Positive electrode material, electrochemical device, and electronic device
By forming a cladding layer of P63mc and R-3m crystal structures on the lithium-cobalt composite oxide positive electrode material and doping Na and Al elements, the problems of impedance increase and capacity decay of lithium-ion batteries under high voltage are solved, significantly improving the Its high temperature storage and cycling performance are achieved.
Patent Information
- Application Number
- PCT/CN2023/093014
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-14
AI Technical Summary
At high voltage, lithium-ion batteries have intensified reactions between the positive electrode material and the electrolyte interface, resulting in increased impedance, capacity loss and rapid attenuation, affecting their high energy density and cycling performance.
Using lithium-cobalt composite oxide as the positive electrode material, a clad layer with P63mc and R-3m crystal structures is formed on its surface, and Na elements are doped in the matrix and the clad layer to expand the lithium ion channel and reduce the interface impedance. And through reasonable molar ratio of Na and Co elements and Al element doping, structural stability is improved, phase transition inactivation and interface side reactions are inhibited.
It significantly reduces the impedance of the electrochemical device, improves the high-temperature storage and cycling performance at high voltages, and extends the cycle life and energy density of lithium-ion batteries.
Smart Images

Figure CN2023093014_14112024_PF_FP_ABST
Abstract
Description
Cathode materials, electrochemical devices, and electronic devices Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a positive electrode material, an electrochemical device, and an electronic device. Background Art
[0002] With the popularity of devices such as laptops, mobile phones, tablets, drones, and electric vehicles, people's requirements for the energy density of lithium-ion batteries are becoming increasingly higher. To meet the demand for high energy density, the voltage platform of lithium-ion batteries continues to increase. However, this voltage increase is accompanied by an intensification of the interfacial reaction between the positive electrode material and the electrolyte. The surface phase change deactivation of the positive electrode material causes an increase in impedance and capacity loss. At the same time, the electrolyte is oxidized on the material surface to form byproducts, which further increases the impedance and causes rapid capacity decay.
[0003] Summary of the Invention
[0004] In view of the above-mentioned problems existing in the prior art, the present application provides a positive electrode material, an electrochemical device and an electronic device to reduce the impedance of the electrochemical device and improve the high-temperature storage performance and cycle performance of the electrochemical device under high voltage.
[0005] In a first aspect, the present application provides a positive electrode material comprising a lithium-cobalt composite oxide, the lithium-cobalt composite oxide comprising a substrate and a coating layer located on a surface of the substrate, the coating layer comprising a first region and a second region, the first region having a P63mc crystal structure and the second region having an R-3m crystal structure, both of which contain the element Na. In the positive electrode material provided herein, the first region having the P63mc crystal structure and the second region having the R-3m crystal structure in the coating layer are both doped with the element Na. The Na element can be doped at the lithium site, thereby expanding lithium ion channels and stabilizing the structure of the surface layer of the lithium-cobalt composite oxide, reducing interfacial impedance during lithium ion insertion and extraction, and improving the cycling performance of the electrochemical device at high voltage. Furthermore, the first region having the P63mc crystal structure has excellent structural stability at high voltage, further suppressing phase change deactivation of the surface layer of the positive electrode material and reducing interfacial side reactions between the positive electrode material and the electrolyte, thereby improving the high-temperature storage performance and cycling performance of the electrochemical device at high voltage.
[0006] In some embodiments, the molar ratio of Na to Co in the first region is K1, satisfying the following: 0.1% ≤ K1 ≤ 2.0%. This improves the stability of the crystal structure of the first region and enhances the cycling performance of the electrochemical device at high voltages. Furthermore, 0.2% ≤ K1 ≤ 1.0%.
[0007] In some embodiments, the molar ratio of Na to Co in the second region is K2, satisfying the following: 0.01% ≤ K2 ≤ 1.0%. This improves the stability of the crystal structure of the second region, thereby enhancing the cycling performance of the electrochemical device at high voltages. Furthermore, 0.04% ≤ K2 ≤ 0.5%.
[0008] In some embodiments, 1.1≤K1 / K2≤5.
[0009] In some embodiments, the first region and the second region are both located on the surface of the substrate.
[0010] In some embodiments, the first regions are dispersed in the second regions in the form of islands.
[0011] In some embodiments, the coating layer has a thickness of 10 nm to 200 nm.
[0012] In some embodiments, the thickness of the first region is 10 nm to 200 nm.
[0013] In some embodiments, the thickness of the second region is 10 nm to 200 nm.
[0014] In some embodiments, a grain boundary exists between the first region and the second region, and the angle between the transition metal layer in the first region and the transition metal layer in the second region at the grain boundary is greater than or equal to 150°. This facilitates lithium ion transport between the first and second regions and reduces interfacial impedance during lithium ion insertion and extraction. Furthermore, because the first region, having the P63mc crystal structure, has high structural stability at high voltages, it can provide a stable channel for lithium ion insertion and extraction, thereby improving the cycling performance of the electrochemical device at high voltages.
[0015] In some embodiments, the matrix further includes Na, and the molar ratio of Na to Co in the matrix is K3, satisfying the following: 0.01% ≤ K3 ≤ 0.2%. Doping the matrix with Na expands the lithium ion channels in the lithium-cobalt composite oxide matrix and stabilizes its layered structure, reducing the impedance and stress concentration during lithium ion insertion and extraction, thereby improving the power performance, high-voltage, high-temperature storage performance, and cycling performance of the electrochemical device.
[0016] In some embodiments, the second region further comprises Al, and the molar ratio of Al to Co in the second region is B, satisfying the following: 0.1% ≤ B ≤ 1%. The further doping of the second region with Al further enhances the structural stability of the second region having an R-3m crystal structure at high voltages, thereby improving the high-temperature storage performance and cycling performance of the electrochemical device at high voltages.
[0017] In some embodiments, the matrix further comprises a Q element, wherein the Q element comprises at least one of Al, Mg, Ti, Ca, La, Y, Zr, Fe, Mn, Ni, Nb, Mo, W, Ta, Zn, Cr, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, or Cu. The molar ratio of the Q element to the Co element in the matrix is C, satisfying the following: 0.1% ≤ C ≤ 10%. By doping the matrix with the Q element, the structural stability of the matrix at high voltage can be further improved, thereby enhancing the high-temperature storage performance and cycling performance of the electrochemical device at high voltage.
[0018] In some embodiments, the mole percentage of the Co element in the lithium-cobalt composite oxide is 90% to 99% based on the mole amount of the metal elements other than the Li element in the lithium-cobalt composite oxide.
[0019] In some embodiments, the coating layer further includes a third region, which includes an oxide of element M, where element M includes at least one of Al, Mg, Ti, Zr, Y, Nb, Ca, Ni, Mn, or Ce, and satisfies at least one of the following conditions: (1) the third region is located on the surface of the second region facing away from the substrate; (2) the third region is located on the surface of the first region facing away from the substrate; or (3) the third region is located on the surface of the substrate. This can further enhance the protection of the lithium-cobalt composite oxide, inhibit its surface phase change deactivation, reduce its interfacial side reactions with the electrolyte, and further improve the high-temperature storage performance and cycling performance of the electrochemical device at high voltage.
[0020] In some embodiments, a lithium-cobalt composite oxide includes a first lithium-cobalt composite oxide and a second lithium-cobalt composite oxide, wherein the volume average particle size Dv50 of the first lithium-cobalt composite oxide is greater than the volume average particle size Dv50' of the second lithium-cobalt composite oxide; based on the mass of the first lithium-cobalt composite oxide, the mass percentage of the Na element in the first lithium-cobalt composite oxide is E; based on the mass of the second lithium-cobalt composite oxide, the mass percentage of the Na element in the second lithium-cobalt composite oxide is F; and the following conditions are satisfied: 0.3 ≤ E / F ≤ 1.5. This can reduce the kinetic difference between the first lithium-cobalt composite oxide with a large particle size and the second lithium-cobalt composite oxide with a small particle size, thereby reducing the impedance of the electrochemical device and improving the high-temperature storage performance and cycling performance of the electrochemical device at high voltage. Furthermore, in some embodiments, 0.5 ≤ E / F ≤ 0.9.
[0021] In some embodiments, 0.01%≤E≤0.3%.
[0022] In some embodiments, 0.04%≤F≤0.5%.
[0023] In some embodiments, the first lithium cobalt composite oxide has a volume average particle size Dv50 of 12 μm to 25 μm.
[0024] In some embodiments, the second lithium cobalt composite oxide has a volume average particle size Dv50' of 2 μm to 8 μm.
[0025] In some embodiments, the volume average particle size Dv50 of the first lithium cobalt composite oxide and the volume average particle size Dv50' of the second lithium cobalt composite oxide satisfy 3 ≤ Dv50 / Dv50' ≤ 6. This facilitates the filling of the small-sized second lithium cobalt composite oxide between the large-sized first lithium cobalt composite oxide particles, thereby improving the energy density of the electrochemical device.
[0026] In some embodiments, the mass ratio of the first lithium cobalt composite oxide to the second lithium cobalt composite oxide is 70:30 to 95:5.
[0027] A second aspect of the present application provides an electrochemical device comprising a positive electrode, the positive electrode comprising a positive electrode material layer, the positive electrode material layer comprising the aforementioned positive electrode material. Thus, the electrochemical device of the present application has low impedance and excellent high-temperature storage performance and cycling performance at high voltage.
[0028] A third aspect of the present application provides an electronic device comprising the aforementioned electrochemical device.
[0029] BRIEF DESCRIPTION OF THE DRAWINGS
[0030] FIG1 is a transmission electron microscope image of the positive electrode material of Example 1 of the present application. DETAILED DESCRIPTION
[0031] To make the purpose, technical solutions, and advantages of this application more clear, the technical solutions of this application will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of this application, rather than all the embodiments. The relevant embodiments described herein are illustrative and are used to provide a basic understanding of this application. The embodiments of this application should not be interpreted as limiting this application.
[0032] For the sake of clarity, only some numerical ranges are specifically disclosed herein. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value may itself serve as a lower limit or upper limit and be combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.
[0033] In the description herein, unless otherwise stated, "above" and "below" are inclusive. Unless otherwise stated, the terms used in this application have the commonly understood meanings commonly understood by those skilled in the art. Unless otherwise stated, the numerical values of the various parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).
[0034] A list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.
[0035] 1. Cathode Materials
[0036] An embodiment of the present application provides a positive electrode material, including a lithium cobalt composite oxide, the lithium cobalt composite oxide including a substrate and a coating layer located on the surface of the substrate, the coating layer including a first region and a second region, the first region having a P63mc crystal structure, the second region having an R-3m crystal structure, and both the first region and the second region containing the Na element.
[0037] The positive electrode material provided in the present application has a first region with a P63mc crystal structure and a second region with an R-3m crystal structure in the coating layer, both of which are doped with the Na element. The Na element can be doped at the lithium site, thereby expanding the lithium ion channel and stabilizing the structure of the surface layer of the lithium-cobalt composite oxide, reducing the interfacial impedance during lithium ion deintercalation and deintercalation, and improving the cycle performance of the electrochemical device at high voltage; at the same time, the first region with the P63mc crystal structure has excellent structural stability at high voltage, which can further inhibit the phase change deactivation of the surface layer of the positive electrode material and reduce the interfacial side reactions between it and the electrolyte, thereby improving the high-temperature storage performance and cycle performance of the electrochemical device at high voltage.
[0038] In some embodiments, the molar ratio of the Na element to the Co element in the first region is K1, satisfying: 0.1% ≤ K1 ≤ 2.0%; illustratively, the molar ratio K1 of the Na element to the Co element in the first region is 0.1%, 0.2%, 0.4%, 0.5%, 0.6%, 0.8%, 1.0%, 1.2%, 1.5%, 1.8%, 2.0% or a range consisting of any two of the above values. It will be understood that the Na element can exist in the form of lithium sodium cobalt composite oxide. Controlling the molar content of the Na element in the first region within the above range is beneficial to improving the stability of the crystal structure of the first region and improving the high temperature storage performance and cycle performance of the electrochemical device at high voltage. Further, in some embodiments, 0.2% ≤ K1 ≤ 1.0%.
[0039] In some embodiments, the molar ratio of the Na element to the Co element in the second region is K2, satisfying: 0.01% ≤ K2 ≤ 1.0%; illustratively, the molar ratio of the Na element to the Co element in the second region, K2, is 0.01%, 0.02%, 0.04%, 0.05%, 0.06%, 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.8%, 1.0% or a range consisting of any two of the above values. Controlling the molar content of the Na element in the second region within the above range is beneficial to improving the stability of the crystal structure of the second region, improving the high-temperature storage performance and cycle performance of the electrochemical device at high voltage; at the same time, it can reduce the loss of lithium capacity, thereby improving the energy density of the electrochemical device. Further, in some embodiments, 0.04% ≤ K2 ≤ 0.5%.
[0040] In some embodiments, the molar ratio K1 of the Na element to the Co element in the first region and the molar ratio K2 of the Na element to the Co element in the second region satisfy: 1.1≤K1 / K2≤5. Exemplarily, K1 / K2 is 1.1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 or a range consisting of any two of the above values. The relatively high content of the local Na element in the coating layer is conducive to the local phase transformation to form a first region with a P63mc crystal structure; at the same time, K1 / K2≤5 is conducive to reducing the difference in lithium ion insertion and extraction rate and structural stability between the first region and the second region, reducing the risk of rupture between the first region and the second region due to stress concentration during charging and discharging, thereby improving the high-temperature storage performance and cycle performance of the electrochemical device at high voltage.
[0041] In some embodiments, the first region and the second region are both located on the surface of the substrate.
[0042] In some embodiments, the first regions are dispersed in the second regions in an island-like form.
[0043] In certain embodiments, the thickness of the coating is between 10 nm and 200 nm. Exemplary, the thickness of the coating is between 10 nm, 20 nm, 40 nm, 50 nm, 60 nm, 80 nm, 100 nm, 120 nm, 150 nm, 180 nm, 200 nm or the range of any two of the above values. Further, in certain embodiments, the thickness of the coating is between 50 nm and 150 nm.
[0044] Those skilled in the art will appreciate that the thickness in the first region and the second region may be the same or different in the coating. In certain embodiments, the thickness in the first region is 10nm to 200nm. Exemplary, the thickness in the first region is 10nm, 20nm, 40nm, 50nm, 60nm, 80nm, 100nm, 120nm, 150nm, 180nm, 200nm or the scope of any two values formed. Further, in certain embodiments, the thickness in the first region is 10nm to 100nm. In certain embodiments, the thickness in the second region is 10nm to 200nm. Exemplary, the thickness in the second region is 10nm, 20nm, 40nm, 50nm, 60nm, 80nm, 100nm, 120nm, 150nm, 180nm, 200nm or the scope of any two values formed. Further, in certain embodiments, the thickness in the second region is 50nm to 150nm.
[0045] In some embodiments, there is a grain boundary between the first region and the second region, and the angle between the transition metal layer of the first region and the transition metal layer of the second region at the grain boundary is greater than or equal to 150°. Exemplarily, the angle between the transition metal layer of the first region and the transition metal layer of the second region at the grain boundary is 150°, 155°, 160°, 165°, 170°, 175°, 178°, 180°, or a range consisting of any two of the above values. Further, in some embodiments, the angle between the transition metal layer of the first region and the transition metal layer of the second region at the grain boundary is greater than or equal to 160°. The angle between the transition metal layer of the first region and the transition metal layer of the second region at the grain boundary is within the above range, which can promote lithium ion transport between the first region and the second region and reduce the interfacial impedance during lithium ion insertion and extraction. Moreover, since the first region having the P63mc crystal structure has high structural stability at high voltage, it can provide a stable channel for lithium ion insertion and extraction, thereby improving the cycling performance of the electrochemical device at high voltage.
[0046] In some embodiments, the second region further comprises an Al element, and the molar ratio of the Al element to the Co element in the second region is B, satisfying the following: 0.1% ≤ B ≤ 1%; illustratively, the molar ratio B of the Al element to the Co element in the second region is 0.1%, 0.2%, 0.4%, 0.5%, 0.6%, 0.8%, 0.9%, 1%, or a range consisting of any two of the foregoing values. Further doping the second region with the Al element can further enhance the structural stability of the second region having the R-3m crystal structure at high voltages, thereby improving the high-temperature storage performance and cycling performance of the electrochemical device at high voltages.
[0047] In some embodiments, the matrix further comprises a Na element, and the molar ratio of the Na element to the Co element in the matrix is K3, satisfying: 0.01% ≤ K3 ≤ 0.2%. Exemplarily, the molar ratio K3 of the Na element to the Co element in the matrix is 0.01%, 0.02%, 0.04%, 0.05%, 0.06%, 0.08%, 0.1%, 0.12%, 0.15%, 0.18%, 0.2%, or a range consisting of any two of the above values. By doping the Na element into the matrix, the lithium ion channels in the lithium cobalt composite oxide matrix can be expanded and its layered structure can be stabilized, reducing the impedance and stress concentration during the lithium ion insertion and extraction process, thereby improving the power performance, high-temperature storage performance under high voltage, and cycle performance of the electrochemical device.
[0048] In some embodiments, the matrix further comprises a Q element, wherein the Q element comprises at least one of Al, Mg, Ti, Ca, La, Y, Zr, Fe, Mn, Ni, Nb, Mo, W, Ta, Zn, Cr, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, or Cu, and the molar ratio of the Q element to the Co element in the matrix is C, satisfying: 0.1% ≤ C ≤ 10%. Exemplarily, the molar ratio C of the Q element to the Co element in the matrix is 0.1%, 0.2%, 0.4%, 0.5%, 0.6%, 0.8%, 0.9%, 1%, 2%, 4%, 5%, 6%, 8%, 10%, or a range consisting of any two of the above values. By doping the matrix with the Q element, the structural stability of the matrix at high voltage can be further improved, and the high-temperature storage performance and cycle performance of the electrochemical device at high voltage can be improved.
[0049] In some embodiments, the molar percentage of Co in the lithium-cobalt composite oxide is 90% to 99% based on the molar amount of the metal elements other than Li in the lithium-cobalt composite oxide. Exemplarily, the molar percentage of Co in the lithium-cobalt composite oxide is 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, or a range consisting of any two of the foregoing values, based on the molar amount of the metal elements other than Li in the lithium-cobalt composite oxide.
[0050] In some embodiments, the coating layer further comprises a third region comprising an oxide of element M, wherein element M comprises at least one of Al, Mg, Ti, Zr, Y, Nb, Ca, Ni, Mn, or Ce. In some embodiments of the present application, the third region is located on the surface of the second region facing away from the substrate; in other embodiments of the present application, the third region is located on the surface of the first region facing away from the substrate; and in still other embodiments of the present application, the third region is located on the surface of the substrate. It is understood that the presence of the oxide of element M can further enhance the protection of the lithium-cobalt composite oxide, inhibit phase transition deactivation of its surface layer, reduce interfacial side reactions between it and the electrolyte, and further improve the high-temperature storage performance and cycling performance of the electrochemical device at high voltage.
[0051] In some embodiments, the lithium cobalt composite oxide includes the first lithium cobalt composite oxide and the second lithium cobalt composite oxide of the aforementioned embodiments, wherein the volume average particle size Dv50 of the first lithium cobalt composite oxide is greater than the volume average particle size Dv50' of the second lithium cobalt composite oxide. Based on the mass of the first lithium cobalt composite oxide, the mass percentage of the Na element in the first lithium cobalt composite oxide is E; based on the mass of the second lithium cobalt composite oxide, the mass percentage of the Na element in the second lithium cobalt composite oxide is F; and the following conditions are satisfied: 0.3 ≤ E / F ≤ 1.5; illustratively, the ratio E / F of the mass percentage of the Na element in the first lithium cobalt composite oxide to the mass percentage of the Na element in the second lithium cobalt composite oxide is 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, or a range consisting of any two of the above values. In this way, the kinetic difference between the large-particle size of the first lithium-cobalt composite oxide and the small-particle size of the second lithium-cobalt composite oxide can be reduced, thereby reducing the impedance of the electrochemical device and improving the high-temperature storage performance and cycle performance of the electrochemical device under high voltage. The first lithium-cobalt composite oxide and the second lithium-cobalt composite oxide can be distinguished by screening the positive electrode material using a 1500-mesh sieve. The material above the sieve is the first lithium-cobalt composite oxide, and the material below the sieve is the second lithium-cobalt composite oxide.
[0052] In some embodiments, 0.5≤E / F≤0.9.
[0053] In some embodiments, 0.01%≤E≤0.3%; illustratively, the mass percentage E of the Na element in the first lithium cobalt composite oxide is 0.01%, 0.02%, 0.03%, 0.05%, 0.06%, 0.08%, 0.10%, 0.12%, 0.14%, 0.16%, 0.18%, 0.20%, 0.22%, 0.24%, 0.26%, 0.28%, 0.30% or a range consisting of any two of the above values.
[0054] In some embodiments, 0.04%≤F≤0.5%; illustratively, the mass percentage F of the Na element in the second lithium cobalt composite oxide is 0.04%, 0.05%, 0.06%, 0.08%, 0.10%, 0.12%, 0.15%, 0.16%, 0.18%, 0.20%, 0.22%, 0.24%, 0.26%, 0.28%, 0.03%, 0.35%, 0.40%, 0.45%, 0.50%, or a range consisting of any two of the above values.
[0055] In some embodiments, the volume average particle size Dv50 of the first lithium cobalt composite oxide is 12 μm to 25 μm; illustratively, the volume average particle size Dv50 of the first lithium cobalt composite oxide is 12 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, 25 μm, or a range consisting of any two of the above values.
[0056] In some embodiments, the volume average particle size Dv50' of the second lithium cobalt composite oxide is 2 μm to 8 μm; illustratively, the volume average particle size Dv50' of the second lithium cobalt composite oxide is 2 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 8 μm, or a range consisting of any two of the above values.
[0057] In some embodiments, the volume average particle size Dv50 of the first lithium cobalt composite oxide and the volume average particle size Dv50' of the second lithium cobalt composite oxide satisfy 3 ≤ Dv50 / Dv50' ≤ 6. Exemplarily, the ratio Dv50 / Dv50' of the volume average particle size Dv50 of the first lithium cobalt composite oxide to the volume average particle size Dv50' of the second lithium cobalt composite oxide is 3, 3.5, 4, 4.5, 5, 5.5, 6, or a range consisting of any two of the foregoing values. This facilitates the filling of the small-sized second lithium cobalt composite oxide between the large-sized first lithium cobalt composite oxide particles, thereby improving the energy density of the electrochemical device.
[0058] In some embodiments, the mass ratio of the first lithium cobalt composite oxide to the second lithium cobalt composite oxide is 70:30 to 95:5; illustratively, the mass ratio of the first lithium cobalt composite oxide to the second lithium cobalt composite oxide is 70:30, 75:25, 80:20, 85:15, 90:10, 95:5, or a range consisting of any two of the above values.
[0059] 2. Preparation method of positive electrode material
[0060] The present application also provides a method for preparing a positive electrode material, which is used to prepare the positive electrode material of the aforementioned embodiment, comprising: step 1, sintering a mixture comprising a lithium source, a cobalt source, and an optional Q element source to obtain a primary positive electrode material; step 2, sintering the primary positive electrode material with a sodium source and an optional M element source in an atmosphere with an oxygen volume percentage of greater than 50% to obtain a final positive electrode material. By sintering the primary positive electrode material with the sodium source in an atmosphere with an oxygen volume percentage of greater than 50%, the local phase transformation of the Na element-rich region on the surface of the primary positive electrode material can be promoted to form a first region having a P63mc crystal structure, thereby obtaining the positive electrode material of the present application.
[0061] In some embodiments, the lithium source includes but is not limited to at least one of lithium carbonate, lithium hydroxide, and lithium fluoride.
[0062] In some embodiments, the cobalt source includes but is not limited to at least one of cobalt trioxide and cobalt hydroxide.
[0063] In some embodiments, the source of the Q element includes, but is not limited to, an oxide of the Q element.
[0064] In some embodiments, the sodium source includes but is not limited to at least one of sodium carbonate, sodium chloride, sodium sulfate, sodium sulfite, sodium fluoride, sodium phosphate, sodium nitrate, and sodium acetate.
[0065] In some embodiments, the source of the M element includes, but is not limited to, an oxide of the M element.
[0066] In some embodiments, the primary sintering atmosphere is an air atmosphere or an oxygen atmosphere.
[0067] In some embodiments, the primary sintering temperature T1 is 800° C. to 1200° C., and the primary sintering time t1 is 4 h to 20 h.
[0068] In some embodiments, the secondary sintering temperature T2 is 600° C. to 950° C., and the secondary sintering time t2 is 4 h to 20 h.
[0069] 3. Electrochemical Device
[0070] A second aspect of the present application provides an electrochemical device, comprising a positive electrode, the positive electrode comprising a positive electrode active layer, and the positive electrode active layer comprising the aforementioned positive electrode material.
[0071] The electrochemical device provided herein also includes a negative electrode, comprising a negative electrode current collector and a negative electrode active layer located on the surface of the negative electrode current collector. In some embodiments, the negative electrode active layer comprises a negative electrode material and a binder, and optionally a conductive agent. In some embodiments, the negative electrode material may include a material that reversibly intercalates and deintercalates lithium ions, lithium metal, a lithium metal alloy, or a transition metal oxide. In some embodiments, the negative electrode material comprises at least one of a carbon material or a silicon-based material, wherein the carbon material comprises at least one of graphite, hard carbon, or soft carbon, and the silicon-based material comprises at least one of silicon, a silicon-oxygen composite, a silicon-carbon composite, or a silicon alloy. In some embodiments, the binder comprises at least one of styrene-butadiene rubber, polyacrylic acid, a polyacrylate, an acrylate polymer, a polyamide, or a styrene-acrylate copolymer. In some embodiments, the conductive agent comprises at least one of conductive carbon black, acetylene black, Ketjen black, carbon nanotubes, or graphene. In some embodiments, the negative electrode current collector comprises copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, or any combination thereof.
[0072] The electrochemical device of the present application further includes an electrolyte, which includes a lithium salt and a non-aqueous solvent.
[0073] In some embodiments of the present application, the lithium salt includes but is not limited to one or more of LiPF6, LiBF4, LiPO2F2, LiN(SO2CF3)2, LiN(SO2F)2, LiB(C2O4)2 or LiBF2(C2O4).
[0074] The non-aqueous solvent includes, but is not limited to, one or more of a carbonate compound or a carboxylate compound.
[0075] Exemplary carbonate compounds include, but are not limited to, one or more of linear carbonate compounds or cyclic carbonate compounds. Specifically, linear carbonate compounds include, but are not limited to, one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), or ethylmethyl carbonate (MEC); cyclic carbonate compounds include, but are not limited to, one or more of ethylene carbonate (EC), propylene carbonate (PC), or butylene carbonate (BC).
[0076] Exemplary carboxylic acid ester compounds include, but are not limited to, one or more of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanoic acid lactone, valerolactone, or caprolactone.
[0077] According to some embodiments of the present application, in the electrochemical device of the present application, an isolation membrane is provided between the positive electrode and the negative electrode to prevent short circuit. The material and shape of the isolation membrane used in the embodiments of the present application are not particularly limited, and it may be any technology disclosed in the prior art. In some embodiments, the isolation membrane includes a polymer or inorganic substance formed from a material that is stable to the electrolyte of the present application. For example, the isolation membrane may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, a film or a composite film having a porous structure, and the material of the substrate layer includes at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Specifically, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film can be selected. A surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer may be an adhesive layer or a heat-resistant layer. The heat-resistant layer includes inorganic particles and a binder, wherein the inorganic particles include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, or barium sulfate. The binder includes at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polytetrafluoroethylene, or polyhexafluoropropylene. The bonding layer includes a polymer, and the polymer material includes at least one of polyamide, polyacrylonitrile, an acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, or a copolymer of vinylidene fluoride and hexafluoropropylene.
[0078] According to some embodiments of the present application, the electrochemical device of the present application includes, but is not limited to, all types of primary batteries or secondary batteries. In some embodiments, the electrochemical device is a lithium secondary battery. In some embodiments, the lithium secondary battery includes, but is not limited to, a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.
[0079] 4. Electronic Devices
[0080] An embodiment of the present application further provides an electronic device, which includes the electrochemical device of the aforementioned embodiment.
[0081] In some embodiments, the electronic devices of the present application include but are not limited to: mobile phones, laptops, tablet computers, drones, electric cars, electric bicycles, power tools, Bluetooth headsets, etc.
[0082] Hereinafter, the cathode material and the preparation method thereof of the present application will be further described in combination with specific embodiments and comparative examples.
[0083] Examples and Comparative Examples
[0084] 1. Preparation of positive electrode
[0085] 1.1 Preparation of positive electrode materials
[0086] Example 1
[0087] 240g of lithium carbonate and 500g of cobalt oxide were weighed, mixed, and sintered at 1050°C in an air atmosphere for 9 hours to obtain a primary positive electrode material. The obtained primary positive electrode material was mixed with 0.89g of sodium carbonate and then sintered again at 850°C in a 50vol% oxygen atmosphere for 7 hours. After crushing and screening, a positive electrode material with a Dv50 of 15μm was obtained. The surface layer of the positive electrode material includes a first region with a P63mc crystal structure and a second region with an R-3m crystal structure. The first region is dispersed in the second region in an island-like manner, as shown in Figure 1. Both the first and second regions contain Na. The molar ratio K1 of Na to Co in the first region is 0.45%, while the molar ratio K2 of Na to Co in the second region is 0.22%.
[0088] Examples 2 and 3
[0089] The preparation method is the same as that of Example 1, except that the amount of sodium carbonate added is controlled to adjust the Na element content in the first and second regions of the surface layer of the positive electrode material. The amounts of sodium carbonate added are 0.73 g and 1.12 g, respectively.
[0090] Example 4
[0091] 240g of lithium carbonate, 500g of cobalt trioxide, and 0.29g of sodium carbonate were weighed, mixed, and sintered at 1050°C in air for 8 hours to obtain a primary positive electrode material. The primary positive electrode material was mixed with 0.32g of sodium carbonate and sintered at 800°C in a 50 vol% oxygen atmosphere for 8 hours. After crushing and screening, a positive electrode material with a Dv50 of 15μm was obtained.
[0092] Examples 5-12
[0093] The preparation method is the same as that of Example 4, except that the amount of sodium carbonate added is controlled to adjust the Na element content in the first and second regions of the surface layer of the positive electrode material. The amount of sodium carbonate added in the first sintering step is 0.05g, 0.12g, 0.19g, 0.36g, 0.42g, 0.48g, 0.50g, and 0.44g, respectively; the amount of sodium carbonate added in the secondary sintering step is 0.26g, 0.32g, 0.37g, 0.42g, 0.86g, 0.89g, 0.93g, and 1.08g, respectively.
[0094] Example 13
[0095] 240g of lithium carbonate, 500g of cobalt oxide, and 0.29g of sodium carbonate were weighed, mixed, and sintered at 900°C in air for 9 hours to obtain a primary positive electrode material. The primary positive electrode material was mixed with 0.60g of sodium carbonate and sintered at 800°C in a 50 vol% oxygen atmosphere for 8 hours. After crushing and screening, a positive electrode material with a Dv50 of 5μm was obtained.
[0096] Examples 14-16
[0097] The method is basically the same as that in Example 2, except that alumina is further added in the secondary sintering step, and the Al element content in the second area of the surface layer of the positive electrode material is adjusted by the amount of alumina added. The amount of alumina added is 0.18g, 0.37g, and 0.55g, respectively.
[0098] Examples 17-20
[0099] A method basically the same as that in Example 15 was adopted, except that after the secondary sintering step, alumina was further added and sintered at 800°C for 8 hours, and the amount of alumina coating on the surface of the positive electrode material was adjusted by the amount of alumina added. The amounts of alumina added were 2.14g, 2.90g, 3.82g, and 5.04g, respectively.
[0100] Example 21
[0101] The method was basically the same as that of Example 19, except that after the secondary sintering step, 0.14 g of zirconium oxide and 3.82 g of aluminum oxide were further added and sintered at 800° C. for 8 hours.
[0102] Example 22
[0103] The positive electrode material in Example 4 was used as the first positive electrode material, and the positive electrode material in Example 13 was used as the second positive electrode material.
[0104] The prepared first positive electrode material and the second positive electrode material were mixed in a mass ratio of 8:2 to obtain a positive electrode material.
[0105] Examples 23-26
[0106] The preparation method is basically the same as that of Reference Example 22, except that the volume average particle size Dv50 of cobalt trioxide is changed to adjust the Dv50 of the first positive electrode material and the Dv50' of the second positive electrode material.
[0107] Examples 27-30
[0108] The preparation method is basically the same as that of Reference Example 22, except that the positive electrode materials in Examples 5, 6, 8, and 9 are used as the first positive electrode material.
[0109] Comparative Example 1
[0110] Weigh 240 g of lithium carbonate and 500 g of cobalt trioxide, mix them, sinter them at 1060° C. in an air atmosphere for 12 hours, cool them to 700° C., and continue sintering at 700° C. for 10 hours. After crushing and screening, a positive electrode material with a Dv50 of 15 μm was obtained.
[0111] Comparative Example 2
[0112] The preparation method is basically the same as that of Comparative Example 1, except that 0.17 g of sodium carbonate is further added to mix with lithium carbonate and cobalt oxide, and the positive electrode material is obtained through the same sintering steps.
[0113] Comparative Example 3
[0114] Weigh 240 g of lithium carbonate and 500 g of cobalt trioxide, mix them, sinter them at 900° C. in an air atmosphere for 9 hours, cool them to 800° C., and continue sintering at 800° C. for 8 hours. After crushing and screening, a positive electrode material with a Dv50 of 5 μm was obtained.
[0115] Comparative Example 4
[0116] The preparation method is basically the same as that of Example 1, except that the secondary sintering is carried out in an air atmosphere.
[0117] Comparative Example 5
[0118] The positive electrode material prepared in Comparative Example 1 was used as the first positive electrode material.
[0119] The positive electrode material prepared in Comparative Example 3 was used as the second positive electrode material.
[0120] The first positive electrode material and the second positive electrode material are mixed in a mass ratio of 9:1 to obtain a positive electrode material.
[0121] 1.2 Preparation of positive electrode
[0122] The positive electrode material, acetylene black, and polyvinylidene fluoride (PVDF) were mixed in a weight ratio of 94:3:3, and N-methylpyrrolidone (NMP) was added. The mixture was stirred thoroughly to obtain a positive electrode slurry. The positive electrode slurry was applied to one side of the positive electrode current collector aluminum foil and dried at 85°C. The above steps were repeated on the other side of the aluminum foil to obtain a positive electrode sheet coated with a positive electrode active layer on both sides. The positive electrode was then cold pressed, cut into pieces, and welded to the tabs.
[0123] 2. Preparation of negative electrode
[0124] Artificial graphite, sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were thoroughly stirred and mixed in an appropriate amount of deionized water at a weight ratio of 96:2:2 to obtain a negative electrode slurry. This negative electrode slurry was applied to one side of the negative electrode current collector copper foil and dried at 85°C. The above steps were repeated on the other side of the copper foil to obtain a negative electrode sheet coated with a negative electrode active layer on both sides. The negative electrode was then cold pressed, cut into pieces, and the tabs were welded to obtain the negative electrode.
[0125] 3. Preparation of electrolyte
[0126] Under a dry argon environment, LiPF6 was added to a solvent mixed with propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) (weight ratio of 1:1:1) and mixed evenly. Then, based on the total weight of the electrolyte, 4% of fluoroethylene carbonate, 2% of 1,3-propane sultone, 3% of adiponitrile and 1% of 1,3,6-hexanetrinitrile were added, wherein the mass percentage of LiPF6 was 12.5%, to obtain an electrolyte.
[0127] 4. Preparation of isolation membrane
[0128] A polyethylene porous polymer film with a thickness of 10 μm was used as the separator.
[0129] 5. Preparation of lithium-ion batteries
[0130] The positive electrode, separator, and negative electrode are stacked in order, wound, and placed in an aluminum-plastic film package. Electrolyte is then injected and packaged. After a series of processes including resting, formation, degassing, and trimming, a lithium-ion battery is obtained.
[0131] 2. Test Method
[0132] 1. Test method for element content and coating thickness
[0133] The cathode electrode was transferred to the chamber of a scanning electron microscope (FEI Vion Plasma FIB) equipped with a focused ion beam. Samples were processed to obtain samples suitable for transmission scanning electron microscopy (STEM) analysis (FEI Titan3G2 60-300). The sample surface was protected with Pt and processed using a Ga ion beam, with a thickness of no more than 100 nm. Cleaning was performed using low-voltage mode to remove residual surface residue from processing. The sample was observed under STEM, and the crystal structure of the first and second regions of the cathode material surface layer was determined by electron diffraction analysis. Electron micrographs of the lattice fringes in the first and second regions were taken at an appropriate magnification. Image processing software was used to measure the angle between the lattice fringes in the first and second regions at the grain boundaries. Simultaneously, the thickness of the first and second regions was measured, with the larger of the two regions used as the coating thickness. Data were collected using energy dispersive X-ray spectroscopy (EDS) at an appropriate magnification to determine the elemental content of the first and second regions of the cathode material surface layer, as well as the matrix. Data were collected from at least three different locations, and the average value was used as the final result.
[0134] 2. Test method for volume average particle size Dv50 of positive electrode materials
[0135] 0.5g of the sample powder to be tested was added to water and ultrasonically dispersed. The sample dispersion was added to the circulation pool of the laser particle size analyzer for testing to obtain the volume average particle size Dv50 of the positive electrode material particles.
[0136] 3. Test method for Na element content E and F in the first positive electrode material and the second positive electrode material
[0137] The cathode material sample was added to aqua regia for digestion, and the content of Na element in the cathode material was obtained by inductively coupled plasma optical emission spectrometry (ICP-OES).
[0138] 4. EIS impedance test method
[0139] At 25°C, the lithium-ion battery was charged at a constant current rate of 0.5C to 3.85V. After the voltage reached 3.85V, constant voltage charging was performed to a current of 0.025C and allowed to stand for 5 minutes. An alternating current impedance (EIS) test was then performed using an EIS impedance tester. The frequency range of the EIS test was set to 0.1kHz-10kHz, and the amplitude was set to 5mV. The Rct impedance value of the lithium-ion battery was obtained through the EIS test.
[0140] 5. Test method for high temperature storage expansion rate
[0141] At 25°C, charge the lithium-ion battery at a constant current rate of 0.5C to 4.50V. Then charge it at a constant voltage rate of 4.50V to a current of 0.05C, bringing it to a fully charged state at 4.50V. Measure the thickness of the fully charged battery before storage, which is recorded as D0. Then, store the fully charged lithium-ion battery in an 85°C oven for 24 hours. Immediately after removing the lithium-ion battery, measure its post-storage thickness, which is recorded as D1. High-temperature storage expansion ratio = (D1 - D0) / D0 × 100%.
[0142] 6. Test method for cycle capacity retention rate
[0143] At 25°C, charge the lithium-ion battery to 4.50V at a constant current of 0.5C at a charge rate, then charge it to 0.025C at a constant voltage. After standing for 5 minutes, discharge it to 3.0V at a constant current of 0.5C at a rate of 0.5C. Record the discharge capacity value of the first cycle. Use the same steps to charge and discharge the lithium-ion battery 800 times, and record the discharge capacity value of the 800th cycle. Cycle capacity retention = (discharge capacity of the 800th cycle / discharge capacity of the first cycle) × 100%.
[0144] Table 1
[0145] Referring to Table 1, a comparison of Comparative Examples 1-2 with Example 1 shows that the positive electrode material of the present application, because the surface layer has a first region of a P63mc crystal structure and a second region of an R-3m crystal structure, and both the first region and the second region contain the Na element, can effectively reduce the impedance and high-temperature storage expansion rate of the lithium-ion battery, and improve the cycle capacity retention rate of the lithium-ion battery at high voltage. Although the positive electrode material of Comparative Example 2 has enhanced ionic conductivity due to the doping of the Na element, which can reduce the impedance of the lithium-ion battery to a certain extent and improve the rate performance of the lithium-ion battery; however, because the surface layer of the positive electrode material of Comparative Example 2 only has the Na-doped R-3m phase, the R-3m phase is structurally unstable at high voltage, resulting in the lithium-ion battery formed by the positive electrode material of Comparative Example 2 still not being effectively improved in terms of high-temperature storage expansion rate and cycle capacity retention rate at high voltage. Compared with the positive electrode material of Comparative Example 2, the surface layer of the positive electrode material of the present application has both the first region of the P63mc phase and the second region of the R-3m phase, which not only makes the structure of the surface layer of the positive electrode material more stable, but also further improves the ionic conductivity of the positive electrode material, thereby significantly improving the power performance, high-temperature storage performance under high voltage, and cycle performance of the lithium-ion battery.
[0146] As shown in Table 1, Examples 1-13 show that because the first region having the P63mc crystal structure in the positive electrode material of the present application is formed by an in-situ phase transformation, the angle between the transition metal layer of the first region and the transition metal layer of the second region at the grain boundary is greater than or equal to 150°. This facilitates lithium ion transport between the first region and the second region, reducing the interfacial impedance during lithium ion insertion and extraction. Furthermore, because the first region having the P63mc crystal structure has high structural stability at high voltages, it can provide a stable channel for lithium ion insertion and extraction, thereby improving the cycling performance of lithium-ion batteries at high voltages.
[0147] The molar ratio K1 of the Na element and the Co element in the first region of the positive electrode material of the present application satisfies 0.1%≤K1≤1.0%, the molar ratio K2 of the Na element and the Co element in the second region satisfies 0.04%≤K2≤0.5%, and the relationship between K1 and K2 satisfies 1.1≤K1 / K2≤5, which are all beneficial to improving the power performance of the lithium-ion battery and the high-temperature storage performance and cycle performance at high voltage. In addition, by comparing Examples 1-3 with Examples 4-13, it can be seen that by further doping the Na element in the matrix, the impedance of the lithium-ion battery can be further reduced, and the high-temperature storage performance and cycle performance of the lithium-ion battery at high voltage can be improved. The reason is that by doping the Na element in the matrix, the lithium ion channels in the lithium-cobalt composite oxide matrix can be expanded and its layered structure can be stabilized, reducing the impedance and stress concentration during the lithium ion insertion and extraction process, thereby improving the power performance, high-temperature storage performance at high voltage and cycle performance of the lithium-ion battery.
[0148] Table 2
[0149] Referring to Table 2, it can be seen from the comparison between Example 2 and Examples 14-16 that by further doping the coating layer with Al element so that the molar ratio B of Al element to Co element in the second region satisfies 0.1%≤B≤1%, the high-temperature storage expansion rate of the lithium-ion battery can be further reduced, and its cycle capacity retention rate at high voltage can be improved, thereby further improving the safety performance and cycle performance of the lithium-ion battery.
[0150] Referring to Table 2, a comparison of Example 15 with Examples 17-20 shows that by further coating the surface of the positive electrode material with an oxide of the element M, the high-temperature storage expansion rate of the lithium-ion battery can be further reduced, and its cycle capacity retention rate at high voltage can be improved, thereby further improving the safety performance and cycle performance of the lithium-ion battery.
[0151] Table 3
[0152] Referring to Table 1 and Table 3, it can be seen from the comparison of Examples 4-13 with Examples 22-30 that the positive electrode materials formed by mixing different particle sizes in the present application make the first positive electrode material Dv50 and the second positive electrode material Dv50' satisfy 3≤Dv50 / Dv50'≤6, which can further reduce the impedance and high-temperature storage expansion rate of the lithium-ion battery, and improve its cycle capacity retention rate, thereby improving the power performance, safety performance and cycle performance of the lithium-ion battery.
[0153] Referring to Table 3, from the comparison of Example 22 and Examples 27-30, it can be seen that when the mass percentage E of the Na element in the first positive electrode material and the mass percentage F of the Na element in the second positive electrode material satisfy 0.5≤E / F≤0.9, the lithium-ion battery can have a lower impedance and an improved high-temperature storage expansion rate and cycle capacity retention rate. As a result, the lithium-ion battery has improved power performance, safety performance and cycle performance.
[0154] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present application should be included in the scope of protection of the present application.
Claims
1. A positive electrode material, comprising a lithium cobalt composite oxide, the lithium cobalt composite oxide comprising a substrate and a coating layer located on the surface of the substrate, the coating layer comprising a first region and a second region, the first region having a P6 3 The first region has an R-3m crystal structure, the second region has an R-3m crystal structure, and both the first region and the second region contain Na element.
2. The positive electrode material according to claim 1, in, The molar ratio of the Na element to the Co element in the first region is K1, the molar ratio of the Na element to the Co element in the second region is K2, and the positive electrode material satisfies at least one of the following conditions: (1)0.1%≤K1≤2.0%; (2)0.01%≤K2≤1.0%; (3)1.1≤K1 / K2≤5.
3. The positive electrode material according to claim 2, in, The positive electrode material satisfies at least one of the following conditions: (1)0.2%≤K1≤1.0%; (2)0.04%≤K2≤0.5%。 4. The positive electrode material according to claim 1, in, The positive electrode material satisfies at least one of the following conditions: (1) Both the first region and the second region are located on the surface of the substrate; (2) The first regions are dispersed in the second regions in the form of islands; (3) The coating layer has a thickness of 10 nm to 200 nm; (4) The thickness of the first region is 10 nm to 200 nm; (5) The thickness of the second region is 10 nm to 200 nm.
5. The positive electrode material according to claim 1, in, There is a grain boundary between the first region and the second region, and an angle between the transition metal layer in the first region and the transition metal layer in the second region at the grain boundary is greater than or equal to 150°.
6. The positive electrode material according to claim 1, in, The positive electrode material satisfies at least one of the following conditions: (1) The matrix further comprises Na element, and the molar ratio of Na element to Co element in the matrix is K3, satisfying: 0.01%≤K3≤0.2%; (2) The second region further includes Al element, and the molar ratio of Al element to Co element in the second region is B, satisfies: 0.1% ≤ B ≤ 1%; (3) The matrix further comprises a Q element, wherein the Q element comprises at least one of Al, Mg, Ti, Ca, La, Y, Zr, Fe, Mn, Ni, Nb, Mo, W, Ta, Zn, Cr, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba or Cu, and the molar ratio of the Q element to the Co element in the matrix is C, satisfying: 0.1%≤C≤10%; (4) The molar percentage of the Co element in the lithium-cobalt composite oxide is 90% to 99% based on the molar amount of the metal elements other than the Li element in the lithium-cobalt composite oxide.
7. The positive electrode material according to claim 1, in, The coating layer further includes a third region, the third region includes an oxide of an M element, the M element includes at least one of Al, Mg, Ti, Zr, Y, Nb, Ca, Ni, Mn or Ce, and satisfies at least one of the following conditions: (1) The third region is located on the surface of the second region away from the substrate; (2) the third region is located on the surface of the first region facing away from the substrate; (3) The third region is located on the surface of the substrate.
8. The positive electrode material according to claim 1, in, The lithium cobalt composite oxide includes a first lithium cobalt composite oxide and a second lithium cobalt composite oxide, the volume average particle size Dv50 of the first lithium cobalt composite oxide is greater than the volume average particle size Dv50' of the second lithium cobalt composite oxide; based on the mass of the first lithium cobalt composite oxide, the mass percentage of the Na element in the first lithium cobalt composite oxide is E; based on the mass of the second lithium cobalt composite oxide, the mass percentage of the Na element in the second lithium cobalt composite oxide is F; Satisfies: 0.3≤E / F≤1.
5.
9. The positive electrode material according to claim 8, in, The positive electrode material satisfies at least one of the following conditions: (1) the volume average particle size Dv50 of the first lithium cobalt composite oxide is 12 μm to 25 μm; (2) the volume average particle size Dv50' of the second lithium cobalt composite oxide is 2 μm to 8 μm; (3) the volume average particle size Dv50 of the first lithium cobalt composite oxide and the volume average particle size Dv50' of the second lithium cobalt composite oxide satisfy 3≤Dv50 / Dv50'≤6; (4) the mass ratio of the first lithium cobalt composite oxide to the second lithium cobalt composite oxide is 70:30 to 95:5; (5)0.01%≤E≤0.3%; (6)0.04%≤F≤0.5%; (7)0.5≤E / F≤0.
9. 10 . An electrochemical device comprising a positive electrode, wherein the positive electrode comprises a positive electrode material layer, wherein the positive electrode material layer comprises the positive electrode material according to claim 1 .
11. An electronic device comprising the electrochemical device according to claim 10.
Citation Information
Patent Citations
Positive electrode active material, electrochemical device, and electronic device
CN114373900A
Positive electrode active material, electrochemical device, and electronic device
CN114497525A
Positive electrode active material, positive electrode plate, electrochemical device comprising positive electrode plate, and electronic device
CN115104204A
Nonaqueous electrolyte battery
JP2010129509A
Non-aqueous electrolyte secondary battery
WO2014083834A1
Cited By
Lithium cobalt oxide positive electrode material and preparation method and application thereof
CN120613382A