Porous polyimide cage material having gradient pore structure and preparation method therefor, and bearing

By designing a gradient pore structure in a porous polyimide cage, the problem of excessive oil output in the prior art under vacuum or high temperature conditions is solved, the high precision and long life of the bearing are achieved, and the on-demand slow release is met Long oil and lubrication life requirements.

WO2024227327A1PCT designated stage expired Publication Date: 2024-11-07LUOYANG BEARING RES INST CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/119560
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-29
Filing Date
2023-09-19
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

The existing porous polyimide cages produce a lot of oil under vacuum or high temperature conditions, which causes friction torque fluctuations or exceeds the index requirements, and cannot have the requirements of both slow release of oil on demand and long lubrication life.

Method used

Porous polyimide cage material with gradient pore structure is adopted, with low porosity close to the guide surface side and high porosity far away from the guide surface side. The porosity structure is designed through bearing guidance to achieve slow oil release on demand, and The lubrication life is extended by staying away from the high porosity and high oil content of the material on the guide surface side.

Benefits of technology

It effectively avoids the problem of high porosity cages producing too much oil under vacuum or high temperature conditions, ensures high accuracy and reliability of bearings, and extends the service life of bearings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023119560_07112024_PF_FP_ABST
    Figure CN2023119560_07112024_PF_FP_ABST
Patent Text Reader

Abstract

A porous polyimide cage material having a gradient pore structure and a preparation method therefor, and a bearing. The porous polyimide cage material comprises at least two porous polyimide layers which are combined from inside out; the porosity of the porous polyimide layer close to a guide surface side is low; and the porosity of the porous polyimide layer distant from the guide surface side is high.
Need to check novelty before this filing date? Find Prior Art

Description

Porous polyimide cage material with gradient pore structure, preparation method thereof, and bearing Technical Field

[0001] The present invention belongs to the field of bearing cages, and in particular relates to a porous polyimide cage material with a gradient pore structure, a preparation method thereof, and a bearing. Background Art

[0002] Porous polyimide cage materials have the characteristics of high mechanical strength, excellent tribological properties, aging resistance, radiation resistance, etc., and also have good high and low temperature adaptability and lubricant compatibility. The lubricant can form a good circulation in the interconnected pores inside the material, achieving the effect of long-term on-demand oil supply, which greatly improves the stability, reliability and life of the bearing operation. It is now widely used in long-life spacecraft gyro motors, navigators, and momentum wheel bearings.

[0003] The applicant has previously conducted relatively systematic research on the aperture adjustment (CN111763429A) and aperture concentration (CN113563626A) of porous polyimide retainers. The relevant products have been well applied in aerospace products, and civilian products based on this technology have also significantly improved the performance of related bearings.

[0004] At present, the pore structure of porous polyimide retainers is uniform as a whole. However, in actual applications, it is found that if the porosity of the material is low, the oil content is low, and the ground running-in test meets the technical indicators, but the theoretical lubrication life is short; if the porosity of the material is high, the oil content is high, and the theoretical lubrication life is long, but more oil is released during running-in in vacuum or at high temperature, resulting in fluctuations in friction torque or exceeding the index requirements.

[0005] With the development of my country's aerospace industry, main engine users have put forward higher requirements on the life and reliability of bearings. The existing porous polyimide cages can no longer meet the requirements of on-demand slow release of oil and long lubrication life.

[0006] Summary of the Invention

[0007] The purpose of the present invention is to provide a porous polyimide cage material with a gradient pore structure to solve the problem that the existing porous polyimide cage cannot achieve both on-demand slow release of oil and long lubrication life.

[0008] The second object of the present invention is to provide a method for preparing the porous polyimide retainer material to solve the above problems.

[0009] The third object of the present invention is to provide a bearing to further improve the service life and reliability of the bearing.

[0010] In order to achieve the above objectives, the technical solution adopted by the present invention is:

[0011] A porous polyimide retainer material with a gradient pore structure comprises at least two porous polyimide layers combined together in the inner and outer directions, the porous polyimide layer close to the guide surface has a low porosity, and the porous polyimide layer away from the guide surface has a high porosity.

[0012] The porous polyimide cage material with a gradient pore structure provided by the present invention features a gradient design of the cage pore structure based on the bearing guidance method. When the bearing is externally guided, the gap between the inner diameter of the bearing outer ring and the outer diameter of the cage is small. When the bearing rotates, lubricating oil overflows due to friction or temperature. When the outer layer of the porous polyimide cage (near the guide surface) has a low porosity and low oil content, oil leakage is minimal. However, the inner layer of the cage (away from the guide surface) has a high porosity and high oil content, meeting the theoretical lubrication life. Similarly, when the bearing is internally guided, the gap between the outer diameter of the bearing inner ring and the inner diameter of the cage is small. When the inner layer of the porous polyimide cage has a low porosity and low oil content, oil leakage is minimal. However, the outer layer of the cage has a high porosity and high oil content, meeting the theoretical lubrication life.

[0013] Utilizing these characteristics, the cage can release oil slowly and on demand, preventing excessive oil release from high-porosity cages during vacuum or high-temperature running-in, which could cause friction torque fluctuations or exceed specification requirements, thereby ensuring high precision and reliability during bearing operation. Furthermore, by leveraging the high porosity and high oil content of the material farther from the guide surface, lubricant is continuously delivered to the side closer to the guide surface as it is consumed, thereby extending the lubrication life.

[0014] To further optimize the performance of the retainer material in terms of slow oil release and improved lubrication life, preferably, the porosity of the porous polyimide layer farthest from the guide surface is 1.2 to 2 times the porosity of the porous polyimide layer closest to the guide surface.

[0015] More preferably, the porosity of the porous polyimide layer on the side farthest from the guide surface is 20-35%. Maintaining the porosity within the above range can meet the use requirements of most bearings.

[0016] Preferably, the pore size of the porous polyimide layer near the guide surface is small, while the pore size of the porous polyimide layer far from the guide surface is large. Further making the pore size present a gradient change can further optimize its slow release of oil and lubrication life performance.

[0017] More preferably, the pore size of the porous polyimide layer farthest from the guide surface is 1.1 to 2.5 times the pore size of the porous polyimide layer closest to the guide surface. Controlling the pore size variation within the above range facilitates manufacturing and has better performance.

[0018] More preferably, the pore size of the porous polyimide layer on the side farthest from the guide surface is 0.9 to 2.5 μm. Maintaining the pore size within the above range can meet the use requirements of most bearings.

[0019] The method for preparing the porous polyimide cage material having a gradient pore structure comprises the following steps:

[0020] (1) preparing raw materials for retainers with different pore structures, first feeding and pre-pressing the raw materials corresponding to one of the pore structure retainers to obtain a preform; then feeding and pre-pressing the raw materials corresponding to the remaining pore structure retainers inside or outside the preform to obtain a retainer preform;

[0021] (2) Sintering the retainer preform.

[0022] The present invention's method for preparing a porous polyimide retainer material with a gradient pore structure primarily involves sequentially preparing preforms to create a highly consistent and well-bonded preform. This preform is then sintered to produce the final product. This method is easy to implement, utilizing existing molds, and has minimal impact on retainer production costs.

[0023] Preferably, the pre-pressing is an integral pressing, and the pressure of the first pre-pressing is 500-2000 kN / cm 2 The final pre-pressing pressure is 2 to 7 times that of the first pre-pressing pressure. The holding time between the first and final pre-pressing is 3 to 8 minutes. This pressing scheme improves the integrity of the retainer preform and ensures the bonding strength between the different layers of material.

[0024] Preferably, in step (2), the sintering temperature is 360-380°C and the holding time is 30-60 minutes. By adopting the above sintering conditions, a better molding effect can be achieved.

[0025] Preferably, the raw materials are composed of the following components by mass fraction: 80-100% of monoether anhydride polyimide and 0-20% of polytetrafluoroethylene molding powder. The raw materials used for retainers with different pore structures can be easily prepared by using the above raw materials.

[0026] The bearing comprises a retaining frame, wherein the retaining frame is made of the above-mentioned porous polyimide retaining frame material with a gradient pore structure.

[0027] Bearings using the above-mentioned retainer will not have the problem of excessive oil discharge during high-oil-content bearing running-in at high temperatures, thereby avoiding friction torque fluctuations or exceeding index requirements caused by excessive oil discharge, thereby improving bearing operation reliability; because it also has a porous polyimide layer with high porosity, it can increase the oil content and extend the service life of the bearing. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] FIG1 is a physical picture of a porous polyimide cage material prepared in Example 1 of the present invention;

[0029] FIG2 is a diagram of a finished cage made from the cage material of Example 1;

[0030] FIG3 is an appearance diagram of a retainer made of the material of Example 1 after a 600-hour bearing bench running-in test. DETAILED DESCRIPTION

[0031] The present invention provides a porous polyimide cage material with a gradient pore structure, which can achieve on-demand slow release of oil while having high porosity and high oil content, meeting the needs of high-precision, long-life and high-reliability bearings.

[0032] The structural feature of the porous polyimide retainer is that the porous polyimide retainer includes at least two porous polyimide layers combined together in the inner and outer directions, the porous polyimide layer close to the guide surface has a low porosity, and the porous polyimide layer away from the guide surface has a high porosity.

[0033] The difference in porosity between the inner and outer directions creates a gradient pore structure. The position of the guide surface is related to the bearing's guidance method, namely, whether it is externally or internally guided. With external guidance, the side closest to the guide surface is the outer side of the cage, and the side further away from the guide surface is the inner side. With internal guidance, the side closest to the guide surface is the inner side of the cage, and the side further away from the guide surface is the outer side.

[0034] Taking the internal guide as an example, the gap between the outer diameter of the bearing inner ring and the inner diameter of the cage is small. When the porosity of the inner layer of the porous polyimide cage is small and the oil content is low, the oil output is small. The porosity of the outer layer of the cage is large and the oil content is high, which can meet the theoretical lubrication life.

[0035] The following further describes the manufacturing process of the porous polyimide cage with a gradient pore structure.

[0036] A porous polyimide cage material with a gradient pore structure, the preparation of which includes the following five steps:

[0037] Step 1: Selection of monoether anhydride polyimide molding powder

[0038] The structural formula of monoether anhydride polyimide is as follows:

[0039]

[0040] Monoether anhydride polyimide molding powder is prepared by polycondensation, cyclodehydration and dehydration of 4,4-oxydiphthalic anhydride (ODPA) and 4,4-diaminodiphenyl ether (ODA).

[0041] Generally speaking, the particle size of the molding powder used for small porosity structures is 8 to 20 μm, and the particle size of the molding powder used for large porosity structures is 15 to 40 μm.

[0042] Step 2: Prepare the polyimide blend by weight percentage

[0043] Prepare a polyimide blend by mixing 80-100% monoether anhydride polyimide molding powder and 0-20% polytetrafluoroethylene molding powder, respectively, in an FM high-speed mixer. Observe the color difference of the polyimide blend under a 20x microscope. A polyimide blend with no noticeable color difference is considered acceptable and should be vacuum-sealed and stored for future use. No further preparation is required for 100% polyimide.

[0044] Generally speaking, porous polyimide materials with varying pore structures can be produced by adjusting the particle size of monoether anhydride polyimide molding powder and the relative amounts of polytetrafluoroethylene molding powder. For example, a porous polyimide material with a low porosity structure can be obtained by using monoether anhydride polyimide molding powder with a larger particle size and increasing the relative amount of polytetrafluoroethylene molding powder.

[0045] Step 3: Mold Construction

[0046] In the following embodiments, the porous polyimide retainer has a porosity of 15-35% and a pore size of 0.7-2.5 μm. The retainer has an inner diameter d of 15-60 mm, an outer diameter D of 20-70 mm, with D / d = 1.1-1.4, and a height H of 7-16 mm. The present invention can be used to produce finished retainers of larger or smaller dimensions.

[0047] In the retainer mold: the outer diameter of the core shaft of the outer tube blank mold = the outer diameter of the core shaft of the inner tube blank mold = the said (d-2) mm, the inner diameter of the outer shell of the outer tube blank mold = the said (D+3) mm, the inner diameter of the outer shell of the inner tube blank mold < the inner diameter of the outer shell of the outer tube blank mold, the height of the inner and outer shells = the core shaft height > 4(H+3), the outer diameters of the inner and outer layer mold punches respectively match the inner diameters of their outer shells, the inner diameters of the inner and outer layer mold punches respectively match the outer diameters of their core shafts, the heights of the inner and outer layer mold punches are the same as their outer shells, the inner diameters of the inner and outer layer mold bases respectively match the outer diameters of their core shafts, the outer diameters of the inner and outer layer mold bases respectively match the inner diameters of their outer shells, and all are slidably matched with the mold cavity.

[0048] In the above cage molds, the outer tube mold is used to form the outer layer of the cage, while the inner tube mold is used to form the inner layer of the cage. The structure of the outer and inner tube molds is similar to that of existing porous polyimide forming molds (including an outer sleeve, core, punch, and base; for example, see CN109808114A for an introduction to traditional tubular forming molds). The cage preform is produced primarily by switching between the outer and inner tube molds (see step 4 for details).

[0049] Step 4: Pre-pressing of monoether anhydride polyimide molding powder

[0050] Place the inner tube mold filled with polyimide mixture on a program-controlled press and press it to 500-2000 kN / cm 2 , hold the pressure for 3-8 minutes and demould, put the inner tube preform after demoulding onto the core shaft of the outer tube mold, and then put another polyimide mixture into the mold, add a certain height limit fixture to the mold punch, that is, on the mold core shaft, and the limit fixture height is h 限位 , h 限位 =h 预制体 +h 底座 +h 冲头 -h 芯轴 , place the mold in the upper and lower clamps, place it on a program-controlled press and press it to 1000~5000kN / cm 2 and fix it with screws, keeping the pressure for 3-8 minutes.

[0051] Step 5: Double-layer matching fixed volume sintering molding

[0052] Place it in a sintering furnace, heat it to 360-380℃ after 60-90 minutes, keep it warm for 30-60 minutes and then the process ends. After taking it out, cool it to room temperature, remove the upper and lower clamps, and demold to obtain a porous polyimide cage material with a gradient pore structure.

[0053] The material prepared using the above method has the advantages of slow oil release and long lubrication life. At the same time, the interface between the two microporous structures is clear, the interface bonding force is strong, and it is not easy to delaminate.

[0054] The implementation process of the present invention is described in detail below with reference to specific embodiments.

[0055] 1. Specific embodiments of the porous polyimide cage material with a gradient pore structure, its preparation method, and bearing of the present invention are as follows:

[0056] Example 1

[0057] The porous polyimide retainer material with a gradient pore structure in this embodiment includes two inner and outer porous polyimide layers, the inner layer having a small porosity structure and the outer layer having a large porosity structure. The porosity and pore size characteristics of the inner and outer layers are detailed in Table 1. The porous polyimide retainer is suitable for an internal guidance method.

[0058] The method for preparing the porous polyimide cage material with a gradient pore structure of this embodiment includes the following steps:

[0059] ① Selection of monoether anhydride polyimide molding powder

[0060] Monoether anhydride polyimide molding powder is prepared by polycondensation and cyclization dehydration of 4.4-oxydiphthalic anhydride (ODPA) and 4.4 diaminodiphenyl ether (ODA). The molding powder particle size (D 50 )8μm, and the particle size of the molding powder used for the large porosity structure was obtained by graded sieving (D 50 )15μm.

[0061] ② Prepare polyimide blend according to weight percentage

[0062] The mixture used in the small porosity structure is divided into particle size (D 50 97% 8μm polyimide molding powder and 3% polytetrafluoroethylene molding powder were mixed in an FM high-speed mixer to prepare a polyimide blend. The polyimide blend was observed for color difference using a 20x microscope. A polyimide blend with no noticeable color difference was considered acceptable and was vacuum-sealed for future use. The macroporous structure was made of 100% polyimide.

[0063] ③Mold composition

[0064] The retainer's inner diameter is set to d = 29.0 mm, its outer diameter is set to D = 35.0 mm, and its height is set to H = 11.0 mm. In the retainer mold, the outer diameter of the mandrel of the outer tube mold is equal to the outer diameter of the mandrel of the inner tube mold, which is (d - 2) mm, which is 27.0 mm. The inner diameter of the outer shell of the outer tube mold is equal to (D + 3) mm, which is 38.0 mm. The inner diameter of the outer shell of the inner tube mold is less than the inner diameter of the outer shell of the outer tube mold. The inner diameter of the inner shell of the inner tube mold is controlled to be 32.0 mm. The height of the inner and outer shells is equal to the mandrel height > 4 (H + 3) = 56.0 mm. The outer shell height of the inner and outer molds is controlled to be 60 mm, the mandrel height is controlled to be 60 mm, the punch height is controlled to be 60 mm, and the base height is controlled to be 15 mm. The outer diameters of the inner and outer layer mold punches respectively match the inner diameters of their outer sleeves, the inner diameters of the inner and outer layer mold punches respectively match the outer diameters of their core shafts, the heights of the inner and outer layer mold punches are the same as their outer sleeves, the inner diameters of the inner and outer layer mold bases respectively match the outer diameters of their core shafts, the outer diameters of the inner and outer layer mold bases respectively match the inner diameters of their outer sleeves, and all are slidably matched with the mold cavity.

[0065] ④Monoether anhydride polyimide molding powder is pre-pressed

[0066] The mixture used for the small porosity structure is placed into the inner tube blank mold and placed on a program-controlled press to press to 500kN / cm 2 , hold the pressure for 3 minutes and demould, the height of the inner tube preform is 26.5mm, put the inner tube preform on the core shaft of the outer tube mold, and then put the mixture used for the large porosity structure into the outer tube mold, add a certain height limit fixture on the mold punch, that is, the mold core shaft, and the limit fixture height is h 限位 , h 限位 =h 预制体 +h 底座 +h 冲头 -h 芯轴 = (26.5 + 15 + 60 - 60) = 41.5 mm. Place the mold in the upper and lower fixtures and press it on a program-controlled press to 1000 kN / cm 2 , and fix it with screws and maintain pressure for 3 minutes.

[0067] ⑤Double-layer matching constant volume sintering molding

[0068] The material was placed in a sintering furnace, heated to 370° C. after 60 minutes, kept warm for 30 minutes, and the process ended. The material was taken out and cooled to room temperature, and demolded to obtain a porous polyimide cage material with a gradient pore structure.

[0069] Example 2

[0070] The porous polyimide retainer material with a gradient pore structure in this embodiment includes two inner and outer porous polyimide layers, the inner layer having a large porosity structure and the outer layer having a small porosity structure. The porosity and pore size characteristics of the inner and outer layers are detailed in Table 1. The porous polyimide retainer is suitable for external guidance.

[0071] The porous polyimide cage material with a gradient pore structure of this embodiment was prepared according to the method of Example 1. The difference from Example 1 is that:

[0072] In step ①, the particle size of the molding powder used for the small porosity structure is obtained by graded sieving (D 50 )13μm, the molding powder used for the macroporous structure was purchased from Shanghai Synthetic Resin Research Institute, the particle size (D 50 ) is 25μm.

[0073] In step ②, the mixture used for the small porosity structure is selected according to the weight percentage of the particle size (D 50 ) 90% of 13μm polyimide molding powder and 10% of polytetrafluoroethylene molding powder; the mixture used for the macroporous structure is selected by weight percentage. 50 ) 25μm polyimide molding powder 95%, polytetrafluoroethylene molding powder 5%.

[0074] In step ③, the inner diameter of the retainer is set to d = 51.0 mm, the outer diameter is set to D = 58.5 mm, and the height is set to H = 14.0 mm. In the retainer mold, the outer diameter of the mandrel of the outer tube mold is equal to the outer diameter of the mandrel of the inner tube mold, which is (d - 2) mm, which is 49.0 mm. The inner diameter of the outer shell of the outer tube mold is equal to (D + 3) mm, which is 61.5 mm. The inner diameter of the outer shell of the inner tube mold is controlled at 55.0 mm. The height of the inner and outer shells is equal to the mandrel height > 4 (H + 3) = 68.0 mm. The outer shell height of the inner and outer molds is controlled at 70 mm, the mandrel height is controlled at 70 mm, the punch height is controlled at 70 mm, and the base height is controlled at 15 mm.

[0075] In step ④, the mixture used for the large porosity structure is placed into the inner tube blank mold and placed on a program-controlled press to press to 1500kN / cm 2 , hold the pressure for 8 minutes and demould, the height of the inner tube preform is 32.0mm, put the inner tube preform on the core shaft of the outer tube mold, and then put the mixture used for the small porosity structure into the outer tube mold, the limit tooling height is h 限位 , h 限位 =h 预制体 +h 底座 +h 冲头 -h 芯轴 = (32.0 + 15 + 70 - 70) = 47.0 mm, placed on a program-controlled press and pressurized to 3000 kN / cm2 , maintain pressure for 5 minutes.

[0076] In step ⑤, the sintering process is to heat to 375°C after 70 minutes and keep at this temperature for 45 minutes before the program ends.

[0077] Example 3

[0078] The porous polyimide retainer material with a gradient pore structure in this embodiment includes two inner and outer porous polyimide layers, the inner layer having a small porosity structure and the outer layer having a large porosity structure. The porosity and pore size characteristics of the inner and outer layers are detailed in Table 1. The porous polyimide retainer is suitable for an internal guidance method.

[0079] The porous polyimide cage material with a gradient pore structure of this embodiment was prepared according to the method of Example 1. The difference from Example 1 is that:

[0080] In step ①, the particle size of the molding powder used for the small porosity structure is obtained by graded sieving (D 50 )17μm, the molding powder used for the macroporous structure was purchased from Shanghai Synthetic Resin Research Institute, the particle size (D 50 ) is 35μm.

[0081] In step ②, the mixture used for the small porosity structure is selected according to the weight percentage of the particle size (D 50 ) 17μm polyimide molding powder 90%, polytetrafluoroethylene molding powder 10%; the mixture used in the macroporous structure is selected according to the weight percentage of the particle size (D 50 ) 35μm polyimide molding powder 90%, polytetrafluoroethylene molding powder 10%.

[0082] In step ③, the retainer's inner diameter is set to d = 16.0 mm, its outer diameter is set to D = 21.5 mm, and its height is set to H = 7.5 mm. In the retainer mold, the outer diameter of the outer tube mold's mandrel is equal to the outer diameter of the inner tube mold's mandrel, which is (d - 2) mm, or 14.0 mm. The inner diameter of the outer shell of the outer tube mold is equal to (D + 3) mm, or 24.5 mm. The inner diameter of the inner tube mold's outer shell is controlled at 20.0 mm. The height of the inner and outer shells is equal to the mandrel height > 4 (H + 3) = 42.0 mm. The outer shell height of the inner and outer molds is controlled at 50 mm, the mandrel height is controlled at 50 mm, the punch height is controlled at 50 mm, and the base height is controlled at 15 mm.

[0083] In step ④, the mixture used for the small porosity structure is placed into the inner tube blank mold and placed on a program-controlled press to press to 1000kN / cm 2 , hold the pressure for 5 minutes and demould, the height of the inner tube preform is 23.5mm, put the inner tube preform on the core shaft of the outer tube mold, and then put the mixture used for the large porosity structure into the outer tube mold, the limit tooling height is h限位 , h 限位 =h 预制体 +h 底座 +h 冲头 -h 芯轴 = (23.5 + 15 + 50 - 50) = 38.5 mm, placed on a program-controlled press and pressurized to 4000 kN / cm 2 , maintain pressure for 5 minutes.

[0084] In step ⑤, the sintering process is to heat to 370°C after 70 minutes and keep at this temperature for 40 minutes before the program ends.

[0085] Example 4

[0086] The porous polyimide retainer material with a gradient pore structure in this embodiment includes two inner and outer porous polyimide layers, the inner layer having a large porosity structure and the outer layer having a small porosity structure. The porosity and pore size characteristics of the inner and outer layers are detailed in Table 1. The porous polyimide retainer is suitable for external guidance.

[0087] The porous polyimide cage material with a gradient pore structure of this embodiment was prepared according to the method of Example 1. The difference from Example 1 is that:

[0088] In step ①, the particle size of the molding powder used for the small porosity structure is obtained by graded sieving (D 50 ) 10 μm, the molding powder used for the macroporous structure was purchased from Shanghai Synthetic Resin Research Institute, the particle size (D 50 ) is 40μm.

[0089] In step ②, the mixture used for the small porosity structure is selected according to the weight percentage of the particle size (D 50 ) 10μm polyimide molding powder 97%, polytetrafluoroethylene molding powder 3%; the mixture used in the macroporous structure is selected according to the weight percentage of the particle size (D 50 ) 40μm polyimide molding powder 80%, polytetrafluoroethylene molding powder 20%.

[0090] In step ③, the inner diameter of the retainer is set to d = 40.0 mm, the outer diameter is set to D = 49.5 mm, and the height is set to H = 11.5 mm. In the retainer mold, the outer diameter of the mandrel of the outer tube mold is equal to the outer diameter of the mandrel of the inner tube mold, which is (d - 2) mm, which is 38.0 mm. The inner diameter of the outer shell of the outer tube mold is equal to (D + 3) mm, which is 52.5 mm. The inner diameter of the outer shell of the inner tube mold is controlled at 43.0 mm. The height of the inner and outer shells is equal to the mandrel height > 4 (H + 3) = 58.0 mm. The height of the inner and outer molds is controlled at 60 mm, the mandrel height is controlled at 60 mm, the punch height is controlled at 60 mm, and the base height is controlled at 15 mm.

[0091] In step ④, the mixture used for the large porosity structure is placed into the inner tube blank mold and placed on a program-controlled press to press to 2000kN / cm 2 , hold the pressure for 8 minutes and demould, the height of the inner tube preform is 37.0mm, put the inner tube preform on the core shaft of the outer tube mold, and then put the mixture used for the small porosity structure into the outer tube mold, the limit tooling height is h 限位 , h 限位 =h 预制体 +h 底座 +h 冲头 -h 芯轴 = (37.0 + 15 + 60 - 60) = 52.0 mm, placed on a program-controlled press and pressurized to 4000 kN / cm 2 , maintain pressure for 5 minutes.

[0092] In step ⑤, the sintering process is to heat to 380°C after 60 minutes and keep warm for 50 minutes before the program ends.

[0093] Example 5

[0094] The porous polyimide retainer material with a gradient pore structure in this embodiment includes two inner and outer porous polyimide layers, the inner layer having a small porosity structure and the outer layer having a large porosity structure. The porosity and pore size characteristics of the inner and outer layers are detailed in Table 1. The porous polyimide retainer is suitable for an internal guidance method.

[0095] The porous polyimide cage material with a gradient pore structure of this embodiment was prepared according to the method of Example 1. The difference from Example 1 is that:

[0096] In step ①, the particle size of the molding powder used for the small porosity structure is obtained by graded sieving (D 50 ) 20 μm, the molding powder used for the macroporous structure was purchased from Shanghai Synthetic Resin Research Institute, the particle size (D 50 ) is 30μm.

[0097] In step ②, the mixture used for the small porosity structure is selected according to the weight percentage of the particle size (D 50 ) 20μm polyimide molding powder 80%, polytetrafluoroethylene molding powder 20%; the mixture used in the macroporous structure is selected according to the weight percentage of the particle size (D 50 ) 30μm polyimide molding powder 95%, polytetrafluoroethylene molding powder 5%.

[0098] In step ③, the inner diameter of the retainer is set to d = 58.5 mm, the outer diameter is set to D = 68.0 mm, and the height is set to H = 15.5 mm. In the retainer mold, the outer diameter of the mandrel of the outer tube mold is equal to the outer diameter of the mandrel of the inner tube mold, which is (d - 2) mm, which is 56.5 mm. The inner diameter of the outer shell of the outer tube mold is equal to (D + 3) mm, which is 71.0 mm. The inner diameter of the outer shell of the inner tube mold is controlled at 65.0 mm. The height of the inner and outer shells is equal to the mandrel height > 4 (H + 3) = 74.0 mm. The height of the inner and outer molds is controlled at 80 mm, the mandrel height is controlled at 80 mm, the punch height is controlled at 80 mm, and the base height is controlled at 15 mm.

[0099] In step ④, the mixture used for the small porosity structure is placed into the inner tube blank mold and placed on a program-controlled press to press to 800kN / cm 2 , hold the pressure for 6 minutes and demould, the height of the inner tube preform is 39.5mm, put the inner tube preform on the core shaft of the outer tube mold, and then put the mixture used for the large porosity structure into the outer tube mold, the limit tooling height is h 限位 , h 限位 =h 预制体 +h 底座 +h 冲头 -h 芯轴 = (39.5 + 15 + 60 - 60) = 54.5 mm, placed on a program-controlled press and pressurized to 5000 kN / cm 2 , maintain pressure for 8 minutes.

[0100] In step ⑤, the sintering process is to heat to 370°C after 90 minutes and keep at this temperature for 60 minutes before the program ends.

[0101] Based on the above cage materials, conventional methods such as machining are used to process the cage, and then bearings of different specifications are produced.

[0102] 2. Experimental Examples

[0103] Experimental Example 1

[0104] The physical picture of the porous polyimide cage material prepared in Example 1 is shown in Figure 1. As can be seen from Figure 1, the interface between the two microporous structures is clear, and the interface can be located at the center line of the finished cage or at any position according to the bearing design.

[0105] In addition, since both structural materials are monoether anhydride polyimide, they have consistent molecular structures and strong interface bonding strength. After sintering and bonding, delamination is not likely to occur during the processing of the cage. The finished cage made using the cage material of Example 1 is shown in Figure 2.

[0106] Experimental Example 2

[0107] This experimental example illustrates the pore structure characteristics of the porous polyimide cages of various embodiments and tests their tensile strength. The test method is based on the GJB 9288-2017 standard. The specific results are shown in Table 1 below. To measure the porosity of the inner and outer layers, the remaining outer and inner layers were machined away, leaving the remaining portions for testing.

[0108] Table 1 Performance test results of porous polyimide cages in different embodiments

[0109] The results in Table 1 demonstrate that the porous polyimide cage material prepared by the present invention exhibits a distinct gradient pore structure, and the pore sizes of the outer and inner layers of the cage can be tailored to the operating requirements of the bearing. Furthermore, the porous polyimide cage material prepared by the present invention exhibits high tensile strength, lacks delamination at the fracture surface, and demonstrates excellent interfacial bonding.

[0110] The porous polyimide retainer with a gradient pore structure prepared in Example 1 was used to conduct a 600-h bearing bench running-in test. Under high temperature conditions (50°C), the current was stable. After the second disassembly, there was no excess lubricating oil inside the bearing, no wear marks on the outer diameter of the retainer, and clear wear marks on the pockets without diffusion, as shown in Figure 3.

[0111] The porous polyimide cage with gradient pore structure can be widely used in the field of controlled torque gyroscopes, momentum wheels, reaction flywheels, aerospace long-life bearing cages, meeting the future development needs of my country's aerospace long-life bearings, with significant economic and social benefits.

Claims

1. Porous polyimide cage material with gradient pore structure, It is characterized in that The porous polyimide retainer includes at least two porous polyimide layers combined together in the inner and outer directions, the porous polyimide layer close to the guide surface has a low porosity, and the porous polyimide layer away from the guide surface has a high porosity.

2. The porous polyimide cage material with gradient pore structure according to claim 1, It is characterized in that The porosity of the porous polyimide layer on the side farthest from the guide surface is 1.2 to 2 times the porosity of the porous polyimide layer on the side closest to the guide surface.

3. The porous polyimide cage material with gradient pore structure as claimed in claim 2, It is characterized in that The porous polyimide layer on the side farthest from the guide surface has a porosity of 20 to 35%.

4. The porous polyimide cage material having a gradient pore structure according to any one of claims 1 to 3, It is characterized in that The pore size of the porous polyimide layer on the side close to the guide surface is small, and the pore size of the porous polyimide layer on the side far from the guide surface is large.

5. The porous polyimide cage material with gradient pore structure as claimed in claim 4, It is characterized in that The pore size of the porous polyimide layer on the side farthest from the guide surface is 1.1 to 2.5 times the pore size of the porous polyimide layer on the side closest to the guide surface.

6. The porous polyimide cage material with gradient pore structure as claimed in claim 5, It is characterized in that The pore size of the porous polyimide layer on the side farthest from the guide surface is 0.9-2.5 μm.

7. A method for preparing a porous polyimide cage material having a gradient pore structure according to any one of claims 1 to 6, It is characterized in that The following steps are involved: (1) preparing raw materials for retainers with different pore structures, first feeding and pre-pressing the raw materials corresponding to one of the retainers with pore structures to obtain a preform; then feeding and pre-pressing the raw materials corresponding to the retainers with other pore structures inside or outside the preform to obtain a retainer preform; (2) Sintering the retainer preform.

8. The method for preparing the porous polyimide cage material with gradient pore structure according to claim 7, It is characterized in that The pre-pressing is an integral pressing, and the pressure of the first pre-pressing is 500-2000 kN / cm 2 The pressure of the last pre-pressing is 2 to 7 times of the pressure of the first pre-pressing; the holding time of the first pre-pressing and the last pre-pressing is 3 to 8 minutes.

9. The method for preparing the porous polyimide cage material with gradient pore structure according to claim 7, It is characterized in that In step (2), the sintering temperature is 360-380° C., and the heat preservation time is 30-60 minutes.

10. A method for preparing a porous polyimide cage material having a gradient pore structure as claimed in claim 7, 8 or 9, It is characterized in that The raw material consists of the following components in mass fraction: 80-100% of monoether anhydride type polyimide and 0-20% of polytetrafluoroethylene molding powder.

11. Bearings, including cages, It is characterized in that The retainer is made of the porous polyimide retainer material with a gradient pore structure according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Porous polyimide composite material for bearing retainer, preparation method of porous polyimide composite material and bearing retainer

    CN111763429A

  • Porous polyimide oil storage and retention structure and preparation method and application thereof

    CN113147105A

  • Two-stage porous polyimide material, preparation method thereof, two-stage porous polyimide retainer and application of two-stage porous polyimide retainer

    CN113510891A

  • Porous oil-containing intelligent lubricating material as well as preparation method and application thereof

    CN114149842A

  • Bearing holder

    JP1997236128A