing the rate performance of the composite material to decrease and unable to achieve rapid charging and discharging. In addition, if the proportion of carbon material is too high, it will reduce the specific capacity of the composite material and reduce the energy density of the sodium ion battery.
[0053] Typically but not limiting, the thickness of the coating layer can be, for example, 2nm, 3nm, 5nm, 8nm, 10nm, 12nm, 14nm, 16nm, 18nm, 19nm, 20nm, 30nm, 40nm or 50nm, or any value within the range of 2nm to 50nm.
[0054] Furthermore, the content of boron in the composite material is 0.1 wt.% to 5 wt.%.
[0055] When the content of boron in the composite material is less than 0.1wt.%, it has little effect on the graphitization degree of the carbon source, and provides fewer holes in the coating layer, which has a slight improvement on the rate performance; when the content of boron in the composite material is higher than 5wt.%, the mass proportion of carbon is reduced, and it will react with Na in the core layer. 3 Fe 2 PO 4 P 2 O 7 Reaction, generating B 2 O 3 Impurities cause the specific capacity of the composite material to decrease.
[0056] Typically but not limiting, the boron content in the composite material may be, for example, 0.1 wt.%, 0.5 wt.%, 1 wt.%, 2 wt.%, 3 wt.%, 4 wt.% or 5 wt.%, or any value within the range of 0.1 wt.% to 5 wt.%.
[0057] The content of phosphorus in the composite material is 0.1wt.% to 5wt.%.
[0058] When the content of phosphorus in the composite material is less than 0.1wt.%, the carrier effect formed in the coating layer is weak, and the improvement of rate performance is also weak. When the content of phosphorus in the composite material is higher than 5wt.%, PO is easily generated. 4 3- With P 2 O 7 4- , making Na 3 Fe 2 PO 4 P 2 O 7 The chemical ratio is unbalanced, and PO 4 3- With P 2 O 7 4- Overdosage will cause a sharp drop in capacity.
[0059] Typically but not limiting, the phosphorus content in the composite material may be, for example, 0.1 wt.%, 0.5 wt.%, 1 wt.%, 2 wt.%, 3 wt.%, 4 wt.% or 5 wt.%, or any value within the range of 0.1 wt.% to 5 wt.%.
[0060] The second aspect of the present invention provides a method for preparing the composite material, which comprises adding a carbon source, a boron source and a phosphorus source to an aqueous solution of a raw material for preparing sodium ferric pyrophosphate, mixing the mixture evenly, and then sand-milling, spray-drying, pre-burning and calcining to obtain the composite material;
[0061] At least one of the boron source and the phosphorus source is in the form of a coupling agent.
[0062] The preparation method provided by the present invention realizes the dual doping of boron and phosphorus by using a coupling agent, improves the crosslinking between sodium ferric pyrophosphate and the carbon source, improves the coating effect of the carbon source, and increases the bonding force between the coating layer and the core layer. The preparation method has a simple process, a high degree of mechanization, a large batch processing volume, and is suitable for large-scale industrial production.
[0063] It should be noted that at least one of the boron source and the phosphorus source is in the form of a coupling agent, and there are three situations: the first situation is that the boron source is a boron-containing coupling agent and the phosphorus source is a phosphorus-containing compound; the second situation is that the boron source is a boron-containing compound and the phosphorus source is a phosphorus-containing coupling agent; the third situation is that the boron source is a boron-containing coupling agent and the phosphorus source is a phosphorus-containing coupling agent. The coupling agent can improve the bonding force between the core layer and the coating layer and thus improve the stability of the composite material of sodium iron pyrophosphate-modified carbon.
[0064] The composite material of the present invention is prepared by coating and modifying the carbon layer while preparing the sodium ferric pyrophosphate, so it is directly carried out in the aqueous solution of the raw material for preparing the sodium ferric pyrophosphate. The present invention does not limit the raw material for preparing the sodium ferric pyrophosphate, and any raw material that can prepare the sodium ferric pyrophosphate can be used.
[0065] Further, the boron-containing coupling agent includes a borate coupling agent.
[0066] or,
[0067] The boron-containing non-coupling agent includes at least one of boric acid, borax and boron trioxide.
[0068] Furthermore, the phosphorus-containing coupling agent includes a phosphate coupling agent.
[0069] or,
[0070] The phosphorus-containing non-coupler is sodium phytate.
[0071] The brands of the borate coupling agent include LD-100P, LD-1060 or LD-12655.
[0072] The phosphate coupling agent includes 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate.
[0073] The carbon source includes at least one of sucrose, glucose, starch, cyclodextrin and citric acid. The carbon source has a low carbonization temperature, low cost and good effect on improving electrical conductivity, and can provide carbon with relatively high purity. The CO generated by the carbon source during the sintering process is a reducing gas, which helps to reduce the trivalent iron in the iron phosphate in the raw material to divalent iron.
[0074] The added amount of the carbon source is 3wt.%-20wt.% of the total mass of the sodium ferric pyrophosphate, the carbon source, the boron source and the phosphorus source.
[0075] Typically but not limiting, the amount of carbon source added may be, for example, 3wt.%, 7wt.%, 9wt.%, 11wt.%, 13wt.%, 15wt.%, 17wt.% or 20wt.%, or any value within the range of 3wt.%-20wt.%.
[0076] The added amount of the boron source is 0.1wt.%-5wt.% of the total mass of the sodium ferric pyrophosphate, the carbon source, the boron source and the phosphorus source.
[0077] Typically but not limiting, the amount of boron source added may be, for example, 0.1 wt.%, 0.5 wt.%, 1 wt.%, 2 wt.%, 3 wt.%, 4 wt.% or 5 wt.%, or any value within the range of 0.1 wt.% to 5 wt.%.
[0078] The added amount of the phosphorus source is 0.1wt.%-5wt.% of the total mass of the sodium ferric pyrophosphate, the carbon source, the boron source and the phosphorus source.
[0079] Typically but not limiting, the added amount of phosphorus source may be, for example, 0.1 wt.%, 0.5 wt.%, 1 wt.%, 2 wt.%, 3 wt.%, 4 wt.% or 5 wt.%, or any value within the range of 0.1 wt.% to 5 wt.%.
[0080] Furthermore, a sand mill is used for the sand grinding, which can quickly reduce the particle size of the slurry and improve the dispersion efficiency.
[0081] The rotation speed of the sand mill is 1500 rpm to 3500 rpm, and the time is 0.5 h to 2 h.
[0082] Furthermore, the pre-firing temperature is 200° C. to 350° C., and the pre-firing time is 1 h to 4 h.
[0083] The calcination temperature is 400° C. to 600° C., and the calcination time is 3 h to 8 h.
[0084] The third aspect of the present invention provides the use of the above-mentioned sodium iron pyrophosphate-modified carbon composite material in the positive electrode material of a sodium ion battery.
[0085] The application of the composite material provided by the present invention, in view of the advantages of the above-mentioned composite material, enables it to have better conductivity, stability and rate performance as a positive electrode material for sodium ion batteries, promotes the development of sodium ion batteries, and expands the application scenarios of sodium ion batteries.
[0086] In the following, some embodiments of the present invention are described in detail in conjunction with the embodiments. In the absence of conflict, the following embodiments and the features in the embodiments can be combined with each other. The raw materials used in the present invention can be obtained by commercial purchase unless otherwise specified.
[0087] Example 1
[0088] This embodiment provides a composite material of sodium iron phosphate pyrophosphate-modified carbon, and the preparation process is as follows:
[0089] 1. Weigh 226.5g FePO4 (1.5 mol, M = 151), 213 g Na 2 HPO 4 (1.5 mol, M = 142), 90 g of ferrous oxalate dihydrate (0.5 mol, M = 180), and 56.6 g of starch for later use;
[0090] 2. Add 213g Na 2 HPO 4 Dissolve in 1.5L deionized water to form a concentration of 1mol / L Na 2 HPO 4 Aqueous solution;
[0091] 3. FePO 4 , ferrous oxalate dihydrate, and starch were mixed evenly, and 1.2 L of Na 2 HPO 4 The aqueous solution, carbon source, boron source and phosphorus source are mixed evenly. The boron source is 0.26g of borate coupling agent LD-100P and 0.38g of sodium phytate, which are mixed evenly to form a slurry.
[0092] 4. Pour the slurry into a sand mill and grind it at a speed of 3500 rpm until the particle size is 0.3-2 μm.
[0093] 5. The sand-milled slurry is spray-dried in a spray dryer to obtain dry and uniform precursor particles.
[0094] 6. Pre-sinter the precursor particles at 300°C for 3h and calcine at 500°C for 4h under nitrogen protection to obtain Na 3 Fe 2 (PO 4 )(P 2 O 7 )@B / PC.
[0095] Example 2
[0096] The present embodiment provides a composite material of sodium ferric pyrophosphate-modified carbon. The difference from Example 1 is that in step 3, 0.44 g of boric acid and 0.58 g of 2-methyl-2-acrylic acid-2-hydroxyethyl phosphate (Zhengzhou Alpha Chemical Co., Ltd.) are added to the aqueous solution of the raw materials for preparing sodium ferric pyrophosphate, and the mixture is evenly mixed to form a slurry. The remaining raw materials and steps are the same as those in Example 1 and will not be repeated here.
[0097] Example 3
[0098] The present embodiment provides a composite material of sodium iron phosphate pyrophosphate-modified carbon. The difference from Example 1 is that in step 3, 1.26 g of borate coupling agent LD-1060 and 1.16 g of 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate (Zhengzhou Alpha Chemical Co., Ltd.) are added to the aqueous solution of the raw materials for preparing sodium iron phosphate pyrophosphate, and the mixture is evenly mixed to form a slurry. The remaining raw materials and steps are the same as those in Example 1 and are not repeated here.
[0099] Example 4
[0100] The present embodiment provides a composite material of sodium iron phosphate pyrophosphate-modified carbon. The difference from Example 1 is that in step 3, 2.24 g of borate coupling agent LD-12655 and 1.56 g of 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate (Zhengzhou Alpha Chemical Co., Ltd.) are added to the aqueous solution of the raw materials for preparing sodium iron phosphate pyrophosphate, and the mixture is evenly mixed to form a slurry. The remaining raw materials and steps are the same as those in Example 1 and are not repeated here.
[0101] Example 5
[0102] The present embodiment provides a composite material of sodium ferric pyrophosphate-modified carbon. The difference from Example 1 is that in step 3, 1.26 g of boron oxide and 1.74 g of 2-methyl-2-acrylic acid-2-hydroxyethyl phosphate (Zhengzhou Alpha Chemical Co., Ltd.) are added to the aqueous solution of the raw materials for preparing sodium ferric pyrophosphate, and the mixture is evenly mixed to form a slurry. The remaining raw materials and steps are the same as those in Example 1 and will not be repeated here.
[0103] Example 6
[0104] This embodiment provides a sodium iron phosphate pyrophosphate-modified carbon composite material. The difference from Example 1 is that glucose is used instead of starch, the amount of glucose used is 62.4 kg, and the remaining raw materials and steps are the same as Example 1, which will not be repeated here.
[0105] Example 7
[0106] This embodiment provides a sodium iron phosphate pyrophosphate-modified carbon composite material. The difference from Example 1 is that the amount of borate coupling agent LD-100P used is 0.86 g, and the remaining raw materials and steps are the same as those in Example 1, which will not be repeated here.
[0107] Example 8
[0108] This embodiment provides a composite material of sodium iron phosphate pyrophosphate-modified carbon. The difference from Example 1 is that the amount of sodium phytate used is 3.8 g, and the remaining raw materials and steps are the same as those in Example 1, which will not be repeated here.
[0109] Example 9
[0110] The present embodiment provides a composite material of sodium iron phosphate pyrophosphate-modified carbon. The difference from Example 1 is that in step 3, 6.5 g of borate coupling agent LD-100P and 9.5 g of sodium phytate are added to the aqueous solution of raw materials for preparing sodium iron phosphate pyrophosphate, and the mixture is mixed evenly to form a slurry. The remaining raw materials and steps are the same as those in Example 1 and are not repeated here.
[0111] Example 10
[0112] The present embodiment provides a composite material of sodium iron phosphate pyrophosphate-modified carbon. The difference from Example 1 is that in step 3, 13 g of borate coupling agent LD-100P and 19 g of sodium phytate are added to the aqueous solution of raw materials for preparing sodium iron phosphate pyrophosphate, and the mixture is evenly mixed to form a slurry. The remaining raw materials and steps are the same as those in Example 1 and will not be repeated here.
[0113] Comparative Example 1
[0114] This comparative example provides a kind of sodium ferric pyrophosphate.
[0115] Comparative Example 2
[0116] This comparative example provides a composite material of sodium iron phosphate pyrophosphate-modified carbon. The difference from Example 1 is that 0.52 g of a borate coupling agent LD-100P is added to the aqueous solution of the raw materials for preparing sodium iron phosphate pyrophosphate in step 3 and mixed evenly to form a slurry. The remaining raw materials and steps are the same as those in Example 1 and are not repeated here.
[0117] Comparative Example 3
[0118] This comparative example provides a composite material of sodium ferric pyrophosphate-modified carbon. The difference from Example 1 is that in step 3, 0.58 g of 2-methyl-2-acrylic acid-2-hydroxyethyl phosphate (Zhengzhou Alpha Chemical Co., Ltd.) is added to the aqueous solution of the raw materials for preparing sodium ferric pyrophosphate and mixed evenly to form a slurry. The remaining raw materials and steps are the same as those in Example 1 and are not repeated here.
[0119] Comparative Example 4
[0120] This comparative example provides a composite material of sodium iron phosphate pyrophosphate-modified carbon. The difference from Example 1 is that in step 3, 1.26 g of boron oxide and 0.76 g of sodium phytate are added to the aqueous solution of raw materials for preparing sodium iron phosphate pyrophosphate and mixed evenly to form a slurry. The remaining raw materials and steps are the same as those in Example 1 and are not repeated here.
[0121] Test Example 1
[0122] The Na prepared in Example 10 3 Fe 2 (PO 4 )(P 2 O7 )@B / PC was observed by scanning electron microscope (FESEM, JSM-6700F). Figure 1 shown.
[0123] like Figure 1 As shown, we can see that Na 3 Fe 2 (PO 4 )(P 2 O 7 ) The particles are coarser, which is why they are coated with a carbon layer.
[0124] Continue to adjust the magnification of the scanning electron microscope to obtain Figure 2 .from Figure 2 The carbon coating on the particles can be more clearly seen.
[0125] Test Example 2
[0126] The Na prepared in Example 10 3 Fe 2 (PO 4 )(P 2 O 7 )@B / PC was observed by transmission electron microscopy (Hitachi800TEM, 200kV). Figure 3 As shown, through transmission electron microscopy testing, it can be seen that the thickness of the carbon layer is about 2nm.
[0127] Test Example 3
[0128] The Na prepared in Example 10 3 Fe 2 (PO 4 )(P 2 O 7 )@B / PC and the materials obtained in Comparative Example 1 were subjected to Raman spectroscopy. The D peak and G peak in the Raman spectrum were located at 1 346 cm -1 and 1 587cm -1 The D peak reflects the defects and regularity of the carbon layer, and the G peak comes from the E 2g Phonon plane vibration reflects the symmetry and order of the material. The larger the peak area D / G ratio, the lower the degree of graphitization. Figure 4 ZhongNa 3 Fe 2 (PO 4 )(P 2 O 7 )@The peak area D / G ratio of B / PC sample is smaller than that of Na 3 Fe 2 (PO 4 )(P 2 O 7), this is because boron doping catalyzes the graphitization of the carbon layer, which increases the degree of graphitization of the carbon layer. Carbon with a higher degree of graphitization has better electronic conductivity, which is also the reason for Na 3 Fe 2 (PO 4 )(P 2 O 7 )@B / PC has higher charge and discharge capacity and better cycle retention rate.
[0129] Test Example 4
[0130] The materials prepared in Example 10 and Comparative Example 1 were subjected to X-ray diffraction (SHIMADZU XRD-7000) test. The experimental conditions were as follows: copper target (λ = 0.1518 nm), 2θ angle range of 10-80°. The XRD spectrum is as follows: Figure 5 shown.
[0131] from Figure 5 It can be seen from the XRD spectrum in that boron / phosphorus dual doping has an effect on Na 3 Fe 2 (PO 4 )(P 2 O 7 ) has no influence on the crystallinity, which is consistent with Comparative Example 1.
[0132] Experimental Example 1
[0133] The positive electrode materials prepared in Examples 1-10 and Comparative Examples 1-4 were respectively pressed into cylinders at a molding pressure of 30 MPa at 25°C, and then the height h, ground diameter d and resistance R of the cylinders were measured respectively. The formula σ = 4h / (πR·d 2 ) to calculate the electronic conductivity σ.
[0134] The obtained data are shown in Table 1 below.
[0135] Table 1
[0136]
[0137] As can be seen from Table 1, the use of boron / phosphorus dual doping can well improve its electronic conductivity. The electronic conductivity of Examples 1-10 is significantly improved compared with that of Comparative Example 1. This is attributed to the formation of B / P pairs by boron / phosphorus dual doping in the coating layer, which makes it easier for electrons to escape and embed, thereby greatly enhancing the conductivity of the composite material and effectively improving the Na 3 Fe 2 (PO 4 )(P 2 O 7)@C's electronic conductivity. In addition, as the amount of B source and phosphorus source used in the embodiment increases, the improvement effect becomes gradually obvious. At the same time, we can also observe from Comparative Examples 2 and 3 that the performance improvement of the material is limited when B and P are doped alone. This is because no electron pair of B and P is formed, and there is no synergistic improvement effect. Comparative Example 4 shows that only through the dispersing effect of the coupling agent can the carbon layer surface be better dispersed and doped.
[0138] Experimental Example 2
[0139] 0.4 g of the materials provided in the examples and comparative examples, 0.05 g of a conductive agent (acetylene black), and 0.05 g of a binder polyvinylidene fluoride (PVDF) were mixed in 0.5 g of N-methylpyrrolidone (NMP) to obtain the desired positive electrode slurry. Subsequently, the slurry was coated on the treated aluminum foil and dried in a vacuum drying oven at 90° C. for 10 h to obtain a positive electrode sheet.
[0140] The above-mentioned electrode and sodium sheet were assembled into a button battery in a glove box. The electrolyte was 1 mol·L -1 NeA 6 The sodium salt of ethylene carbonate (EC) and ethylene methyl carbonate (EMC) was dissolved in a solution of 1:1 by volume, and 5% fluoroethylene carbonate (FEC) additive was added to the electrolyte. Subsequent electrochemical performance tests will focus on button cells.
[0141] The button cell was subjected to a charge and discharge test. The current was 0.1C (1C is 150 mA / g) and the charge and discharge temperature was 30°C. The charge and discharge specific capacity of the button cell was measured, and the results are shown in Table 1.
[0142] The button cell was subjected to a cycle performance test. The current was 1C (1C = 150 mA / g) and the charge and discharge temperature was 30°C. Before the 1C formal cycle, it was activated with a small current of 0.5C for 3 cycles. The discharge specific capacity of the button cell was measured, and the discharge specific capacity was continued to be measured after 100 cycles. The capacity retention rate was calculated, and the results are shown in Table 2.
[0143] Table 2
[0144]
[0145] As can be seen from Table 2, the use of boron / phosphorus dual doping can greatly improve its charge and discharge capacity, and the cycle performance is also improved, which shows that boron / phosphorus dual doping has a significant effect on Na 3 Fe 2 (PO 4 )(P 2 O 7)@C can significantly improve its charge and discharge capacity. At the same time, as the amount of B source and phosphorus source used increases, the electronic conductivity gradually increases, and the improvement effect is better, with higher charge and discharge performance and cycle performance.
[0146] Result Example 1
[0147] The charging and discharging results of the buckle of Example 10 and Comparative Example 1 in the test example are plotted to obtain Figure 6 ,from Figure 6 It can be seen that it is precisely because of the effect of B / P dual doping that the Na 3 Fe 2 (PO 4 )(P 2 O 7 )@C polarization makes it more conductive, which in turn improves its capacity.
[0148] Result Example 2
[0149] For Example 10 and Comparative Example 1 in the test example, the cycle number and cycle retention rate data obtained by the test are plotted to obtain Figure 7 ,from Figure 7 It can be seen that the cycling performance is improved by B / P dual doping, which is attributed to the improvement of its conductivity and the improvement of cycling performance brought about by the reduction of polarization degree.
[0150] Result Example 3
[0151] For Example 10 and Comparative Example 1 in the test example, the number of cycles and capacity data obtained by testing are plotted to obtain Figure 8 ,from Figure 8 It can be seen that its rate discharge is improved, which is attributed to the increased conductivity brought about by B / P dual doping.
[0152] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A composite material of sodium ferric pyrophosphate-modified carbon, characterized in that: The composite material comprises a core layer and a coating layer, the core layer is made of sodium ferric pyrophosphate, and the coating layer is a modified carbon coating layer; The chemical formula of the sodium iron phosphate pyrophosphate is Na3Fe2(PO4)(P2O7); The material of the modified carbon coating layer is boron-phosphorus dual-doped modified carbon.
2. The composite material according to claim 1, characterized in that The coating layer has a thickness of 2 nm to 50 nm.
3. The composite material according to claim 1, characterized in that The content of boron in the composite material is 0.1wt.% to 5wt.%; The content of phosphorus in the composite material is 0.1wt.% to 5wt.%.
4. A method for preparing the composite material according to any one of claims 1 to 3, characterized in that: A carbon source, a boron source and a phosphorus source are added to a raw material aqueous solution for preparing sodium ferric phosphate pyrophosphate, and the mixture is evenly mixed, and then sand-milled, spray-dried, pre-burned and calcined to obtain the composite material; At least one of the boron source and the phosphorus source is in the form of a coupling agent.
5. The preparation method according to claim 4, characterized in that: Boron-containing coupling agents include borate coupling agents; or, The boron-containing non-coupling agent includes at least one of boric acid, borax and boron trioxide.
6. The preparation method according to claim 4, characterized in that: Phosphorus-containing coupling agents include phosphate coupling agents; or, Phosphorus-containing non-couplers include sodium phytate.
7. The preparation method according to any one of claims 4 to 6, characterized in that: The carbon source comprises at least one of sucrose, glucose, starch, cyclodextrin, ascorbic acid, polyethylene glycol and citric acid; The amount of the carbon source added is 3wt.%-20wt.% of the total mass of the sodium ferric pyrophosphate, the carbon source, the boron source and the phosphorus source; The amount of the boron source added is 0.1wt.%-5wt.% of the total mass of the sodium ferric pyrophosphate, the carbon source, the boron source and the phosphorus source; The added amount of the phosphorus source is 0.1wt.%-5wt.% of the total mass of the sodium ferric pyrophosphate, the carbon source, the boron source and the phosphorus source.
8. The preparation method according to any one of claims 4 to 6, characterized in that: Performing the sanding using a sand grinder; The rotation speed of the sand mill is 1500 rpm to 3500 rpm, and the time is 0.5 h to 2 h.
9. The preparation method according to any one of claims 4 to 6, characterized in that: The pre-burning temperature is 150°C to 350°C, and the time is 1h to 4h; The calcination temperature is 400° C. to 600° C., and the calcination time is 3 h to 8 h.
10. Application of a composite material of sodium iron pyrophosphate-modified carbon in a positive electrode material for a sodium ion battery, characterized in that: The sodium iron phosphate pyrophosphate-modified carbon composite material is the composite material described in any one of claims 1 to 3, or a composite material prepared by the preparation method described in any one of claims 4 to 9.
Citation Information
Patent Citations
Lithium iron phosphate / carbon composite material with surface modified by coupling agent and preparation method thereof
CN101964412A
Preparation method of sodium ion battery positive electrode material Na3Fe2 (PO4) P2O7
CN115611258A
Heteroatom-doped carbon-coated Na4MxFe3-x (PO4) 2P2O7 composite material as well as preparation method and application thereof
CN117276494A
Polyanionic positive electrode composite material as well as preparation method and application thereof
CN117766743A
Positive electrode material and preparation method therefor
WO2023227035A1
Cited By
Modification method of sodium battery positive active material
CN122444153A
Boron-coated sodium ferric phosphate, preparation method thereof, sodium ion battery positive electrode material and sodium ion battery
CN122520024A