Copolymerized silicon having comb-like structure and controllable branched chain length, and preparation method therefor and use thereof
By preparing comb-shaped structure copolymer silicon with controllable branch length, the problems of poor compatibility and insufficient interface adhesion of polymer materials in functional surface modification and processability adjustment are solved, and the hydrophobic and oil-eating of the materials are achieved and chemical solvent resistance, suitable for a variety of application fields, especially in wearable materials.
Patent Information
- Application Number
- PCT/CN2023/092477
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-11-14
AI Technical Summary
Existing polymer materials have problems such as poor compatibility, insufficient interface adhesion and high surface polarity in functional surface modification and processability adjustment, especially in the field of wearable materials, which are difficult to meet hydrophobic, oleophobic and chemical solvent resistance. demand.
Using a comb-like structure with controll length, acrylate monomer, olefin-terminal silicone, initiator and water are prepared by mixing and heating polymerizing aromatic vinyl monomer, acrylate monomer, olefin-terminal silicone, initiator and water. The branched comb-like structure copolymer silicon uses water as an environmentally friendly solvent. It has a simple process and low cost, ensuring product stability and wide application.
It has achieved low surface polarity of polymer materials, obtained hydrophobic and oleophobic properties, improved processing rheology, improved outdoor service life of materials, and is suitable for smart wearable fields, with broad application prospects and industrial value.
Smart Images

Figure CN2023092477_14112024_PF_FP_ABST
Abstract
Description
A comb-like structured copolymer silicon with controllable branch chain length and its preparation method and application Technical Field
[0001] The invention relates to a preparation method and application of a comb-structured copolymer silicon with controllable branch chain length, which can be used for surface modification and processability adjustment of functional polymers, and belongs to the field of polymer materials. Background Art
[0002] With the advancement of modern industrial and agricultural science and technology, the use of polymer materials has gradually penetrated into all areas of industrial and agricultural production. However, with the development of industries such as automobiles and home appliances, people's demand for more aesthetically pleasing and higher-performance polymer materials continues to grow. In particular, with the development of artificial intelligence, the demand for wearable materials has increased rapidly. The new generation of high-performance polymer materials must not only possess excellent mechanical properties, but also a series of new characteristics such as high surface quality, good tactile feel, and self-cleaning properties.
[0003] Silicone materials combine the properties of both organic and inorganic materials, boasting low surface tension, low surface energy, high temperature resistance, and oxidation resistance. Consequently, they are gaining increasing attention in the modification of functional materials, being used to improve surface properties or impart special properties such as self-cleaning. However, compatibility issues exist between silicone-based resins and conventional polymer materials. A common approach involves adding compatibilizers, such as those described in CN108219447A and CN111234467A, which use ethylene acrylic acid copolymer (EAA) or conventional maleic anhydride grafts as compatibilizers. However, these compatibilizers lack silicon chains and are linear in structure, resulting in poor compatibility with polysiloxanes.
[0004] Copolymerization of an organopolysiloxane containing a free radical polymerizable group and a free radical polymerizable monomer is also a feasible means. The prior art proposes a vinyl polymer obtained by copolymerizing a reactive dimethyl polysiloxane and an alkyl acrylate, which can be used as a compatibilizer or a special coating. However, the compatibility of this linear structure containing silicone with other raw materials is still low, resulting in poor stability and poor interfacial adhesion. CN201380049545.5 and CN201510526256.0 respectively proposed a dendritic and branched silicone resin, which have better interfacial bonding strength than a linear structure, but their structural design is not conducive to fully utilizing the low surface energy characteristics of silicone. CN202110082325.9 discloses a method for preparing an organosiloxane and a polyester elastomer by reactive extrusion. When this structure is used as a compatibilizer, the interfacial strength is effectively improved, but the structure of the polyester elastomer is limited in applicability. In addition, the reactive extrusion process makes it difficult to increase the silicon content, making it difficult to achieve low surface polarity. This greatly limits its applications in high-surface, good touch, and wearable applications. Technical issues
[0005] In response to the deficiencies in the prior art, the present invention aims to provide a method for preparing and applying a comb-like copolymerized silicon with controllable branch length. The copolymerized silicon of the present invention can be applied to the surface modification of functional materials to obtain surface hydrophobicity, oleophobicity, chemical solvent resistance, and a special feel, as well as to improve processability in blending and modification. The process route selected in the present invention is easy to control, has low production costs, is easily available for equipment, uses water as the reaction medium, has low environmental pollution, and is simple to use. The product can be widely used in the fields of home appliances, automobiles, packaging, medical treatment, wearables, aviation, etc. It has very broad application prospects and industrial value. Technical Solutions
[0006] The present invention is achieved through the following technical solutions:
[0007] A comb-like structured copolymer silicon with controllable branch chain length, the preparation method of which comprises the following steps: mixing an aromatic vinyl monomer, an acrylate monomer, an olefin-terminated organosilicon, an initiator, a molecular weight regulator and water, and then heating and polymerizing the mixture to prepare a comb-like structured copolymer silicon with controllable branch chain length.
[0008] The comb-like structured copolymer silicon with controllable branch chain length disclosed in the present invention overcomes the defects of the existing technology. It is a green, environmentally friendly, simple process, with controllable branch chain molecular weight, regular branch chain structure, low residue, and easy to use comb-like structured copolymer silicon product. It can be used to reduce the surface polarity of polymers to obtain hydrophobic and oleophobic properties, and can also be used to obtain a special surface touch. It is suitable for applications such as smart wearables. It can also be used to improve the processing rheology and reduce the processing temperature of polymer materials. It can also be used to reduce the water absorption rate of materials and increase the outdoor service life of materials such as polyester and polyamide.
[0009] In the present invention, the sum of the mass of the aromatic vinyl monomer, the acrylate monomer, and the olefin-terminated silicone is 100%, wherein the mass percentage of the olefin-terminated silicone is 1 to 50%, preferably 5 to 40%. The ratio of raw materials has an important influence on the structure and performance of the product, especially on the surface polarity, thereby affecting the application effect. The length of the copolymerized silicone side chains prepared by the present invention is controllable, the side chain structure is regular, there is no local gel problem, and the polymer production is stable; the lower the polarity of the product, the better the processing performance of the polymer and the acquisition of surface characteristics, avoiding the problem that the silicone on the molecular chain is prone to phase separation during the polymerization process and the production process is difficult to control.
[0010] In the present invention, the molecular weight regulator is used in an amount of 0.1 to 3% by weight of the monomer, preferably 0.3 to 1%, and more preferably 0.3 to 0.7%; the initiator is used in an amount of 0.1 to 2% by weight of the monomer, preferably 0.1 to 1%, and more preferably 0.4 to 0.6%. The monomer mass is the sum of the mass of the aromatic vinyl monomer, the acrylate monomer, and the olefin-terminated silicone.
[0011] In the present invention, the aromatic vinyl monomer includes a styrene monomer, such as styrene or substituted styrene, which can be selected from styrene monomer, α-methylstyrene monomer, α-chlorostyrene monomer or p-methylstyrene monomer; the acrylate monomer includes one or more of methyl methacrylate (MMA), ethyl methacrylate (EMA), butyl methacrylate and tert-butyl methacrylate; the initiator and molecular weight regulator are conventional additives in the art, such as the molecular weight regulator includes dodecyl mercaptan; the initiator includes azobisisobutyronitrile (AIBN) or dibenzoyl peroxide (BPO).
[0012] The present invention discloses a comb-like structured copolymer silicone with controllable branch length, wherein the main molecular chain contains a plurality of silicone pendant branches, and the overall structure is comb-like. The number average molecular weight of the olefin-terminated silicone of the present invention is 1000 to 5000, preferably 2000 to 5000, and the olefin functional group can be vinyl, propylene, etc. The olefin functional group of the olefin-terminated silicone is located at the end, and the olefin functionality is ≤2, preferably the olefin functionality of the olefin-terminated silicone is <2, and it is not easy to cause problems such as cross-linking and gelation. When mixed with polymers such as ABS, the main chain is compatible with the polymer, and the silicone branches tend to extend out of the surface, which can give full play to the low surface energy characteristics of silicone to obtain functional materials with special surfaces. In the present invention, the functionality is the average functionality, which generally refers to the average number of functional groups contained in each molecular chain.
[0013] In the present invention, the temperature of the heating polymerization is 65-110° C., and the time is 2-10 hours. Preferably, the heating polymerization is performed at 65-80° C. for 2-6 hours, and then the temperature is raised to 90-110° C. to continue polymerization for 0.5-3 hours. The material is washed with deionized water after discharge. The present invention uses water as a solvent, which is green and environmentally friendly, low in price, and easy to obtain equipment. The obtained product has few residual monomers and excellent stability, which is more conducive to later processing and downstream use. The amount of water used is conventionally selected and can be 1-5 times the mass of the monomer, such as 1-3 times. Beneficial effects
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] 1. The copolymerized silicon of the present invention has a moderate degree of polymerization, and a single molecular chain has multiple pendant organic silicon molecular chains, the branch chain lengths are controllable, and they do not interfere with each other and are not prone to gelation;
[0016] 2. In the copolymerized silicon of the present invention, the organosilicon exists in a long-chain branched state on the surface or at the interface, which is conducive to giving full play to the low surface energy characteristics of the organosilicon and making it easy to obtain materials with special surface requirements;
[0017] 3. The copolymerized silicone resin of the present invention has a main chain of styrene and acrylate copolymers, and its polarity is close to that of conventional polymer resins, and it has compatibility; the branched structure is more conducive to the anchoring of the copolymerized silicone resin in the matrix resin, and migration will not occur, thus avoiding the problem of precipitation during use;
[0018] 4. The present invention uses water as the medium in the process route, which requires little investment, is easy to obtain equipment and raw materials, has little discharge, is simple in proportion, and has a stable composition;
[0019] 4. The monomers selected in the present invention are non-toxic or low-toxic, the raw monomers are easily available, and the process route is conducive to reducing residual materials. It is suitable for high-end applications related to medical devices and food and drug packaging;
[0020] 5. The comb-like copolymerized silicon with controllable side chain length of the present invention has a wide range of applications: it can be applied to polymers to reduce surface polarity to achieve properties such as hydrophobicity, oleophobicity, and chemical solvent resistance; it can also be used in applications such as smart wearables to achieve a special surface feel; it can also be used in polymer materials to improve the water absorption rate of materials, especially polyester materials, to extend the outdoor service life;
[0021] 6. The comb-like structured copolymer silicon with controllable side chain length of the present invention is easy to use and can be widely used in medical devices, packaging, home appliances, automobiles, aviation and other fields, and has very broad application prospects and industrial value. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Other features, objects and advantages of the present invention will become more apparent upon reading the detailed description of non-limiting embodiments with reference to the following drawings:
[0023] Figure 1 is the infrared spectrum of comb-structured copolymer silicon with controllable branch chain length. Modes for Carrying Out the Invention
[0024] The present invention will be described in detail below with reference to specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those skilled in the art, several variations and improvements can be made without departing from the scope of the present invention. These all fall within the scope of protection of the present invention.
[0025] The present invention discloses a method for preparing a comb-shaped copolymer silicon with controllable branch chain length. The method comprises the following steps: placing an aromatic vinyl monomer, an acrylate monomer, an olefin-terminated organosilicon, an initiator, a molecular weight regulator and water into a reaction kettle, mixing them uniformly, reacting them at 65-80° C. for 2-8 hours under conventional stirring, and then continuing to react at 90-110° C. for 0.5-2 hours. After the material is discharged, it is filtered, washed with water and dried to obtain a comb-shaped copolymer silicon with controllable branch chain length. The preparation process does not require any organic solvent, pressurization or special atmosphere protection.
[0026] A method for preparing a modified polymer comprises the following steps: mixing a polymer raw material and the aforementioned comb-like structured copolysilicon with controllable branch lengths, followed by extrusion, to obtain the modified polymer. Preferably, the comb-like structured copolysilicon with controllable branch lengths is used in an amount of 0.5-2% by mass of the polymer raw material. The polymer raw material can be pure particles or a blended plastic; it can be used to improve the processability and flowability of polymer materials, or to modify the surface properties of polymer materials to achieve superhydrophobic and oleophobic properties, or to reduce the hygroscopicity of water-absorbent materials.
[0027] The test conditions are as follows:
[0028] Weight average molecular weight (Mw): tested by GPC using PS as the standard sample;
[0029] Infrared structure (IR): tested by Fourier-infrared spectrometer;
[0030] RTVM: Tested according to ASTM D790 using GC-MS;
[0031] Contact angle: tested with a water contact angle tester;
[0032] Aging stability: Bake in an oven at 80°C for 6 hours. If there is no stickiness or precipitation, it is considered excellent. The stability is judged to be poor based on the degree of stickiness and precipitation.
[0033] Water absorption rate: The injection molded specimens were dried at 105℃ for 2 hours, then refluxed in deionized water at 100℃ for 2 hours. After removal, the surface water stains were removed and weighed to calculate the water absorption rate.
[0034] Tensile strength: tested in accordance with GB1039 test standard;
[0035] Tensile strength retention rate: tensile strength after 48 hours of boiling aging / original tensile strength*100%.
[0036]
[0037] ①: Olefin-terminated silicone with Mn of 4000 and olefin functionality of 1;
[0038] ②: Olefin-terminated silicone with Mn of 500 and olefin functionality of 1;
[0039] ③: Active silicone with Mn of 3000 and olefin functionality of 3, located at the end group and side chain.
[0040] The chemical structure of the above-mentioned "ene-terminated silicone" with a functionality of 1 is as follows:
[0041]
[0042] By designing double bonds at the end groups and / or side chains, olefin-terminated silicones with different functionalities can be obtained.
[0043] The above-mentioned copolymer silicon is prepared as follows: styrene, acrylate monomer (if any), olefin-terminated organosilicon, initiator azobisisobutyronitrile, molecular weight regulator dodecyl mercaptan and 200 kg of water are placed in a reactor, mixed evenly, and reacted at 70°C for 5 hours under conventional stirring, and then continued to react at 95°C for 1 hour. After discharge, the material is filtered, washed with deionized water three times, and dried to obtain the copolymer silicon. The preparation process does not require organic solvents, pressurization, or special atmosphere protection.
[0044] The present invention copolymerizes styrene, MMA, and olefin-terminated organosilicon to form a long-chain branched organosilicon copolymer, in which the organosilicon is a branched chain, dangling from the styrene-MMA main chain, forming a comb-like structure. Organosilicon has low polarity, and when blended with conventional polymers, the organosilicon segments tend to migrate to the surface or interface, thereby improving the surface properties of the polymer material, providing super-hydrophobic and oleophobic properties, and also enhancing resistance to chemical solvents. When the organosilicon molecular chain is long enough, it also creates a unique tactile feel on the polymer surface.
[0045] The structures of the copolymerized silicon in the above embodiment and the comparative example were tested under the above conventional test conditions and infrared analysis was performed. The analysis results are shown in FIG1 . It can be seen that the infrared spectroscopy at 1260 cm -1 The absorption peak is the characteristic peak of organosilicon grafted onto the polystyrene main chain. It can be seen that the intensity of the absorption peak increases with the increase of organosilicon concentration; the polystyrene raw material in the figure is commercially available conventional polystyrene.
[0046] The molecular weight (Mw) and residual monomer content (RTVM) of the copolymerized silicon of the above examples and comparative examples were tested according to the above conventional test conditions. The test results are shown in Table 2.
[0047] The molecular weight of the comb-structured copolymer of the present invention is within a controllable range. However, the molecular weight of Comparative Example 4 could not be measured due to crosslinking of the molecular chains and implosion. Compared with the comparative example, the monomer ratio compatibility of the embodiment is better, and the RTVM is significantly reduced, indicating that the reaction is more complete.
[0048]
[0049] Examples 1-4, the comparative example, the commercially available silicone LYSI-306 (50% silicone content, Comparative Example 6), and the commercially available high-molecular-weight silicone Pellet S (Comparative Example 7) were used as surface modifiers with polypropylene (PP) and pelletized using a high-vacuum twin-screw extruder at 210°C. Specifically, the surface modifier and polypropylene were added to a twin-screw extruder (the surface modifier amount was 1% of the polypropylene mass) and pelletized at 210°C to produce polymer particles. The resulting particles were then tableted and tested for surface contact angle and aging stability. The test results are shown in Table 3.
[0050]
[0051] As shown in Table 3, by comparing Example 1 with Comparative Example 3, it can be seen that the two samples have little difference in silicone content and molecular weight, but the silicone side chain of Example 1 shows better hydrophobicity in the contact angle test.
[0052] Compared with Comparative Example 2, Example 1 exhibits significantly better surface effects. This is because, despite similar organosilicon chain lengths and concentrations, Comparative Example 2 struggles to migrate to the surface. Compared with Comparative Example 3, Examples 2 and 3 also exhibit significantly lower surface polarity. This indicates that reduced surface polarity is related to the ability of organosilicon chain segments to migrate to the surface, such as their number and length. Therefore, the Examples exhibited better surface hydrophobicity improvement than the Comparative Example.
[0053] Furthermore, based on the formulation of Example 3, ethylene-terminated silicone with an Mn of 2000, 2500, 3000 or 3500 was used. Under the same preparation method, the surface water contact angle of the modified polypropylene was also significantly improved, similar to that of the embodiment, and the aging stability was excellent.
[0054] In the aging test, Comparative Example 6 has poor compatibility and is easily precipitated onto the surface, resulting in poor aging stability, which manifests as a defect of surface stickiness.
[0055] Examples 1-4, the comparative example, and commercially available silicone LYSI-306 (50% silicone content, comparative example 6) were used as flow modifiers with glass fiber-reinforced nylon (30% GF) and pelletized at 260°C using a high-vacuum twin-screw extruder. Specifically, the flow modifier and glass fiber-reinforced nylon (30% GF) were added to a twin-screw extruder (the flow modifier amount was 1% of the mass of the glass fiber-reinforced nylon) and pelletized at 260°C using a twin-screw extruder to produce polymer particles. The melt index (MI) and mechanical properties of the resulting particles were tested. The test results are shown in Table 4.
[0056]
[0057] The chemical resistance test is to press the particles into conventional tablets (0.5 mm), immerse them in a mixture of ethanol and ethyl acetate with a volume ratio of 3:1 at room temperature, and take them out after 30 minutes. If the tensile strength retention rate is 80% or above, it is rated as +++; if it is 75% or above, it is rated as ++; if it is 70% or above, it is rated as +; and if it is below 70%, it is rated as -.
[0058] As shown in Table 4, compared to the PA-reinforced raw material, the water absorption rates of all samples were reduced. The examples showed a significant reduction in water absorption compared to the comparative examples, with the improvement in Examples 1-3 being even more pronounced compared to Comparative Example 3. Correspondingly, the chemical resistance tests of the examples and Comparative Example 3 also outperformed the other reference samples, with Example 3 demonstrating the highest chemical solvent resistance. This demonstrates that low surface polarity effectively repels chemical solvents, thereby enhancing chemical solvent resistance.
[0059] Due to the improvement of chemical resistance, the performance retention rate is also improved. After adding long-chain branched copolymer silicone, its toughness is improved, which may be related to the toughening effect of long-chain branched silicone. As the chemical solvent resistance is improved, the performance retention rate is also better.
[0060] Combined with Tables 1 to 4, the effects of improving surface properties and processability are related to molecular weight, silicone side chain concentration, silicone side chain length, etc. For example, when comparing Example 1 with Comparative Example 2, although the silicone content is the same, the difference in molecular weight control leads to a large difference in viscosity, which affects the mobility of the silicone side chains. The surface effect of Example 1 is more obvious, which shows that an appropriate molecular weight is conducive to the migration reaction of molecular segments.
[0061] The present invention proposes for the first time that the organosilicon content affects the surface modification effect. In Comparative Example 1, the organosilicon content is too low, the number of organosilicon segments migrating to the surface is small, and the surface modification effect is poor. As the organosilicon content increases, the surface polarity decreases. However, more is not necessarily better. Excessively high organosilicon content will cause instability in the polymerization process, which is not conducive to production (Comparative Example 5).
[0062] Although the branch chain concentrations are similar, the surface modification effects vary greatly depending on the branch chain lengths. However, the comb-like structure has obvious advantages over the existing structure, such as Example 3 and Comparative Examples 6 and 7. Comparative Examples 6 and 7 are both silicone oil products with good conventional application performance. Although their concentrations are higher, their surface modification effects are even lower than those of Example 4.
[0063]
[0064] Copolysilicon was prepared according to the above-mentioned copolysilicon preparation method using the proportions in Table 5. The copolysilicon was used as a surface modifier and granulated with polypropylene (PP) at 210°C using a high-vacuum twin-screw extruder. Specifically, the surface modifier and polypropylene were added to a twin-screw extruder (the surface modifier amount was 1% of the weight of the polypropylene). Granulation was performed at 210°C using a twin-screw extruder to produce polymer particles. The resulting particles were tableted and the surface contact angle was measured. The test results are shown in Table 5. Comparison of Example 5 and Example 1 with Comparative Example 8 demonstrates that the MMA monomer improves compatibility.
[0065] The existing methyl methacrylate-silicone-styrene copolymer (S-2001) is a shell / core structured impact modifier with characteristics such as low-temperature resistance and weather resistance. However, when used for the above-mentioned PP surface modification (1wt%), it has almost no effect on the water contact angle, which was tested to be 83.6°. It has no effect on the surface and only has a toughening effect.
[0066] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various variations or modifications within the scope of the claims, which do not affect the essence of the present invention.
[0067] Compared with the prior art, the present invention has the following beneficial effects: 1. The copolymerized silicon of the present invention has a comb-like structure, with multiple long-chain silicone branches on a single molecular chain. The density of the silicone branches is appropriate, which can significantly reduce the surface polarity and improve the surface hydrophobicity and oleophobicity; 2. When used as a chemical resistance modifier, it can effectively improve the chemical solvent resistance, and has no obvious side effects on the mechanical properties; 3. The process route selected by the present invention only uses water as the medium, with low investment, easy equipment acquisition, low process route emissions, simple process control, low reaction temperature, easy heat transfer, high product yield, and stable composition; 4. The chain extender of the present invention is a polymer with adjustable branch length, which can be applied to a variety of processing technologies and conditions, avoiding adaptability problems in the production process; 5. The monomers selected by the present invention have the characteristics of non-toxic or low toxicity, and the process route is conducive to further reducing residual monomers, and can be applied to high-end applications such as medical devices and food and drug packaging.
[0068] This invention, a completely innovative design, leads to technological advancement and green production in this field, contributes to structural and technological upgrades in the relevant domestic industrial chain, enhances the technical support and innovation capabilities for functional polymer modification, and positively promotes the development of the chemical industry towards refined, high-value-added products. Furthermore, the technical route of this invention provides a high-yield synthesis route that can be industrialized, environmentally friendly, and can achieve high yields.
Claims
1. A method for preparing a comb-shaped copolymer silicon with controllable branch chain length, It is characterized in that The method comprises the following steps: mixing aromatic vinyl monomer, acrylate monomer, olefin-terminated silicone, initiator, molecular weight regulator and water, and then heating and polymerizing to prepare a comb-shaped copolymer silicone with controllable branch chain length; the mass sum of aromatic vinyl monomer, acrylate monomer and olefin-terminated silicone is 100%, wherein the mass percentage of olefin-terminated silicone is 1-50%.
2. The method for preparing the comb-like structured copolymer silicon with controllable branch chain length as claimed in claim 1, It is characterized in that The mass percentage of aromatic vinyl monomer, acrylate monomer and olefin-terminated organic silicon is 100%, wherein the mass percentage of olefin-terminated organic silicon is 5-40%; the amount of the initiator is 0.1-2% of the mass of the monomer; and the amount of the molecular weight regulator is 0.1-3% of the mass of the monomer.
3. The method for preparing the comb-like structured copolymer silicon with controllable branch chain length as claimed in claim 1, It is characterized in that The number average molecular weight of the olefin-terminated organosilicon is 500 to 10,000, and the functionality of the olefin group of the olefin-terminated organosilicon is ≤2.
4. The method for preparing the comb-like structured copolymer silicon with controllable branch chain length as claimed in claim 3, It is characterized in that The number average molecular weight of the olefin-terminated organosilicon is 1000-5000, and the functionality of the olefin group of the olefin-terminated organosilicon is less than 2.
5. The method for preparing the comb-like structured copolymer silicon with controllable branch chain length as claimed in claim 1, It is characterized in that The heating polymerization is carried out at 65-80°C for 2-6 hours, and then the temperature is raised to 90-110°C to continue polymerization for 0.5-3 hours.
6. The method for preparing the comb-like structured copolymer silicon with controllable branch chain length as claimed in claim 1, It is characterized in that The aromatic vinyl monomers include styrene monomers; the acrylate monomers include one or more of methyl methacrylate, ethyl methacrylate, butyl methacrylate, and tert-butyl methacrylate.
7. The comb-like copolymer silicon with controllable branch chain length prepared by the method for preparing the comb-like copolymer silicon with controllable branch chain length as claimed in claim 1.
8. The comb-like structured copolymer silicon with controllable branch chain length as claimed in claim 7 is used as a surface modifier in the modification of functional polymers.
9. A method for preparing a modified polymer, It is characterized in that The method comprises the following steps: mixing a polymer raw material and the comb-shaped copolymer silicon with controllable branch chain length as claimed in claim 7 and then extruding the mixture to obtain a modified polymer.
10. The method for preparing the modified polymer according to claim 9, It is characterized in that The amount of the comb-shaped copolymer silicon with controllable branch chain length is 0.5-5% of the mass of the polymer raw material.
Citation Information
Patent Citations
Design and preparation for controllable hydrophobic material
CN101070388A
Novel organic silicon water repellent and preparing method thereof
CN105218762A
Organosilicone-maleic anhydride resin novel copolymer
CN107573460A
Polymerization process for silicone and acrylic monomers
CN112352004A
Acrylic acid modified vinyl organic silicon resin and preparation method thereof
CN113136013A
Cited By
Dendritic cross-linked structure fluoride-free oil-proofing agent and preparation method thereof
CN121108423A