Dibenzylideneacetone modified hydrophobic butyl rubber damping composite material and preparation method therefor
By introducing NaH to activate butyl rubber and adding dibenzyl acetone and lignin-modified phenolic resin, a damping material with high thermal stability and hydrophobic properties was prepared, which solved the problem of poor performance of traditional damping materials at room temperature and above, and broadened the application field.
Patent Information
- Application Number
- PCT/CN2024/078251
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2024-02-23
- Publication Date
- 2024-11-14
AI Technical Summary
Existing damping materials do not perform well at room temperature and above, and traditional hydrophobic materials are complex or costly to prepare, making it difficult to meet the requirements for efficient hydrophobicity and damping performance.
A method for preparing hydrophobic butyl rubber damping composite material modified with dibenzyl acetone was adopted. By adding NaH to activate butyl rubber and introducing dibenzyl acetone, combined with lignin-modified phenolic resin and montmorillonite filler, a hydrophobic damping material with rigid groups was prepared.
It broadens the damping temperature range, improves the damping factor, achieves high thermal stability and hydrophobic properties, simplifies the preparation process, and reduces costs.
Smart Images

Figure CN2024078251_14112024_PF_FP_ABST
Abstract
Description
A dibenzylideneacetone modified hydrophobic butyl rubber damping composite material and preparation method thereof
[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on May 11, 2023, with application number CN202310528702.6 and invention name “A dibenzylideneacetone modified hydrophobic butyl rubber damping composite material and its preparation method”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application relates to a dibenzylidene acetone modified hydrophobic butyl rubber damping composite material and a preparation method thereof, belonging to the field of polymer-based damping materials. Background Art
[0003] At present, many new materials and technologies have been continuously applied to damping and shock absorption. Among them, polymer materials, especially rubber damping and shock absorption materials, are attracting more and more attention due to their excellent performance. The use of rubber damping materials can minimize mechanical noise and reduce mechanical vibration, improve work efficiency, and improve product quality. Some commonly used asphalt-based damping pads for vehicles will emit carcinogens such as naphthalene, anthracene, and phenanthrene when in use, and the damping effect is relatively poor, which does not meet the requirements of the comfortable, healthy, and quiet travel experience we need. Polymer-based damping materials greatly reduce the emission of toxic substances in the vehicle, have good damping effects at room temperature and above, and can also use renewable raw materials. They have the advantages of sustainable development, safety, health, and environmental protection.
[0004] Water exists in every corner of nature, but in some areas, its presence is undesirable for extended periods, which is why hydrophobic materials are needed. Hydrophobic materials have a wide range of applications, appearing in all aspects of life, including aerospace, military, transportation, agriculture, construction, healthcare, and daily textiles, offering a promising future. The contact angle of hydrophobic materials is generally above 90°, and their preparation mainly revolves around two aspects. On the one hand, low surface energy substances are added to the material, such as substances containing long alkyl chains or fluorine-containing substances, and on the other hand, a rough surface with a micro-nano structure is prepared. However, these two methods of preparing hydrophobic materials have advantages and disadvantages. Generally, the current industrial production of hydrophobic materials mainly involves adding hydrophobic masterbatch, that is, adding low surface energy substances, but the hydrophobic effect of this method is general and can only meet general hydrophobic requirements. The method of preparing hydrophobic materials by constructing a rough interface, although the prepared hydrophobic material has better effect, the preparation process is relatively cumbersome, and the rough interface is easily destroyed, which greatly reduces the hydrophobic effect and requires regular replacement, so the cost is relatively high. At present, the ideal preparation method for producing hydrophobic materials is a combination of the two aspects to play a synergistic role, that is, not only constructing a rough surface, but also covering its surface with low surface energy substances, but the process is relatively speaking, and has not yet reached the capacity for full industrialization and large-scale production.
[0005] Traditional asphalt-based or viscoelastic damping materials, due to the polar functional groups in butyl rubber, are generally hydrophilic and often absorb moisture during use. This, combined with poor thermal stability, results in a typically short service life for these damping materials. Developing a damping material with excellent moisture resistance and high thermal stability is imperative. However, research on the hydrophobicity of damping materials is limited. Chen Bo from Beijing University of Chemical Technology (Chen Bo. Study on silicone-modified polybutadiene-based polyurethane damping materials and their properties [D], Beijing University of Chemical Technology, 2017) used hydroxy-terminated polydimethylsiloxane (HTPDMS) and hydroxy-terminated polybutadiene (HTPB) as blended soft segments to carry out block copolymerization with diphenylmethane diisocyanate (MDI), dipropylene glycol (DPG) and glycerol (GLY) as chain extenders, and used the prepolymer method and casting method to prepare PU damping materials. The hydrophobicity of the material surface was increased, and heptamethyl trisiloxane grafted hydroxy-terminated polybutadiene (HTMS-g-HTPB) and polytetramethylene ether diol (PTMEG2000) were used as mixed segments, and then the polyurethane damping elastomer was prepared by the prepolymer method with diphenylmethane diisocyanate (MDI) and chain extender dipropylene glycol (DPG). By adjusting the ratio between the two phases of the soft segment, as the content of HMTS-g-HTPB increases, the mechanical properties of the material are comprehensively improved and the hydrophobicity of the surface is enhanced. Zang Yu (Zang Yu, Lei Tianyang, Aoki Junshu, et al. Research on Polyester Modified by Grafting of Fluorinated Acrylic Macromonomers [J]. Journal of Qiqihar University (Natural Science Edition), 2020, 36(03): 77-80) et al. studied the effect of methyl methacrylate and tridecyl methacrylate grafted fluorinated side chains on the hydrophilicity of the material and found that the contact angle of the material increased to 128.8° after grafting modification, changing from a hydrophilic material to a hydrophobic material. Although these two methods can improve the hydrophobicity of the damping material, the preparation of the damping material is too complicated and the price is high, which limits its industrial application.
[0006] Summary of the Invention
[0007] The purpose of the present application is to provide a method for preparing a dibenzylideneacetone-modified hydrophobic butyl rubber damping composite material, by adding a bio-based phenolic resin, activating the modified butyl rubber with NaH, and introducing a rigid group benzene ring, thereby broadening the damping temperature range of the butyl rubber, improving the damping performance, and preparing a green and environmentally friendly hydrophobic damping composite material with simple operation.
[0008] The technical solution of this application is:
[0009] The present application provides a method for preparing a dibenzylidene acetone-modified hydrophobic butyl rubber damping composite material, comprising the following steps:
[0010] (1) Add butyl rubber (IIR) and NaH in proportion to the torque rheometer and react for 10 to 15 minutes, then add dibenzylidene acetone and continue to react for 10 to 15 minutes. After the reaction is completed, take out the rubber;
[0011] (2) plasticizing the rubber obtained in step (1) on a two-roll mixer, adding stearic acid, zinc oxide, tetramethylthiuram TMTD, tetramethylthiuram disulfide DM, sulfur, lignin-modified phenolic resin, and montmorillonite filler in sequence, blending uniformly, making triangular packages, thinning, unrolling, and standing to remove bubbles to obtain raw rubber;
[0012] (3) vulcanizing the raw rubber obtained in step (2) on a flat vulcanizer to obtain a dibenzylideneacetone-modified hydrophobic butyl rubber damping composite material.
[0013] Preferably, in step (1), the butyl rubber is 100 parts, the dibenzylideneacetone is 5-20 parts, and the NaH is 5-20 parts by mass.
[0014] Preferably, in step (2), when the butyl rubber in step (1) is 100 parts, the substances in step (2) are calculated by mass as follows: montmorillonite filler is 20-40 parts, lignin-modified phenolic resin is 10-20 parts, stearic acid is 1-3 parts, zinc oxide is 3-7 parts, TMTD is 1-4 parts, DM is 0.5-2 parts, and sulfur is 1-4 parts.
[0015] Preferably, in step (2), the time for removing bubbles is 24 to 36 hours.
[0016] Preferably, in step (3), the vulcanization temperature is 140-160° C., and the vulcanization pressure is 10-16 MPa.
[0017] Preferably, in step (1), the torque rheometer is replaced by an internal mixer.
[0018] Preferably, the raw materials of the preparation method are free of solvent.
[0019] The present application also provides a dibenzylideneacetone modified hydrophobic butyl rubber damping composite material, which is prepared by the preparation method described in the above technical solution.
[0020] Preferably, the high-temperature damping temperature range of the dibenzylideneacetone modified hydrophobic butyl rubber damping composite material is ≥70°C.
[0021] Preferably, the damping factor at 70°C of the dibenzylideneacetone modified hydrophobic butyl rubber damping composite material is 0.37 or 0.35.
[0022] Preferably, the water contact angle of the dibenzylidene acetone modified hydrophobic butyl rubber damping composite material is 94.6°, 97.8°, 101.9° or 103.1°.
[0023] Preferably, the dibenzylideneacetone modified hydrophobic butyl rubber damping composite material includes unsaturated double bond functional groups and rigid group benzene rings introduced into the main chain of the macromolecule.
[0024] The beneficial effects of this application are:
[0025] Using lignin to replace some petroleum raw materials to synthesize biomass-based phenolic resins can not only fully utilize renewable resources but also reduce environmental pollution. Using lignin to replace phenol to synthesize phenolic resins has become an important direction to solve the problems of resin environmental protection and reproducibility.
[0026] The biggest advantage of chemically modifying the rubber during processing is that the reaction can be carried out in common rubber processing equipment (such as torque rheometer, internal mixer, etc.). It is a solvent-free modification method with a simple preparation process and low requirements for experimental equipment.
[0027] The butyl rubber damping composite material prepared in this application solves the problem that traditional asphalt-based damping materials have poor damping effect at room temperature and above, broadens the damping temperature range, improves the damping factor, prepares a new type of hydrophobic butyl rubber damping composite material, and further broadens the application field of damping composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 shows the tanδ~T relationship curve of pure butyl rubber;
[0029] FIG2 is a graph showing the water contact angle of butyl rubber after adding 10 parts of lignin-modified phenolic resin to Comparative Example 1;
[0030] FIG3 is a graph showing the water contact angle of butyl rubber after adding 20 parts of lignin-modified phenolic resin in Comparative Example 2;
[0031] Figure 4 is a tanδ-T relationship curve of the damping rubber with lignin-modified phenolic resin; 1-Comparative Example 1; 2-Comparative Example 2;
[0032] FIG5 is a graph showing the contact angle of butyl rubber with water after adding 15 parts of dibenzylideneacetone in Example 3;
[0033] FIG6 is a tanδ-T relationship curve of the damping rubber of Examples 1 to 4;
[0034] Figure 7 is an infrared spectra of the damping composite materials obtained with different additives, where 1 is pure butyl rubber; 2 is comparative example 1 with the addition of filler and bio-based phenolic resin; 3 is example 1 with the addition of NaH and dibenzylideneacetone; and 4 is comparative example 4 with the addition of dibenzylideneacetone without the addition of NaH. DETAILED DESCRIPTION
[0035] In the present invention, butyl rubber (100 parts) and NaH (5-20 parts) are added to a torque rheometer to react for 10-15 minutes, and then dibenzylideneacetone (5-20 parts) is added to continue the reaction for 10-15 minutes. After the reaction is completed, the rubber material is taken out; the obtained rubber material is plasticized on a two-roll mixer, and stearic acid (1-3 parts), zinc oxide (3-7 parts), tetramethylthiuram (TMTD) (1-4 parts), tetramethylthiuram disulfide ( DM) (0.5-2 parts), sulfur (1-4 parts), lignin-modified phenolic resin (10-20 parts), and montmorillonite filler (20-40 parts) are uniformly blended, packaged in a triangle, thinly passed, and sliced. The raw rubber is left for 24-36 hours to remove bubbles, thereby obtaining a raw rubber. Finally, the obtained raw rubber is vulcanized on a flat vulcanizer at a vulcanization temperature of (140-160° C.) and a vulcanization pressure of (10-16 MPa) to obtain a wide-temperature-range hydrophobic butyl rubber damping composite material.
[0036] The present application will be further described in detail below in conjunction with specific embodiments. The specific embodiments described are only used to explain the present application and are not used to limit the present application. Throughout the specification, references to "one embodiment," "an embodiment," "an example," or "an example" mean that the specific features, structures, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment of the present application. Therefore, the phrases "one embodiment," "an embodiment," "an example," or "an example" that appear in various places throughout the specification do not necessarily refer to the same embodiment or example.
[0037] Figure 1 shows the tanδ~T relationship curve of pure butyl rubber. It can be seen from Figure 1 that the damping effect of pure butyl rubber is not good at room temperature and above.
[0038] Comparative Example 1:
[0039] Take 100 parts of butyl rubber, 10 parts of lignin-modified phenolic resin, 30 parts of montmorillonite filler, 2 parts of stearic acid, 5 parts of zinc oxide, 2 parts of TMTD, 1 part of DM, and 2 parts of sulfur.
[0040] The butyl rubber was plasticized on a two-roll mixer, and stearic acid, zinc oxide, TMTD, DM, sulfur, lignin-modified phenolic resin, and montmorillonite filler were added in sequence, mixed evenly, made into triangular packages, thinly passed, and sheeted. The raw rubber was left for 24 hours to remove bubbles to obtain the raw rubber. Finally, the obtained raw rubber was vulcanized on a flat vulcanizer at a vulcanization temperature of 160°C, a vulcanization pressure of 14 MPa, and a vulcanization time of 16 minutes to obtain a wide-temperature-range butyl rubber damping composite material.
[0041] The modified butyl rubber prepared in Comparative Example 1 has a high-temperature damping temperature range of >60°C and a damping factor of 0.33 at 60°C, as shown in curve 1 of FIG4 . The water contact angle is 86.9°, indicating no hydrophobicity, as shown in FIG2 .
[0042] Comparative Example 2:
[0043] Take 100 parts of butyl rubber, 20 parts of lignin-modified phenolic resin, 30 parts of montmorillonite filler, 2 parts of stearic acid, 5 parts of zinc oxide, 2 parts of TMTD, 1 part of DM, and 2 parts of sulfur.
[0044] The butyl rubber was plasticized on a two-roll mixer, and stearic acid, zinc oxide, TMTD, DM, sulfur, lignin-modified phenolic resin, and montmorillonite filler were added in sequence, mixed evenly, made into triangular packages, thinly passed, and sheeted. The raw rubber was left for 24 hours to remove bubbles to obtain the raw rubber. Finally, the obtained raw rubber was vulcanized on a flat vulcanizer at a vulcanization temperature of 160°C, a vulcanization pressure of 14 MPa, and a vulcanization time of 16 minutes to obtain a wide-temperature-range butyl rubber damping composite material.
[0045] The high-temperature damping temperature range of the modified butyl rubber prepared in Comparative Example 2 is greater than 60°C, and the damping factor at 60°C is 0.31, as shown in curve 2 of FIG4 ; the water contact angle is 80.2°, and it does not exhibit hydrophobic properties, as shown in FIG3 .
[0046] As can be seen from Figures 2 and 3, after adding lignin-modified phenolic resin, the damping composite material does not show hydrophobic properties because the lignin-modified phenolic resin contains a certain amount of hydroxyl groups on the modified resin molecular chain.
[0047] Example 1:
[0048] Take 100 parts of butyl rubber, 5 parts of dibenzylideneacetone, 5 parts of NaH, 10 parts of lignin-modified phenolic resin, 30 parts of montmorillonite filler, 2 parts of stearic acid, 5 parts of zinc oxide, 2 parts of TMTD, 1 part of DM, and 2 parts of sulfur.
[0049] Butyl rubber and NaH were added to a torque rheometer and reacted for 10 minutes, and then dibenzylidene acetone was added and the reaction was continued for 10 minutes. After the reaction was completed, the rubber material was taken out; the obtained rubber material was plasticized on a two-roll mixer, and stearic acid, zinc oxide, TMTD, DM, sulfur, lignin-modified phenolic resin, and montmorillonite filler were added in sequence, blended evenly, made into triangular packages, thinly passed, and sheeted. The rubber material was left for 24 hours to remove bubbles to obtain a raw rubber; finally, the obtained raw rubber was vulcanized on a flat vulcanizer at a vulcanization temperature of 160°C and a vulcanization pressure of 14 MPa to obtain a wide-temperature-range hydrophobic butyl rubber damping composite material.
[0050] The high-temperature damping temperature range of the modified butyl rubber prepared in Example 1 is ≥70° C., and the damping factor at 70° C. is 0.30, as shown in curve 1 of FIG6 ; and the water contact angle is 94.6°.
[0051] Example 2:
[0052] Take 100 parts of butyl rubber, 10 parts of dibenzylideneacetone, 10 parts of NaH, 10 parts of lignin-modified phenolic resin, 30 parts of montmorillonite filler, 2 parts of stearic acid, 5 parts of zinc oxide, 2 parts of TMTD, 1 part of DM, and 2 parts of sulfur.
[0053] Butyl rubber and NaH were added to a torque rheometer and reacted for 10 minutes, and then dibenzylidene acetone was added and the reaction was continued for 10 minutes. After the reaction was completed, the rubber material was taken out; the obtained rubber material was plasticized on a two-roll mixer, and stearic acid, zinc oxide, TMTD, DM, sulfur, lignin-modified phenolic resin, and montmorillonite filler were added in sequence, blended evenly, made into triangular packages, thinly passed, and sheeted. The rubber material was left for 24 hours to remove bubbles to obtain a raw rubber; finally, the obtained raw rubber was vulcanized on a flat vulcanizer at a vulcanization temperature of 160°C and a vulcanization pressure of 14 MPa to obtain a wide-temperature-range hydrophobic butyl rubber damping composite material.
[0054] The high-temperature damping temperature range of the modified butyl rubber prepared in Example 2 is greater than 70° C., and the damping factor at 70° C. is 0.35, as shown in curve 2 of FIG6 ; the water contact angle is 97.8°.
[0055] Example 3:
[0056] Take 100 parts of butyl rubber, 15 parts of dibenzylideneacetone, 15 parts of NaH, 10 parts of lignin-modified phenolic resin, 30 parts of montmorillonite filler, 2 parts of stearic acid, 5 parts of zinc oxide, 2 parts of TMTD, 1 part of DM, and 2 parts of sulfur.
[0057] Butyl rubber and NaH were added to a torque rheometer and reacted for 10 minutes, and then dibenzylidene acetone was added and the reaction was continued for 10 minutes. After the reaction was completed, the rubber material was taken out; the obtained rubber material was plasticized on a two-roll mixer, and stearic acid, zinc oxide, TMTD, DM, sulfur, lignin-modified phenolic resin, and montmorillonite filler were added in sequence, blended evenly, made into triangular packages, thinly passed, and sheeted. The rubber material was left for 24 hours to remove bubbles to obtain a raw rubber; finally, the obtained raw rubber was vulcanized on a flat vulcanizer at a vulcanization temperature of 160°C and a vulcanization pressure of 14 MPa to obtain a wide-temperature-range hydrophobic butyl rubber damping composite material.
[0058] The high-temperature damping temperature range of the modified butyl rubber prepared in Example 3 is greater than 70° C., and the damping factor at 70° C. is 0.37, as shown in curve 3 of FIG6 ; the water contact angle is 101.9°.
[0059] Example 4:
[0060] Take 100 parts of butyl rubber, 20 parts of dibenzylideneacetone, 20 parts of NaH, 10 parts of lignin-modified phenolic resin, 30 parts of montmorillonite filler, 2 parts of stearic acid, 5 parts of zinc oxide, 2 parts of TMTD, 1 part of DM, and 2 parts of sulfur.
[0061] Butyl rubber and NaH were added to a torque rheometer and reacted for 10 minutes, and then dibenzylidene acetone was added and the reaction was continued for 10 minutes. After the reaction was completed, the rubber material was taken out; the obtained rubber material was plasticized on a two-roll mixer, and stearic acid, zinc oxide, TMTD, DM, sulfur, lignin-modified phenolic resin, and montmorillonite filler were added in sequence, blended evenly, made into triangular packages, thinly passed, and sheeted. The rubber material was left for 24 hours to remove bubbles to obtain a raw rubber; finally, the obtained raw rubber was vulcanized on a flat vulcanizer at a vulcanization temperature of 160°C and a vulcanization pressure of 14 MPa to obtain a wide-temperature-range hydrophobic butyl rubber damping composite material.
[0062] The high-temperature damping temperature range of the modified butyl rubber prepared in Example 4 is greater than 70° C., and the damping factor at 70° C. is 0.35, as shown in curve 4 of FIG6 ; the water contact angle is 103.1°, as shown in FIG5 .
[0063] As can be seen from Figure 5, the addition of lignin-modified phenolic resin combined with NaH-activated modified butyl rubber introduces a large number of rigid group benzene rings on the main chain of butyl rubber. Due to the presence of a large number of aromatic group benzene rings, the damping composite material has hydrophobic properties.
[0064] As shown in Figure 6, increasing the amount of dibenzylidene acetone added to the NaH-activated modified butyl rubber increases the damping temperature range and damping factor of the damping composite. In Example 3, when 15 parts of dibenzylidene acetone were added, the damping factor reached as high as 0.37 at 75°C. The addition of lignin-modified phenolic resin combined with NaH-activated modified butyl rubber with the introduction of rigid benzyl ring groups improves the damping performance of the butyl rubber, broadens the damping temperature range, and imparts hydrophobic properties to the damping composite.
[0065] Comparative Example 3:
[0066] Take 100 parts of butyl rubber, 10 parts of NaH, 10 parts of lignin-modified phenolic resin, 30 parts of montmorillonite filler, 2 parts of stearic acid, 5 parts of zinc oxide, 2 parts of TMTD, 1 part of DM, and 2 parts of sulfur.
[0067] Butyl rubber and NaH were added to a torque rheometer and reacted for 10 minutes. After the reaction was completed, the rubber was taken out; the obtained rubber was plasticized on a two-roll mixer, and stearic acid, zinc oxide, TMTD, DM, sulfur, lignin-modified phenolic resin, and montmorillonite filler were added in sequence, blended evenly, made into triangular packages, thinly passed, and sheeted. The rubber was left for 24 hours to remove bubbles to obtain a raw rubber; finally, the raw rubber was vulcanized on a flat vulcanizer at a vulcanization temperature of 160°C and a vulcanization pressure of 14 MPa to obtain a wide-temperature-range butyl rubber damping composite material.
[0068] The modified butyl rubber prepared in Comparative Example 3 has a high-temperature damping temperature range of ≥60°C, a damping factor of 0.31 at 60°C, and a water contact angle of 82.4°.
[0069] Comparative Example 4:
[0070] Take 100 parts of butyl rubber, 10 parts of dibenzylideneacetone, 10 parts of lignin-modified phenolic resin, 30 parts of montmorillonite filler, 2 parts of stearic acid, 5 parts of zinc oxide, 2 parts of TMTD, 1 part of DM, and 2 parts of sulfur.
[0071] Butyl rubber and NaH were added to a torque rheometer and reacted for 10 minutes. After the reaction was completed, the rubber was taken out; the obtained rubber was plasticized on a two-roll mixer, and stearic acid, zinc oxide, TMTD, DM, sulfur, lignin-modified phenolic resin, and montmorillonite filler were added in sequence, blended evenly, made into triangular packages, thinly passed, and sheeted. The rubber was left for 24 hours to remove bubbles to obtain a raw rubber; finally, the raw rubber was vulcanized on a flat vulcanizer at a vulcanization temperature of 160°C and a vulcanization pressure of 14 MPa to obtain a wide-temperature-range butyl rubber damping composite material.
[0072] The wide temperature range damping hydrophobic butyl rubber prepared by the methods described in Examples 1 to 4 and Comparative Examples 1 to 3 of the present application was compared with the butyl rubber to which only lignin phenolic resin and filler were added. For specific performance, please refer to Figures 1 to 7 and Table 1.
[0073] [Corrected 07.04.2024 in accordance with Rule 91] Table 1
[0074] Table 1 and Figure 4 show that the addition of lignin-modified phenolic resin improves the tensile and fracture strength of the damping composite. The addition of lignin-modified phenolic resin improves the damping properties of butyl rubber composites. The numerous polar hydroxyl groups contained in the molecular chains of the lignin-modified phenolic resin, upon incorporation into the rubber matrix, significantly enhance the internal friction forces that contribute to the molecular chain's motion. The lignin-modified phenolic resin and butyl rubber interpenetrate each other, forming a distinct interpenetrating network structure.
[0075] As can be seen from Figure 7, a comparison between curves 1 and 2 shows that the addition of lignin-modified phenolic resin and montmorillonite filler does not change the main chain structure of butyl rubber; curve 3 uses NaH to activate butyl rubber and introduce dibenzylideneacetone, while curve 4 only adds dibenzylideneacetone without using NaH to activate the double bonds in butyl rubber. By comparison, it can be found that unsaturated double bond functional groups and rigid group benzene rings are introduced into the main chain of the macromolecule.
[0076] Although the above embodiment provides a detailed description of the present application, it is only a part of the embodiments of the present application rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the scope of protection of the present application.
Claims
1. A method for preparing a dibenzylideneacetone modified hydrophobic butyl rubber damping composite material, characterized in that: The steps include: (1) Add butyl rubber and NaH in proportion to a torque rheometer and react for 10 to 15 minutes, then add dibenzylideneacetone and continue to react for 10 to 15 minutes. After the reaction is completed, take out the rubber; (2) plasticizing the rubber obtained in step (1) on a two-roll mixer, adding stearic acid, zinc oxide, tetramethylthiuram, tetramethylthiuram disulfide, sulfur, lignin-modified phenolic resin, and montmorillonite filler in sequence, blending evenly, making triangle packages, thinning, putting down sheets, and leaving them to remove bubbles, thereby obtaining raw rubber; (3) vulcanizing the raw rubber obtained in step (2) on a flat vulcanizer to obtain a dibenzylideneacetone-modified hydrophobic butyl rubber damping composite material.
2. The preparation method according to claim 1, characterized in that: In step (1), the butyl rubber is 100 parts, the dibenzylideneacetone is 5 to 20 parts, and the NaH is 5 to 20 parts by mass.
3. The preparation method according to claim 1, characterized in that: When the butyl rubber in step (1) is 100 parts, the substances in step (2) are, by weight, 20 to 40 parts of montmorillonite filler, 10 to 20 parts of lignin-modified phenolic resin, 1 to 3 parts of stearic acid, 3 to 7 parts of zinc oxide, 1 to 4 parts of tetramethylthiuram, 0.5 to 2 parts of tetramethylthiuram disulfide, and 1 to 4 parts of sulfur.
4. The preparation method according to claim 1, characterized in that: In step (2), the time for removing bubbles is 24 to 36 hours.
5. The preparation method according to claim 1, characterized in that: In step (3), the vulcanization temperature is 140-160° C., and the vulcanization pressure is 10-16 MPa.
6. The preparation method according to claim 1, characterized in that: In step (1), the torque rheometer is replaced by an internal mixer.
7. The preparation method according to claim 1, characterized in that: The raw materials of the preparation method are free of solvent.
8. A dibenzylideneacetone modified hydrophobic butyl rubber damping composite material, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 7.
9. The dibenzylideneacetone modified hydrophobic butyl rubber damping composite material according to claim 8, characterized in that: The high-temperature damping temperature range of the dibenzylideneacetone modified hydrophobic butyl rubber damping composite material is ≥70°C.
10. The dibenzylideneacetone modified hydrophobic butyl rubber damping composite material according to claim 8 or 9, characterized in that: The 70°C damping factor of the dibenzylideneacetone modified hydrophobic butyl rubber damping composite material is 0.37 or 0.
35.
11. The dibenzylideneacetone modified hydrophobic butyl rubber damping composite material according to claim 8 or 9, characterized in that: The water contact angle of the dibenzylideneacetone modified hydrophobic butyl rubber damping composite material is 94.6°, 97.8°, 101.9° or 103.1°.
12. The dibenzylideneacetone modified hydrophobic butyl rubber damping composite material according to claim 8, characterized in that: The dibenzylideneacetone modified hydrophobic butyl rubber damping composite material comprises an unsaturated double bond functional group and a rigid group benzene ring introduced into the main chain of the macromolecule.
Citation Information
Patent Citations
Preparation method of citral modified isobutylene-isoprene rubber compound
CN106751058A
Preparation method of benzoxazine modified butyl rubber wide-temperature-range damping composite material
CN112457544A
Dibenzylidene acetone modified hydrophobic butyl rubber damping composite material and preparation method thereof
CN116444906A
Modified butyl rubber composition
JP2007231244A
Cited By
Damping rubber composition for track fastener and preparation method of damping rubber composition
CN119912755A