Preparation method for large-dimension lithium niobate crystal
By selecting suitable seed crystal axial direction, mixing raw materials and controlling the growth process, the temperature field regulation and inheritance defects in the growth of large-sized lithium niobate crystals are solved, the high quality and stability of the crystal are achieved, and the production efficiency is improved Consistent with application.
Patent Information
- Application Number
- PCT/CN2023/117596
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-06
- Filing Date
- 2023-09-08
- Publication Date
- 2024-11-14
AI Technical Summary
The prior art has difficulty in controlling the temperature field of the growth interface, many inheritance defects, large crystal thermal stress, and high lithium ions volatilize at high temperatures, resulting in many intrinsic defects and unstable Curie temperature, affecting the crystal. Quality and application areas.
Reduce the stress at the bottom of the crystal by selecting the appropriate seed crystal axial direction, mixing raw materials to control Curie temperature, using preheating and finishing processes to stabilize the convection of the molten liquid, and using a heat field sub-heater and insulation layer to uniformize the temperature during in-situ annealing, reducing the stress at the bottom of the crystal and risk of cracking.
It reduces the risk of crystal defects and cracking, improves the stability of Curie temperature, ensures high-quality growth and application consistency of crystals, and reduces production costs and efficiency.
Smart Images

Figure PCTCN2023117596-FTAPPB-I100001 
Figure PCTCN2023117596-FTAPPB-I100002 
Figure PCTCN2023117596-FTAPPB-I200001
Abstract
Description
A method for preparing large-size lithium niobate crystals Technical Field
[0001] The present invention relates to the field of piezoelectric crystals, and specifically relates to a method for preparing large-sized lithium niobate crystals. Background Art
[0002] In recent years, the widespread use of high-frequency and multi-band communications in wireless communications, particularly mobile phones, has significantly increased demand for surface acoustic wave (SAW) filters, leading to higher quality requirements. With the continuous advancement of SAW technology, the application areas of SAW devices have continued to expand, including applications in mobile phones, multimedia data broadcasting systems (such as VOD), automotive electronics, wireless LAN, and digital television, increasing market demand for SAW devices. Furthermore, the miniaturization of communications equipment requires increasingly precise manufacturing of individual components, which in turn drives the miniaturization of SAW filters.
[0003] The existing lithium niobate products in China are mainly 4 inches. For the growth of large-sized (6-inch, 8-inch, 10-inch) lithium niobate single crystals, there are problems such as difficulty in controlling the temperature field of the growth interface, many inherited defects, and large thermal stress in the crystal, which can easily lead to crystal cracking. At the same time, large-sized lithium niobate crystals have a higher marginal temperature, which makes lithium ions easily volatilize at high temperatures, resulting in a large number of intrinsic defects in the lithium niobate crystals, and the crystal Curie temperature is unstable and has poor consistency, which seriously affects the quality of the crystal and limits its application in many fields. The invention patent with publication number CN113529170A discloses a method for growing ultra-large-sized lithium niobate single crystals. Small-sized crystals are prepared by the pulling method. After the growth of the small-sized crystals is completed, a thin neck is pulled, and then the shoulder expansion, equal diameter and tailing stages are entered to complete the growth of the ultra-large-sized lithium niobate single crystals, thereby solving the problem of unfavorable central heat convection. This patent uses small-sized crystals to grow large-sized crystals, which easily leads to the extension of crystal intrinsic defects. Invention patent publication number CN111206282A discloses a method for producing 8-inch lithium niobate crystals. The method uses a multi-layer temperature field to ensure uniform temperature without sudden changes, thus avoiding polycrystalline and cracking of the crystals. Multiple mixing and firing are performed when preparing polycrystalline raw materials to ensure a stable Curie temperature of the crystals. This patent does not describe the regulation of the Curie temperature during continuous growth. Invention patent publication number CN105525355B discloses an in-situ annealing process for large-sized sapphire crystals. After the sapphire crystals are grown, the crystals remain in place, and staged heat preservation annealing is used to reduce the dislocation sealing of the large-sized sapphires and eliminate the stress within the crystals to the greatest extent possible. This patent does not adjust the heat field insulation structure during in-situ annealing.
[0004] Summary of the Invention
[0005] The object of the present invention is to provide a method for preparing large-sized lithium niobate crystals.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing large-sized lithium niobate crystals comprises the following steps:
[0008] a) Seed crystal processing: A seed crystal is selected based on the axial direction of the lithium niobate crystal to be grown. After orienting the seed crystal, it is cut into a rectangular block and illuminated on all six sides. At the same time, vein defects in the seed crystal block are marked under a spotlight. When cutting the rectangular block into seed crystals, the seed crystal seeding surface is made to avoid vein defects;
[0009] b) Mixing raw materials: Determine whether there is residual bottom material from the previous growth furnace in the crystal growth furnace. If there is no residual bottom material, mix the raw materials according to the mass ratio of niobium oxide to lithium carbonate of 1000:261-263; If there is residual bottom material, measure the Curie temperature a and mass A of the residual bottom material in the crucible, and preliminarily determine the mass B of the added raw materials and the Curie temperature target value b according to the mass ratio of niobium oxide to lithium carbonate of 1000:261-263. The estimated Curie temperature of the grown crystal is c, where If the estimated value c is lower than the target value b, then lithium carbonate needs to be added with a mass fraction Bθ(bc), where θ is 0.8‰ to 1‰; if the estimated value c is higher than the target value b, then niobium oxide needs to be added with a mass fraction Bγ(bc), where γ is 1% to 1.5%, ultimately making the estimated value equal to the target value to obtain the optimal Curie temperature;
[0010] c) Crystal growth: The prepared raw materials are placed in a platinum crucible, which is then placed in a hot field. The temperature is increased to melt the lithium niobate raw materials to form a melt, which is then preheated. After preheating, a seed crystal is lowered into contact with the melt. The seed crystal is necked and then kept warm, allowing the crystal to grow automatically.
[0011] d) Crystal finishing: When the crystal reaches the target length, adjust the temperature and rotation speed to finish the crystal growth, and then pull the crystal out of the liquid surface at a pulling rate of 30-60mm / min;
[0012] e) Crystal annealing: After the crystal leaves the liquid surface, the temperature gradient inside the thermal field is controlled at 5-10°C / dm, and the temperature is kept at 1200-1250°C for 10-12 hours to complete the crystal annealing, and then cooled to room temperature at 30-50°C / h.
[0013] In step a), a suitable seed crystal is selected according to the axial direction of the lithium niobate crystal to be grown. Since lithium niobate crystals have a high degree of intrinsic defects and are inherited, a biased crystal is generally used to process the seed crystal growth according to the axial direction of the crystal to be grown. For example, if a Y-oriented lithium niobate crystal is grown, an X- or Z-oriented seed crystal is selected; if a Z-oriented lithium niobate crystal is grown, an X- or Y-oriented seed crystal is selected; and if an X-oriented lithium niobate crystal is grown, a Y- or Z-oriented seed crystal is selected. Since vein defects are inherent defects of lithium niobate crystals, using a crystal with vein defects for seeding will inevitably increase the probability of crystal twinning and cause crystal cracking. Therefore, after the seed crystal is oriented, it is cut into a rectangular seed crystal block and inspected with six-sided illumination. The vein defects of the seed crystal block are marked under a spotlight to ensure that the seed crystal seeding surface does not involve vein defects when it is subsequently cut into seed crystals.
[0014] In step b), it is determined whether there is residual bottom material from the previous crystal growth process in the crystal growth furnace. If there is no residual bottom material in the furnace, the raw materials can be directly mixed at a mass ratio of 1000:261-263 between niobium oxide and lithium carbonate and then crystal growth can be directly carried out, so that the Curie temperature of the grown lithium niobate crystals is controlled within the target value of 1141-1143°C. If there is residual bottom material from the previous crystal growth process in the crystal growth furnace, and this residual bottom material produces perion volatilization in a high temperature environment, if the raw materials are still mixed at a mass ratio of 1000:261-263 between niobium oxide and lithium carbonate and then crystal growth is carried out, the crystal quality will be affected, resulting in a difference in the Curie temperature of the subsequently grown crystals, or even deviation from the target value. In this patent, the influence of the residual bottom material in the crystal growth furnace on the next crystal growth furnace is taken into account, the Curie temperature and quality of the residual bottom material in the crystal growth furnace are measured, and the raw materials are further adjusted based on the calculated Curie temperature estimate, so that the Curie temperature of the lithium niobate crystal is controlled between the target 1141 and 1143°C, and continuous crystal growth is achieved while ensuring the quality of crystal growth.
[0015] In step c), the heating rate is controlled at 100-200° C. / h, and the lithium niobate raw material is heated to 1200-1400° C. to melt to form a melt. The temperature is detected and regulated using an infrared thermometer, and the melt is preheated. After preheating, the seed crystal is lowered into contact with the melt at a rate of 8-10 mm / min, and the seed crystal is necked to 2-3 mm. The temperature is kept for 1-2 hours. At this time, the seed crystal necking is completed and automatic growth begins. The rotation speed in the crystal growth stage is controlled at 4-8 rpm, and the pulling speed is controlled at 0.5-1 mm / h.
[0016] In step c), the preheating time of the raw material melt is 90-100 minutes, and the preheating temperature is 1350-1380°C. In order to better convect the raw materials and improve the seeding quality, a preheating process is introduced. At the same time, too high a preheating temperature will cause the Curie temperature to drop, so the time needs to be controlled;
[0017] In step d), the growth parameters are adjusted before the crystal is cut, wherein the temperature is increased by 10-20° C., the rotation speed is increased by 1-2 rpm, and the temperature is kept for 10-15 minutes for finishing, which can reduce the bottom convexity of the crystal and reduce the stress at the bottom of the crystal;
[0018] Among them, in step e), after the crystal growth is completed, according to the conventional in-situ annealing in the furnace, due to the large thermal field gradient used during crystal growth, the uniformity of the thermal field at the crystal location is difficult to control within 2-3°C. This patent adds a secondary heater on the upper part of the thermal field and uses a thermocouple to monitor the temperature of the position where the crystal is located after cutting in real time. At the same time, according to the monitoring results, a thermal insulation layer is added to the upper part of the thermal field to reduce the temperature difference and ensure the uniformity of the thermal field temperature.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) During the seed crystal processing process, by selecting the seed crystal processing axis and controlling the seed crystal processing vein defects, the generation of intrinsic inherited defects during the growth of large-sized lithium niobate crystals is reduced, and crystal defects and cracking are reduced;
[0021] (2) This process takes into account the influence of the residual bottom material after the actual crystal growth is completed on the growth of the next batch of crystals in the crystal growth furnace. Therefore, by adjusting the filler ratio, the stability of the Curie temperature, a key characteristic indicator of the crystal, is improved;
[0022] (3) This process adopts a crystal preheating control process and a crystal finishing process to make the convection of the melt more stable, reduce the difficulty of seeding operation, ensure the stability of the interface temperature of the crystal during growth, and grow the crystal according to the flat interface. At the same time, it reduces the bottom convexity of the crystal when it is cut, reduces the stress at the bottom of the crystal, and reduces the risk of crystal cracking;
[0023] (4) During the in-situ annealing of the crystal, the auxiliary heater and the thermal insulation layer on the upper part of the thermal field act simultaneously, reducing the temperature gradient difference inside the thermal field and realizing in-situ annealing of large-sized lithium niobate crystals, greatly improving production efficiency and reducing costs. DETAILED DESCRIPTION
[0024] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.
[0025] Example 1
[0026] (a) Seed crystal processing: Process the Y-direction crystal, select the Z-direction seed crystal, and use a laser pen to inspect the Z-direction seed crystal to confirm that there are no bubbles, flashes, or cracks inside. Then fix the Z-direction crystal with a fixture and use an orienter to confirm the specific position of the Z-direction end face. Then use a single-line cut to cut the Z-direction end face of the crystal head and tail. After cutting, use a flat grinder to trim the crystal Z-direction end face and pass the light. The deviation is within 6'. Then fix the trimmed crystal with a fixture again and use an orienter to confirm the specific position of the Y-face end face. Then, use a single-line cut to cut the upper and lower Y-direction end faces of the crystal. After cutting, use a surface grinder to trim the crystal direction of the Y-direction end face of the crystal and make it transparent, with a deviation within 6'. Finally, use a single-line cut to vertically cut the remaining two end faces along the Y and Z-direction end faces, and use a surface grinder to flatten and make it transparent to obtain a rectangular seed crystal block with six sides transparent to light. Under strong light, the vein defect position is marked. Then, when the rectangular seed crystal block is cut into seed crystals with a size of 7*10*50mm using an internal circular machine, the seed crystal seeding surface is made to avoid the vein defect.
[0027] (b) Mixing raw materials: After determining whether the crystal growth furnace contains residual bottom material from the previous growth process, first preliminarily determine the mass B of the added raw material and the target Curie temperature b based on the mass ratio of niobium oxide to lithium carbonate of 1000:261-263. Then, subtract the weight of the crystal from the weight of the filling material to obtain the mass A of the residual bottom material in the crystal growth furnace. Measure the Curie temperature a of the residual bottom material and calculate the estimated Curie temperature c of the growing crystal. If the estimated value c is lower than the target value b, lithium carbonate needs to be added with a mass fraction Bθ(bc), where θ is 0.8‰ to 1‰; if the estimated value c is higher than the target value b, niobium oxide needs to be added with a mass fraction Bγ(bc), where γ is 1% to 1.5%. Finally, the raw materials are adjusted to make the estimated Curie temperature of the crystal equal to the target value to obtain the optimal Curie temperature;
[0028] (c) Crystal Growth: The prepared raw materials were placed in a crucible and heated to 1200-1400°C at a heating rate of 100-200°C / h. When the liquid surface became a melt and convection occurred, the temperature was adjusted to between 1350-1380°C to ensure stable and uniform convection. Preheating was performed before seeding for 90-100 min. The seed crystal was then lowered at a rate of 8-10 mm / min. The temperature control was adjusted to allow the seed crystal to neck to 2-3 mm at the seeding end. This state was maintained stable for 1-2 h. At this point, the seed crystal necking was complete and automatic growth began. The rotation speed during the crystal growth stage was controlled at 4-8 rpm and the pulling speed was controlled at 0.5-1 mm / h.
[0029] (d) Crystal finishing: After the crystal automatically grows to the target length, the temperature is raised by 10-20°C based on the current value, the rotation speed is increased by 1-2 rpm, and the temperature is kept at this temperature for 10-15 minutes. The crystal is then pulled out of the liquid at a rate of 30-60 mm / min.
[0030] (e) Crystal annealing: When the crystal leaves the liquid surface, turn on the auxiliary heater on the upper part of the hot field and add a set of heat preservation hot field on the upper part of the hot field to control the internal gradient of the hot field at 5-10℃ / dm. Then adjust the temperature control to keep the crystal at 1200-1250℃ for 10-12h to complete the crystal annealing, and then reduce it to room temperature at 30-50℃ / h.
[0031] The large-sized lithium niobate crystal grown in this example showed no cracks, a regular shape, and 0-5 vein defects. Laser pen inspection revealed no flashes or bubbles within the crystal. The Curie temperature at the head of the crystal was 1142°C, and at the tail it was 1142.5°C, showing good consistency.
[0032] In order to highlight the beneficial effects of the present invention, the following comparative example experiments were also carried out.
[0033] Comparative Example 1
[0034] (a) Seed crystal processing: Process the Y-direction crystal, select the Z-direction seed crystal, and use a laser pen to inspect the Z-direction seed crystal to confirm that there are no bubbles, flashes, or cracks inside; then fix the Z-direction crystal with a fixture, use an orienter to confirm the specific position of the Z-face end face, and then use a single-line cut to cut the head and tail Z-direction end faces of the crystal. After cutting, use a surface grinder to trim the crystal Z-direction end face, with a deviation within 6'; then fix the trimmed crystal with a fixture again, use an orienter to confirm the specific position of the Y-face end face, and then use a single-line cut to cut the upper and lower Y-direction end faces of the crystal. After cutting, use a surface grinder to trim the crystal Y-direction end face, with a deviation within 6'; finally, use a single-line cut to vertically cut the remaining two end faces along the Y and Z-direction end faces, and use a surface grinder to flatten them to obtain a rectangular seed crystal block, and then use an internal circular machine to cut the rectangular seed crystal block into specifications of 7*10*50mm to make a seed crystal;
[0035] (b) Preparation of raw materials: same as in Example 1;
[0036] (c) Crystal growth: same as in Example 1;
[0037] (d) Crystal finishing: same as in Example 1;
[0038] (e) Crystal annealing: same as in Example 1.
[0039] The large-sized lithium niobate crystal grown in this comparative example was found to be uncracked during inspection, but had serious internal vein defects, 5-10 in number; this was determined to be due to the failure to avoid vein defects during seed crystal selection.
[0040] Comparative Example 2
[0041] (a) Seed crystal processing: same as in Example 1;
[0042] (b) Mixing raw materials: If there is residual bottom material from the previous growth furnace in the crystal growth furnace, the raw materials are mixed according to the mass ratio of niobium oxide to lithium carbonate of 1000:261-263;
[0043] (c) Crystal growth: same as in Example 1;
[0044] (d) Crystal tailing: same as in Example 1;
[0045] (e) Crystal annealing: same as in Example 1;
[0046] The large lithium niobate crystals grown in this comparative example showed no cracks, a regular shape, and 0-5 vein defects. Laser inspection revealed no internal flashes or bubbles. The Curie temperatures at the head and tail of the crystals were 1140°C and 1142.5°C, respectively. This significant deviation was attributed to a failure to consider the impact of lithium ion volatilization from residual bottom material in the growth furnace on subsequent crystal growth. The raw material ratio was not adjusted based on the estimated Curie temperature, resulting in a drop in the Curie temperature of the grown crystals, which did not meet the target value.
[0047] Comparative Example 3
[0048] (a) Seed crystal processing: same as in Example 1;
[0049] (b) Preparation of raw materials: same as in Example 1;
[0050] (c) Crystal Growth: The prepared raw materials were placed in a crucible and heated to 1200-1400°C at a heating rate of 100-200°C / h. When the liquid surface became molten and convection occurred, a seed crystal was lowered at a rate of 8-10 mm / min. The temperature was adjusted to allow the seed crystal to neck to 2-3 mm at the seeding end. This state was maintained stable for 1-2 hours. At this point, the seed crystal necking was complete and automatic growth began. The rotation speed during the crystal growth stage was controlled at 4-8 rpm and the pulling speed was controlled at 0.5-1 mm / h.
[0051] (d) Crystal tailing: same as in Example 1;
[0052] (e) Crystal annealing: same as in Example 1.
[0053] The large-sized lithium niobate crystal grown in this comparative example showed cracks and irregular shapes during appearance inspection. It was determined that the lack of preheating before seeding resulted in uneven convection, which reduced the crystal quality and caused the cracks.
[0054] Comparative Example 4
[0055] (a) Seed crystal processing: same as in Example 1;
[0056] (b) Preparation of raw materials: same as in Example 1;
[0057] (c) Crystal growth: same as in Example 1;
[0058] (d) Crystal annealing: After the crystal automatically grows to the target length, it is pulled out of the liquid surface at a rate of 30-60 mm / min. When the crystal is out of the liquid surface, the auxiliary heater on the upper part of the hot field is turned on and a set of heat preservation hot field is added on the upper part of the hot field to control the internal gradient of the hot field at 5-10 ° C / dm. Then, the temperature control is adjusted to keep the crystal at 1200-1250 ° C for 10-12 hours to complete the crystal annealing, and then it is cooled to room temperature at 30-50 ° C / h.
[0059] The large lithium niobate crystal grown in this comparative example showed cracks on the surface. The crystal had a convex bottom, with significant rain streaks and even turbidity on the convex portion. The cracks also extended upwards from the bottom. This was attributed to excessive stress at the bottom of the crystal due to the lack of finishing.
[0060] Comparative Example 5
[0061] (a) Seed crystal processing: same as Example 1
[0062] (b) Preparation of raw materials: same as in Example 1;
[0063] (c) Crystal growth: same as in Example 1;
[0064] (d) Crystal finishing: After the crystal automatically grows to the target length, the temperature is raised by 10-20°C according to the current value, the rotation speed is increased by 1-2 rpm, and the temperature is kept at this temperature for 10-15 minutes. Then, the crystal is pulled out of the liquid surface at a rate of 30-60 mm / min. After the crystal is out of the liquid surface, the temperature is cooled to room temperature at a rate of 30-50°C / h, and then the crystal is removed.
[0065] The large-sized lithium niobate crystals grown in this comparative example cracked due to discharge after being taken out of the furnace. This is because the large-sized lithium niobate crystals have high static electricity, and the crystals that have not been annealed are easily affected by the external environment and crack.
[0066] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing large-sized lithium niobate crystals, Features: The following steps are involved: a) Seed crystal processing: Select a suitable seed crystal according to the axial direction of the lithium niobate crystal to be grown, orient the seed crystal and cut it into a rectangular block, and then when cutting the rectangular block into seed crystals, make the seed crystal seeding surface avoid vein defects; b) Prepare raw materials: Determine whether there is residual bottom material from the previous crystal growth furnace in the crystal growth furnace. If there is no residual bottom material, prepare the raw materials according to the mass ratio of niobium oxide to lithium carbonate of 1000:261-263; if there is residual bottom material, measure the Curie temperature a and mass A of the residual bottom material in the crucible, and preliminarily determine the mass B of the added raw materials and the Curie temperature target value b according to the mass ratio of niobium oxide to lithium carbonate of 1000:261-263. The estimated Curie temperature of the grown crystal is c, where, If the estimated value c is lower than the target value b, the mass of lithium carbonate to be added is Bθ(bc), where θ is 0.8‰ to 1‰; if the estimated value c is higher than the target value b, the mass fraction of niobium oxide to be added is Bγ(bc), where γ is 1% to 1.5%; c) Crystal growth: Put the prepared raw materials into a crucible in a hot field, heat up to melt the lithium niobate raw materials to form a molten liquid, keep the molten liquid warm and preheat it, then lower the seed crystal to contact the molten liquid, keep the seed crystal warm after shrinking the neck, and then the crystal will automatically grow; d) Crystal finishing: adjust the temperature and rotation speed to finish the crystal growth, and then pull the crystal out of the liquid surface; e) Crystal annealing: When the crystal is separated from the liquid surface, it is annealed in situ in the furnace and then cooled to room temperature. During annealing, there are auxiliary heaters and insulation layers on the upper part of the heat field, and the temperature gradient inside the heat field is controlled at 5-10℃ / dm.
2. The method for preparing large-sized lithium niobate crystals according to claim 1, Features: In the step a), the specific method of selecting the seed crystal according to the axial direction of the lithium niobate crystal to be grown is: when growing a Y-direction lithium niobate crystal, select the X-direction or Z-direction seed crystal; when growing a Z-direction lithium niobate crystal, select the X-direction or Y-direction seed crystal; when growing an X-direction lithium niobate crystal, select the Y-direction or Z-direction seed crystal.
3. The method for preparing large-sized lithium niobate crystals according to claim 1, Features: In the step a), the six sides of the rectangular block are inspected by light transmission, and vein defects are marked under a spotlight. When the rectangular block is cut into seed crystals, the seed crystal seeding surface is made to avoid the vein defects.
4. The method for preparing large-sized lithium niobate crystals according to claim 1, Features: In the step c), the heating rate is controlled at 100-200°C / h, and the lithium niobate raw material is heated to 1200-1400°C to melt and form a molten liquid. An infrared thermometer is used to detect the temperature, adjust the temperature, and preheat the molten liquid.
5. The method for preparing large-sized lithium niobate crystals according to claim 4, Features: The preheating time of the molten liquid is 90-100 minutes, and the preheating temperature is 1350-1380°C.
6. The method for preparing large-sized lithium niobate crystals according to claim 4, Features: After the preheating is completed, the seed crystal is lowered at a rate of 8-10 mm / min to contact the melt, the seed crystal is necked to 2-3 mm, and kept warm for 1-2 hours to enter automatic growth. The rotation speed of the crystal growth stage is controlled at 4-8 rpm, and the pulling speed is controlled at 0.5-1 mm / h.
7. The method for preparing large-sized lithium niobate crystals according to claim 1, Features: In the step d), the temperature is raised by 10-20° C., the rotation speed is increased by 1-2 rpm, and after keeping the temperature for 10-15 minutes, the crystal is finished, and then the crystal is pulled away from the liquid surface at a pulling rate of 30-60 mm / min.
8. The method for preparing large-sized lithium niobate crystals according to claim 1, Features: In the step e), the temperature is kept at 1200-1250° C. for 10-12 hours to complete the crystal annealing, and then the temperature is lowered to room temperature at a rate of 30-50° C. / h.
Citation Information
Patent Citations
Lithium niobate crystal and preparation method thereof
CN113913937A
Large-size lithium niobate single crystal and crystal growth method thereof
CN114686967A
Preparation method of large-size lithium niobate crystal
CN116200828A
Method for growing lithium niobate single crystal
JP2020147459A