Energy storage device electrode using a cellulose ester binder

WO2024229781A1PCT designated stage expired Publication Date: 2024-11-14EASTMAN CHEM CHINA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/093400
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-14

Smart Images

  • Figure CN2023093400_14112024_PF_FP_ABST
    Figure CN2023093400_14112024_PF_FP_ABST
Patent Text Reader

Abstract

An electrode plate for an electrochemical energy storage device, comprising: a current collector plate; and an active material layer formed on at least a portion of the current collector plate; wherein the active material layer comprises a binder and an active material; wherein the binder comprises a cellulose ester (CE), which has one or more substituents selected from acetyl, propionyl, and butyryl; and wherein the cellulose ester has a glass transition temperature (Tg) of 80 to 200℃, a melting temperature (Tm) of 120 to 260℃, and a ball drop viscosity of 0.1 to 50 seconds as measured according to ASTM D-1343.
Need to check novelty before this filing date? Find Prior Art

Description

ENERGY STORAGE DEVICE ELECTRODE USING A CELLULOSE ESTER BINDERTECHNICAL FIELD

[0001] Embodiments of the present disclosure generally relate to an electrode for an electrochemical energy storage device, and more particularly, to an electrode composition comprising a cellulose ester binder that is particularly suitable for rechargeable lithium-ion batteries. The cellulose ester can be used as a replacement or partial replacement for polyvinylidene difluoride (PVDF) commonly used as a binder for the electrode to bind electrochemical active materials to the current collector.BACKGROUND

[0002] Electrochemical energy storage devices play an important role in modern everyday life. Lithium-ion batteries, in particular, have been widely used in computer, mobile devices, and, more recently, electric vehicles due to their higher energy capacity and higher operating voltages. Lithium-ion battery (LIB) is typically composed of an anode, a cathode, a separator, and an electrolyte mixture. The anode (negative electrode) is typically made of a copper current collector coated with graphite / carbon, while the cathode (positive electrode) is typically made of aluminum current collector coated with various lithium metal oxides.

[0003] A binder may be required to coat the electrochemical active materials, such as, graphite for the anode and lithium metal oxides for the cathode, to the current collectors. The binder plays an important role in holding the particles of the active materials together and in adhering the coating to the current collector metal. In addition, the binder must remain stable inside the harsh environment of a battery during the electrochemical charging and discharging cycles in order to maintain the energy capacity of the battery. The binder must also have good mechanical strength and a certain degree of pliability to withstand the battery manufacturing process.

[0004] Accordingly, there remains a need for binder materials that can provide improved adhesion and cohesion among active materials and the current collectors, tensile strength, ionic conductivity, swelling resistance, and / or ease of production.SUMMARY

[0005] Disclosed in embodiments herein are electrode plates for an electrochemical energy storage device. The electrode plates comprise: a current collector plate; and an active material layer formed on at least a portion of the current collector plate; wherein the active material layer comprises a binder and an active material; wherein the binder comprises a cellulose ester (CE) , which has one or more substituents selected from acetyl, propionyl, and butyryl; and wherein the cellulose ester has a glass transition temperature (Tg) of 80 to 200℃, a melting temperature (Tm) of 120 to 260℃, and a ball drop viscosity of 0.1 to 50 seconds as measured according to ASTM D-1343.

[0006] Also disclosed in embodiments herein are methods of coating a current collector plate. The methods comprise coating at least a portion of a current collector plate with an active material composition comprising an active material and a binder, wherein the binder comprises a cellulose ester (CE) , which has one or more substituents selected from acetyl, propionyl, and butyryl; and wherein the cellulose ester has a glass transition temperature (Tg) of 80 to 200℃, a melting temperature (Tm) of 120 to 260℃, and a ball drop viscosity of 0.1 to 50 seconds as measured according to ASTM D-1343.

[0007] Further disclosed in in embodiments herein are rechargeable lithium-ion batteries. The rechargeable lithium-ion batteries comprise the electrode plates as described herein.

[0008] Additional features and advantages of the embodiments will be set forth in the detailed description which follows, and in part will be readily apparent to those skilled in the art from that description or recognized by practicing the embodiments described herein. It is to be understood that both the foregoing and the following  description describe various embodiments and are intended to provide an overview or framework for understanding the nature and character of the claimed subject matter.BRIEF DESCRIPTION OF THE DRAWINGS

[0009] FIG. 1 graphically depicts the voltage stability of inventive binder solutions of the present invention as compared to a comparative binder solution.DETAILED DESCRIPTION

[0010] Reference will now be made in detail to embodiments of electrode plates, methods of coating a current collector plate, as well as rechargeable lithium-ion batteries. The electrode plates may be used in the manufacture of rechargeable lithium-ion batteries. It is noted, however, that this is merely an illustrative implementation of the embodiments disclosed herein. The embodiments are applicable to other electrochemical technologies that are susceptible to similar problems as those discussed above.

[0011] In embodiments herein, the electrode plate comprises a current collector plate and an active material layer formed on at least a portion of the current collector plate. The current collector plate may be made of a conductive material such as aluminum, aluminum alloy, titanium, titanium alloy, silver, silver alloy, stainless steel, nickel, nickel alloy, copper or copper alloy. The current collector plate may specifically be an anode or a cathode. The anode may be made of a conductive material such as aluminum, aluminum alloy, titanium, titanium alloy, silver, silver alloy, stainless steel, nickel, nickel alloy, copper or copper alloy. The cathode may be made of a conductive material such as aluminum or an aluminum alloy. In some embodiments, the current collector plate is made of aluminum. In other embodiments, the current collector plate is made of copper.

[0012] The active material layer comprises a binder and an active material. In one or more embodiments herein, the active material layer may have a weight ratio of binder to active material of from 0.01: 1 to 0.1: 1. All individual values and subranges are  included and disclosed herein. For example, in some embodiments, the active material layer may have a weight ratio of binder to active material of from 0.01: 1 to 0.09: 1 or 0.02: 1 to 0.09: 1, or 0.02: 1 to 0.08: 1.

[0013] Examples of suitable active materials may include, but are not limited to, lithium cobalt-based oxides, lithium manganese-based oxides, lithium nickel-based oxides, lithium nickel manganese-based oxides, lithium nickel cobalt manganese-based oxides, lithium nickel cobalt aluminum-based oxides, graphite, graphene, silicon, and combinations thereof.

[0014] In some embodiments, the current collector plate is a cathode (or positive electrode) , and the active material comprises lithium cobalt-based oxides, lithium manganese-based oxides, lithium nickel-based oxides, lithium nickel manganese-based oxides, lithium nickel cobalt manganese-based oxides, lithium nickel cobalt aluminum-based oxides, or combinations thereof. Specific examples of active materials, may include LiFePO4 (LFP) , LiCoO2 (LCO) , LiMn2O (LMO) , Li (NiCoMn) O2 (NCM) , Li (NiCoAl) O2 (NCA) , LiNiO2, LiMnO2, LiCrO2, LiMn2O4, and LiFeO2. In other embodiments, the current collector plate is an anode (or negative electrode) , and the active material comprises graphite, graphene, silicon, and combinations thereof. In one or more embodiments, the active material layer may further comprise an additive. Examples of additives may include carbon or a carbon-based material. In some embodiments, the active material layer further comprises carbon black as a conductive material.

[0015] The binder comprises a cellulose ester (CE) . In one or more embodiments herein, the binder comprises at least 40 wt. %of CE. All individual values and subranges are included and disclosed herein. For example, the binder may comprise at least 50 wt. %, at least 65 wt. %, at least 75 wt. %, at least 85 wt. %, at least 90 wt. %, at least 95 wt. %, or at least 99 wt. %of CE.

[0016] CEs are derived from the renewable polysaccharide cellulose. There have been persistent interests in replacing petroleum-based materials with CE-based materials as the society continues to look for biodegradable, compostable,  environmental-friendly materials for use in modern technology. The conversion of cellulose-to-cellulose ester is a critical step to enable the material to be soluble in common organic solvents and to become melt processible into various useful forms, such as film and fiber. The cellulose backbone provides three hydroxyl (OH) groups per anhydroglucose unit (AGU) , which are replaced with acyl groups during esterification. The extent of this replacement of the hydroxyl group can be expressed as degree of substitution with a range of 0 (cellulose) to 3 (tri-ester) . A wide variety of cellulose esters can be prepared by varying the substituents, the degree of substitution (DS) , the functionality, and the molecular weight to obtain the desirable properties such as solubility, compatibility, viscosity, and hardness.

[0017] In embodiments herein, the CE has one or more substituents selected from acetyl, propionyl, and butyryl. In one or more embodiments, the CE may be selected from the group consisting of cellulose acetate (CA) , cellulose diacetate (CDA) , cellulose triacetate (CTA) , cellulose acetate butyrate (CAB) , cellulose acetate propionate (CAP) , and combinations thereof. In some embodiments, the CE is selected from the group consisting of cellulose acetate (CA) , cellulose diacetate (CDA) , cellulose triacetate (CTA) , and combinations thereof. In other embodiments, the CE is CAP. In further embodiments, the CE is CAB.

[0018] In one or more embodiments, the CE may have an average degree of substitution for the acetyl substituent (DSAC) of 0.5 to 3, an average degree of substitution for the butyryl substituent (DSbu) of 0 to 2.5, an average degree of substitution for the propionyl substituent (DSpr) of 0 to 2.5, and an average degree of substitution for the unsubstituted hydroxyl group (DSOH) of 0 to 2.5. As used herein, the term “degree of substitution” or “DS” refers to the average number of acyl substituents per anhydroglucose ring of the cellulose polymer, wherein the maximum degree of substitution is 3.0, as described above.

[0019] In some embodiments, the cellulose ester is one or more selected from the group consisting of cellulose acetate (CA) , cellulose diacetate (CDA) , and cellulose triacetate (CTA) , and wherein the cellulose ester has an average degree of substitution  for the acetyl substituent (DSAC) of 0.5 to 3 and an average degree of substitution for the unsubstituted hydroxyl group (DSOH) of 0 to 2.5.

[0020] In other embodiments, the cellulose ester is a cellulose acetate propionate (CAP) , and wherein the cellulose ester has an average degree of substitution for the acetyl substituent (DSAC) of 0.5 to 2.5, an average degree of substitution for the propionyl substituent (DSpr) of 0.5 to 2.5, and an average degree of substitution for the unsubstituted hydroxyl group (DSOH) of 0 to 2.

[0021] In further embodiments, the cellulose ester is a cellulose acetate butyrate (CAB) , and wherein the cellulose ester has an average degree of substitution for the acetyl substituent (DSAC) of 0.5 to 2.5, an average degree of substitution for the butyryl substituent (DSbu) of 0.5 to 2.5, and an average degree of substitution for the unsubstituted hydroxyl group (DSOH) of 0 to 2.

[0022] The cellulose esters described herein may have unsubstituted hydroxyl groups. When the cellulose ester (CA, CDA, CTA, CAP, or CAB) has unsubstituted hydroxyl groups, the cellulose ester may further comprise a substituent that results from a reaction of at least some of the unsubstituted hydroxyl groups with another substituent, such as an anhydride (e.g., phthalic anhydride, hexahydrophthalic anhydride, trimellitic anhydride, and succinic anhydride) , a carboxymethyl ether, a carboxyl, an aryl, or combinations thereof.

[0023] In some embodiments, the cellulose ester further comprises a carboxyl group directly attached to the cellulose ester ring, and wherein the cellulose ester has an average degree of substitution for the carboxyl substituent (DScb) of 0.1 to 2. The carboxyl group can provide water dispersibility for the binder to be used in water-based slurries. It can also provide strong adhesion to the active materials and ionic conductivity for the electrodes to improve their electrochemical performance. In other embodiments, the cellulose ester further comprises a carboxyl group directly attached to the cellulose ester ring, and wherein the cellulose ester has an average degree of substitution for the carboxyl substituent (DScb) of 0.1 to 2; and wherein the cellulose ester has an acid number of 10 to 200 mg KOH / g. All individual values and subranges  are included and disclosed herein. For example, the CE may have an acid number of from 20 to 180, 30 to 160, 40 to 140, or 50 to 120 mg KOH / g.

[0024] In some embodiments, the cellulose ester has unsubstituted hydroxyl groups, and the cellulose ester further comprises a substituent that results from a reaction of at least some of the unsubstituted hydroxyl groups with an anhydride selected from the group consisting of phthalic anhydride, hexahydrophthalic anhydride, trimellitic anhydride, and succinic anhydride, and wherein the cellulose ester has an average degree of substitution for the anhydride substituent (DSah) of 0.5 to 2. In other embodiments, the cellulose ester has unsubstituted hydroxyl groups, and the cellulose ester further comprises a substituent that results from a reaction of at least some of the unsubstituted hydroxyl groups with an anhydride selected from the group consisting of phthalic anhydride, hexahydrophthalic anhydride, trimellitic anhydride, and succinic anhydride, and wherein the cellulose ester has an average degree of substitution for the anhydride substituent (DSah) of 0.5 to 2; and wherein the cellulose ester has an acid number of 10 to 200 mg KOH / g. All individual values and subranges are included and disclosed herein. For example, the CE may have an acid number of from 20 to 180, 30 to 160, 40 to 140, or 50 to 120 mg KOH / g.

[0025] In some embodiments, the cellulose ester further comprises a carboxymethyl ether substituent, and wherein the cellulose ester has an average degree of substitution for the carboxymethyl substituent (DScm) of 0.1 to 2. In other embodiments, the cellulose ester further comprises a carboxymethyl ether substituent, and wherein the cellulose ester has an average degree of substitution for the carboxymethyl substituent (DScm) of 0.1 to 1; and wherein the cellulose ester has an acid number of 10 to 200 mg KOH / g. All individual values and subranges are included and disclosed herein. For example, the CE may have an acid number of from 20 to 180, 30 to 160, 40 to 140, or 50 to 120 mg KOH / g.

[0026] In some embodiments, the cellulose ester has unsubstituted hydroxyl groups, and the cellulose ester further comprises a substituent that results from a reaction of at least some of the unsubstituted hydroxyl groups with an aromatic compound, and  wherein the cellulose ester has an average degree of substitution for the aryl substituent (DSar) of 0.1 to 2. Cellulose esters having aromatic groups can be desirable to provide coating porosity to the electrodes for improved access to the active materials. In other embodiments, the cellulose ester has unsubstituted hydroxyl groups, and the cellulose ester further comprises a substituent that results from a reaction of at least some of the unsubstituted hydroxyl groups with an aryl group, and wherein the cellulose ester has an average degree of substitution for the aryl substituent (DSar) of 0.1 to 2, or 0.1 to 1.5, or 0.1 to 1, or 0.1 to 0.5.

[0027] The cellulose esters described herein have a glass transition temperature (Tg) of 80 to 200℃, a melting temperature (Tm) of 120 to 260℃, and a ball drop viscosity of 0.1 to 50 seconds as measured according to ASTM D-1343. All individual values and subranges are included and disclosed herein. For example, in some embodiments, the CE may have a Tg of from 85 to 190℃, 90 to 180℃, 95 to 170℃, 100 to 160℃, 105 to 150℃, or 110 to 140℃; a Tm of from 125 to 250℃, 130 to 240℃, 135 to 230℃, 140 to 220℃, 145 to 220℃, 150 to 210℃, 155 to 200℃, or 160 to 200℃; and a ball drop viscosity of from 0.2 to 45 seconds, 0.2 to 40 seconds, 0.3 to 35 seconds, 0.4 to 30 seconds, 0.5 to 25 seconds, 0.6 to 20 seconds, 0.7 to 15 seconds, or 0.8 to 10 seconds.

[0028] In some embodiments, the binder as previously described herein may further comprises one or more polymers selected from the group consisting of polyvinylidene fluoride (PVDF) , polyvinyl butyral (PVB) , polyacrylic acid, styrene butadiene rubber (SBR) , carboxymethyl cellulose (CMC) , polyacrylonitrile, polyamide, polyimide, polytetrafluoroethylene (PTFE) , polyvinyl alcohol, polyethylene oxide, cyclic olefin polymer (COP) , and polyvinylidene fluoride-co-hexafluoropropylene.

[0029] In some embodiments, the binder further comprises: (i) a cellulose ester in an amount of 5%to 95%, based on the total weight of (i) and (ii) ; and (ii) polyvinylidene difluoride (PVDF) in an amount of 95%to 5%, based on the total weight of (i) and (ii) . All individual values and subranges are included and disclosed herein. For example, in some embodiments, the cellulose ester is in an amount of 10%to 90%, 20%to 80%,  30%to 70%, or 40%to 60%and said PVDF is in an amount of 90%to 10%, 80%to 20%, 70%to 30%, 60%to 40%.

[0030] In one or more embodiments herein, the binder may exhibit at least one of the following properties: a binder solution viscosity at 10 wt. %in n-methyl pyrrolidone (NMP) of 0.5 to 100 Pa. s; and a change in the binder solution viscosity after 7 days, as measured at a shear rate of 0.01 to 1000 / second, of less than 10%. In some embodiments, the binder exhibits both properties.

[0031] The active material layer may be formed on the current collector plate by any methods known in the art. For example, in an organic solvent-based process, a slurry with suitable viscosity is first prepared by mixing the binder (s) , the active materials, and other additives with an organic solvent. The slurry thus obtained is then coated on the current collector plate by one of the following methods --spraying, dipping, spinning, roller, and flow coating.

[0032] Examples of suitable organic solvents for the preparation of the slurry may include N-methyl pyrrolidone (NMP) , N-butylpyrrolidone, N, N’-dimethylacetamide, N, N’-dimethylformamide, pyridine, tetrahydrofuran, acetonitrile, methyl ethyl ketone, cyclopentanone, toluene, methyl isobutyl ketone, methylene chloride, chloroform, 1, 2-dichloroethane, methyl amyl ketone, methyl isopropyl ketone, methyl isoamyl ketone, ethyl acetate, n-butyl acetate, propylene glycol methyl ether acetate, and a mixture thereof.

[0033] Alternatively, water may be used to replace organic solvents to prepare the slurry provided that a binder used is water dispersible, and may include additional substituents as described herein, such as those having hydrophilic carboxyl groups.

[0034] The active material layer may also be formed on the current collector plate by a dry process without solvents, in which the binder, the active materials, and the additives are blended to yield a homogeneous mixture in powder form. The powder can then be applied to the current collector plate by a method such as, for example, electrostatic spraying. The powder layer can then be pressed by feeding the coated  metal through a hot roller to obtain the desirable coating properties –e.g., adhesion and thickness.

[0035] Also disclosed in embodiments described herein is a rechargeable lithium-ion battery comprising the electrode plate of any embodiment described herein.

[0036] TEST METHODS

[0037] Glass Transition Temperature (Tg)

[0038] A resin sample is placed in a differential scanning calorimeter (TA Instruments DSC Q2000 V24.9 Build 121) . On the first heating cycle, the sample is heated under nitrogen atmosphere from 30℃ to 150-300℃ depending on the samples at a rate of 10℃ / min. The sample is then quench cooled to 30℃. For the second heating cycle, the sample is heated under the same conditions as those used in the first heating cycle. The midpoint of the baseline shift of the second heating cycle is reported as the Tg of the sample. The results are reported in ℃.

[0039] Peak Melting Temperature (Tm)

[0040] In the above DSC test, in addition to Tg, Tm may be present and is recorded as an endothermic peak. The midpoint of the peak in the second heating cycle is reported as the Tm of the sample. The results are reported in ℃.

[0041] Ball Drop Viscosity

[0042] Ball drop viscosity is measured according to ASTM D1343. The results are reported in seconds.

[0043] Nuclear Magnetic Resonance (NMR)

[0044] The relative degree of substitution (RDS) at C6, C3, and C2 in the cellulose ester of the present invention is determined by carbon 13 NMR following the general methods described in “Cellulose Derivatives” , ACS Symposium Series 688, 1998, T.J. Heinze and W.G. Glasser, Editors, herein incorporated by reference to the  extent it does not contradict the statements herein. Briefly, the carbon 13 NMR data is obtained using a JEOL NMR spectrometer operating at 100 MHz or a Bruker NMR spectrometer operating at 125 MHz. The sample concentration is 100 mg / mL of DMSO-d6. Five mg of Cr (OAcAc) 3 per 100 mg of sample are added as a relaxation agent. The spectra are collected at 80 ℃. using a pulse delay of 1 second. Normally, 15,000 scans are collected in each experiment. Conversion of a hydroxyl to an ester results in a downfield shift of the carbon bearing the hydroxyl and an upfield shift of a carbon gamma to the carbonyl functionality. Hence, the RDS of the C2 and C6 ring carbons are determined by direct integration of the substituted and unsubstituted C1 and C6 carbons. The RDS at C3 is determined by subtraction of the sum of the C6 and C2 RDS from the total DS. The carbonyl RDS is determined by integration of the carbonyl carbons using the general assignments described in Macromolecules, 1991, 24, 3050-3059, herein incorporated by reference to the extent it does not contradict the statements herein. In the case of cellulose mixed esters containing a plurality of acyl groups, the cellulose ester is first converted to fully substituted cellulose mixed p-nitrobenzoate ester. The position of the p-nitrobenzoate esters indicate the location of the hydroxyls in the cellulose mixed ester.

[0045] EXAMPLES

[0046] The following specific examples are given to illustrate the process and performance properties associated with conductive paste compositions and its components. The inventive and comparative examples are provided below with the details of the formulations and results are provided in the Tables below.

[0047] Table 1 –Raw Materials & Properties

[0048] Sample preparation and purification

[0049] The CE powders (C-A-P, CA-398-30) and PVB powders are washed with isopropyl alcohol (the weight of isopropyl alcohol is around 20 times of the weight of CE) whiling stirring at room temperature, and the washing is done 3 times (washing time is around 5 hours for each time) . Then, the isopropyl alcohol is decanted, and the powders in the bottom are transferred onto an aluminum pan and dried in a house vacuum at 100 ℃ for 1 day.

[0050] To prepare a neutralized C-A-P sample, the C-A-P powders are added into methanol (the weight of methanol is around 20 times of the weight of C-A-P) whiling stirring at room temperature, and LiOH is added until the pH is 7. The mixture is precipitated in n-butyl acetate. The precipitation is washed with isopropyl alcohol (the weight of isopropyl alcohol is around 20 times of the weight of C-A-P) whiling stirring at room temperature, and the washing is done 3 times (washing time is around 5 hours for each time) . Then, the isopropyl alcohol is decanted, and the neutralized C-A-P  powders in the bottom are transferred onto an aluminum pan and dried in a house vacuum at 100 ℃ for 1 day.

[0051] Binder solution preparation

[0052] The CE and PVB powders are dried overnight in a vacuum oven at 90 ℃. 10%stock solutions of the CE and PVB powders are prepared by mixing with n-methyl pyrrolidone (NMP) in a centrifugal mixer (FlackTek SpeedMixer) . 10%PVDF is used on its own and in combination with 10%CE or CE / PVB binders as described below in Table 2. In separate containers portions of the 10%PVDF solution is mixed with each 10%CE binder in a 75: 25 mass ratio. NMP is used to dilute the binder solution if it is too thick to coat (viscosities > 10 Pa·sat 3 1 / s) . Approximately ~0.5 m length of each binder solution is coated on a table with a knife coater at a 50 μm gap. Adjustments to gap is made if dilution is required for some of the binder mixtures. The coating is dried on the table at 70 –80 ℃, then overnight at 110 ℃ under vacuum.

[0053] Table 2. Binder solution components

[0054] Testing coin cell preparation

[0055] Half-cells with binders coating on aluminum foil are constructed to test voltage stability of binders. 5 / 8” diameter samples of dried binder on aluminum foil and coin cell components (316SS anode / cathode can, 316SS spacers and conical spring, Celgard 2320 separator) are dried overnight under vacuum at 80 ℃. The vacuum oven is backfilled with argon, and cell components are transferred to glove box. 16 mm diameter lithium disc surfaces are brushed with stainless steel bristles and placed in anode can. 150 μL electrolyte (1 M LiPF6 in EC / EMC, 3 / 7 wt ratio from SoulBrain, MI) is added via pipette. The rear side (bare foil) of all samples is lightly abraded with fine grit sandpaper to improve electrical contact with the cathode can of the coin cell assembly. A 3 / 4" diameter Celgard 2320 separator is positioned on top of anode can. The sample is placed on top of Celgard separator with binder side down. Spacers and conical spring are positioned on top of binder sample, followed by cathode can. Cell is crimped to seal. Coin cells are aged 12 hours at room temperature to ensure full wetting of all components with electrolyte.

[0056] Voltage stability evaluation

[0057] Sequential 1 mA charging steps are applied, using constant current / constant voltage mode with a 50 μA current cutoff, across the voltage range of 3.5 -4.7 V in increments of 0.1 V. The cell voltage is held at the setpoint for 1 hour or until the end current value reached, whichever comes first. A ten-minute rest is implemented between charging steps to allow polarization to dissipate. Three repeats are tested for each sample and the average energy is plotted in FIG. 1. All of the CE / PVDF binder solutions demonstrated equivalent stability to the PVDF control. None of the samples in the voltage stability assessment showed any indication of instability in contact with electrolyte across the voltage range evaluated.

[0058] Electrode Preparation and Testing Using Cellulose Ester as the Binder

[0059] An NCM cathode slurry is prepared by mixing lithium nickel cobalt manganese oxide with one or more cellulose esters as disclosed in the specification as  the binder in the presence of N-methyl pyrrolidinone (NMP) solvent. The resulting slurry is then cast onto an aluminum foil at a loading of 2 mAh / cm2 and 4 mAh / cm2 respectively and subsequently dried. The electrode thus prepared is then punched, calendared to yield 3 g / cm3, and assembled into half cells vs. lithium metal for electrochemical testing. Additional electrode samples are prepared for physical testing: 1 / 8” –1 / 16” mandrel bend testing to assess the degree of cracking / delamination that occurs, and tape peel (adhesion) testing to compare peel force and coating mass loss. Lastly, the through-plane electrical conductivity of the electrode is assessed utilizing a range of applied currents.

[0060] Comparative Example: Electrode Preparation and Testing Using PVDF as the Binder

[0061] The above procedure is repeated using PVDF as the binder instead of the cellulose ester.

[0062] Evaluation of the Slurries

[0063] The inventive CE and comparative PVDF slurries prepared are compared as follows:

[0064] 1. Dissolution Time –The time required to dissolve the binder is assessed using standardized solvent volumes, binder masses, and mixing conditions. The complete dissolution is defined as complete transparency of the solution (visually assessed) and stable viscosity.

[0065] 2. Binder Solution Viscosity –Viscosity of the fully dissolved binder solutions at a standard concentration, 6 weight %binder in NMP, is measured. A small amount of each binder solution is cast on aluminum foil for use in voltage stability assessment (see electrochemical testing details, below)

[0066] 3. Mixing Time vs. Dispersion –Hegman gauge (FOG) measurements are made every 15 minutes during the conductive additive and active material dispersion steps.

[0067] 4. Viscosity vs. Solids / Solvent content –The NCM cathode slurry with PVDF binder is prepared at 60 –62 weight %solids. The solids mass fraction of the NCM cathode slurry with the CE binder is adjusted such that the final viscosity matches that of the PVDF based as closely as possible.

[0068] Electrochemical Testing

[0069] Voltage Stability Assessment -Binder solutions without conductive additive or active material cast on aluminum foil are constructed into coin cells with a lithium metal reference electrode and standard lithium-ion battery electrolyte. Voltages ranging from 3.8 –4.9 V are applied to the binder-coated aluminum foil to assess the voltage stability windows of both binders in the presence of the electrolyte.

[0070] Half Cell Performance -NCM cathode half cells are tested using identical procedures to compare gravimetric capacity, coulombic efficiency, DCIR cell resistance, power performance, and cyclic capacity fade rate.

[0071] Physical / Electrical Testing

[0072] Peel Testing -1.5” square electrode samples from each electrode type are calendared to yield 3.0 g / cm3. Electrode coating adhesion / cohesion is assessed using a 180° tape peel apparatus in accordance with ASTM D3359. Peel force and electrode coating mass loss are assessed.

[0073] Bend Testing -Electrode samples are cut to 60 mm wide (roughly the width of the electrode in a wound 18650 cell) , calendared to yield 3.0 g / cm3, and tightly wrapped around the 0.125" and 0.0625" mandrels. The degrees of cracking / delamination are assessed.

[0074] Through-plane Conductivity Testing –5 / 8” (15.9 mm) diameter electrodes from each formulation and coat loading are punched and calendared to yield 3.0 g / cm3. Electrodes are placed between the 16 mm diameter stainless steel positive and negative contacts and a constant force of 100 pounds is applied. Short duration current pulse is applied, and the voltage is recorded in order to calculate the conductivity.

[0075] The dimensions and values disclosed herein are not to be understood as being strictly limited to the exact numerical values recited. Instead, unless otherwise specified, each such dimension is intended to mean both the recited value and a functionally equivalent range surrounding that value. For example, a dimension disclosed as “40 mm” is intended to mean “about 40 mm. ”

[0076] Every document cited herein, if any, including any cross-referenced or related patent or application and any patent application or patent to which this application claims priority or benefit thereof, is hereby incorporated herein by reference in its entirety unless expressly excluded or otherwise limited. The citation of any document is not an admission that it is prior art with respect to any invention disclosed or claimed herein or that it alone, or in any combination with any other reference or references, teaches, suggests or discloses any such invention. Further, to the extent that any meaning or definition of a term in this document conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this document shall govern.

[0077] While particular embodiments of the present invention have been illustrated and described, it would be obvious to those skilled in the art that various other changes and modifications can be made without departing from the spirit and scope of the invention. It is therefore intended to cover in the appended claims all such changes and modifications that are within the scope of this invention.

Claims

1.An electrode plate for an electrochemical energy storage device, comprising:a current collector plate; andan active material layer formed on at least a portion of the current collector plate;wherein the active material layer comprises a binder and an active material;wherein the binder comprises a cellulose ester (CE) , which has one or more substituents selected from acetyl, propionyl, and butyryl; andwherein the cellulose ester has a glass transition temperature (Tg) of 80 to 200℃, a melting temperature (Tm) of 120 to 260℃, and a ball drop viscosity of 0.1 to 50 seconds as measured according to ASTM D-1343.2.The electrode plate of claim 1, wherein the active material layer has a weight ratio of binder to active material of 0.01: 1 to 0.1: 1.3.The electrode plate of claims 1 or 2, wherein the binder exhibits at least one of the following properties:a binder solution viscosity at 10 wt. %in n-methyl pyrrolidone (NMP) of 0.5 to 100 Pa·s; anda change in the binder solution viscosity after 7 days, as measured at a shear rate of 0.01 to 1000 / second, of less than 10%.4.The electrode plate of claims 1-3, wherein the cellulose ester is one or more selected from the group consisting of cellulose acetate (CA) , cellulose diacetate (CDA) , cellulose triacetate (CTA) , and combinations thereof; and wherein the cellulose ester has an average degree of substitution for the acetyl substituent (DSAC) of 0.5 to 3 and an average degree of substitution for the unsubstituted hydroxyl group (DSOH) of 0 to 2.5.5.The electrode plate of claims 1-3, wherein the cellulose ester is a cellulose acetate propionate (CAP) , and wherein the cellulose ester has an average degree of substitution for the acetyl substituent (DSAC) of 0.5 to 2.5, an average degree of  substitution for the propionyl substituent (DSpr) of 0.5 to 2.5, and an average degree of substitution for the unsubstituted hydroxyl group (DSOH) of 0 to 2.6.The electrode plate of claims 1-3, wherein the cellulose ester is a cellulose acetate butyrate (CAB) , and wherein the cellulose ester has an average degree of substitution for the acetyl substituent (DSAC) of 0.5 to 2.5, an average degree of substitution for the butyryl substituent (DSbu) of 0.5 to 2.5, and an average degree of substitution for the unsubstituted hydroxyl group (DSOH) of 0 to 2.7.The electrode plate of claims 4-6, wherein the cellulose ester has unsubstituted hydroxyl groups, and the cellulose ester further comprises a substituent that results from a reaction of at least some of the unsubstituted hydroxyl groups with an anhydride selected from the group consisting of phthalic anhydride, hexahydrophthalic anhydride, trimellitic anhydride, and succinic anhydride, and wherein the cellulose ester has an average degree of substitution for the anhydride substituent (DSah) of 0.5 to 2; and wherein the cellulose ester has an acid number of 10 to 200 mg KOH / g.8.The electrode plate of claims 4-6, wherein the cellulose ester further comprises a carboxymethyl ether substituent, and wherein the cellulose ester has an average degree of substitution for the carboxymethyl substituent (DScm) of 0.1 to 2; and wherein the cellulose ester has an acid number of 10 to 200 mg KOH / g.9.The electrode plate of claims 4-6, wherein the cellulose ester further comprises a carboxyl group directly attached to the cellulose ester ring, and wherein the cellulose ester has an average degree of substitution for the carboxyl substituent (DScb) of 0.1 to 2;and wherein the cellulose ester has an acid number of 10 to 200 mg KOH / g.10.The electrode plate of claims 4-6, wherein the cellulose ester has unsubstituted hydroxyl groups, and the cellulose ester further comprises a substituent that results from a reaction of at least some of the unsubstituted hydroxyl groups with an aromatic compound; and wherein the cellulose ester has an average degree of substitution for the aryl substituent (DSar) of 0.1 to 2.11.The electrode plate of claims 1-10, wherein the binder further comprises one or more polymers selected from the group consisting of polyvinylidene fluoride (PVDF) ,  polyvinyl butyral, polyacrylic acid, styrene butadiene rubber (SBR) , carboxymethyl cellulose (CMC) , polyacrylonitrile, polyamide, polyimide, polytetrafluoroethylene (PTFE) , polyvinyl alcohol, polyethylene oxide, cyclic olefin polymer (COP) , and polyvinylidene fluoride-co-hexafluoropropylene.12.The electrode plate of claims 1-11, wherein the binder comprises:i. a cellulose ester in an amount of 5%to 95%, based on the total weight of (i) and (ii) andii. a polyvinylidene difluoride (PVDF) in an amount of 95%to 5%, based on the total weight of (i) and (ii) .13.The electrode plate of claims 1-12, wherein the current collector plate is a cathode, and the active material comprises lithium cobalt-based oxides, lithium manganese-based oxides, lithium nickel-based oxides, lithium nickel manganese-based oxides, lithium nickel cobalt manganese-based oxides, lithium nickel cobalt aluminum-based oxides, or combinations thereof.14.The electrode plate of claims 1-12, wherein the current collector plate is an anode, and the active material comprises graphite, graphene, silicon, and combinations thereof.15.The electrode plate of claims 1-14, wherein the active material layer further comprises carbon black as a conductive material.16.The electrode plate of claim 13, wherein the current collector plate is made of aluminum.17.The electrode plate of claim 14, wherein the current collector plate is made of copper.18.A rechargeable lithium-ion battery comprising the electrode plate of any of the preceding claims.

Citation Information

Patent Citations

  • Electrode with enhanced safety and electrochemical device having the same

    CN101313428A

  • Pouch-type flexible film battery and method of manufacturing the same

    CN102437339A

  • Hot melt and pressure-sensitive adhesives that include highly-plasticized cellulose esters and methods and articles relating thereto

    CN105073928A

  • Preparation method of cellulose acetate butyrate nitrate

    CN106317230A

  • Cellulose Ester Film, Production Method of the Same, Polarizing Plate and Liquid Crystal Display

    US20080118667A1