ABS rubber powder and preparation method therefor, ABS material and vehicle interior trim part

By preparing ABS powder with high loss modulus, the noise problem in the vehicle is solved by using its damping performance, achieving a lasting anti-noise effect.

WO2024230014A1PCT designated stage expired Publication Date: 2024-11-14KINGFA SCI & TECH CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/115598
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2023-08-29
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The noise in the vehicle mainly comes from the extrusion of the combined components in the vehicle and the friction between the components. The existing methods cannot achieve a lasting anti-noise effect.

Method used

A ABS rubber powder is used, which includes a continuous phase and a dispersed phase, the continuous phase is an acrylonitrile-styrene copolymer, and the dispersed phase is polybutadiene, the polybutadiene is composed of a first butadiene rubber and a second butadiene The ene rubber is composed of olefin rubber, prepared by emulsion graft copolymerization reaction, to form ABS powder with high loss modulus, thereby improving damping performance.

Benefits of technology

It achieves good noise reduction performance of ABS powder, can achieve long-lasting anti-noise effect, improves the damping performance of the material, and reduces noise.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023115598-APPB-I100001
    Figure PCTCN2023115598-APPB-I100001
  • Figure PCTCN2023115598-APPB-I100002
    Figure PCTCN2023115598-APPB-I100002
  • Figure PCTCN2023115598-APPB-I100003
    Figure PCTCN2023115598-APPB-I100003
Patent Text Reader

Abstract

An ABS rubber powder and a preparation method therefor, an ABS material and a vehicle interior trim part. The ABS rubber powder comprises a continuous phase and a dispersed phase dispersed in the continuous phase, wherein the continuous phase comprises an acrylonitrile-styrene copolymer, and the dispersed phase comprises polybutadiene, the polybutadiene comprising a first butadiene rubber and a second butadiene rubber. The average particle size of the first butadiene rubber is 250-350 nm, and the average particle size of the second butadiene rubber is 800-2000 nm; and the weight ratio of the first butadiene rubber to the second butadiene rubber is (40-50): (3-7). The ABS rubber powder has relatively good damping performance and a good long-acting anti-noise effect.
Need to check novelty before this filing date? Find Prior Art

Description

ABS rubber powder and preparation method thereof, ABS material and vehicle interior parts Technical Field

[0001] The present invention relates to the technical field of engineering plastics, in particular to ABS rubber powder and a preparation method thereof, ABS material and vehicle interior decoration parts. Background Art

[0002] In recent years, the automotive industry has paid increasing attention to in-vehicle noise. This noise primarily originates from the compression and friction between interlocking components within the vehicle. High in-vehicle noise can directly impact the physical and mental health of drivers and passengers, and can even affect driving safety.

[0003] In order to improve the noise problem, the usual method is to apply grease or felt on the extrusion surface or friction surface of the component to prevent direct contact between the components, so as to achieve the purpose of reducing noise, but this method cannot achieve a lasting anti-noise effect.

[0004] Summary of the Invention

[0005] Based on this, the present invention provides an ABS rubber powder and a preparation method thereof, an ABS material and a vehicle interior trim.

[0006] The first aspect of the present invention provides an ABS rubber powder, and its technical solution is as follows:

[0007] An ABS rubber powder, comprising a continuous phase and a dispersed phase dispersed in the continuous phase;

[0008] The continuous phase comprises acrylonitrile-styrene copolymer, and the dispersed phase comprises polybutadiene;

[0009] The polybutadiene includes a first butadiene rubber and a second butadiene rubber;

[0010] The average particle size of the first butadiene rubber is 250 nm to 350 nm, and the average particle size of the second butadiene rubber is 800 nm to 2000 nm;

[0011] The weight ratio of the first butadiene rubber to the second butadiene rubber is (40-50):(3-7).

[0012] In some embodiments, one or more of the following conditions are met:

[0013] 1) The second butadiene rubber is selected from butadiene rubber, styrene butadiene rubber or a combination thereof.

[0014] 2) The polybutadiene accounts for 49 wt% to 70 wt% of the ABS rubber powder;

[0015] 3) The acrylonitrile-styrene copolymer accounts for 30wt% to 51wt% of the ABS rubber powder, and the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(50-400).

[0016] The second aspect of the present invention provides a method for preparing ABS rubber powder, and its technical solution is as follows:

[0017] Mixing a first butadiene latex and a second butadiene latex to prepare a seed latex, wherein the first butadiene latex includes a first butadiene rubber, the average particle size of the first butadiene rubber is 250 nm to 350 nm, the second butadiene latex includes a second butadiene rubber, the average particle size of the second butadiene rubber is 800 nm to 2000 nm, and in the seed latex, the weight ratio of the first butadiene rubber to the second butadiene rubber is (40 to 50):(3 to 7);

[0018] The seed latex, acrylonitrile monomer and styrene monomer are mixed, and an emulsion graft copolymerization reaction is carried out under the action of a chain transfer agent, an initiator, an emulsifier, a reducing agent and a solvent to obtain a grafted latex. The grafted latex is flocculated, and the solid is collected and then dried.

[0019] In some embodiments, the solid content of the first butadiene latex is 50 wt % to 65 wt %; and / or the solid content of the second butadiene latex is 15 wt % to 25 wt %.

[0020] In some embodiments, the second butadiene rubber is selected from butadiene rubber, styrene butadiene rubber, or a combination thereof.

[0021] In some embodiments, the second butadiene latex further includes a solvent, and the solvent is styrene monomer.

[0022] In some embodiments, the first butadiene latex is prepared by emulsion polymerization of butadiene monomer.

[0023] In some embodiments, one or more of the following conditions are met:

[0024] 1) controlling the weight of the seed latex so that the proportion of the polybutadiene in the ABS rubber powder is 49 wt% to 70 wt%;

[0025] 2) controlling the weight of the acrylonitrile monomer and the styrene monomer so that the proportion of the acrylonitrile-styrene copolymer in the ABS rubber powder is 30 wt% to 51 wt%, and the polymerized monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(50-400).

[0026] In some embodiments, the emulsion graft copolymerization reaction satisfies one or more of the following conditions:

[0027] 1) The chain transfer agent used in the emulsion graft copolymerization reaction is one or more selected from tert-dodecyl mercaptan, n-dodecyl mercaptan, tetradecyl mercaptan, tridecyl mercaptan, undecyl mercaptan and decanyl mercaptan;

[0028] 2) The initiator used in the emulsion graft copolymerization reaction is selected from one or more of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile;

[0029] 3) the emulsifier used in the emulsion graft copolymerization reaction is selected from one or more of naphthalenesulfonic acid formaldehyde condensate sodium salt, naphthalenesulfonic acid formaldehyde condensate potassium salt, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzenesulfonate and sodium dodecylsulfonate;

[0030] 4) the reducing agent used in the emulsion graft copolymerization reaction is selected from one or more of sodium edetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite;

[0031] 5) The solvent used in the emulsion graft copolymerization reaction is water;

[0032] 6) The flocculant used in the flocculation treatment is one or more selected from magnesium sulfate, sulfuric acid and calcium chloride.

[0033] A third aspect of the present invention provides an ABS material, comprising the above-mentioned ABS rubber powder or the ABS rubber powder prepared by the above-mentioned preparation method, and SAN resin.

[0034] In some embodiments, the weight ratio of the ABS rubber powder to the SAN resin is (15-35): (65-85).

[0035] A fourth aspect of the present invention provides a vehicle interior trim component, the components of which include the above-mentioned ABS rubber powder or the ABS rubber powder prepared by the above-mentioned preparation method or the above-mentioned ABS material.

[0036] Compared with the traditional solution, the present invention has the following beneficial effects:

[0037] The dispersed phase of the ABS rubber powder of the present invention includes polybutadiene, which includes a first butadiene rubber and a second butadiene rubber. The first butadiene rubber has an average particle size of 250 nm to 350 nm, and the second butadiene rubber has an average particle size of 800 nm to 2000 nm. The weight ratio of the first butadiene rubber to the second butadiene rubber is controlled to be (40-50):(3-7). In the presence of the small-particle first butadiene rubber and the large-particle second butadiene rubber, a dispersed phase with cavities can be formed, thereby increasing the loss modulus and dissipation factor of the synthesized ABS rubber powder, thereby facilitating noise reduction. The ABS rubber powder of the present invention has good damping properties, thereby providing excellent noise reduction performance and achieving a long-lasting noise reduction effect. DETAILED DESCRIPTION

[0038] The present invention will be further described in detail below with reference to specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to provide a more thorough and comprehensive understanding of the present disclosure.

[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0040] the term

[0041] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0042] In the present invention, "plurality", "multiple", "multiple times", "multiple", etc., unless otherwise specified, refer to a number greater than or equal to 2. For example, "one or more" means one or more than or equal to two.

[0043] In the present invention, “preferred”, “better”, “more preferred” and “suitable” are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of the present invention.

[0044] In the present invention, the terms “further”, “further”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present invention.

[0045] In this disclosure, the terms "optionally," "optional," and "optional" are optional and refer to either option, i.e., to the selection of either option from the two parallel options of "optional" or "optional." If multiple "optional" terms appear in a technical solution, each "optional" term is independent unless otherwise specified and there are no conflicts or constraints.

[0046] In the present invention, in the "first aspect," "second aspect," "third aspect," "fourth aspect," etc., the terms "first," "second," "third," "fourth," etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or quantity, nor as implicitly indicating the importance or quantity of the technical features indicated. Furthermore, "first," "second," "third," "fourth," etc. serve only as non-exhaustive enumeration and description and should be understood not to constitute a closed-ended limitation on quantity.

[0047] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0048] In the present invention, when referring to a numerical interval (i.e., a numerical range), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval and includes the two numerical endpoints of the numerical range (i.e., the minimum value and the maximum value), as well as each numerical value between the two numerical endpoints. Unless otherwise specified, when a numerical interval refers only to integers within the numerical interval, it includes the two endpoint integers of the numerical range, as well as each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1 to 10, indicating that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be merged. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all subranges included therein.

[0049] The temperature parameters in the present invention, unless otherwise specified, may be either constant temperature or fluctuating within a certain temperature range. It should be understood that the constant temperature treatment allows for temperature fluctuations within the precision range of the instrument control. Fluctuations within ranges such as ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are permitted.

[0050] In the present invention, when referring to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the percentage of the added component in the system after the addition of the component.

[0051] In the present invention, wt% represents weight percentage, and wt‰ represents weight thousandth.

[0052] In the present invention, normal temperature refers to 20 to 30°C.

[0053] In the present invention, the first butadiene rubber and the second butadiene rubber in the ABS rubber powder can be characterized and observed by SEM.

[0054] In the present invention, the average particle size of the first butadiene rubber in the first butadiene latex, the average particle size of the second butadiene rubber in the second butadiene latex, and the weight ratio of the first butadiene rubber to the second butadiene rubber are tested according to the following method:

[0055] The first butadiene latex and the second butadiene latex were dissolved in acetone and then ultrasonically dispersed. The particle size analysis dynamic light scattering (DLS) method according to GB / T 29022-2012 was used to measure the particle size.

[0056] Increasing the damping of materials is a way to reduce noise. Compared with applying grease or felt on the extrusion and friction surfaces of components to prevent direct contact between components for noise reduction, increasing the damping of the materials used in the components can achieve a more lasting anti-noise effect.

[0057] An embodiment of the present invention provides an ABS rubber powder, which improves the anti-noise effect of the ABS rubber powder from the perspective of improving the damping of the ABS rubber powder. The ABS rubber powder includes a continuous phase and a dispersed phase dispersed in the continuous phase;

[0058] The continuous phase comprises acrylonitrile-styrene copolymer, and the dispersed phase comprises polybutadiene;

[0059] The polybutadiene includes a first butadiene rubber and a second butadiene rubber;

[0060] The average particle size of the first butadiene rubber is 250 nm to 350 nm, and the average particle size of the second butadiene rubber is 800 nm to 2000 nm;

[0061] The weight ratio of the first butadiene rubber to the second butadiene rubber is (40-50):(3-7).

[0062] The damping of a material is generally measured by the loss tangent (tanδ) (also known as the loss factor or damping factor), which represents the ratio of the material's loss modulus to its storage modulus. Because polymers possess both viscous and elastic properties, when an external force acts on a polymer material, some energy is stored (the storage modulus), resulting in the material exhibiting elastic recovery. Another portion of energy is dissipated due to viscous heat generation (the loss modulus), and this energy cannot be recovered. Therefore, the damping performance of a material primarily stems from the internal friction of the polymer. A larger loss factor indicates that more mechanical energy is converted into heat and dissipated, resulting in better vibration and noise reduction.

[0063] The dispersed phase in the ABS rubber powder comprises polybutadiene, which comprises a first butadiene rubber and a second butadiene rubber. The first butadiene rubber has an average particle size of 250 nm to 350 nm, and the second butadiene rubber has an average particle size of 800 nm to 2000 nm. The weight ratio of the first butadiene rubber to the second butadiene rubber is controlled to be (40-50):(3-7). The presence of the small-particle first butadiene rubber and the large-particle second butadiene rubber increases the loss modulus and dissipation factor of the synthesized ABS rubber powder, thereby increasing the noise generated by the ABS rubber powder. The ABS rubber powder of the present invention inherently has good damping properties, thereby providing excellent noise reduction performance and achieving a long-lasting noise reduction effect.

[0064] It can be understood that the average particle size of the first butadiene rubber includes but is not limited to: 250 nm, 280 nm, 300 nm, 330 nm, and 350 nm.

[0065] It can be understood that the average particle size of the second butadiene rubber includes but is not limited to: 800 nm, 900 nm, 1000 nm, 1100 nm, 1200 nm, 1300 nm, 1400 nm, 1500 nm, 1600 nm, 1700 nm, 1800 nm, and 2000 nm.

[0066] It can be understood that the weight ratio of the first butadiene rubber to the second butadiene rubber includes but is not limited to 40:4, 44:4, 47:4, 40:5, 44:5, 47:5, 40:6, 44:6, and 47:6.

[0067] Optionally, the second butadiene rubber is selected from butadiene rubber, styrene butadiene rubber or a combination thereof. Preferably, the second butadiene rubber is butadiene rubber.

[0068] Optionally, the ABS rubber powder can be ABS high-rubber powder or ABS low-rubber powder. Preferably, the ABS rubber powder is ABS high-rubber powder, and the content of polybutadiene is 49wt% to 70wt%.

[0069] Optionally, the content of acrylonitrile-styrene copolymer in the ABS rubber powder is 30 wt% to 51 wt%, and the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(50-400).

[0070] One embodiment of the present invention further provides a method for preparing ABS rubber powder, which improves the anti-noise effect of the ABS rubber powder from the perspective of increasing the damping of the ABS rubber powder, and comprises the following steps:

[0071] Mixing a first butadiene latex and a second butadiene latex to prepare a seed latex, wherein the first butadiene latex includes a first butadiene rubber, the average particle size of the first butadiene rubber is 250 nm to 350 nm, the second butadiene latex includes a second butadiene rubber, the average particle size of the second butadiene rubber is 800 nm to 2000 nm, and the weight ratio of the first butadiene rubber to the second butadiene rubber is (40 to 50):(3 to 7);

[0072] The seed latex, acrylonitrile monomer and styrene monomer are mixed, and an emulsion graft copolymerization reaction is carried out under the action of a chain transfer agent, an initiator, an emulsifier, a reducing agent and a solvent to obtain a grafted latex. The grafted latex is flocculated, and the solid is collected and then dried.

[0073] In this embodiment, a first butadiene latex and a second butadiene latex are used as seed latexes, wherein the first butadiene latex includes a first butadiene rubber having an average particle size of 250 nm to 350 nm, and the second butadiene latex includes a second butadiene rubber having an average particle size of 800 nm to 2000 nm. The weight ratio of the first butadiene rubber to the second butadiene rubber is controlled to be (40 to 50):(3 to 7). The presence of the first butadiene rubber with a small particle size and the second butadiene rubber with a large particle size is conducive to the formation of a dispersed phase with voids during the subsequent graft copolymerization process, thereby increasing the loss modulus of the synthesized ABS rubber powder, thereby increasing the loss factor of the ABS rubber powder, and thus facilitating the reduction of noise of the ABS rubber powder.

[0074] It can be understood that the weight ratio of the first butadiene rubber to the second butadiene rubber includes but is not limited to 40:4, 44:4, 47:4, 40:5, 44:5, 47:5, 40:6, 44:6, and 47:6.

[0075] Optionally, the solid content of the first butadiene latex is 50 wt% to 65 wt%.

[0076] Optionally, the solid content of the second butadiene latex is 15 wt% to 25 wt%.

[0077] In this embodiment, the first butadiene latex provides a latex system environment. Optionally, the first butadiene latex can be prepared by emulsion polymerization of butadiene monomers. However, the particle size of the first butadiene latex prepared by emulsion polymerization of butadiene monomers is generally small. In this embodiment, the average particle size of the first butadiene rubber is 250 nm to 350 nm. It is understood that the average particle size of the first butadiene rubber includes, but is not limited to, 250 nm, 280 nm, 300 nm, 330 nm, and 350 nm.

[0078] Optionally, in the presence of an electrolyte, an initiator, an emulsifier and a chain transfer agent, butadiene monomer undergoes an emulsion polymerization reaction to obtain a first butadiene latex.

[0079] Optionally, the reaction time of the emulsion polymerization reaction is 20 hours to 40 hours, and the reaction temperature is 51° C. to 93° C.

[0080] In some examples, the method for preparing the first butadiene latex comprises the following steps:

[0081] The butadiene monomer, electrolyte, initiator, emulsifier and chain transfer agent are mixed, and the temperature of the obtained mixed system is raised from 51° C. to 61° C. to 83° C. to 93° C. within 20 h to 40 h.

[0082] Optionally, the initiator used in the emulsion polymerization is one or more selected from the group consisting of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile.

[0083] Optionally, the initiator accounts for 0.2 wt% to 1.5 wt% of the butadiene monomer.

[0084] Optionally, the electrolyte used in the emulsion polymerization is one or more selected from sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate, and potassium hydroxide.

[0085] Optionally, the electrolyte accounts for 2 wt% to 15 wt% of the butadiene monomer.

[0086] Optionally, the emulsifier used in the emulsion polymerization is one or more selected from the group consisting of sodium salt of naphthalenesulfonic acid formaldehyde condensate, potassium salt of naphthalenesulfonic acid formaldehyde condensate, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzenesulfonate and sodium dodecylsulfonate.

[0087] Optionally, the emulsifier accounts for 2 wt% to 15 wt% of the butadiene monomer.

[0088] Optionally, the chain transfer agent used in the emulsion polymerization is one or more selected from tert-dodecyl mercaptan, n-dodecyl mercaptan, tetradecyl mercaptan, tridecyl mercaptan, undecyl mercaptan and decanyl mercaptan.

[0089] Optionally, the chain transfer agent accounts for 0.5 wt% to 5 wt% of the butadiene monomer.

[0090] To increase the damping of the ABS rubber powder, this embodiment introduces a second butadiene rubber with a larger particle size by adding a second butadiene latex to the latex system provided by the first butadiene latex. In this embodiment, the average particle size of the second butadiene rubber is 800 nm to 2000 nm. It is understood that the average particle size of the second butadiene rubber includes, but is not limited to, 800 nm, 900 nm, 1000 nm, 1100 nm, 1200 nm, 1300 nm, 1400 nm, 1500 nm, 1600 nm, 1700 nm, 1800 nm, and 2000 nm.

[0091] Optionally, the second butadiene rubber is selected from butadiene rubber, styrene butadiene rubber or a combination thereof. Preferably, the second butadiene rubber is butadiene rubber.

[0092] Optionally, the second butadiene latex further comprises a solvent, and the solvent is styrene monomer.

[0093] In this embodiment, after the seed latex is obtained, the seed latex, acrylonitrile monomer and styrene monomer undergo emulsion graft copolymerization in the presence of a reducing agent, an emulsifier, an initiator, a chain transfer agent and a solvent to obtain a grafted latex.

[0094] Optionally, the reaction time of the emulsion graft copolymerization reaction is 5 hours to 9 hours, and the reaction temperature is 10° C. to 72° C.

[0095] In some examples, the method for preparing the grafted latex comprises the following steps:

[0096] The seed latex and the reducing agent are mixed, and the resulting mixed system is heated to 62° C. to 72° C., and acrylonitrile monomer, styrene monomer, emulsifier, initiator, chain transfer agent and solvent are added. After keeping the temperature for 1 to 3 hours, the mixture is naturally cooled and reacted for 4 to 6 hours.

[0097] Optionally, the weight of the seed latex is controlled so that the proportion of the polybutadiene in the ABS rubber powder is 49 wt % to 70 wt %.

[0098] Optionally, the weight of the acrylonitrile monomer and the styrene monomer is controlled so that the proportion of the acrylonitrile-styrene copolymer in the ABS rubber powder is 30wt% to 51wt%, and the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(50-400).

[0099] Optionally, the chain transfer agent used in the emulsion graft copolymerization reaction is one or more selected from tert-dodecyl mercaptan, n-dodecyl mercaptan, tetradecyl mercaptan, tridecyl mercaptan, undecyl mercaptan and decanyl mercaptan.

[0100] The chain transfer agent accounts for 0.2 wt‰ to 10 wt‰ of the seed latex.

[0101] Optionally, the initiator used in the emulsion graft copolymerization reaction is one or more selected from the group consisting of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile.

[0102] Optionally, the initiator accounts for 1 wt‰ to 10 wt‰ of the seed latex.

[0103] Optionally, the emulsifier used in the emulsion graft copolymerization reaction is one or more selected from the group consisting of sodium salt of naphthalenesulfonic acid formaldehyde condensate, potassium salt of naphthalenesulfonic acid formaldehyde condensate, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzenesulfonate and sodium dodecylsulfonate.

[0104] Optionally, the emulsifier accounts for 2 wt‰ to 20 wt‰ of the seed latex.

[0105] Optionally, the reducing agent used in the emulsion graft copolymerization reaction is selected from one or more of sodium ethylenediaminetetraacetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite.

[0106] Optionally, the reducing agent accounts for 0.01 wt‰ to 0.05 wt‰ of the seed latex.

[0107] Optionally, the solvent used in the emulsion graft copolymerization reaction is water.

[0108] In this embodiment, a flocculant is added to the grafted latex to perform flocculation treatment to prepare a flocculated slurry.

[0109] Optionally, the flocculation treatment time is 2 hours to 6 hours, and the reaction temperature is 70°C to 100°C.

[0110] Optionally, the flocculant used in the flocculation treatment is selected from one or more of magnesium sulfate, sulfuric acid and calcium chloride.

[0111] Optionally, the weight ratio of the grafted latex to the flocculant is 1000:(40-50).

[0112] It can be understood that the flocculant is added to the graft latex in the form of an aqueous flocculant solution.

[0113] In some examples, the method for preparing the flocculated slurry comprises the following steps:

[0114] The grafted latex is heated to 70-80° C., and a flocculant aqueous solution is added. The flocculant aqueous solution is added within 1-3 hours, and then the temperature is raised to 90-100° C. and kept warm for 1-3 hours.

[0115] Optionally, the concentration of the flocculant in the flocculant aqueous solution is 0.5 wt% to 5 wt%.

[0116] In this embodiment, the method further includes adding a washing liquid to the flocculated slurry for washing.

[0117] Optionally, the washing liquid is water.

[0118] In this embodiment, after washing, the solid can be collected by centrifugation, filtration, etc., and the solid can be dried to obtain ABS rubber powder.

[0119] The above preparation method requires less modification to the original emulsion production line, has less impact on the production cycle and energy consumption, is conducive to continuous large-scale production, has low preparation cost, and high production efficiency.

[0120] Optionally, the product prepared by the above preparation method is ABS rubber powder, which can be ABS high-rubber powder or ABS low-rubber powder. Preferably, the prepared ABS rubber powder is ABS high-rubber powder, and the polybutadiene content is 49wt% to 70wt%.

[0121] One embodiment of the present application further provides an ABS material, comprising the above-mentioned ABS rubber powder or the ABS rubber powder prepared by the above-mentioned preparation method, and SAN resin.

[0122] By blending ABS rubber powder with SAN resin, the content of acrylonitrile, butadiene and styrene can be flexibly adjusted, leaving a large room for modification.

[0123] Optionally, the weight ratio of ABS rubber powder to SAN resin can be adjusted according to actual use requirements. In some embodiments, the weight ratio of ABS rubber powder to SAN resin is (15-35): (65-85).

[0124] It is understood that the ABS material can be prepared by extruding and pelletizing a powder containing ABS rubber powder and SAN resin. Optionally, the extrusion temperature is 180°C to 210°C, the screw speed is 200 rpm to 300 rpm, and the screw aspect ratio is (35-45):1.

[0125] One embodiment of the present invention provides a vehicle interior trim component, the components of which include the aforementioned ABS rubber powder or the ABS rubber powder prepared by the aforementioned preparation method or the aforementioned ABS material.

[0126] The following is further described in conjunction with specific examples and comparative examples. The raw materials involved in the following specific examples and comparative examples, unless otherwise specified, can all be sourced from commercial sources. The instruments used, unless otherwise specified, can all be sourced from commercial sources. The processes involved, unless otherwise specified, are all routinely selected by those skilled in the art. The number of parts involved in the following examples and comparative examples, unless otherwise specified, are all parts by weight. The particle sizes involved in the following examples and comparative examples, unless otherwise specified, are all average particle sizes.

[0127] [Corrected 19 / 09 / 2023 according to Rule 26] Among them, the butadiene monomer is industrial-grade butadiene with a purity greater than 96%, sourced from Huarui Chemical; butadiene rubber 35AE and 55AE are sourced from Asahi Kasei Corporation of Japan; butadiene rubber 50AF and 30AF are sourced from Dushanzi Petrochemical Company; butadiene rubber 565T and 8497 are sourced from Lanxess of Germany. Styrene monomer is sourced from Aladdin Reagents with a purity greater than or equal to 99%; acrylonitrile monomer is sourced from Aladdin Reagents with a purity greater than or equal to 99%; tert-dodecyl mercaptan (TDM) is a chain transfer agent; and SAN resin is a styrene-acrylonitrile copolymer, brand PN-128, sourced from Chi Mei of Taiwan, China.

[0128] Example 1

[0129] This embodiment provides an ABS rubber powder, an ABS material, and a preparation method thereof, and the steps are as follows:

[0130] Step 1: Preparation of the first butadiene latex

[0131] 100 parts of butadiene monomer, 0.5 parts of sodium persulfate (initiator), 5 parts of sodium carbonate (electrolyte), 5 parts of potassium disproportionate rosinate (emulsifier) ​​and 2 parts of tert-dodecyl mercaptan (chain transfer agent) were mixed, the temperature was raised to 56° C. to start emulsion polymerization reaction, and the temperature was continuously raised to 88° C. within 30 hours. The reaction was completed after 30 hours to obtain a first butadiene latex with a particle size of 310 nm and a solid content of 58 wt%.

[0132] Step 2: Preparation of the second butadiene latex

[0133] Butadiene rubber 35AE was mixed with styrene monomer in a weight ratio of 20:80, and stirred at room temperature for 24 hours to obtain a second butadiene latex with a particle size of 1000 nm and a solid content of 20 wt%.

[0134] Step 3: Prepare seed latex

[0135] The first butadiene latex and the second butadiene latex are mixed in a weight ratio of 80:20 to obtain a seed latex.

[0136] Step 4: Prepare ABS material

[0137] 1000 parts of seed latex were added to a reactor, 0.015 parts of ferrous sulfate were added to the reactor and stirred evenly, the reactor was heated to 67°C, and 2.51 parts of cumene hydroperoxide, 100 parts of acrylonitrile monomer, 140 parts of styrene monomer, 1.5 parts of TDM, 5 parts of potassium disproportionate rosinate and 175 parts of deionized water were added, and the mixture was kept warm for 2 hours, and then naturally cooled and reacted for 5 hours to obtain a grafted latex.

[0138] Take 1000 parts of grafted latex and add it to the flocculation reactor, start stirring and heat to 75°C, gradually add 450 parts of 10wt% magnesium sulfate aqueous solution, add it over 2 hours, and heat to 95°C and maintain the temperature for 2 hours. Filter the product with a 325-mesh filter to obtain a flocculation slurry.

[0139] The flocculated slurry was washed with deionized water at a flow rate of 2 tons / h and 1 ton / h. The mixed solution was dehydrated in a centrifuge and then dried in a fluidized bed at 60°C for 6 hours to obtain ABS rubber powder 1 with a moisture content of <1 wt%.

[0140] 25 parts of the above-mentioned ABS rubber powder 1 and 75 parts of SAN resin were mixed, extruded through a twin-screw extruder, cooled, and pelletized to obtain ABS material 1, wherein the extrusion temperature was 200°C, the screw speed was 250 r / min, and the screw aspect ratio was 40:1.

[0141] Example 2

[0142] This embodiment provides an ABS rubber powder, an ABS material, and a preparation method thereof. These methods are substantially the same as those of Example 1, with the primary differences being that, in step 3, the first butadiene latex and the second butadiene latex are mixed in a weight ratio of 70:30 to obtain a seed latex; and in step 4, 1080 parts of the seed latex are added to a reactor, along with 40.8 parts of styrene monomer. This embodiment produces ABS rubber powder 2 and ABS material 2.

[0143] Example 3

[0144] This example provides an ABS rubber powder, an ABS material, and a preparation method thereof. These methods are substantially the same as those in Example 1, with the primary difference being that, in step 2, butadiene rubber 35AE is replaced with butadiene rubber 55AE, yielding a second butadiene latex having a particle size of 2000 nm and a solids content of 20 wt%. This example produces ABS rubber powder 3 and ABS material 3.

[0145] Example 4

[0146] This embodiment provides an ABS rubber powder, an ABS material, and a preparation method thereof. These methods are substantially the same as those of Example 3, with the primary differences being that, in step 3, the first butadiene latex and the second butadiene latex are mixed in a weight ratio of 70:30 to obtain a seed latex. In step 4, 1080 parts of the seed latex are added to a reactor, along with 40.8 parts of styrene monomer. This embodiment produces ABS rubber powder 4 and ABS material 4.

[0147] Example 5

[0148] This example provides an ABS rubber powder, an ABS material, and a preparation method thereof. These methods are substantially the same as those in Example 1, with the primary difference being that, in step 2, cis-1,4-butadiene rubber 35AE is replaced with cis-1,4-butadiene rubber 50AF, yielding a second butadiene latex having a particle size of 1500 nm and a solids content of 20 wt%. This example yields ABS rubber powder 5 and ABS material 5.

[0149] Example 6

[0150] This example provides an ABS rubber powder, an ABS material, and a preparation method thereof. These methods are substantially the same as those in Example 1, with the primary difference being that, in step 2, cis-1,4-butadiene rubber 35AE is replaced with cis-1,4-butadiene rubber 565T, yielding a second butadiene latex having a particle size of 800 nm and a solids content of 20 wt%. This example produces ABS rubber powder 6 and ABS material 6.

[0151] Example 7

[0152] This embodiment provides an ABS rubber powder, an ABS material, and a preparation method thereof. These methods are substantially the same as those of Example 1, with the primary difference being that in step 4, the seed latex is adjusted from 1000 parts to 1100 parts, the acrylonitrile monomer is adjusted from 100 parts to 150 parts, and the styrene monomer is adjusted from 140 parts to 50 parts. This embodiment produces ABS rubber powder 7 and ABS material 7.

[0153] Example 8

[0154] This embodiment provides an ABS rubber powder, an ABS material, and a preparation method thereof. These methods are essentially the same as those in Example 1, with the primary difference being that in step 4, the seed latex is adjusted from 1000 parts to 900 parts, the acrylonitrile monomer is adjusted from 100 parts to 50 parts, and the styrene monomer is adjusted from 140 parts to 200 parts. 20 parts of the aforementioned ABS rubber powder 1 and 80 parts of SAN resin are mixed, extruded through a twin-screw extruder, cooled, and pelletized. This embodiment produces ABS rubber powder 8 and ABS material 8.

[0155] Example 9

[0156] This embodiment provides an ABS rubber powder, an ABS material, and a preparation method thereof. These methods are substantially the same as those of Example 1, with the primary differences being that, in step 3, a first butadiene latex and a second butadiene latex are mixed in a weight ratio of 75:25 to obtain a seed latex; and in step 4, 1040 parts of the seed latex are added to a reactor, along with 92 parts of styrene monomer. This embodiment produces ABS rubber powder 9 and ABS material 9.

[0157] Comparative Example 1

[0158] This comparative example provides an ABS rubber powder, an ABS material, and a preparation method thereof, which are substantially the same as those in Example 1, except that in step 2, cis-1,4-butadiene rubber 35AE is replaced with cis-1,4-butadiene rubber 30AF, resulting in a second butadiene latex having a particle size of 500 nm and a solid content of 20 wt%. This comparative example produces ABS rubber powder 10 and ABS material 10.

[0159] Comparative Example 2

[0160] This comparative example provides an ABS rubber powder, an ABS material, and a preparation method thereof, which are basically the same as those in Example 1, except that no second butadiene latex is added. The steps are as follows:

[0161] Step 1: Prepare ABS material

[0162] 869 parts of the first butadiene latex prepared in step 1 of Example 1 were added to a reactor, 0.015 parts of ferrous sulfate was added to the reactor and stirred evenly, the reactor was heated to 67° C., and 2.51 parts of cumene hydroperoxide, 100 parts of acrylonitrile monomer, 300 parts of styrene monomer, 1.5 parts of TDM, 5 parts of potassium disproportionate rosinate, and 175 parts of deionized water were added dropwise continuously for 2 hours. After heating was completed, the reaction was continued for 5 hours to obtain a grafted latex.

[0163] Take 1000 parts of grafted latex and add it to the flocculation reactor, start stirring and heat to 75°C, gradually add 450 parts of 10wt% magnesium sulfate aqueous solution, add it over 2 hours, and heat to 95°C and maintain the temperature for 2 hours. Filter the product with a 325-mesh filter to obtain a flocculation slurry.

[0164] The flocculated slurry was washed with deionized water at a flow rate of 2 tons / h and 1 ton / h. The mixed solution was dehydrated in a centrifuge and then dried in a fluidized bed at 60°C for 6 hours to obtain ABS rubber powder 11 with a moisture content of less than 1 wt%.

[0165] 25 parts of the above-mentioned ABS rubber powder 8 and 75 parts of SAN resin were mixed, extruded through a twin-screw extruder, cooled, and pelletized to obtain ABS material 11, wherein the extrusion temperature was 200°C, the screw speed was 250 r / min, and the screw aspect ratio was 40:1.

[0166] Comparative Example 3

[0167] This comparative example provides an ABS rubber powder, an ABS material, and a preparation method thereof. These methods are substantially the same as those in Example 1, with the primary difference being that cis-1,4-butadiene rubber 35AE is replaced with cis-1,4-butadiene rubber 8497, resulting in a second butadiene latex having a particle size of 3000 nm and a solids content of 20 wt%. This comparative example yielded ABS rubber powder 12 and ABS material 12.

[0168] The ABS materials of the above embodiments and comparative examples were subjected to performance tests. The test items and methods are as follows. The test results are shown in Tables 1 and 2.

[0169] Tensile strength refers to ISO 527-2012 50mm / min;

[0170] Bending strength refers to ISO 178-2010 2mm / min;

[0171] Charpy notched impact strength refers to ISO 179-2010 23℃;

[0172] The loss factor tanδ (damping factor) is tested according to the free vibration attenuation method;

[0173] The noise risk factor (RPN) is tested according to the German automotive industry standard VDA 230-206-2005, with a force of 40N and a speed of 1mm / s. A risk factor of 1-3 indicates low noise risk, a risk factor of 4-6 indicates medium noise risk, and a risk factor of 7-10 indicates high noise risk.

[0174] Table 1

[0175] Table 2

[0176] As shown in Tables 1 and 2, in Examples 1-9, ABS rubber powder and, in turn, ABS materials were prepared using the first and second butadiene latexes as seed latexes. The particle size of the second butadiene rubber ranged from 800 nm to 2000 nm. Within this particle size range, the ABS materials achieved a relatively low RPN value of 1-3 and a relatively high loss factor (tan δ) of 0.021-0.033, which facilitated noise reduction in the ABS materials. Furthermore, the ABS materials maintained relatively good mechanical properties, such as tensile strength and flexural strength. In conjunction with Examples 1, 3, 5, 7, 8, and 9, when the particle size of the second butadiene rubber ranged from 1500 nm to 2000 nm, the RPN value was 1-2 and the loss factor (tan δ) was 0.027-0.028, achieving even better noise reduction. In combination with Examples 1, 2, and 9 or in combination with Examples 3 and 4, adjusting the ratio of the first butadiene rubber to the second butadiene rubber is also beneficial to enhancing the noise reduction effect of the ABS material. The smaller the weight ratio of the first butadiene rubber to the second butadiene rubber, the better the noise reduction effect.

[0177] Comparative Example 1 added a second butadiene rubber with a particle size of 500 nm, Comparative Example 2 did not add a second butadiene, and Comparative Example 3 added a second butadiene with a particle size of 3000 nm. The noise reduction effects were all inferior to that of Example 1.

[0178] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0179] The above-described embodiments merely illustrate several implementations of the present invention, and while their descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art would be able to make numerous variations and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be determined by the appended claims.

Claims

1. An ABS rubber powder, It is characterized in that The ABS rubber powder comprises a continuous phase and a dispersed phase dispersed in the continuous phase; The continuous phase comprises acrylonitrile-styrene copolymer, and the dispersed phase comprises polybutadiene; The polybutadiene includes a first butadiene rubber and a second butadiene rubber; The average particle size of the first butadiene rubber is 250nm to 350nm, and the average particle size of the second butadiene rubber is 800nm ​​to 2000nm; The weight ratio of the first butadiene rubber to the second butadiene rubber is (40-50):(3-7).

2. The ABS rubber powder according to claim 1, It is characterized in that One or more of the following conditions are met: 1) the second butadiene rubber is selected from butadiene rubber, styrene butadiene rubber or a combination thereof; 2) The polybutadiene accounts for 49wt% to 70wt% of the ABS rubber powder; 3) The acrylonitrile-styrene copolymer accounts for 30wt% to 51wt% of the ABS rubber powder, and the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50 to 150): (50 to 400).

3. A method for preparing ABS rubber powder, It is characterized in that The following steps are involved: Mixing a first butadiene latex and a second butadiene latex to prepare a seed latex, wherein the first butadiene latex includes a first butadiene rubber, the average particle size of the first butadiene rubber is 250nm-350nm, the second butadiene latex includes a second butadiene rubber, the average particle size of the second butadiene rubber is 800nm-2000nm, and in the seed latex, the weight ratio of the first butadiene rubber to the second butadiene rubber is (40-50):(3-7); The seed latex, acrylonitrile monomer and styrene monomer are mixed, and an emulsion graft copolymerization reaction is carried out under the action of a chain transfer agent, an initiator, an emulsifier, a reducing agent and a solvent to obtain a grafted latex, and the grafted latex is flocculated and the solid is collected and then dried.

4. The method for preparing ABS rubber powder according to claim 3, It is characterized in that The solid content of the first butadiene latex is 50 wt% to 65 wt%; and / or the solid content of the second butadiene latex is 15 wt% to 25 wt%.

5. The method for preparing ABS rubber powder according to claim 3, It is characterized in that The second butadiene rubber is selected from butadiene rubber, styrene butadiene rubber or a combination thereof.

6. The method for preparing ABS rubber powder according to claim 5, It is characterized in that The second butadiene latex further includes a solvent, and the solvent is a styrene monomer.

7. The method for preparing ABS rubber powder according to claim 3, It is characterized in that The first butadiene latex is prepared by emulsion polymerization of butadiene monomer.

8. A method for preparing ABS rubber powder according to any one of claims 3 to 7, It is characterized in that One or more of the following conditions are met: 1) controlling the weight of the seed latex so that the proportion of the polybutadiene in the ABS rubber powder is 49wt% to 70wt%; 2) The weight of the acrylonitrile monomer and the styrene monomer is controlled so that the proportion of the acrylonitrile-styrene copolymer in the ABS rubber powder is 30wt% to 51wt%, and the polymerized monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(50-400).

9. The method for preparing the ABS rubber powder according to any one of claims 3 to 7, It is characterized in that The emulsion graft copolymerization reaction satisfies one or more of the following conditions: 1) The chain transfer agent used in the emulsion graft copolymerization reaction is selected from one or more of tert-dodecyl mercaptan, n-dodecyl mercaptan, tetradecyl mercaptan, tridecyl mercaptan, undecyl mercaptan and decanyl mercaptan; 2) The initiator used in the emulsion graft copolymerization reaction is selected from one or more of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile; 3) the emulsifier used in the emulsion graft copolymerization reaction is selected from one or more of naphthalenesulfonic acid formaldehyde condensate sodium salt, naphthalenesulfonic acid formaldehyde condensate potassium salt, potassium oleate, potassium stearate, disproportionated potassium rosin acid, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate; 4) The reducing agent used in the emulsion graft copolymerization reaction is selected from one or more of sodium ethylenediaminetetraacetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite; 5) The solvent used in the emulsion graft copolymerization reaction is water; 6) The flocculant used in the flocculation treatment is one or more selected from magnesium sulfate, sulfuric acid and calcium chloride.

10. The ABS material according to claim 1, It is characterized in that The ABS material comprises the ABS rubber powder according to any one of claims 1 to 2 or the ABS rubber powder prepared by the preparation method according to any one of claims 3 to 9, and SAN resin.

11. The ABS material according to claim 10, It is characterized in that The weight ratio of the ABS rubber powder to the SAN resin is (15-35):(65-85).

12. A vehicle interior component, It is characterized in that Its components include the ABS rubber powder described in any one of claims 1-2, or the ABS rubber powder prepared by the preparation method described in any one of claims 3-9, or the ABS material described in any one of claims 10-11.

Citation Information

Patent Citations

  • Method for preparing acrylonitrile butadiene-styrene (ABS) resin through double peak emulsion grafting

    CN102199253A

  • Modified double-peak ABS resin preparation method

    CN103923430A

  • Rubber-modified styrene resin composition and molded article formed by same

    CN106496919A

  • Method for preparing ABS toughened resin by adopting emulsion grafting method based on controllable double-particle-size distribution latex

    CN111117096A

  • ABS (Acrylonitrile Butadiene Styrene) rubber powder and preparation method thereof, ABS material and vehicle interior trim part

    CN116554410A