Method for comprehensive utilization of lateritic nickel ore

By optimizing the smelting process of laterite nickel ore, combining wet and ignition smelting, and using iron and aluminum slag for resource recycling, the problems of high energy consumption and environmental pollution in the existing smelting process are solved, and efficient recycling and resources of nickel and cobalt are achieved. Comprehensive use of.

WO2024229597A1PCT designated stage expired Publication Date: 2024-11-14GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/092283
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The existing fire and wet smelting processes have problems such as high energy consumption, high cost, environmental pollution and equipment maintenance difficulties in the smelting process of laterite nickel ore, and it is difficult to effectively recover cobalt resources.

Method used

By optimizing the fire and wet smelting technology, wet and ignition smelting are carried out separately after ore separation, iron and aluminum slag in wet smelting is used as raw materials for fire smelting, water treatment and resource recycling are carried out, and nickel and Cobalt recovery rate and smelting of high ice nickel through pyrogenic method, reducing energy consumption and cost.

Benefits of technology

It has achieved low-cost and efficient smelting of laterite nickel ore, improved the recovery rate of nickel and cobalt, reduced environmental pollution, and improved resource utilization and product value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023092283_14112024_PF_FP_ABST
    Figure CN2023092283_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure relates to a method for comprehensive utilization of lateritic nickel ore, comprising the following steps: (1) carrying out ore dressing on lateritic nickel ore to obtain chromium concentrate, low-nickel low-magnesium ore and high-nickel high-magnesium ore; (2) pulping the low-nickel low-magnesium ore to obtain ore pulp, carrying out leaching, neutralization, continuous countercurrent washing, and solid-liquid separation on the ore pulp to obtain a filtrate and filter residues, carrying out neutralization and impurity removal on the filtrate to obtain iron-aluminum residues and a solution containing nickel and cobalt, and performing nickel and cobalt precipitation to obtain nickel-cobalt hydroxide; and (3) crushing, screening, drying and calcining the high-nickel high-magnesium ore, adding gypsum, smelting to obtain low-grade nickel matte, and carrying out oxidation blowing to obtain high-grade nickel matte; and (4) adding the filter residues and the iron-and aluminum residues obtained in step (2) to a sulfuric acid solution, filtering to obtain a filtrate and filter residues, evaporating and concentrating the obtained filtrate to obtain a water treatment coagulant, and separating gypsum from the obtained filter residues and reusing the gypsum in the smelting process in step (3).
Need to check novelty before this filing date? Find Prior Art

Description

A comprehensive utilization method of laterite nickel ore Technical Field

[0001] The present invention relates to the technical field of laterite nickel ore metallurgy, and in particular to a comprehensive utilization method of laterite nickel ore. Background Art

[0002] In recent years, with the continued promotion and popularization of new energy electric vehicles and consumer electronics, global demand for lithium-ion secondary batteries has exploded. This has led to a surge in demand for nickel and nickel-based compounds, key materials for lithium-ion secondary batteries. Currently, laterite nickel ore is the primary raw material for nickel products on the market, accounting for over 65%.

[0003] The smelting of laterite nickel ore mainly falls into two categories: pyrometallurgy and hydrometallurgy. Conventional pyrometallurgy mainly uses the rotary kiln pre-reduction-electric furnace smelting process (RKEF). The advantages of this process are high-quality nickel-iron products and a relatively simple process flow. However, its disadvantages are high energy consumption, and it is only suitable for processing laterite nickel ores with higher nickel grades, and it cannot recover cobalt. Hydrometallurgy mainly utilizes the high-pressure acid leaching process. The high-pressure acid leaching process has great advantages in processing low-grade laterite nickel ores with high cobalt and iron content, and it consumes less energy. However, its disadvantages are high plant construction costs, and due to the proneness of corrosion and scaling during the production process, the autoclave equipment must be regularly maintained. Therefore, the existing pyrometallurgy and hydrometallurgy processes have obvious shortcomings in the smelting process of laterite nickel ore.

[0004] Summary of the Invention

[0005] The present disclosure aims to address at least one of the technical problems existing in the related art. To this end, the present disclosure proposes a comprehensive utilization method for laterite nickel ore. This method rationally optimizes the processes of pyrometallurgical and hydrometallurgical smelting based on their process characteristics. The method processes the ferroaluminum slag produced during hydrometallurgical smelting and uses it as a raw material for pyrometallurgical smelting and water treatment. This method transforms the ferroaluminum slag, previously treated as hazardous waste, into valuable resources, increasing its economic value and reducing environmental pollution.

[0006] The above technical objectives of the present disclosure are achieved through the following technical solutions:

[0007] A comprehensive utilization method of laterite nickel ore comprises the following steps:

[0008] (1) beneficiating laterite nickel ore to obtain chromium concentrate, low-nickel and low-magnesium ore, and high-nickel and high-magnesium ore, wherein the chromium content in the chromium concentrate is ≥20wt%, the nickel content in the low-nickel and low-magnesium ore is ≤1.5wt%, and the magnesium content is ≤3wt%, and the nickel content in the high-nickel and high-magnesium ore is ≥1.5wt%, and the magnesium content is >3wt%;

[0009] (2) Wet smelting: pulping the low-nickel, low-magnesium ore obtained in step (1) to obtain a pulp, leaching the pulp, neutralizing it, continuously countercurrent washing it, and performing solid-liquid separation to obtain a filtrate and a filter residue, neutralizing and removing impurities from the filtrate to obtain an iron-aluminum slag and a solution containing nickel and cobalt, and precipitating nickel and cobalt to obtain nickel cobalt hydroxide;

[0010] (3) pyrometallurgy: crushing, screening, drying, calcining, adding gypsum, smelting to obtain low-grade nickel matte, and then oxidizing and blowing to obtain high-grade nickel matte;

[0011] (4) adding the filter residue and iron-aluminum slag obtained in step (2) into a sulfuric acid solution, filtering to obtain a filtrate and filter residue, evaporating and concentrating the obtained filtrate to obtain a water treatment coagulant, separating gypsum from the obtained filter residue and recycling it to the smelting process of step (3).

[0012] In one embodiment, in step (1), the ore dressing is carried out by using one of a trough ore washer, a spiral chute or a shaking table.

[0013] In one embodiment, in step (2), the solid content of the slurry is 30 wt%-40 wt%, and the mass ratio of particles with a particle size of 8 μm to the total solids is greater than 80%.

[0014] In one embodiment, the moisture content of the high-nickel and high-magnesium ore is 30wt%-40wt%, and the particle size of the high-nickel and high-magnesium ore after crushing is less than 25mm.

[0015] In one embodiment, in step (2), the leaching includes oxygen pressure leaching or high pressure leaching.

[0016] In one embodiment, the temperature of the oxygen pressure leaching is 170-185° C., the leaching pressure is 1.8-2.0 MPa, and the leaching time is 0.5-2.0 h.

[0017] In one embodiment, the high-pressure leaching temperature is 250-260° C., the leaching pressure is 4.3-5.2 MPa, and the leaching time is 0.5-2.0 h.

[0018] In one embodiment, in step (2), the neutralization before the continuous countercurrent washing refers to adding limestone slurry for neutralization, and the pH value after the neutralization with the limestone slurry is 1.5-2.0.

[0019] In one embodiment, in step (2), the continuous countercurrent washing refers to performing six or seven stages of countercurrent washing using a thickener, wherein the overflow of the first stage thickener is fed into the iron and aluminum removal process, and the bottom flow of the final stage thickener is fed into the tailings neutralization process.

[0020] In one embodiment, in step (2), the neutralization and impurity removal refers to adding limestone slurry and a mixed gas containing SO2 to the filtrate for neutralization and impurity removal, controlling the pH of the reaction to be 3.5-4.5 and the reaction temperature to be 55-65°C.

[0021] In one embodiment, in step (2), the mixed gas is a mixture of compressed air and SO2 gas, the volume proportion of SO2 in the mixed gas is 0.5%-1%, and the pressure of the mixed gas is 0.2-0.5 MPa.

[0022] In one embodiment, in step (2), magnesium oxide is added to the nickel-cobalt-containing solution to precipitate nickel and cobalt, and the pH of the reaction is controlled to be 6.5-7.5.

[0023] In one embodiment, in step (3), the drying temperature is 350-400° C., and the moisture content of the high-nickel and high-magnesium ore after drying is 20wt%-22wt%.

[0024] In one embodiment, in step (3), a reducing agent and limestone are added during calcination to obtain roasted sand, and the reducing agent is at least one of blue coke and anthracite.

[0025] In one embodiment, in step (3), the calcination is carried out in a rotary kiln, the calcination temperature is 750-850°C, the calcination time is 1-3 hours, and the temperature of the roasted sand is 700-750°C when it is taken out of the kiln after calcination.

[0026] In one embodiment, in step (3), the mass ratio of the high-nickel and high-magnesium ore, the reducing agent, and the limestone added during calcination is 100:(5-10):(1-10).

[0027] In one embodiment, in step (3), the smelting is carried out in a side-blown furnace, specifically, roasted sand is added to the side-blown furnace, and sulfur, reducing agent and gypsum are added by side blowing.

[0028] In one embodiment, in step (3), the smelting temperature is 1500-1600° C., and the smelting time is 2-3 hours.

[0029] In one embodiment, in step (3), the mass ratio of calcined sand: sulfur: reducing agent: gypsum added during smelting is 100: (2-10): (5-10): (5-10).

[0030] In one embodiment, in step (3), the nickel content in the obtained low-grade nickel matte is 12 wt%-30 wt%.

[0031] In one embodiment, in step (3), after being smelted out of the furnace, the temperature of the low-grade nickel matte is 1400-1500°C.

[0032] In one embodiment, in step (3), the steel is transferred from a ladle to a converter for intermittent blowing or a top-blown furnace is used for continuous operation to produce high-grade nickel matte.

[0033] In one embodiment, in step (3), the temperature of the oxidative blowing is 1300-1400° C., and the blowing time is 6-8 hours.

[0034] In one embodiment, in step (3), the nickel content in the obtained high-grade nickel matte is 60wt%-75wt%.

[0035] In one embodiment, in step (3), the converted slag produced by the converting process is returned to the smelting process for preparing low-grade nickel matte. The nickel content in the converted slag is 0.6 wt% to 1.5 wt%.

[0036] In one embodiment, in step (3), the high-temperature flue gas generated in the side-blown furnace in the smelting process is returned to the rotary kiln in the calcining process and used as a heat source. The temperature of the high-temperature flue gas generated in the smelting process is 1100-1300°C.

[0037] In one embodiment, in step (3), the flue gas after heat utilization in the calcination process is treated with limestone desulfurization and then discharged.

[0038] In one embodiment, in step (3), the gypsum slag left after the treatment of the flue gas from the rotary kiln in the calcining process is dried and added to the side-blown furnace in the smelting process to participate in the sulfidation and slag formation of the low-grade nickel matte.

[0039] In one embodiment, in step (4), the concentration of the sulfuric acid solution is 10 wt%-30 wt%.

[0040] In one embodiment, a comprehensive utilization method of laterite nickel ore comprises the following steps:

[0041] (1) beneficiating laterite nickel ore to obtain chromium concentrate, low-nickel and low-magnesium ore, and high-nickel and high-magnesium ore, wherein the chromium concentrate has a chromium content of ≥20wt%, the low-nickel and low-magnesium ore has a nickel content of ≤1.5wt% and a magnesium content of ≤3wt%, and the high-nickel and high-magnesium ore has a nickel content of ≥1.5wt% and a magnesium content of >3wt%;

[0042] (2) Wet smelting: the low-nickel, low-magnesium ore obtained in step (1) is pulped to obtain a pulp, and then oxygen pressure leaching or high-pressure leaching is performed, limestone slurry is added for neutralization, and then continuous countercurrent washing is performed, and solid-liquid separation is performed to obtain a filtrate and a filter residue, limestone slurry and a mixed gas containing SO2 are added to the filtrate to obtain iron-aluminum slag and a solution containing nickel and cobalt, and magnesium oxide is added to the nickel and cobalt solution to obtain nickel and cobalt hydroxide;

[0043] (3) pyrometallurgy: crushing the high-nickel and high-magnesium ore obtained in step (1), screening it, drying it, adding a reducing agent and limestone, calcining it to obtain roasted sand, then adding a reducing agent, sulfur and gypsum, and smelting it to obtain low-grade nickel matte, and then oxidizing and blowing the low-grade nickel matte to obtain high-grade nickel matte;

[0044] (4) adding the filter residue and iron-aluminum slag obtained in step (2) into a sulfuric acid solution, filtering to obtain a filtrate and filter residue, evaporating and concentrating the obtained filtrate to obtain a water treatment coagulant, separating gypsum from the obtained filter residue and recycling it to the smelting process of step (3).

[0045] The beneficial effects of the present disclosure are:

[0046] (1) The present invention discloses a comprehensive utilization method of laterite nickel ore, which is to separate the laterite nickel ore by beneficiation, and adopt different smelting methods for laterite nickel ores with different nickel contents, thereby reducing production costs and improving production stability; wherein, chrome concentrate can be directly sold, low-nickel and low-magnesium ore is made into slurry and sent to hydrometallurgy, and high-nickel and high-magnesium ore is sent to pyrometallurgy; in the hydrometallurgy, the slurry is subjected to high-pressure acid leaching or oxygen pressure leaching, leaching neutralization, continuous countercurrent washing, neutralization and impurity removal, and nickel and cobalt precipitation to obtain nickel hydroxide; in the pyrometallurgy, the laterite nickel ore is dried in a drying kiln, calcined in a rotary kiln, smelted in a side-blown furnace, and oxidized and blown in a converter or top-blown furnace to obtain high-grade nickel matte; and at the same time, the process is optimized according to the process characteristics of hydrometallurgy and pyrometallurgy:

[0047] The pH of the filtrate after continuous countercurrent washing in the wet smelting process is about 3, and the Fe ion concentration in the filtrate is 3-5g / L. The present invention adopts a hydrolysis method to remove Fe. Compared with the iron removal by yellow sodium ferroaluminate, the hydrolysis method produces less slag. When removing iron and aluminum from the filtrate, the pH is controlled at 3.5-4.5 and the temperature is 55-65°C. Limestone slurry is added to neutralize the H generated by the hydrolysis reaction. + The reactions are as follows: 2FeSO4+O2+2H2O=2FeOOH+2H2SO4; Al2(SO4)3+6H2O=2Al(OH)3+3H2SO4; H2SO4+CaCO3=CaSO4+H2O+CO2;

[0048] The main components of ferroaluminum slag are FeOOH, Al(OH)3, and CaSO4. The ferroaluminum slag produced in the past was treated as hazardous waste, which required a lot of manpower, material and financial resources. The present invention adds dilute sulfuric acid to the ferroaluminum slag, and the iron and aluminum are dissolved into sulfates. The insoluble CaSO4 (gypsum) is separated into solid and liquid and dried before being added to the oxygen-enriched side-blown furnace smelting process. At high temperatures, CaSO4 decomposes into calcium oxide and sulfur dioxide, participating in the sulfidation of low-matte nickel, and calcium oxide is used as a slag-forming agent. The iron and aluminum sulfate solution is evaporated and concentrated and used as a coagulant for water treatment. A small amount of nickel and cobalt entrained in the ferroaluminum slag enters the water treatment together with the ferroaluminum sulfate solution and enters the recycling process.

[0049] (2) The present invention adopts wet smelting and pyrometallurgical smelting according to the different nickel contents in laterite nickel ore. Among them, the pyrometallurgical smelting adopts the oxygen-enriched side-blowing method to produce high-grade nickel matte, which replaces the traditional RKEF smelting of nickel iron. Compared with the oxygen-enriched side-blowing method, the energy consumption is lower and the requirement for the grade of laterite nickel ore is also lower. The high-grade nickel matte product has higher economic value in subsequent production. At the same time, according to the process characteristics of the pyrometallurgical and wet metallurgical methods, the process is optimized, and the iron-aluminum slag produced in the wet smelting is separated. The obtained calcium sulfate is dried and added to the oxygen-enriched side-blowing furnace to participate in the sulfidation and slagging of low-grade nickel matte, and the iron and aluminum are converted into sulfate solution as a coagulant for water treatment in the smelter. The gypsum slag produced after flue gas desulfurization in the wet smelting is also added to the oxygen-enriched side-blowing furnace for utilization. This method realizes the comprehensive utilization of resources, improves the mining value of laterite nickel ore, and reduces product costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] FIG1 is a flow chart of Example 1 of the present disclosure. DETAILED DESCRIPTION

[0051] The present disclosure is further described below with reference to specific embodiments.

[0052] Example 1:

[0053] A comprehensive utilization method of laterite nickel ore, as shown in FIG1 , comprises the following steps:

[0054] (1) The laterite nickel ore is beneficiated by a trough-type ore washer to obtain chromium concentrate, low-nickel and low-magnesium ore and high-nickel and high-magnesium ore, wherein the chromium content in the chromium concentrate is ≥20wt%, which can be directly sold. The mass proportion of the components of the low-nickel and low-magnesium ore is as shown in Table 1-1:

[0055] Table 1-1: Composition of low nickel and low magnesium ores

[0056] The mass ratio of the components of high nickel and high magnesium ore is shown in Table 1-2:

[0057] Table 1-2: Composition of high nickel and high magnesium ore

[0058] (2) Wet smelting: The low-nickel, low-magnesium ore obtained in step (1) is modulated into a slurry with a solid content of 35%, and the mass ratio of particles with a particle size of 8 μm to the total solid is greater than 80%. The ore is subjected to high-pressure leaching at a temperature and pressure of 250° C. and 4.5 MPa for 1 hour. After high-pressure leaching, limestone slurry is added to neutralize the excess acid in the leaching process. The pH value after neutralization is controlled at 1.5. After six-stage continuous countercurrent washing, solid-liquid separation is performed to obtain a filtrate and a filter residue. Limestone slurry and a mixed gas composed of compressed air and SO2 are added to the filtrate. The volume ratio of SO2 in the mixed gas is 0.8%, the pressure of the mixed gas is 0.3 MPa, the pH of the reaction is controlled to 4, and the reaction temperature is 60° C. to obtain iron-aluminum slag and a solution containing nickel and cobalt. Magnesium oxide is added to the solution containing nickel and cobalt to control the pH of the reaction to 7 to obtain a nickel-cobalt intermediate product. The mass ratios of the components of the nickel-cobalt intermediate product are shown in Table 1-3 below.

[0059] Table 1-3: Composition of nickel-cobalt intermediate products

[0060] (3) Fire smelting: The high nickel and high magnesium ore obtained in step (1) has a moisture content of 35 wt%. The high nickel and high magnesium ore is crushed to a particle size of less than 20 mm, sieved, and passed through a drying kiln to remove free water and part of the crystal water. The moisture content of the dry ore is 20%. After drying, blue coke and limestone are added. The high nickel and high magnesium ore: blue coke: limestone are added in a mass ratio of 100:10:5 and calcined in a rotary kiln. The calcination temperature is 800 ° C. The calcination time is 2 h. The calcined sand is obtained by pre-reduction and then enters an oxygen-enriched side-blown furnace. Gypsum separated from the wet smelting iron and aluminum slag and gypsum slag produced by flue gas desulfurization are added. Sulfur and blue coke are added for smelting. The smelting temperature is 1550 ° C. The time is 3h to obtain low-grade nickel matte, wherein the mass ratio of roasted sand: semi-coke: sulfur: gypsum is 100:10:6:8, and the low-grade nickel matte is transferred to the converter through the ladle and enters the converter for oxidation blowing to obtain high-grade nickel matte product. The oxidation blowing temperature is 1300℃, and the blowing time is 8h. The blowing slag is returned to the oxygen-enriched side-blowing furnace. The nickel content in the blowing slag is 1.0wt%. The high-temperature flue gas generated in the side-blowing furnace in the smelting process is returned to the rotary kiln in the calcining process as a heat source. The temperature of the high-temperature flue gas generated in the smelting process is about 1200℃. The flue gas after heat utilization in the calcining process is discharged after limestone desulfurization treatment. The mass proportion of the components of the obtained high-grade nickel matte product is as shown in Table 1-4 below;

[0061] Table 1-4: Composition of high-grade nickel matte products

[0062] (4) The filter residue and iron-aluminum slag obtained in step (2) are added to a 20 wt% sulfuric acid solution, filtered to obtain a filtrate and filter residue, the obtained filtrate is evaporated and concentrated to obtain a water treatment coagulant, and the gypsum is separated from the obtained filter residue and reused in the smelting process of step (3).

[0063] The nickel recovery rate of the hydrometallurgy in Example 1 is 94%, and the nickel recovery rate of the pyrometallurgy is 90%.

[0064] Example 2:

[0065] A comprehensive utilization method of laterite nickel ore comprises the following steps:

[0066] (1) The laterite nickel ore is beneficiated through a spiral chute to obtain chromium concentrate, low-nickel and low-magnesium ore and high-nickel and high-magnesium ore. The chromium content in the chromium concentrate is ≥20wt%, which can be sold directly. The mass proportion of the components of the low-nickel and low-magnesium ore is as shown in Table 2-1:

[0067] Table 2-1: Composition of low nickel and low magnesium ores

[0068] The mass ratio of the components of high nickel and high magnesium ore is shown in Table 2-2:

[0069] Table 2-2: Composition of high nickel and high magnesium ore

[0070] (2) Wet smelting: The low-nickel, low-magnesium ore obtained in step (1) is modulated into a slurry with a solid content of 35%, and the mass ratio of particles with a particle size of 8 μm to the total solid is greater than 80%. The ore is subjected to oxygen pressure leaching at a temperature and pressure of 180°C and 1.8 MPa for 1 hour. After high-pressure leaching, limestone slurry is added to neutralize the excess acid in the leaching process. The pH value after neutralization is controlled at 1.5. After six-stage continuous countercurrent washing, solid-liquid separation is performed to obtain a filtrate and a filter residue. Limestone slurry and a mixed gas composed of compressed air and SO2 are added to the filtrate. The volume ratio of SO2 in the mixed gas is 0.8%, the pressure of the mixed gas is 0.3 MPa, the pH of the reaction is controlled to 4, and the reaction temperature is 60°C to obtain iron-aluminum slag and a solution containing nickel and cobalt. Magnesium oxide is added to the nickel-cobalt solution to control the pH of the reaction to 7 to obtain a nickel-cobalt intermediate product. The mass ratios of the components of the nickel-cobalt intermediate product are shown in Table 2-3 below.

[0071] Table 2-3: Composition of nickel-cobalt intermediate products

[0072] (3) Fire smelting: The high nickel and high magnesium ore obtained in step (1) has a moisture content of 35 wt%. The high nickel and high magnesium ore is crushed to a particle size of less than 20 mm, sieved, and passed through a drying kiln to remove free water and part of the crystal water. The moisture content of the dry ore is 20%. After drying, blue coke and limestone are added. The high nickel and high magnesium ore: blue coke: limestone are added in a mass ratio of 100:10:5 and calcined in a rotary kiln. The calcination temperature is 800 ° C. The calcination time is 2 h. The calcined sand is obtained by pre-reduction and then enters an oxygen-enriched side-blown furnace. Gypsum separated from the wet smelting iron and aluminum slag and gypsum slag produced by flue gas desulfurization are added. Sulfur and blue coke are added for smelting. The smelting temperature is 1550 ° C. The time is 3 hours to obtain low-grade nickel matte, wherein the mass ratio of roasted sand: semi-coke: sulfur: gypsum is 100:10:6:8, and the low-grade nickel matte is transferred to the converter through the ladle and enters the converter for oxidation blowing to obtain high-grade nickel matte product. The oxidation blowing temperature is 1400°C, and the blowing time is 6 hours. The blowing slag is returned to the oxygen-enriched side-blowing furnace, and the nickel content in the blowing slag is 1.0wt%. The high-temperature flue gas generated in the side-blowing furnace in the smelting process is returned to the rotary kiln in the calcining process as a heat source. The temperature of the high-temperature flue gas generated in the smelting process is about 1200°C. The flue gas after heat utilization in the calcining process is discharged after desulfurization treatment with limestone. The mass proportion of the components of the obtained high-grade nickel matte product is as shown in Table 2-4 below;

[0073] Table 2-4: Composition of high-grade nickel matte products

[0074] (4) The filter residue and iron-aluminum slag obtained in step (2) are added to a 20 wt% sulfuric acid solution, filtered to obtain a filtrate and filter residue, the obtained filtrate is evaporated and concentrated to obtain a water treatment coagulant, and the gypsum is separated from the obtained filter residue and reused in the smelting process of step (3).

[0075] The nickel recovery rate of the hydrometallurgy in Example 2 is 93.5%, and the nickel recovery rate of the pyrometallurgy is 89%.

Claims

1. A comprehensive utilization method of laterite nickel ore, Features: The following steps are involved: (1) beneficiating laterite nickel ore to obtain chromium concentrate, low-nickel and low-magnesium ore and high-nickel and high-magnesium ore, wherein the chromium content in the chromium concentrate is ≥20wt%, the nickel content in the low-nickel and low-magnesium ore is ≤1.5wt%, and the magnesium content is ≤3wt%, and the nickel content in the high-nickel and high-magnesium ore is ≥1.5wt%, and the magnesium content is >3wt%; (2) hydrometallurgy: pulping the low-nickel and low-magnesium ore obtained in step (1) to obtain ore pulp, leaching the ore pulp, neutralizing, continuously countercurrent washing, solid-liquid separation to obtain filtrate and filter residue, neutralizing and removing impurities from the filtrate to obtain iron-aluminum slag and a solution containing nickel and cobalt, and precipitating nickel and cobalt to obtain nickel-cobalt hydroxide; (3) pyrometallurgy: crushing, screening, drying, calcining, adding gypsum, smelting to obtain low-grade nickel matte, and then oxidizing and blowing to obtain high-grade nickel matte; (4) adding the filter residue and iron-aluminum slag obtained in step (2) into a sulfuric acid solution, filtering to obtain a filtrate and a filter residue, evaporating and concentrating the obtained filtrate to obtain a water treatment coagulant, separating gypsum from the obtained filter residue and recycling it to the smelting process of step (3).

2. A comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (1), the ore dressing is carried out by using one of a trough ore washer, a spiral chute or a shaking table.

3. A comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (2), the solid content of the slurry is 30wt%-40wt%, and the mass ratio of particles with a particle size of 8um to the total solids is greater than 80%.

4. A comprehensive utilization method of laterite nickel ore according to claim 1, Features: The water content of the high-nickel and high-magnesium ore is 30wt%-40wt%, and the particle size of the high-nickel and high-magnesium ore after crushing is less than 25mm.

5. A comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (2), the leaching includes oxygen pressure leaching or high pressure leaching.

6. A comprehensive utilization method of laterite nickel ore according to claim 5, Features: The temperature of the oxygen pressure leaching is 170-185° C., the leaching pressure is 1.8-2.0 MPa, and the leaching time is 0.5-2.0 h.

7. A comprehensive utilization method of laterite nickel ore according to claim 5, Features: The high-pressure leaching temperature is 250-260° C., the leaching pressure is 4.3-5.2 MPa, and the leaching time is 0.5-2.0 h.

8. A comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (2), the neutralization before continuous countercurrent washing refers to adding limestone slurry for neutralization, and the pH value after neutralization by adding limestone slurry is 1.5-2.

0.

9. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: The continuous countercurrent washing refers to using a thickener to perform six-stage or seven-stage countercurrent washing, wherein the overflow of the first-stage thickener enters the iron and aluminum removal process, and the bottom flow of the last-stage thickener enters the tailings neutralization process for treatment.

10. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (2), the neutralization and impurity removal refers to adding limestone slurry and a mixture containing SO 2 The mixed gas is neutralized and impurities are removed, the pH of the reaction is controlled to be 3.5-4.5, and the reaction temperature is 55-65°C.

11. A comprehensive utilization method of laterite nickel ore according to claim 10, Features: In step (2), the mixed gas is compressed air and SO 2 A mixture of gases, wherein SO 2 The volume proportion is 0.5%-1%, and the pressure of the mixed gas is 0.2-0.5MPa.

12. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (2), magnesium oxide is added to the nickel-cobalt-containing solution to precipitate nickel and cobalt, and the pH of the reaction is controlled to be 6.5-7.

5.

13. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), the drying temperature is 350-400° C., and the moisture content of the high-nickel and high-magnesium ore after drying is 20wt%-22wt%.

14. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), a reducing agent and limestone are added during calcination to obtain roasted sand, and the reducing agent is at least one of blue coke and anthracite.

15. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), the calcination is carried out in a rotary kiln, the calcination temperature is 750-850° C., and the calcination time is 1-3 hours.

16. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), the mass ratio of the high-nickel and high-magnesium ore, the reducing agent and the limestone added during calcination is 100:(5-10):(1-10).

17. The comprehensive utilization method of laterite nickel ore according to claim 14, Features: In step (3), the smelting is carried out in a side-blown furnace, specifically, roasted sand is added into the side-blown furnace, and sulfur, reducing agent and gypsum are added by side blowing at the same time.

18. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), the smelting temperature is 1500-1600°C, and the smelting time is 2-3h.

19. The comprehensive utilization method of laterite nickel ore according to claim 17, Features: In step (3), the mass ratio of roasted sand: sulfur: reducing agent: gypsum added during smelting is 100: (2-10): (5-10): (5-10).

20. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), the nickel content in the obtained low-grade nickel matte is 12wt%-30wt%.

21. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), the steel is transferred from the ladle to a converter for intermittent blowing or a top-blown furnace is used for continuous operation to produce high-grade nickel matte.

22. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), the temperature of the oxidative blowing is 1300-1400° C., and the blowing time is 6-8 hours.

23. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), the nickel content in the obtained high-grade nickel matte is 60wt%-75wt%.

24. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), the blowing slag produced by blowing is returned to the smelting process for preparing low-grade nickel matte, and the nickel content in the blowing slag is 0.6wt%-1.5wt%.

25. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), the high-temperature flue gas generated in the side-blown furnace in the smelting process is returned to the rotary kiln in the calcining process and used as a heat source. The temperature of the high-temperature flue gas generated in the smelting process is 1100-1300°C.

26. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), the flue gas after heat utilization in the calcination process is discharged after being treated with limestone desulfurization.

27. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (3), the gypsum slag left after the treatment of the flue gas in the rotary kiln in the calcining process is dried and added to the side-blown furnace in the smelting process to participate in the sulfidation and slag-making of low-grade nickel matte.

28. The comprehensive utilization method of laterite nickel ore according to claim 1, Features: In step (4), the concentration of the sulfuric acid solution is 10wt%-30wt%.

Citation Information

Patent Citations

  • Comprehensive reutilization method for laterite-nickel ore

    CN101285128A

  • Method for leaching nickel and cobalt form low-iron and high-magnesium and high-iron and low-magnesium laterite-nickel ore by using waste dilute sulphuric acid

    CN102876892A

  • Method for leaching valuable metals from laterite nickel ore by sulfuric acid under normal pressure

    CN111118285A

  • Method for producing battery-grade nickel sulfate by means of laterite nickel ore

    CN112080636A