High-performance lithium battery current collector and preparation method therefor, and conductive paste and preparation method therefor

Through the dumbbell-shaped structure of modified conductive agent and magnetic field induction technology, a three-dimensional network structure of the current collector of lithium battery is constructed, solving the problems of lowering the firming force of conductive coating and coating monitoring, and improving the cycle stability and production efficiency of the battery.

WO2024229972A1PCT designated stage expired Publication Date: 2024-11-14BLUEGLOWNANO TECHNOLOGIES LTD +1

Patent Information

Application Number
PCT/CN2023/107196
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2023-07-13
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The existing lithium battery current collector conductive coating has reduced its fixation force after multiple charges and discharges, which is easy to fall off, resulting in a shortening of battery life and the inability to accurately monitor the coating thickness and coverage, limiting production efficiency and quality stability.

Method used

Use modified conductive agent to form a dumbbell-shaped structure, and use magnetic field to induce it to be arranged obliquely in the coating along the thickness direction 15-45°, to build a three-dimensional network structure, enhance the fixation and conductivity, and improve the coating formula and process Reduce the amount of conductive agent and coating thickness.

Benefits of technology

It improves the cycle stability and rate performance of lithium batteries, extends battery life, reduces internal resistance, and realizes accurate monitoring of coating thickness and coverage, improving production efficiency and quality stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023107196-APPB-I100001
    Figure PCTCN2023107196-APPB-I100001
  • Figure PCTCN2023107196-APPB-I100002
    Figure PCTCN2023107196-APPB-I100002
  • Figure PCTCN2023107196-APPB-I100003
    Figure PCTCN2023107196-APPB-I100003
Patent Text Reader

Abstract

A high-performance lithium battery current collector and a preparation method therefor, and a conductive paste and a preparation method therefor, which belong to the technical field of lithium battery production. A functional coating of the current collector is of a functional layered covering structure, which is formed by means of applying a conductive paste on a surface of metal foil and drying same, and has a thickness of not greater than 800 nm. The functional coating comprises a plurality of strip-shaped modified conductive agents, which are parallel to each other in the functional coating after being cured and molded, and the axes of which are obliquely arranged to form an included angle of 15-45 degrees with respect to the surface of the metal foil in the thickness direction of the coating, wherein the modified conductive agents are interwoven with modified nano-fibers, binders and conductive agents in the coating, so as to form an oriented three-dimensional network connection structure with reinforced fixation, electrical conductivity and thermal conductivity and capable of uniform deformation and automatic reset. The functional coating can automatically adapt to and hedge the volume, and can maintain the relative stability of a connection network and the electrical connection strength during expansion and reduction processes of a charging and discharging active substance, thereby improving the comprehensive performance of a lithium battery.
Need to check novelty before this filing date? Find Prior Art

Description

A high-performance lithium battery current collector, conductive slurry and preparation method thereof Technical Field

[0001] The present invention belongs to the technical field of lithium battery production, and in particular relates to a high-performance lithium-ion battery current collector, a conductive slurry and a preparation method thereof. Background Art

[0002] Power lithium-ion batteries are widely used in industries such as new energy vehicles and large-scale energy storage, and market demand is growing. The current collector in lithium-ion batteries and other secondary batteries refers to the structure or component that collects current. In lithium-ion batteries, this primarily refers to metal foil, such as copper or aluminum foil. The term also broadly includes the tabs. Its primary function is to collect the current generated by the battery's active materials to generate a larger current output. Therefore, the current collector should be in full contact with the active materials and ideally have minimal internal resistance.

[0003] The use of functional coatings to surface-treat conductive battery substrates is a significant technological innovation. Carbon-coated aluminum / copper foil involves uniformly and delicately coating dispersed conductive materials such as nano-conductive graphite, carbon-coated particles, and carbon nanotubes onto aluminum / copper foil. This provides excellent static conductivity, collecting the microcurrent of the active material. This significantly reduces the contact resistance between the positive / negative electrode materials and the current collector, improves the adhesion between the two, reduces the amount of binder used, and significantly improves overall battery performance.

[0004] Currently, safer and cheaper, LiFePO4 is a promising cathode material. However, its inherent low electronic and ionic conductivity, mass density, and tap density result in defects such as poor conductivity and adhesion, and easy powder shedding. Carbon-coated aluminum foil applied to the cathode current collector can reduce interfacial contact impedance, lower battery internal resistance, alleviate internal battery structure, and improve the battery's discharge rate to a certain extent. For lithium-ion battery anodes, the use of carbon-coated copper foil can address the need for high-energy-density battery electrodes with high surface density, high adhesion, and the application of silicon-carbon materials with high expansion properties, as well as the need for laminated battery punching without powder shedding.

[0005] Existing carbon-coated foils are made by compounding conductive materials such as graphite, carbon black, and multi-layer carbon nanotubes, and evenly dispersing them with dispersants and binders in different proportions to form a conductive slurry that is then coated on aluminum foil or copper foil. The carbon coating layer is approximately 2 to 50 μm, the coating is relatively thick, and the peeling resistance during repeated charging is poor. The appearance of the carbon coating varies depending on the proportion of the conductive agent, but generally appears in black or gray of varying depths. When different lithium battery material systems are used, the coating machine cannot use color or color difference to determine the electrode coating coverage and coating thickness through observation or machine vision monitoring methods to improve the quality stability of the current collector product, and cannot accurately monitor the coating coverage in high-speed production quality management, thus limiting the improvement of production efficiency.

[0006] To improve the performance of the current collector's conductive coating, Chinese invention patent application No. 201610410998.1 discloses a carbon nanotube conductive coating current collector and its preparation process. The current collector comprises a metal current collector and a carbon nanotube conductive coating, wherein the carbon nanotube conductive coating is applied to the surface of the metal current collector. The carbon nanotube conductive coating has a thickness of 1 to 50 μm and a surface pattern of network-like microcracks and a rough, porous structure. The carbon nanotube conductive coating of this invention provides a good conductive network for the electrode. By preparing conductive slurries with different dispersion effects, dense microcracks are formed on the surface of the carbon nanotube conductive coating after drying, improving the bonding strength between the carbon nanotube conductive coating and the current collector and reducing the internal resistance of the battery. However, the conductive coating in this technical solution requires the use of more than two conductive materials and has a large thickness of micron level. After multiple charge and discharge cycles, its adhesion (characterizing the durability of the coating) decreases rapidly, which can easily cause the coating to fall off. After it falls off, the current collector metal layer is directly exposed to the active material, which can easily cause the current collector electrode to be corroded and oxidized and fail, shortening the battery life. At the same time, after the material is applied, the conductive coating has poor resettlement properties and appears black or gray. During the coating operation, it is impossible to judge the coating thickness and coverage based on the coating color and color difference. During the coating process, there is a lack of effective coating quality monitoring methods. At the same time, in the subsequent coating and welding process of the battery pole pieces, there is an adverse effect due to the inability to accurately judge the coating color.

[0007] Chinese invention patent application number 201610522526.5 discloses a conductive paste and a method for forming a reticulated carbon thermal and conductive network current collector. The conductive paste is made from the following raw materials by weight: 4-6 parts carbon nanotubes, 8-12 parts conductive carbon black, 1-3 parts flake graphite, and 15-25 parts polyvinyl alcohol. This invention utilizes carbon materials with high thermal and electrical conductivity in one or more dimensions to form a reticulated material, such as carbon nanotubes, graphene, or other high thermal conductivity materials added to conventional conductive carbon black, to form a continuous thermally and electrically conductive network coating on the current collector. This not only improves heat dissipation at high charge and discharge rates, but also meets electrical conductivity requirements, preventing thermal aging and extending system life. However, in the above technical solution, more than two conductive materials need to be used, and the thickness of the conductive network coating formed is still relatively large, the coating has poor resettlement properties, and the color is gray-black and cannot be monitored; the spatial structure of the mesh material is randomly distributed and has no orientation, and its effect on reducing interfacial resistance, enhancing electrical conductivity, thermal conductivity and fixation is also limited.

[0008] During the charge and discharge process of a lithium battery, the relative positions, contact surfaces, and contact points of the various components within it (particularly the active material, conductive material, and current collector) undergo periodic changes based on electrochemical reactions and physical volume changes. During these changes, especially during volume expansion, the distance between the components increases, the number of contact points decreases, and the contact resistance increases, leading to an increase in the battery's internal resistance and a rapid decrease in efficiency. Furthermore, after each cycle, it is difficult to ensure that the various materials can accurately return to their original positions and restore their original connection network and strength. The spatial distribution between the components gradually becomes disordered, and the connection (electrical and thermal conductivity) performance deteriorates, resulting in a decline in various battery performance characteristics after multiple cycles. To overcome this drawback, it is necessary to consider maintaining a strong connection network and strength between the various components within the lithium battery during charge and discharge, as well as after multiple cycles, to reduce the connection network loss caused by physical and chemical reactions, which in turn leads to an increase in the battery's internal resistance and a decrease in capacity.

[0009] The randomly arranged carbon nanotubes used in the aforementioned prior art fail to fully exploit the excellent mechanical, electrical, and thermal conductivity properties of individual carbon nanotubes and their arrays. Furthermore, this irregular distribution easily leads to carbon nanotube agglomeration and increases the contact resistance between carbon nanotubes, resulting in the performance of lithium-ion battery anode materials prepared using this type of conductive coating material falling far short of expectations. However, using existing techniques to regularly arrange carbon nanotubes to create a specific three-dimensional structural framework is difficult to control and achieve. Therefore, simultaneous improvements in the preparation processes of carbon nanotubes, conductive plasma, coating structure, and current collector are required to significantly enhance the overall performance of the current collector. Technical issues

[0010] The present invention addresses the above-mentioned deficiencies in the prior art and provides a high-performance lithium battery current collector, wherein the functional coating uses a modified conductive agent as a conductive material, and based on the dumbbell-shaped structure of the modified conductive agent, a bridge-island structure anchored at both ends is formed in the coating that can automatically adapt to and offset changes in volume and other deformations, and under the action of an external magnetic field, the modified conductive agent is arranged in a specific 15-45° oblique and parallel arrangement along the thickness direction, forming a three-dimensional network structure with enhanced fixation, electrical conductivity, thermal conductivity and high reset characteristics, thereby solving the problem that the network structure of the prior art has no arrangement regularity and cannot simultaneously take into account the enhanced fixation, electrical conductivity and thermal conductivity of the coating. The current collector of the present invention is applied to lithium batteries and can better establish a spatial network structure and reliable connection with the active ingredients. In addition, during the charge and discharge, battery coating and active material expansion and contraction processes, the modified conductive agent can maintain the orderliness of the spatial distribution of the conductive material inside the lithium battery through its angle change and anchoring effect, so as to maintain the relative stability of the connection network and electrical connection strength, thereby solving the problem that the coating fixation decreases rapidly and the coating easily falls off after multiple charge and discharge cycles in the prior art in lithium battery applications.

[0011] The present invention also provides a method for preparing the dumbbell-shaped modified conductive agent, which is formed by oxidizing multi-walled carbon nanotubes, chemically modifying both ends, and pre-connecting other larger-scale conductive agent particles at both ends to form a dumbbell-shaped structure. A bridge-island structure anchored at both ends is formed in the coating, which can automatically adapt to regular arrangement and automatically adjust the tilt angle to offset volume changes and deformations. During the oxidation process, vacancy defects are formed in the single-layer carbon nanotubes due to the oxidation of local CC bonds. The presence of the defects leads to the existence of magnetic moments near the defects, thereby giving the carbon nanotube-modified conductive agent weak magnetism.

[0012] The present invention also provides a conductive slurry for preparing the above-mentioned functional coating and a preparation method thereof. By simultaneously improving the coating formula and preparation process, the amount of modified conductive agent added is reduced and the average thickness of the coating after drying is no more than 800 nanometers. It uses a modified conductive agent with weak magnetism to form a specific 15-45° oblique arrangement structure along the thickness direction in the coating, further increasing its specific surface area in contact with the active material, so as to greatly enhance the adhesion of the coating after multiple charge and discharge cycles, solve the problems of thick coating and poor adhesion in existing batteries, and improve the life and high-rate performance of secondary batteries such as lithium ion batteries.

[0013] The present invention also provides a method for preparing the above-mentioned current collector, which solves the problems of difficulty and complex process in forming an adaptive three-dimensional network connection structure in the coating. The oriented array of magnetic modified conductive agent is realized through a constant magnetic field, thereby enhancing the conductivity and fixation of the functional coating, reducing the amount of modified conductive agent and the thickness of the functional coating; during the coating process of the conductive slurry, the modified conductive agent and the substrate are three-dimensionally structured, which is easy to shape and control; the structure shaping can be completed simultaneously during the coating and drying process, saving steps and obtaining a coating structure in which the oriented modified conductive agent and the substrate are interwoven. Technical Solutions

[0014] To achieve the above object, the present invention provides the following technical solutions:

[0015] A high-performance lithium battery current collector comprises a metal foil and a functional coating, characterized in that the functional coating is a functional layered covering structure having a thickness of no more than 800 nm formed by coating one or both surfaces of the metal foil with a conductive slurry and drying; the functional coating comprises a plurality of strip-shaped modified conductive agents, each of which is a magnetically oriented modified multi-walled carbon nanotube. After curing, the modified conductive agents are parallel to each other in the functional coating, and within the thickness of the coating, their axes are each arranged obliquely at an angle of 15 to 45 degrees with the metal foil surface. The modified conductive agents are interwoven with the modified nanofibers, binder, and conductive agent in the coating to form an oriented three-dimensional network connection structure with enhanced fixation, electrical and thermal conductivity, and uniform deformation and resetting.

[0016] The magnetically oriented modified multi-walled carbon nanotubes in the functional coating are modified multi-walled carbon nanotubes with a dumbbell-shaped structure, an inner diameter of not less than 5 nm, an outer diameter of not more than 20 nm, and a length of not more than 1200 nm. The modified multi-walled carbon nanotubes, after oxidation and chemical modification, have a dumbbell-shaped fiber structure with thicker ends and thinner middle. After orientation, the thicker lower ends are connected to the metal foil surface respectively, and the upper ends are connected to each other. With the cooperation of the adhesive, other conductive particles of different sizes and modified nanofibers are sandwiched between the thinner fiber parts in the middle, so that the parts are connected to each other to form a three-dimensional network bridge-island structure with anchored ends and oriented arrangement. The elastic three-dimensional network limits the deformation and displacement of the modified multi-walled carbon nanotubes and conductive particles during battery operation, so as to automatically adapt to and offset the internal volume changes and deformation and displacement of the conductive particles during the charging and discharging process of the lithium battery, thereby maintaining the reliability of the functional coating for the connection between the metal foil surface and the active material.

[0017] A conductive slurry for preparing the high-performance lithium battery current collector is characterized in that the conductive slurry is an aqueous slurry prepared by dispersing and mixing modified multi-walled carbon nanotubes, nanoconductive agents, modified nanofibers, dispersants, binders and solvents, and the slurry has a solid content of 0.1-5%, a viscosity of 200-1000 mPa·s (25°C), and a pH of 8-11.

[0018] The weight ratio of each raw material component of the conductive paste is modified as follows: modified multi-walled carbon nanotube, nano conductive agent: modified nanofiber: dispersant: binder: solvent = (0.01-1.8): (0.01-0.2): (0.02-2): (0.02-20): (0.05-20): (56-99.89).

[0019] A method for preparing the high-performance lithium battery current collector conductive slurry is characterized in that it comprises the following steps:

[0020] S1: Prepare materials: prepare modified multi-walled carbon nanotubes, nanoconductive agent, modified nanofibers, dispersant, binder, and solvent respectively according to the proportions;

[0021] S2: Preparation of high-concentration modified conductive agent suspension: Weigh the modified nanofibers and dispersant in proportion and add them to 1 / 3 of the solvent. Dissolve them completely by mechanical stirring. Then weigh the desired modified agent into the mixed solution and ultrasonicate it for 30 minutes to obtain a modified conductive agent suspension, which is specifically a modified multi-walled carbon nanotube suspension.

[0022] S3: magnetization: placing the modified multi-walled carbon nanotubes and nano-conductive agent dispersion in a strong external magnetic field for magnetization to further stimulate the magnetic anisotropy of the magnetically modified multi-walled carbon nanotubes and obtain a high-concentration magnetically modified multi-walled carbon nanotube suspension;

[0023] S4: Preliminary dispersion: Add a corresponding proportion of binder to the above-mentioned high-concentration magnetic modified multi-walled carbon nanotube suspension, and replenish the solvent to the required amount; use a high-speed vacuum disperser first and then a sand mill for preliminary dispersion; the shear speed during dispersion in the vacuum disperser is 10-25 m / s, the vacuum degree is not less than 0.085 MPa, and the vacuum dispersion time is 1-5 hours; the diameter of the sand mill beads in the sand mill is 0.2-2 mm, the proportion is 30-90%, the sand mill speed is 600-10000 r / min, and the sand mill time is 0.1-5 hours;

[0024] S5: Secondary dispersion: Use ultrasonic processing equipment to disperse again in the form of ultrasonic resonance, and apply alternating magnetic fields on both sides to further evenly disperse the modified multi-walled carbon nanotubes and nano-conductive agent particles and align them in the same direction under the induction of the magnetic field, thereby obtaining a conductive slurry with magnetic orientation.

[0025] A method for preparing the high-performance lithium battery current collector is characterized in that it comprises the following steps:

[0026] (A1) preparing a current collector metal foil and a dispersed conductive slurry, and setting up a coating device, an ultrasonic device, a constant magnetic field generating device, and a drying device;

[0027] (A2) applying the dispersed conductive paste on the surface of the metal foil to form a liquid colloidal coating having a viscosity of 200 to 1000 mPa·s (25° C.) and a thickness of 500 to 1200 nm on the surface;

[0028] (A3) continuously applying a constant magnetic field perpendicular to the surface of the metal foil to the liquid colloidal coating, so that the orientation-modified conductive agent in the coating is induced by the external magnetic field to align in an orderly manner, gradually straighten from its original coiled state, and form a parallel array, interwoven with the substrate;

[0029] (A4) Drying the coating to evaporate the solvent and volatiles, and continuously applying a constant magnetic field. As the viscosity of the coating rapidly increases, the modified conductive agent maintains its arrangement position and posture and quickly takes shape, and is arranged in parallel at an angle of 15-45 degrees in the thickness direction until the solidified components of the conductive paste of the coating are fixed on the surface of the metal foil to form a dense functional covering structure with a thickness of no more than 800 nm, that is, a three-dimensional network structure with enhanced fixing, electrical conductivity, thermal conductivity and high reset characteristics is formed on the surface of the metal foil. Beneficial effects

[0030] Compared with the prior art, the present invention has the following advantages:

[0031] (1) The functional coating and conductive paste of the present invention use a modified conductive agent as the conductive material. Its unique dumbbell-shaped structure forms a bridge-island structure with two ends anchored in the coating that can automatically adapt to and offset changes in volume and other deformations. It also has magnetic anisotropy and can be arranged in a specific orientation under the induction of a magnetic field. When used in lithium batteries, the modified conductive agent can automatically adjust the tilt angle as the internal volume of the battery changes, better establish a spatial network structure with the active ingredients, and reliably connect. In addition, during the charging and discharging, and expansion and contraction of the battery coating and active materials, the modified conductive agent maintains the orderliness of the spatial distribution to maintain the relative stability of the connection network and electrical connection strength, thereby solving the problem of the prior art that the coating adhesion decreases rapidly and the coating easily falls off after multiple charge and discharge cycles in lithium battery applications.

[0032] (2) The conductive paste provided by the present invention realizes the composite use of modified conductive agent, modified nanocellulose and dispersant in the preparation process. The dispersant modifies the surface of the modified conductive agent in a non-covalent manner, weakening the van der Waals force between molecules and reducing their surface energy, so that it can be better dispersed in the aqueous solution; the modified nanocellulose provides a three-dimensional porous network structure for the modified conductive agent and other components in the functional coating, and the negatively charged groups generate electrostatic repulsion between fibers to form a stable colloid, so that the modified conductive agent is stably bound in its developed pores, playing a role in assisting dispersion. Under the combined action of the two, the magnetic modified conductive agent is well dispersed in the conductive paste, avoiding aggregation, and facilitating the orientation of the modified conductive agent under the induction of a magnetic field in the subsequent process;

[0033] (3) The functional coating of the present invention continuously applies an external magnetic field during the slurry preparation and coating process of the conductive slurry, so that the magnetic modified conductive agent therein is induced to form an induced magnetic moment under the action of a strong magnetic field, thereby achieving ordering of the magnetic modified conductive agent, and finally forming a specific 15-45° oblique and parallel arrangement along the thickness direction in the coating;

[0034] (4) The modified conductive agent in the functional coating of the present invention is composed of modified carbon nanotubes, which can use the relatively larger inner diameter of the carbon nanotubes to act as ion diffusion channels, exerting the channel effect and making Li + Ions quickly penetrate the coating along the internal cavity of the carbon nanotubes, increasing the Li + The diffusion rate of ions shortens the Li + Ion migration path, to enhance the efficiency of electron transfer and thus reduce impedance, applied to lithium batteries to improve battery rate performance and low temperature performance;

[0035] (5) The oriented parallel array of the magnetic modified conductive agent in the functional coating of the present invention gives the functional coating a magnetic orientation. The combination of magnetic current collectors with positive and negative poles forms a battery, so that a stable magnetic field is formed between the positive and negative current collectors in the battery, that is, the magnetic field constraint makes the migration of lithium ions regular. On the other hand, in terms of passing through the lithium battery diaphragm, the regularity of lithium ion movement also improves the permeability of the diaphragm, thereby reducing the diaphragm impedance. The lithium battery assembled with magnetic current collectors with different polarities prepared by the present invention can significantly increase its battery capacity and reduce the battery impedance, while improving the battery cycle performance; in addition, its adaptive hedging volume change and maintaining reliable connection can also increase the safety of lithium batteries in high-power discharge, thereby improving the energy utilization rate and charging efficiency in charging and discharging, and reducing the charging time.

[0036] (6) The functional coating of the present invention constructs a three-dimensional network structure of a modified conductive agent and a flexible adhesive matrix material interwoven, providing a connection layer with high strength, conductive efficiency and good flexibility, which can effectively increase the contact area between the rigid metal current collector and the conductive paste, improve the adhesion of the coating, effectively reduce the interface resistance between the current collector and the battery active material, increase the electrochemical stability of the current collector material, avoid the increase of the battery internal resistance, and reduce the negative impact of the battery performance, especially the negative impact of the performance under high current charge and discharge conditions; at the same time, the three-dimensional interwoven network anchored at both ends of the modified conductive agent is used to buffer the volume change during the charge and discharge process, improve the reliability of the electrical connection, avoid the expansion and separation between the conductive paste and the current collector, enhance the long-term adhesion between the current collector metal foil substrate and the battery active material during repeated charge and discharge, improve the stability of the electrode piece, avoid cycle failure, and thus improve the specific capacity, cycle stability and rate performance of the electrode. Therefore, the functional coating provided by the present invention and the lithium battery prepared therefrom have the advantages of high capacity, long cycle life and good rate performance;

[0037] (7) The present invention provides more contact sites for active particles through the introduction of modified carbon nanotubes and the effective construction of a three-dimensional network, thereby increasing their specific surface area in contact with the active material and significantly enhancing the fixation of the positive / negative electrode materials on the current collector. Therefore, the current collector of the present invention can appropriately reduce the proportion of binder in the positive / negative electrode slurry of the battery, further reducing the internal resistance, which is conducive to improving the energy density of the battery. The positive electrode sheet prepared using the current collector of the present invention has a resistance of only 1 / 3 of that of pure plain foil, but the peeling force is more than 4 times that of pure plain foil. The prepared lithium-ion battery has an AC internal resistance reduced by more than 42% compared to the battery prepared with the plain foil current collector.

[0038] (8) The current collector provided by the present invention can significantly increase the battery energy density, improve the cycle life and rate performance. Under the 1C charge 2C discharge system, after 2000 cycles at room temperature, the capacity retention rate of the lithium-ion battery prepared using the current collector of the present invention can reach 93%, which is much higher than the 80% capacity retention rate of the plain foil current collector. At the same time, the battery cycle consistency is also significantly better than that of the pure plain foil current collector.

[0039] (9) The method for preparing a high-performance lithium battery current collector and a conductive slurry provided by the present invention has readily available materials, simple steps, strong controllability, and low preparation cost. The prepared current collector functional coating has a unique upper and lower double-layer internal aggregation structure and excellent mechanical properties, and has great development potential and application value in the fields of power lithium battery manufacturing and the like. Modes for Carrying Out the Invention

[0040] The present invention is further described in detail below with reference to a number of embodiments.

[0041] Example

[0042] The high-performance lithium-ion battery current collector, conductive slurry and preparation method provided by the present invention can be applied to the manufacture of lithium batteries using technical routes such as lithium cobalt oxide (LCO), lithium manganese oxide (LMO), lithium iron phosphate (LFP), and ternary materials (lithium nickel cobalt manganese oxide (NCM) and lithium nickel cobalt aluminum oxide (NCA)). It can also be adapted to a variety of diaphragms and electrolytes and has a wide range of applications.

[0043] A high-performance lithium battery current collector comprises a metal foil and a functional coating. The functional coating is a functional layered covering structure formed by coating one or both surfaces of the metal foil with a conductive slurry and drying to form a thickness of no more than 800 nm. The functional coating includes a plurality of strips of modified conductive agents, each of which is a magnetically oriented modified multi-walled carbon nanotube. After curing, the modified conductive agents are parallel to each other in the functional coating and arranged obliquely within the thickness of the coating, with their axes each forming an angle of 15 to 45 degrees with the metal foil surface. The modified conductive agents are interwoven with the modified nanofibers, binder, and conductive agent in the coating to form an oriented three-dimensional network connection structure with enhanced fixation, electrical and thermal conductivity, and uniform deformation and resetting.

[0044] The modified conductive agent in the functional coating, i.e., magnetically oriented modified multi-walled carbon nanotubes, is a dumbbell-shaped modified multi-walled carbon nanotube with an inner diameter of not less than 5 nm, an outer diameter of not more than 20 nm, and a length of not more than 1200 nm. The modified multi-walled carbon nanotubes, after oxidation and chemical modification, have a dumbbell-shaped fiber structure with thicker ends and thinner middle. After orientation, the thicker lower ends are connected to the metal foil surface and the upper ends are connected to each other. With the help of an adhesive, other conductive agent particles and modified nanofibers of different sizes are sandwiched between the thinner fiber parts in the middle, so that the parts are connected to each other to form a three-dimensional network bridge-island structure with anchors at both ends and oriented arrangement. The elastic three-dimensional network limits the deformation and displacement of the modified multi-walled carbon nanotubes and conductive agent particles during battery operation, so as to automatically adapt to and offset the internal volume changes and deformation and displacement of the conductive particles during the charging and discharging process of the lithium battery, thereby maintaining the reliability of the functional coating for the connection between the metal foil surface and the active material.

[0045] A conductive slurry for preparing the high-performance lithium battery current collector is characterized in that the conductive slurry is an aqueous slurry prepared by dispersing and mixing a modified conductive agent (modified multi-walled carbon nanotubes), a nanoconductive agent, modified nanofibers, a dispersant, a binder and a solvent, and the slurry has a solid content of 0.1-5%, a viscosity of 200-1000 mPa·s (25°C), and a pH of 8-11.

[0046] The weight ratio of each raw material component of the conductive paste is modified as follows: modified conductive agent (i.e., modified multi-walled carbon nanotubes), nano conductive agent: modified nanofiber: dispersant: binder: solvent = (0.01~1.8): (0.01~0.2): (0.02~2): (0.02~20): (0.05~20): (56~99.89).

[0047] A method for preparing the high-performance lithium battery current collector conductive slurry is characterized in that it comprises the following steps:

[0048] S1: Prepare materials: prepare modified conductive agent (modified multi-walled carbon nanotubes), nano conductive agent, modified nanofiber, dispersant, binder, and solvent respectively according to the proportions;

[0049] S2: Preparation of high-concentration modified conductive agent suspension: Weigh the modified nanofibers and dispersant in proportion and add them to 1 / 3 of the solvent. Dissolve them completely by mechanical stirring. Then weigh the desired modified agent into the mixed solution and ultrasonicate it for 30 minutes to obtain a modified conductive agent suspension, specifically a high-concentration modified multi-walled carbon nanotube suspension.

[0050] S3: magnetization: placing the modified multi-walled carbon nanotubes and nano-conductive agent dispersion in a strong external magnetic field for magnetization to further stimulate the magnetic anisotropy of the magnetically modified multi-walled carbon nanotubes and obtain a high-concentration magnetically modified multi-walled carbon nanotube suspension;

[0051] S4: Preliminary dispersion: Add a corresponding proportion of binder to the above-mentioned high-concentration magnetic modified multi-walled carbon nanotube suspension, and replenish the solvent to the required amount; use a high-speed vacuum disperser first and then a sand mill for preliminary dispersion; the shear speed during dispersion in the vacuum disperser is 10-25 m / s, the vacuum degree is not less than 0.085 MPa, and the vacuum dispersion time is 1-5 hours; the diameter of the sand mill beads in the sand mill is 0.2-2 mm, the proportion is 30-90%, the sand mill speed is 600-10000 r / min, and the sand mill time is 0.1-5 hours;

[0052] S5: Secondary dispersion: Use ultrasonic processing equipment to disperse again in the form of ultrasonic resonance, and apply alternating magnetic fields on both sides to further evenly disperse the modified multi-walled carbon nanotubes and nano-conductive agent particles and align them in the same direction under the induction of the magnetic field, thereby obtaining a conductive slurry with magnetic orientation.

[0053] A method for preparing the high-performance lithium battery current collector is characterized in that it comprises the following steps:

[0054] (A1) preparing a current collector metal foil and a dispersed conductive slurry, and setting up a coating device, an ultrasonic device, a constant magnetic field generating device, and a drying device;

[0055] (A2) applying the dispersed conductive paste on the surface of the metal foil to form a liquid colloidal coating having a viscosity of 200 to 1000 mPa·s at 25° C. and a thickness of 500 to 1200 nm on the surface;

[0056] (A3) continuously applying a constant magnetic field perpendicular to the surface of the metal foil to the liquid colloidal coating, so that the orientation-modified conductive agent in the coating is induced by the external magnetic field to align in an orderly manner, gradually straighten from its original coiled state, and form a parallel array, interwoven with the substrate;

[0057] (A4) Drying the coating to evaporate the solvent and volatiles, and continuously applying a constant magnetic field. As the viscosity of the coating rapidly increases, the modified conductive agent maintains its arrangement position and posture and quickly takes shape, and is arranged in parallel at an angle of 15-45 degrees in the thickness direction until the solidified components of the conductive paste of the coating are fixed on the surface of the metal foil to form a dense functional covering structure with a thickness of no more than 800 nm, that is, a three-dimensional network structure with enhanced fixing, electrical conductivity, thermal conductivity and high reset characteristics is formed on the surface of the metal foil.

[0058] Example 1

[0059] This embodiment is a specific application case. The metal foil substrate used in this embodiment is aluminum foil with a thickness of 10-15 μm.

[0060] The present invention provides a high-performance lithium battery current collector, which includes a metal aluminum foil and a functional coating; the functional coating is a functional covering structure with a thickness of 700 nm formed by coating a conductive slurry on both surfaces of the metal aluminum foil and drying; the functional coating has magnetic orientation;

[0061] In this embodiment, the modified conductive agent in the functional coating and the axes of each modified multi-walled carbon nanotube are arranged obliquely at a specific 45° angle with the surface of the metal aluminum foil along the thickness direction, and are interwoven with the matrix material such as the adhesive to form a three-dimensional network structure with enhanced fixation, electrical conductivity and thermal conductivity.

[0062] The magnetic modified conductive agent used in the present invention forms a parallel distributed array, which can make the carriers move along the direction of the modified conductive agent array, make the carrier propagation speed faster, and avoid the recombination of carriers during the transmission process. It has good directional conductivity and can quickly guide the carriers to the metal foil.

[0063] In this embodiment, the preparation of the modified conductive agent specifically includes the following steps:

[0064] (1) Oxidation of carbon nanotubes: 2 g of multi-walled carbon nanotubes and 200 mL of concentrated sulfuric acid and concentrated nitric acid [V (浓HNO3) :V (浓H2SO4)=1:3] The mixture was placed in a 500mL conical flask and ultrasonically treated for 2h to disperse the carbon nanotubes in the acid solution. The mixture was placed in a constant temperature magnetic stirrer and stirred at 55°C for 6h to oxidize the carbon nanotubes and cut into short tubes of 150 to 400 nm (the specific length in this embodiment is 150 to 300 nm). It was then diluted with deionized water, vacuum filtered with a 0.22μm filter membrane, and repeatedly washed and filtered with deionized water until the pH of the filtrate was close to 7. The black solid on the filter membrane was collected, dried in a vacuum drying oven at 60°C for 24h, and ground through a 200-mesh sieve to achieve the shortening, oxidation and purification of the single-layer carbon nanotubes; during the oxidation process, vacancy defects were formed between the internal grids of the short carbon nanotubes, which gave them local magnetic moments and endowed the multi-walled carbon nanotubes with weak magnetism;

[0065] (2) Amination of carbon nanotubes: Weigh 1g of oxidized carbon nanotubes and 6g of 1,6-hexanediamine in 30mL of acetone, ultrasonically treat for 1h, add 0.4g of condensing agent DCC (dicyclohexylcarbodiimide), mix well, and reflux at 70℃ for 32h. Ultrasonic wash away excess 1,3-hexanediamine, DCC, and reaction by-products with anhydrous ethanol, vacuum filter with a 0.22μm filter membrane and membrane filter, repeatedly wash with anhydrous ethanol, collect the black substance on the filter membrane, and then dry in a vacuum drying oven at 65℃ for 24h. Grind through a 200-mesh sieve to obtain amino-modified magnetic carbon nanotubes;

[0066] (3) Dumbbell-shaped structure: Weigh 0.5g of amino-modified magnetic carbon nanotubes and 0.7g of nano-conductive carbon black and add them to 30mL of acetone, perform ultrasonic dispersion for 1h, add condensation agent DCC, and reflux at 70℃ for 24h. Use anhydrous ethanol to ultrasonically wash away DCC and reaction by-products, vacuum filter with a 0.45μm filter membrane and membrane filter, wash repeatedly with anhydrous ethanol, collect the black substance on the filter membrane, and then dry it in a vacuum drying oven at 65℃ for 24h. Grind it through a 200-mesh sieve to separate the dumbbell-shaped structure-modified conductive agent with thick ends and thin middle.

[0067] The multi-walled carbon nanotubes used in the embodiment of the present invention have an inner diameter of no less than 5 nm, an outer diameter of no more than 20 nm, and a length before cutting of no more than 1200 nm.

[0068] The oxidation step in the embodiment of the present invention utilizes the oxidation effect of the mixed acid to break the unstable five-membered carbon ring and seven-membered carbon ring located at the location where the carbon nanotube is spirally twisted due to its large aspect ratio, and truncate to form short carbon nanotubes with open ends, thereby shortening the treated carbon nanotubes and opening the top ports. Continuous oxidation further oxidizes the C atoms at the ports to form carboxyl groups, thereby providing multiple contact sites at the ports for grafting reactions. At the same time, the truncated carbon nanotubes have vacancy defects formed by the oxidation and opening of local C-C bonds. The presence of the defects leads to the presence of magnetic moments near the defects, thereby giving the carbon nanotubes weak magnetism. At the same time, the high reactivity caused by defects or local high curvature in the structures of carbon nanoparticles, amorphous carbon and graphite fragments is utilized to oxidize impurities with concentrated acid, thereby selectively removing these impurities.

[0069] The diamine compound of the present invention can be one of the diamine compounds such as 1,6-hexanediamine, 1,4-butanediamine, and p-phenylenediamine. Its functional characteristics are that the amino group contained in it reacts with the carboxyl group at the end of the single-walled carbon nanotube to form an amide bond, leaving the other amino group exposed, thus completing the amino modification of the carbon nanotube. The grafted diamine stretches the adjacent and closely packed carbon nanotubes, increasing the gap between the carbon nanotubes. At the same time, the presence of the diamine steric hindrance weakens the hydrogen bonds formed between the multi-walled carbon nanotubes during the acidification process. Therefore, the dispersion of the carbon nanotubes after amination is improved, facilitating the subsequent grafting of nano-conductive particles containing a large number of carboxyl groups. In this embodiment 1, 1,6-hexanediamine is specifically used.

[0070] The condensing agent in the present embodiment can be one of dicyclohexylcarbodiimide (DCC), diisopropylcarbodiimide (DIC), or 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide (EDCI). Its functional characteristic is that it acts as a dehydrating agent to promote the reaction of amino and carboxyl groups to form an amide bond, thereby connecting them. In this embodiment, dicyclohexylcarbodiimide DCC is specifically used.

[0071] The inert solvent in the embodiment of the present invention can be acetone, xylene, etc. In this embodiment, acetone is specifically used.

[0072] The nano-conductive agent particles described herein can be made of carbon black or graphite oxide, with a particle size of 20 to 250 nm. The numerous carboxyl groups on their surfaces can react with the amino-modified carbon nanotubes to form amide bonds, linking them together. In Example 1, nano-conductive carbon black with an average particle size of 120 nm is used.

[0073] A conductive slurry for preparing the aforementioned high-performance lithium battery current collector is an aqueous slurry prepared by dispersing and mixing a modified conductive agent, modified nanofibers, a dispersant, a binder, and a solvent. The slurry has a solid content of 0.1-10%, a viscosity of 200-1000 mPa·s (25°C), and a pH of 8-10. Those skilled in the art can select the slurry according to specific needs. In this embodiment, the slurry has a solid content of 8.5%, a viscosity of 500 mPa·s (25°C), and a pH of 9.

[0074] The thickness of the functional coating after coating and before drying is about 800-1200 nm, which provides sufficient space for the modified conductive agent to untwist, straighten and align in an oriented manner; controlling the viscosity within a specific range is conducive to the modified conductive agent untwisting, straightening and oriented arrangement under the induction of a magnetic field, while preventing it from slipping and floating to the surface. As the volatile matter in the slurry evaporates, it is captured in the grid structure of the substrate and intertwined with the substrate to form a three-dimensional network structure.

[0075] The weight ratio of the raw material components of the conductive paste in Example 1 is: modified multi-walled carbon nanotubes, nano-conductive agent: modified nanofibers: dispersant: binder: solvent = 0.3:0.05:5:20:20:54.65.

[0076] In the embodiment of the present invention, the modified nanofiber can be one of cellulose nanofibers or chitin (ChNF) nanofibers modified by reactions such as carboxylation, sulfonation, phosphorylation, and quaternization, and is dispersed in a deionized water medium with a solid content of 0.1 to 3.0 wt%. The modified nanofiber is suitable for aqueous media, and its functional characteristics are to provide a three-dimensional porous network structure, and the negatively charged groups generate electrostatic repulsion between the fibers to form a stable colloid, so that the magnetic modified conductive agent is stably bound in its developed pores, playing an auxiliary dispersion role; at the same time, it is interwoven with carbon nanotubes in the functional coating to form a three-dimensional network structure, thereby improving the overall performance of the current collector. This embodiment 1 specifically uses carboxylated cellulose nanofibers.

[0077] In the present invention, the dispersant can be a mixture of one of polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA), or poly (N-vinyl acetamide) (PNVA) with a binder resin. The amount of the dispersant (including a single component or a multi-component mixture) used is generally 20 to 1000 times the weight of the dry carbon nanotube powder. The dispersant is suitable for use in aqueous media and is characterized by uniformly dispersing the conductive agent in the conductive paste system. In Example 1, polyvinyl pyrrolidone (PVP) is specifically used.

[0078] The binder in the embodiments of the present invention can be a resin resistant to lithium-ion battery electrolytes and high voltages. This resin is polyacrylic acid (PAA) and its salts with a relatively broad molecular weight distribution, isopropyl alcohol, or a modified acrylic resin or modified polyacrylonitrile (PAN) resin. This resin is dispersed in deionized water to a solid content of 5-30 wt%. This binder is suitable for use in aqueous media and is characterized by bonding the conductive paste between the current collector and the positive / negative electrode materials, while also improving the adhesion between the two. In Example 1, isopropyl alcohol is specifically used.

[0079] The solvent used in Example 1 of the present invention is deionized water;

[0080] A method for preparing the aforementioned high-performance lithium battery current collector conductive slurry comprises the following steps:

[0081] (1) Preparation of materials: Prepare modified conductive agent, modified nanocellulose, dispersant, binder, and solvent respectively according to the ratio; modified multi-walled carbon nanotubes, nanoconductive agent: modified nanofiber: dispersant: binder: solvent = 0.3:0.05:5:20:20:56.45;

[0082] (2) Preparation of high-concentration modified conductive agent suspension: Weigh the modified nanofibers and dispersant in proportion and add them to 1 / 3 of the solvent. Dissolve them completely by mechanical stirring. Then weigh the required modified conductive agent into the mixed solution and ultrasonicate it for 30 minutes to obtain a modified conductive agent suspension, specifically a high-concentration modified multi-walled carbon nanotube suspension.

[0083] (3) Magnetization: The modified conductive agent suspension is placed in a strong external magnetic field for magnetization, so that the vacancy defects of the carbon nanotube part in the modified conductive agent form an induced magnetic moment, thereby further stimulating the magnetic anisotropy of the magnetic modified conductive agent, and obtaining a high-concentration magnetic modified multi-walled carbon nanotube suspension;

[0084] (4) Preliminary dispersion: Add a corresponding proportion of binder to the above-mentioned high-concentration modified conductive agent suspension and replenish the solvent to the required amount. Use a high-speed vacuum disperser first and then a sand mill for preliminary dispersion; the shear speed of the vacuum disperser is 10~25m / s, the vacuum degree is not less than 0.085MPa, and the vacuum dispersion time is 1~5h; the diameter of the sand mill beads in the sand mill is 0.2~2mm, accounting for 30~90%, the sand mill speed is 600~10000r / min, and the sand mill time is 0.1~5h;

[0085] (5) Secondary dispersion: Ultrasonic treatment equipment is used to disperse the material again in an ultrasonic resonance manner, and an alternating magnetic field is applied on both sides to further uniformly disperse the magnetic modified conductive agent and orient it in the same direction under the induction of the magnetic field, thereby obtaining a conductive slurry with magnetic orientation. The ultrasonic treatment equipment is an ultrasonic generator placed in the liquid, and the ultrasonic frequency of each power unit is 20kHz~40kHz and the power is 1kW~3kW. The intensity of the magnetic field is 0.1~5T and the frequency is 40~60Hz.

[0086] In the steps (4) and (5), during the dispersion process, the pH value of the conductive paste is adjusted to 8-11 with ammonia water to maintain the stability of the paste.

[0087] In Example 1 of the present invention, the specific component ratio and some preparation steps of the conductive slurry are as follows: 20 g of 10% polyvinyl pyrrolidone (PVP K30) solution and 5 g of 1% carboxylated nanocellulose solution are added to 13 g of deionized water and mixed thoroughly; then 0.3 g of modified multi-walled carbon nanotubes and 0.05 g of nanoconductive agent are added to the mixed solution and ultrasonically treated for 30 minutes to obtain a magnetic modified conductive agent suspension; the magnetic modified conductive agent suspension is placed in a strong external magnetic field for magnetization; 20 g of isopropyl alcohol and 43.45 g of deionized water are added to the magnetized magnetic modified conductive agent suspension, and pre-dispersed for 30 minutes using a high-speed disperser (first with low speed stirring, then accelerated). After the slurry is basically stirred evenly, it is stirred at 2400 The slurry was vacuum dispersed at 3000 rpm for 120 minutes (the vacuum level must be greater than 0.08 MPa), followed by sand milling. The slurry was then ultrasonically dispersed again, and an alternating magnetic field was applied to both sides to obtain an oriented, water-based conductive slurry with a solids content of 2.1%. By adjusting the amounts of the magnetically modified conductive agent, modified nanocellulose, dispersant, and binder in the above formula, water-based conductive slurries with solids contents of 0.1-6% could also be produced.

[0088] A method for preparing the aforementioned high-performance lithium battery current collector comprises the following steps:

[0089] (1) Prepare the current collector metal foil and the dispersed conductive slurry respectively, and set up coating equipment, ultrasonic equipment, constant magnetic field generating equipment, and drying equipment;

[0090] (2) The dispersed conductive paste is coated on the surface of the current collector metal foil to form a liquid colloidal coating with a viscosity of 200-1000 mPa·s (25°C) and a thickness of 800-1000 nm on the surface; the thickness of the coating after coating and before drying is about 800-1200 nm, which provides sufficient space for the magnetic modified conductive agent to untwist and straighten under the induction of the magnetic field and to be oriented; the viscosity is controlled within a specific range to provide the necessary conditions for the magnetic field-induced orientation effect while preventing the modified conductive agent from sliding and floating to the surface. As the volatile matter in the paste evaporates, it is captured in the grid structure of the matrix and intertwined with the matrix to form a three-dimensional network structure;

[0091] (3) continuously applying a stable magnetic field perpendicular to the surface of the metal foil to the liquid colloidal coating, so that the magnetic orientation modified conductive agent in the coating generates an induced magnetic moment under the induction of the magnetic field, and forms a directional arrangement array under the induction of the magnetic field;

[0092] The specific steps of applying an external magnetic field to induce orientation are as follows: in the first 1 / 3 of the coating production line, an orientation magnetic field is applied at an angle of 45 degrees to the surface of the metal foil, and the magnetic field strength is 200mT~1000mT to complete the first orientation positioning of the magnetic modified conductive agent, so that the magnetic single-layer carbon nanotubes that were disrupted during coating are re-oriented; then in the last 2 / 3 of the coating production line, an orientation magnetic field is applied at an angle of 45-90 degrees to the surface of the metal foil, and the magnetic field strength is 500mT~1000mT to complete the second orientation positioning. As the viscosity of the coating continues to increase, the magnetic modified conductive agent eventually forms a specific 15-45° oblique array along the thickness direction in the coating and is fixed;

[0093] (4) Drying the coating to allow the solvent and volatiles to fully evaporate, continuously applying a constant magnetic field, and maintaining the arrangement position and posture and quickly shaping as the viscosity of the coating rapidly increases, until the solid content of the conductive paste component of the coating is fixed on the surface of the metal foil to form a dense functional covering structure with a thickness of no more than 800 nm, which includes forming a three-dimensional network structure layer with enhanced fixation, electrical conductivity, and thermal conductivity on the surface of the metal foil.

[0094] Said step (3) further comprises the following steps:

[0095] (31) In the first 1 / 3 of the coating production line, the temperature of the conductive paste or the coated coating is raised to 45-65°C for pre-drying to extend the coagulation time, thereby reducing the viscosity of the liquid colloidal coating and increasing the kinetic energy of the untwisting, straightening and directional arrangement of the single-layer carbon nanotubes.

[0096] The high-performance lithium battery current collector prepared in Example 1 was used in the manufacture of lithium-ion batteries and performance tests were performed. The electrodes were manufactured using the following parameters. The positive electrode sheet included a current collector and a positive electrode active material layer coated on the current collector. The current collector was the high-performance lithium battery current collector prepared in Example 1. The positive electrode active material layer was composed of the following raw materials in parts by weight: 93 parts of positive electrode material (LFP); 4 parts of positive electrode conductive agent (SP); and 3 parts of positive electrode binder (PVDF-5130).

[0097] The negative electrode sheet includes a current collector and a negative electrode active material layer coated on the current collector. The current collector is a bare copper foil. The negative electrode active material layer is composed of the following raw materials in parts by weight: 96 parts of negative electrode material (artificial graphite); 1 part of negative electrode conductive agent (SP); 1 part of negative electrode binder 1 (sodium carboxymethyl cellulose CMC); 2 parts of negative electrode binder 2 (styrene-butadiene rubber SBR).

[0098] An 18650 battery was assembled using the positive and negative electrode sheets, a 20 μm polypropylene (PP) separator, and a LiPF6 electrolyte. The measured electrode sheet performance and battery performance are shown in Tables 1 and 2.

[0099] Comparative Example 1

[0100] In Comparative Example 1, the positive electrode current collector was prepared using plain aluminum foil, and other preparation conditions were the same.

[0101] The high-performance lithium battery current collector prepared in Example 1 and the bare aluminum foil were directly used as the positive electrode current collector. The same lithium battery positive and negative electrode formula and process were used to prepare 18650 batteries, and the electrode performance and battery performance tests were carried out. The measured electrode performance and battery performance are shown in Table 1 and Table 2, respectively.

[0102] Table 1: Comparative test data of the high-performance lithium battery current collector of the present invention applied to positive electrode sheets

[0103] Table 2: Comparative test data of high performance lithium battery current collectors used in lithium ion batteries according to embodiments of the present invention

[0104] According to the test results, it is easy to conclude that the high-performance lithium battery current collector provided by the present invention is applied to the manufacture of lithium batteries, and all performances from the electrode to the battery are better than the scheme using plain foil as the current collector in Comparative Example 1; the electrode sheet resistance of the positive electrode prepared in Example 1 is only 1 / 3 of that of the pure plain foil current collector scheme in Comparative Example 1, but the peeling force is more than 4 times that of the pure plain foil current collector scheme; it is measured that the AC internal resistance of the battery in Example 1 is 42% lower than that of the plain foil; at room temperature, the lithium-ion battery prepared in this Example 1 has a capacity retention rate of up to 93% after 2000 cycles of 1C charge and 2C discharge, which is much higher than the 80% capacity retention rate of the plain foil current collector scheme in Comparative Example 1, and the battery cycle consistency is also significantly better than that of the pure plain foil current collector scheme.

[0105] Example 2

[0106] The high-performance lithium battery current collector, conductive slurry and preparation method thereof provided in this embodiment are basically the same as those in Example 1, except that:

[0107] A modified conductive agent for preparing the aforementioned high-performance battery current collector, wherein the modified conductive agent is formed by oxidizing and chemically modifying multi-walled carbon nanotubes and then connecting them with other larger nano-conductive agent particles to form a dumbbell-shaped bridge-island structure anchored at both ends, wherein this embodiment 2 uses 1,4-butanediamine as a modifier and diisopropylcarbodiimide (DIC) as a condensation agent.

[0108] A conductive slurry for preparing the aforementioned high-performance lithium battery current collector is an aqueous slurry prepared by dispersing and mixing a modified conductive agent, modified nanofibers, a dispersant, a binder, and a solvent. The slurry has a solid content of 4-6%, a viscosity of 300-1000 mPa·s (25°C), and a pH of 8-9.

[0109] In this embodiment 2, the weight ratio of the raw material components of the conductive paste is modified multi-walled carbon nanotubes, nano-conductive agent: modified nanofibers: dispersant: binder: solvent = 0.6:0.1:6:20:20:53.3;

[0110] In this Example 2, the modified nanocellulose is carboxylated chitin nanofiber, the binder is modified acrylic resin, and the dispersant is polyvinyl alcohol (PVA).

[0111] This embodiment 2 is coated on copper foil to produce a high-performance lithium battery current collector.

[0112] The preparation parameters for the lithium-ion battery negative electrode sheet used in the comparative test using the current collector prepared in Example 2 are as follows: The negative electrode sheet comprises a current collector and a negative electrode active material layer coated on the current collector. The current collector is the high-performance lithium battery current collector prepared in Example 2. The negative electrode active material layer is composed of the following raw materials in parts by weight: 96 parts negative electrode material (artificial graphite); 1 part negative electrode conductive agent (SP); 1 part negative electrode binder 1 (sodium carboxymethyl cellulose, CMC); and 2 parts negative electrode binder 2 (styrene-butadiene rubber, SBR). The sheet peel strength was tested using an electronic tensile tester, and the sheet resistance was tested using a dual-probe pressing method. The measured sheet performance is shown in Table 3.

[0113] Example 3

[0114] The high-performance lithium battery current collector, conductive slurry, and preparation method thereof provided in this embodiment are substantially the same as those in Examples 1 and 2, except that:

[0115] In a modified conductive agent for preparing the aforementioned high-performance battery current collector, Example 3 uses 1,6-hexanediamine as a modifier and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide (EDCI) as a condensation agent.

[0116] A conductive slurry for preparing the aforementioned high-performance lithium battery current collector is an aqueous slurry prepared by dispersing and mixing a modified conductive agent, modified nanofibers, a dispersant, a binder, and a solvent. The slurry has a solid content of 3-4%, a viscosity of 200-800 mPa·s (25°C), and a pH of 9-10.

[0117] In this embodiment 3, the weight ratio of the raw material components of the conductive paste is modified multi-walled carbon nanotubes, nano-conductive agent: modified nanofibers: dispersant: binder: solvent = 0.3:0.1:4:12:14:69.6;

[0118] In this Example 3, the modified nanocellulose is carboxylated chitin nanofiber, the binder is modified polyacrylonitrile (PAN), and the dispersant is poly (N-vinyl acetamide) (PNVA).

[0119] The present embodiment 3 is coated on copper foil to produce a high-performance lithium battery current collector.

[0120] The preparation parameters for the lithium-ion battery negative electrode sheet used in the comparative testing of the current collector prepared in Example 3 are as follows: the negative electrode sheet comprises a current collector and a negative electrode active material layer coated on the current collector. The current collector is the high-performance lithium battery current collector prepared in Example 2. The negative electrode active material layer is composed of the following raw materials in parts by weight: 97 parts negative electrode material (artificial graphite); 1 part negative electrode conductive agent (SP); 1 part negative electrode binder 1 (sodium carboxymethyl cellulose, CMC); and 1 part negative electrode binder 2 (styrene-butadiene rubber, SBR). The sheet peel strength was tested using an electronic tensile testing machine, and the sheet resistance was tested using a dual-probe pressing method. The measured sheet performance is shown in Appendix 3 (Comparative Test Data for the High-Performance Lithium Battery Current Collector of the Present Invention Applied to the Negative Electrode Sheet).

[0121] Comparative Example 2

[0122] The process parameters for preparing the negative electrode sheet for a lithium-ion battery were the same as those in Example 2, specifically, the negative electrode material (artificial graphite): conductive agent (SP): binder 1 (CMC): binder 2 (SBR) = 96:1:1:2. The difference was that plain copper foil was used as the current collector. The measured electrode sheet properties are shown in Table 3.

[0123] Comparative Example 3

[0124] The process parameters for preparing the negative electrode sheet for a lithium-ion battery were the same as those in Example 3, specifically, the negative electrode material (artificial graphite): conductive agent (SP): binder 1 (CMC): binder 2 (SBR) = 97:1:1:1. The difference was that plain copper foil was used as the current collector. The measured electrode sheet properties are shown in Table 3.

[0125] Table 3

[0126] According to the test results, it is easy to conclude that the negative electrode sheet prepared by using the high-performance lithium battery current collector of the present invention shows higher electrode sheet adhesion at the same amount of negative electrode binder, and the electrode sheet resistance is also lower than that of pure light foil. It can be seen that the high-performance lithium battery current collector of the present invention can appropriately reduce the proportion of binder in the positive / negative electrode slurry of the battery, further reduce the internal resistance, and is conducive to the improvement of the battery energy density.

[0127] In summary, the high-performance lithium battery current collector of the present invention uses a magnetic modified conductive agent to form a parallel distributed array in the functional coating, successfully constructing a three-dimensional network structure of the modified conductive agent interwoven with the flexible substrate, providing a connection layer with high strength, conductive efficiency and good flexibility, which can effectively increase the contact area between the rigid metal current collector and the conductive slurry, improve the adhesion of the coating, and effectively reduce the interface resistance between the current collector and the battery active material. At the same time, the interwoven network is used to buffer the volume changes and automatic reset during the charge and discharge process, thereby avoiding expansion and separation between the conductive slurry and the current collector, enhancing the long-term adhesion between the current collector metal foil substrate and the battery active material during repeated charge and discharge, improving the stability of the electrode, and avoiding cycle failure, thereby improving the specific capacity, cycle stability and rate performance of the electrode, and greatly improving the overall performance of the lithium battery.

[0128] In other embodiments of the present invention, the metal foil may also be copper foil, iron foil, or stainless steel foil as the metal substrate of the current collector. Furthermore, within the aforementioned component ratios and process conditions described in the present invention, those skilled in the art can select the desired specific components, ratios, processes, and operating conditions based on conventional techniques to achieve the technical effects described in the present invention. The embodiments of the present invention are not listed one by one.

[0129] The above are only preferred embodiments of the present invention, and are not intended to limit the scope of protection of the present invention. Any modifications, equivalent replacements, improvements, etc. made to the technical solutions of the present invention within the spirit and principles of the present invention shall be included in the scope of protection of the present invention.

Claims

1. A high-performance lithium battery current collector, comprising a metal foil and a functional coating, characterized in that: The functional coating is a functional layered covering structure with a thickness of no more than 800 nm formed by coating a conductive slurry on one or two surfaces of a metal foil after drying; the functional coating includes a plurality of strip-shaped modified conductive agents, which are magnetically oriented modified multi-walled carbon nanotubes; After the modified conductive agent is cured and formed, it is parallel to each other in the functional coating, and within the thickness of the coating, its axis is arranged obliquely at an angle of 15 to 45 degrees to the surface of the metal foil, and is interwoven with the modified nanofibers, binder, and modified conductive agent in the coating to form an oriented three-dimensional network connection structure with enhanced fixation, electrical and thermal conductivity, and uniform deformation and reset; The magnetically oriented modified multi-walled carbon nanotubes in the functional coating are modified multi-walled carbon nanotubes with a dumbbell-shaped structure, with an inner diameter of not less than 5nm, an outer diameter of not more than 20nm, and a length of not more than 1200nm. The modified multi-walled carbon nanotubes, after being oxidized and chemically modified, have a dumbbell-shaped fiber structure with thicker ends and thinner middle. After being oriented, the thicker lower ends are respectively connected to the metal foil surface and the upper ends are connected to each other. With the help of an adhesive, other nano-conductive agent particles of different sizes and modified nano-fibers are sandwiched between the thinner fiber parts in the middle, so that the parts are connected to each other to form a three-dimensional network bridge-island structure with anchors at both ends and oriented arrangement. The elastic three-dimensional network limits the deformation and displacement of the modified multi-walled carbon nanotubes and nano-conductive agent particles during the operation of the battery, so as to automatically adapt to and offset the internal volume changes and the deformation and displacement of the conductive particles during the charging and discharging of the lithium battery, and maintain the reliability of the functional coating for the connection between the metal foil surface and the active substance.

2. The high performance lithium battery current collector according to claim 1, characterized in that: The modified multi-walled carbon nanotubes are prepared by the following steps: (1) Oxidation of carbon nanotubes: Take an appropriate amount of multi-walled carbon nanotubes, place them in a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:3, and ultrasonically treat them for 2 hours to uniformly disperse the multi-walled carbon nanotubes in the acid solution to obtain a dispersion; place the dispersion in a constant temperature magnetic stirrer and stir it at 55°C for 6 hours to oxidize the carbon nanotubes and cut them into short tubes of 150 to 400 nm; then dilute them with deionized water, vacuum filter them with a 0.22 μm filter membrane and a membrane filter, and repeatedly wash and filter them with deionized water until the pH of the filtrate is close to 7; collect the black solid on the filter membrane, dry it in a vacuum drying oven at 60°C for 24 hours, and grind it through a 100-mesh sieve to obtain truncated and purified oxidized multi-walled carbon nanotubes; (2) Amination of carbon nanotubes: Add the oxidized multi-walled carbon nanotubes and excess diamine compounds to an inert solvent, ultrasonically treat for 1 hour, add a condensing agent, mix well, and reflux at 70°C for 32 hours; use anhydrous ethanol to ultrasonically wash away excess amine, dicyclohexylcarbodiimide (DCC) and reaction by-products, use a 0.22 μm filter membrane and a membrane filter to vacuum filter, repeatedly wash with anhydrous ethanol, collect the black substance on the filter membrane, and then dry it in a vacuum drying oven at 65°C for 24 hours, grind it through a 200-mesh sieve, and obtain amino-modified magnetic multi-walled carbon nanotubes; (3) Constructing a dumbbell-shaped structure: Add amino-modified magnetic multi-walled carbon nanotubes and nano-conductive agent particles to an inert solvent, ultrasonically disperse for 1 hour, add a condensing agent, and reflux at 70°C for 24 hours; use anhydrous ethanol to ultrasonically wash away excess condensing agent and reaction by-products, use a 0.45 μm filter membrane and a membrane filter to vacuum filter, repeatedly wash with anhydrous ethanol, collect the black substance on the filter membrane, and then dry it in a vacuum drying oven at 65°C for 24 hours, grind it through a 200-mesh sieve to obtain modified multi-walled carbon nanotubes with thick ends and a thin middle and a dumbbell-shaped structure.

3. The high performance lithium battery current collector according to claim 2, characterized in that: The carbon nanotube oxidation step (1) utilizes the oxidation effect of the mixed acid to break the unstable five-membered carbon ring and seven-membered carbon ring located at the position where the carbon nanotube is spirally twisted due to its large aspect ratio, and cuts off to form short carbon nanotubes with open ends, thereby shortening the treated carbon nanotubes and opening the top ports. The oxidation is continued to oxidize the C atoms at the ports to form carboxyl groups, thereby providing multiple contact sites at the ports for grafting reactions. At the same time, the truncated carbon nanotubes have vacancy defects formed by the oxidation of local CC bonds, and the presence of the defects leads to the presence of magnetic moments near the defects, thereby giving the carbon nanotubes weak magnetism.

4. The high performance lithium battery current collector according to claim 2, characterized in that: The nano-conductive agent particles in the step (3) of constructing the dumbbell-shaped structure are carbon black or graphite oxide, and have a particle size of 20 to 250 nm. A large number of carboxyl groups on the surface of the nano-conductive agent particles react with the amino-modified carbon nanotubes to form amide bonds and stably connect them together, forming thicker anchoring sites at both ends of the modified multi-walled carbon nanotubes.

5. The high performance lithium battery current collector according to claim 2, characterized in that: The diamine compound in step (2) is one of 1,6-hexanediamine, 1,4-butanediamine, and p-phenylenediamine, and the amino group contained in the diamine compound reacts with the carboxyl group at the end of the carbon nanotube to form an amide bond, and the other amino group is exposed to the outside, thereby completing the amino modification of the carbon nanotube; and the grafted diamine stretches the adjacent and closely connected carbon nanotubes to increase the gap between the carbon nanotubes. At the same time, the presence of the steric hindrance of the diamine weakens the hydrogen bonds formed between the multi-walled carbon nanotubes during the acidification process, thereby improving the dispersibility of the carbon nanotubes after amination, which is conducive to the subsequent grafting of nano-conductive agent particles containing a large number of carboxyl groups; The condensation agent in step (2) is dicyclohexylcarbodiimide (DCC), which acts as a dehydrating agent to promote the reaction of amino groups and carboxyl groups to form amide bonds and stably connect them together; The inert solvent in step (3) is one of acetone and xylene.

6. A conductive slurry for preparing the high-performance lithium battery current collector according to any one of claims 1 to 5, characterized in that: The conductive slurry is an aqueous slurry prepared by dispersing and mixing modified multi-walled carbon nanotubes, nano conductive agents, modified nano fibers, dispersants, binders and solvents, and the slurry has a solid content of 0.1-5%, a viscosity of 200-1000 mPa·s and a pH of 8-11. The weight ratio of the raw material components of the conductive paste is modified multi-walled carbon nanotubes, nano conductive agent: modified nanofiber: dispersant: binder: solvent = (0.01~1.8): (0.01~0.2): (0.02~2): (0.02~20): (0.05~20): (56~99.89).

7. The conductive slurry for high-performance lithium battery current collector according to claim 6, characterized in that: The modified nanofiber is one of cellulose nanofiber and chitin ChNF nanofiber modified by carboxylation, sulfonation, phosphorylation and quaternary ammonium salt reaction, which is dispersed in a deionized water medium with a solid content of 0.1-3.0wt%. The modified nanofiber is suitable for aqueous medium, provides a three-dimensional porous network structure, and the negatively charged groups generate electrostatic repulsion between the fibers to form a stable colloid, so that the modified conductive agent is stably bound in its developed pores; at the same time, it is interwoven with the modified conductive agent in the functional coating to form a three-dimensional network structure, thereby improving the comprehensive performance of the current collector; The dispersant is one of polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA) or poly N-vinyl acetamide (PNVA), and the amount of the dispersant is 20 to 1000 times the weight of the modified conductive agent dry powder. The dispersant is suitable for use in an aqueous medium to make the modified conductive agent evenly dispersed in the conductive slurry system; The binder is a resin that is resistant to lithium-ion battery electrolyte and high voltage. The resin is polyacrylic acid (PAA) and its salt with a relatively wide molecular weight distribution, or a modified acrylic resin, or a modified polyacrylonitrile (PAN) resin or a mixture thereof. The binder is dispersed in a deionized water medium with a solid content of 5 to 30 wt%. The binder is suitable for use in an aqueous medium to bond the conductive slurry between the current collector body and the positive / negative electrode material, while improving the fixation ability between the two. The solvent is deionized water.

8. A method for preparing the high-performance lithium battery current collector conductive slurry according to claim 6 or 7, characterized in that: It includes the following steps: S1: preparing materials: preparing modified multi-walled carbon nanotubes, nano-conductive agent, modified nanofibers, dispersant, binder, and solvent respectively according to proportions; S2: Preparation of high-concentration modified conductive agent suspension: Weigh the modified nanofibers and dispersant in proportion and add them to 1 / 3 of the solvent, stir them mechanically to completely dissolve them, then weigh the required modified conductive agent, add it to the mixed solution and treat it ultrasonically for 30 minutes to obtain a modified conductive agent suspension, specifically a high-concentration modified multi-walled carbon nanotube suspension; S3: magnetization: placing the modified conductive agent suspension in a strong external magnetic field for magnetization to further stimulate the magnetic anisotropy of the magnetically modified multi-walled carbon nanotubes to obtain a high-concentration magnetically modified multi-walled carbon nanotube suspension; S4: Preliminary dispersion: add a corresponding proportion of binder to the above-mentioned high-concentration magnetic modified multi-walled carbon nanotube suspension, and supplement the solvent to the required amount; use a high-speed vacuum disperser first and then a sand mill for preliminary dispersion; the shear speed of the vacuum disperser is 10~25m / s during dispersion, the vacuum degree is not less than 0.085MPa, and the vacuum dispersion time is 1~5h; the diameter of the sand mill beads in the sand mill is 0.2~2mm, accounting for 30~90%, the sand mill speed is 600~10000r / min, and the sand mill time is 0.1~5h; S5: Secondary dispersion: Use ultrasonic processing equipment to disperse again in an ultrasonic resonance manner, and apply an alternating magnetic field on both sides to further evenly disperse the modified multi-walled carbon nanotubes and nano-conductive agent particles and align them in the same direction under the induction of the magnetic field, so as to obtain a conductive slurry with magnetic orientation.

9. The method according to claim 8, characterized in that In the steps S2 and S5, the ultrasonic processing equipment is an ultrasonic generator placed in the liquid, and the ultrasonic frequency of each power unit is 20kHz~40 kHz and the power is 1kW~3kW; in the steps S3 and S5, the intensity of the alternating magnetic field is 0.1~5T and the frequency is 40~60Hz.

10. A method for preparing a high-performance lithium battery current collector according to any one of claims 1 to 5, characterized in that: It includes the following steps: (A1) preparing a current collector metal foil and a dispersed conductive slurry respectively, and setting up a coating device, an ultrasonic device, a constant magnetic field generating device, and a drying device; (A2) applying the dispersed conductive paste on the surface of the metal foil to form a liquid colloidal coating having a viscosity of 200 to 1000 mPa·s at 25° C. and a thickness of 500 to 1200 nm on the surface; (A3) continuously applying a constant magnetic field perpendicular to the surface of the metal foil to the liquid colloidal coating, so that the orientation-modified conductive agent in the coating is orderly arranged under the induction of the external magnetic field, gradually straightened from the original coiled state, and arranged in a parallel array, and intertwined with the substrate; (A4) Drying the coating to evaporate the solvent and volatiles, and continuously applying a constant magnetic field. As the viscosity of the coating increases rapidly, the modified conductive agent maintains its arrangement position and posture and quickly takes shape, and is arranged in parallel at an angle of 15-45 degrees in the thickness direction until the solidified components of the conductive paste of the coating are fixed on the surface of the metal foil to form a dense functional covering structure with a thickness of no more than 800 nm, that is, a three-dimensional network structure with enhanced fixation, electrical conductivity, thermal conductivity and high reset characteristics is formed on the surface of the metal foil.

11. The preparation method according to claim 10, characterized in that: The step (A3) further comprises the following steps: (A3-1) The temperature of the conductive paste or the applied coating is raised to 45-65°C for pre-drying to prolong the coagulation time and thereby reduce the viscosity of the liquid colloidal coating and increase the kinetic energy of the modified conductive agent to untwist, straighten and orientate; and / or ultrasonic waves are simultaneously applied to the liquid colloidal coating to further increase the kinetic energy of the modified conductive agent to untwist, straighten and orientate, accelerate the formation of a parallel array of the modified conductive agent, and increase the density of the three-dimensional connection structure formed between the modified conductive agent and the substrate, thereby forming a three-dimensional network structure on the surface of the metal foil with enhanced fixation, electrical conductivity, thermal conductivity, limited deformation and automatic reset.

Citation Information

Patent Citations

  • Battery electrode, preparation method of battery electrode and battery

    CN108630945A

  • Current collector for secondary battery, conductive paste and preparation method thereof

    CN110783572A

  • Ultralow-temperature high-rate lithium ion battery and preparation method thereof

    CN113793939A

  • High-performance lithium battery current collector, conductive slurry and preparation method thereof

    CN116259929A

  • Binder for electrode of lithium battery and lithium battery containing the binder

    US20130177807A1

Cited By

  • Modified current collector and preparation method and application thereof

    CN119208619A

  • Lithium manganese iron phosphate positive electrode material and preparation method thereof

    CN119361660A

  • Pole piece, secondary battery and electronic device

    CN120690810A

  • Purification method of carbon nanotubes

    CN121449057A