Coating kit, thermosetting coating composition, main agent for thermosetting coating composition, coating film forming method, and coated article

The paint kit uses an acrylic polyol and polyisocyanate-based thermosetting paint composition to form a high-crosslinking-density film that allows easy graffiti removal and stain resistance at low curing temperatures, addressing the inefficiencies of existing compositions and reducing energy costs.

WO2024232438A1PCT designated stage expired Publication Date: 2024-11-14KANSAI PAINT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017485
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2024-05-10
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Existing thermosetting paint compositions struggle with insufficient stain removal properties when cured at low temperatures, and there is a need for a paint kit that can form a removable paint film from which graffiti can be easily and cleanly removed, while also reducing energy costs by curing at lower temperatures and shorter times.

Method used

A paint kit comprising a thermosetting paint composition with a main ingredient of acrylic polyol having an alkoxysilyl group and a curing agent containing a polyisocyanate compound, specifically an isocyanurate trimer, which forms a coating film with high crosslinking density, allowing for easy graffiti removal and improved stain resistance when cured at 80°C for 30 minutes and left to stand for 1 hour.

Benefits of technology

The paint kit achieves high removability and stain resistance of graffiti, even when cured at low temperatures, with a minimum storage modulus of 2.6×10^7 Pa, ensuring the paint film's integrity and ease of removal, while reducing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide a coating kit for a thermosetting coating composition that forms a removable coating film that allows graffiti to be removed easily and cleanly in curing at from low temperature to conventional temperature. The present invention is a coating kit for a thermosetting coating composition comprising a main agent that contains an acrylic polyol (A) having an alkoxysilyl group and a curing agent that contains a polyisocyanate compound (B) containing an isocyanurate trimer, wherein the minimum value E'min of the storage modulus in the 40-200°C range of a coating film formed by curing a thermosetting coating composition obtained from the coating kit by heating for 30 minutes at 80°C and allowing to stand for one hour is 2.6×107Pa or more.
Need to check novelty before this filing date? Find Prior Art

Description

Paint kit, thermosetting paint composition, base agent for thermosetting paint composition, coating film forming method, and coated article

[0001] The present invention relates to a paint kit, a thermosetting paint composition, a base agent for a thermosetting paint composition, a method for forming a coating film, and a coated article.

[0002] Artificial graffiti on various architectural structures, railway vehicles, large vehicles, etc., is a major social problem because it not only damages the aesthetics and scenery but can also lead to a deterioration in public safety. However, removing graffiti painted on substrates with spray paint, oil-based pens, etc., is time-consuming and labor-intensive, and is difficult to remove cleanly, and there is a risk of damaging the existing coating film. Therefore, there is a demand for removable coating compositions that allow graffiti to be easily and cleanly removed. Furthermore, in recent years, there has been a demand for coating compositions that can form coating films at lower curing temperatures and shorter curing times in order to reduce energy costs.

[0003] Patent Document 1 discloses a coating composition containing a resin (A) having hydroxyl groups and alkoxysilyl groups, a curing agent (B), and a dispersion of acrylic resin-coated silica particles (C), in which the dispersion of acrylic resin-coated silica particles (C) is a dispersion of acrylic resin-coated silica particles (C) that is a reaction product of silica particles (c1) having polymerizable unsaturated groups and a polymerizable unsaturated monomer mixture (c2), and the polymerizable unsaturated monomer mixture (c2) contains, as at least a part of its components, a polymerizable unsaturated monomer (c21) having a polysiloxane structure represented by formula (I) and an alkoxysilyl group-containing polymerizable unsaturated monomer (c22). The coating composition is described as being capable of forming a coating film that is excellent in stain removability, scratch resistance, and transparency.

[0004] International Publication No. 2021 / 131444

[0005] The coating composition of Patent Document 1 sometimes exhibits insufficient stain removal properties when cured at low temperatures.

[0006] An object of the present invention is to provide a coating kit for a thermosetting coating composition that can form a removable coating film from which graffiti can be easily and cleanly removed when cured at low to conventional temperatures.

[0007] As a result of intensive research into solving the above-mentioned problems, the present inventors have discovered a coating kit for a thermosetting coating composition, which comprises a base agent containing an acrylic polyol (A) having an alkoxysilyl group and a curing agent component containing a polyisocyanate compound (B), wherein the thermosetting coating composition obtained from the coating kit is heat-cured at 80°C for 30 minutes and allowed to stand for 1 hour to form a coating film having a minimum storage modulus E' in the range of 40 to 200°C. min is 2.6 x 10 7 The present inventors have found that the above-mentioned problems can be solved by a paint kit for a thermosetting paint composition having a modulus of elasticity of 80°C or more, and have completed the present invention. That is, the present invention provides the following paint kit, thermosetting paint composition, base agent for a thermosetting paint composition, method for forming a coating film, and coated article. Item 1. A paint kit for a thermosetting paint composition, comprising a base agent containing an acrylic polyol (A) having an alkoxysilyl group, and a curing agent component containing a polyisocyanate compound (B) containing an isocyanurate trimer, wherein the thermosetting paint composition obtained from the paint kit is heat-cured at 80°C for 30 minutes and allowed to stand for 1 hour, and the coating film formed has a minimum storage modulus E' in the range of 40 to 200°C. min is 2.6 x 10 7Item 2. The paint kit according to Item 1, further comprising at least one catalyst compound (C) selected from amidine compounds, guanidine compounds, phosphazene compounds, and imidazole compounds. Item 3. The paint kit according to Item 1 or 2, further comprising a silicone (D) modified with a hydroxyl group-containing resin. Item 4. The paint kit according to any one of Items 1 to 3, further comprising an organic solvent-dispersed colloidal silica (E). Item 5. The paint kit according to any one of Items 1 to 4, wherein the paint film has stain resistance. Item 6. A thermosetting paint composition comprising a base component containing an acrylic polyol (A) having an alkoxysilyl group, and a curing agent component containing a polyisocyanate compound (B) containing an isocyanurate trimer, wherein the paint film formed by heating and curing at 80°C for 30 minutes and then leaving to stand for 1 hour has a minimum storage modulus E' in the range of 40 to 200°C. min is 2.6 x 10 7 Item 7. A thermosetting coating composition comprising a base agent containing an acrylic polyol (A) having an alkoxysilyl group and a curing agent component containing a polyisocyanate compound (B) containing an isocyanurate trimer, wherein the thermosetting coating composition is heat-cured at 80°C for 30 minutes and allowed to stand for 1 hour to form a coating film having a storage modulus of at least Pa in the range of 40 to 200°C. min is 2.6 x 10 7Item 8. A coating film forming method comprising a coating film forming step of applying to a substrate a thermosetting coating composition obtained from the coating kit according to any one of Items 1 to 5, the thermosetting coating composition according to Item 6, or a thermosetting coating composition obtained by mixing the substrate and curing agent component according to Item 7, to form a wet coating film. Item 9. The coating film forming method according to Item 8, comprising a step of heat-curing the wet coating film at a temperature range of 50°C or higher and 120°C or lower. Item 10. The coating film forming method according to Item 8 or 9, wherein the substrate is at least one selected from automobiles, industrial machinery, construction machinery, railway vehicles, ship hulls, building materials, and housing equipment and parts thereof. Item 11. A coated article obtained by applying to a substrate a thermosetting coating composition obtained from the coating kit according to any one of Items 1 to 5, the thermosetting coating composition according to Claim 6, or a thermosetting coating composition obtained by mixing the substrate and curing agent component according to Claim 7.

[0008] The paint kit of the present invention can form a coating film from which graffiti can be easily and cleanly removed by curing at low to conventional temperatures.

[0009] Hereinafter, embodiments for carrying out the present invention will be described in detail. Note that the present invention is not limited to the following embodiments, and includes various modifications that are implemented within the scope of the present invention. In this specification, "parts" means parts by mass, and "%" means % by mass.

[0010] [Alkoxysilyl group-containing acrylic polyol (A)] The paint kit for the thermosetting paint composition of the present invention (hereinafter sometimes simply referred to as the "paint kit") contains an alkoxysilyl group-containing acrylic polyol (A) as a component in the base material. The content of the acrylic polyol (A), based on the mass of the resin solids contained in the base material, is preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 70 mass% or more. The content of the acrylic polyol (A), based on the mass of the resin solids contained in the entire paint kit (thermosetting paint composition), is preferably 20 to 80 mass%, more preferably 30 to 75 mass%, and even more preferably 40 to 70 mass%.

[0011] The acrylic polyol (A) having the alkoxysilyl group can be produced, for example, by copolymerizing a hydroxyl group-containing polymerizable unsaturated monomer (a11), an alkoxysilyl group-containing polymerizable unsaturated monomer (a12), and another copolymerizable polymerizable unsaturated monomer (a13).

[0012] The hydroxyl group-containing polymerizable unsaturated monomer (a11) is a compound having one or more hydroxyl groups and one or more polymerizable unsaturated groups per molecule. In this specification, the term "polymerizable unsaturated group" refers to an unsaturated group capable of radical polymerization. Examples of the polymerizable unsaturated group include a vinyl group and a (meth)acryloyl group. The hydroxyl group derived from the hydroxyl group-containing polymerizable unsaturated monomer (a11) can function as a crosslinkable functional group in the resulting acrylic polyol (A) having an alkoxysilyl group.

[0013] Specific examples of the hydroxyl group-containing polymerizable unsaturated monomer (a11) include monoesters of acrylic acid or methacrylic acid with dihydric alcohols having 2 to 10 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, caprolactone-modified hydroxyl group-containing (meth)acrylate, and 4-methylolcyclohexyl (meth)acrylate. Commercially available caprolactone-modified hydroxyl group-containing (meth)acrylates include "PLACCEL FM" (trade name, manufactured by Daicel Chemical Industries, Ltd.), and commercially available 4-methylolcyclohexyl acrylates include "CHDMMA" (trade name, manufactured by Nippon Kasei Chemical Industry Co., Ltd.). The hydroxyl group-containing polymerizable unsaturated monomer (a11) may be used alone or in combination of two or more kinds.

[0014] In this specification, "(meth)acrylate" means "acrylate and / or methacrylate." "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid." "(meth)acryloyl" means "acryloyl and / or methacryloyl." "(meth)acrylamide" means "acrylamide and / or methacrylamide."

[0015] As the hydroxyl group-containing polymerizable unsaturated monomer (a11), from the viewpoint of preventing penetration of ink and contaminants, polymerizable unsaturated monomers having a hydroxyl group-containing hydrocarbon group having 2 to 20 carbon atoms are particularly preferred, specifically 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-methylolcyclohexyl acrylate, etc.

[0016] The alkoxysilyl group-containing polymerizable unsaturated monomer (a12) is a compound having one or more alkoxysilyl groups and one or more polymerizable unsaturated groups per molecule. Specific examples include vinyltrimethoxysilane, vinyltriethoxysilane, acryloxyethyltrimethoxysilane, methacryloxyethyltrimethoxysilane, acryloxypropyltrimethoxysilane, methacryloxypropyltrimethoxysilane, acryloxypropyltriethoxysilane, methacryloxypropyltriethoxysilane, and vinyltris(β-methoxyethoxy)silane. Preferred alkoxysilyl group-containing polymerizable unsaturated monomers include vinyltrimethoxysilane, γ-acryloxypropyltrimethoxysilane, and γ-methacryloxypropyltrimethoxysilane. The alkoxysilyl group-containing polymerizable unsaturated monomer (a12) can be used alone or in combination of two or more.

[0017] The other copolymerizable polymerizable unsaturated monomer (a13) is a compound having one or more polymerizable unsaturated groups in one molecule, other than the hydroxyl group-containing polymerizable unsaturated monomer (a11) and the alkoxysilyl group-containing polymerizable unsaturated monomer (a12), and specific examples thereof are listed in the following (1) to (11).

[0018] (1) Aromatic polymerizable unsaturated monomers: for example, styrene, α-methylstyrene, vinyltoluene, etc. (2) Polymerizable unsaturated monomers having a branched hydrocarbon group with 8 or more carbon atoms: for example, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isomyristyl (meth)acrylate, isostearyl (meth)acrylate, etc. Commercially available isostearyl (meth)acrylates include "Isostearyl Acrylate" (trade name, manufactured by Osaka Organic Chemical Industry Ltd.). (3) Polymerizable unsaturated monomers containing an alicyclic hydrocarbon group having 3 to 20 carbon atoms: for example, polymerizable unsaturated monomers containing a bridged alicyclic hydrocarbon group having 10 to 20 carbon atoms, such as isobornyl (meth)acrylate, tricyclodecanyl (meth)acrylate, adamantyl (meth)acrylate, 3,5-dimethyladamantyl (meth)acrylate, and 3-tetracyclododecyl (meth)acrylate; polymerizable unsaturated monomers having an alicyclic hydrocarbon group having 3 to 12 carbon atoms, such as cyclohexyl (meth)acrylate, 4-methylcyclohexylmethyl (meth)acrylate, 4-ethylcyclohexylmethyl (meth)acrylate, 4-methoxycyclohexylmethyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, cyclooctyl (meth)acrylate, cyclododecyl (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate. (4) C1-7 linear or branched alkyl esters of (meth)acrylic acid: methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, etc. (5) C8-22 linear alkyl esters of (meth)acrylic acid: lauryl (meth)acrylate, stearyl (meth)acrylate, etc. (6) Epoxy group-containing polymerizable unsaturated monomers: glycidyl (meth)acrylate, etc. (7) Nitrogen-containing polymerizable unsaturated monomers: (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, vinylpyridine, vinylimidazole, etc.(8) Other vinyl compounds: for example, vinyl acetate, vinyl propionate, vinyl chloride, vinylidene chloride, divinyl ether, and versatate vinyl esters such as "Veova 9" and "Veova 10" (trade names, manufactured by Hexion). (9) Unsaturated group-containing nitrile compounds: for example, (meth)acrylonitrile. (10) Acidic functional group-containing polymerizable unsaturated monomers: for example, carboxyl group-containing unsaturated monomers such as (meth)acrylic acid, crotonic acid, itaconic acid, maleic acid, and maleic anhydride; sulfonic acid group-containing unsaturated monomers such as vinyl sulfonic acid and sulfoethyl (meth)acrylate; and acidic phosphate ester-based unsaturated monomers such as 2-(meth)acryloyloxyethyl acid phosphate, 2-(meth)acryloyloxypropyl acid phosphate, 2-(meth)acryloyloxy-3-chloropropyl acid phosphate, and 2-(meth)acryloyloxyethylphenyl phosphoric acid. (11) Polymerizable unsaturated monomers having a polydimethylsiloxane structure: For example, commercially available products include "Silaplane FM-0721", "Silaplane FM-0711", and "Silaplane FM-0725" (all trade names, manufactured by JNC Corporation), "X-22-174ASX", "X-22-174BX", "KF-2012", "X-22-2426", "X-22-2404", and "X-22-2475" (all trade names, manufactured by Shin-Etsu Chemical Co., Ltd.). The other copolymerizable polymerizable unsaturated monomers (a13) can be used alone or in combination of two or more.

[0019] The proportion of the hydroxyl group-containing polymerizable unsaturated monomer (a11) used is suitably 15 to 55 mass %, preferably 20 to 50 mass %, based on the total mass of the copolymerizable monomer components constituting the acrylic polyol (A) having an alkoxysilyl group, from the viewpoints of stain removability, scratch resistance, water resistance, etc. of the resulting coating film.

[0020] The proportion of the alkoxysilyl group-containing polymerizable unsaturated monomer (a12) used is suitably 5 to 60 mass %, preferably 20 to 50 mass %, based on the total mass of the copolymerizable monomer components constituting the acrylic polyol (A) having an alkoxysilyl group, from the viewpoints of the stain removability, scratch resistance, transparency, etc. of the resulting coating film.

[0021] The other polymerizable unsaturated monomers (a13) are optional components, and among them, acidic functional group-containing polymerizable unsaturated monomers such as carboxyl group-containing unsaturated monomers, sulfonic acid group-containing unsaturated monomers, and acidic phosphate ester-based unsaturated monomers can act as internal catalysts when the resulting alkoxysilyl group-containing acrylic polyol (A) crosslinks with a polyisocyanate compound, and the amount used is preferably within a range of 0 to 5 mass %, more preferably within a range of 0 to 3 mass %, based on the total mass of the copolymerizable monomer components constituting the alkoxysilyl group-containing acrylic polyol (A).

[0022] The copolymerization method for copolymerizing the above-mentioned monomer mixture to obtain the acrylic polyol (A) having an alkoxysilyl group is not particularly limited, and any known copolymerization method can be used. It is preferable to use a solution polymerization method in which polymerization is carried out in an organic solvent in the presence of a polymerization initiator.

[0023] Examples of organic solvents used in the solution polymerization method include aromatic solvents such as toluene, xylene, and high-boiling aromatic hydrocarbons; ester solvents such as ethyl acetate, butyl acetate, 3-methoxybutyl acetate, ethylene glycol ethyl ether acetate, and propylene glycol methyl ether acetate; ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, and methyl amyl ketone; glycol ether solvents such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, ethylene glycol monobutyl ether, and propylene glycol monomethyl ether; alcohol organic solvents such as methanol, ethanol, isopropanol, n-butanol, and isobutanol; propyl propionate, butyl propionate, and ethoxyethyl propionate. Commercially available high-boiling aromatic hydrocarbons include, for example, "Swasol 1000" (trade name, manufactured by Cosmo Oil Co., Ltd., a high-boiling petroleum solvent).

[0024] The organic solvents can be used alone or in combination of two or more. When the acrylic polyol (A) having an alkoxysilyl group has a high hydroxyl value, it is preferable to use a high-boiling ester solvent or ketone solvent as the organic solvent from the viewpoint of resin solubility. Furthermore, a high-boiling aromatic solvent can be used in combination with a high-boiling ester solvent or ketone solvent.

[0025] Examples of polymerization initiators that can be used in copolymerizing the acrylic polyol (A) having an alkoxysilyl group include known radical polymerization initiators such as 2,2'-azobisisobutyronitrile, benzoyl peroxide, 2,2-di(t-amylperoxy)butane, di-t-butyl peroxide, di-t-amyl peroxide, t-butyl peroctoate, 2,2'-azobis(2-methylbutyronitrile), etc. The acrylic polyol (A) having an alkoxysilyl group may be composed of one type of copolymer or two or more types of copolymers.

[0026] The hydroxyl value of the acrylic polyol (A) having an alkoxysilyl group is preferably within the range of 120 to 200 mgKOH / g, more preferably 130 to 200 mgKOH / g, and even more preferably 140 to 200 mgKOH / g, from the viewpoint of stain removal properties.

[0027] The weight average molecular weight of the acrylic polyol (A) having an alkoxysilyl group is preferably within the range of 5,000 to 30,000, more preferably 5,000 to 20,000, and even more preferably 6,000 to 15,000, from the viewpoints of stain removability, scratch resistance, transparency, and the like.

[0028] In this specification, the weight average molecular weight and number average molecular weight are values ​​calculated from a chromatogram measured by gel permeation chromatography using the molecular weight of standard polystyrene as a reference. The gel permeation chromatograph used was "HLC8120GPC" (manufactured by Tosoh Corporation). Four columns, "TSKgel G-4000HXL," "TSKgel G-3000HXL," "TSKgel G-2500HXL," and "TSKgel G-2000HXL" (all trade names, manufactured by Tosoh Corporation), were used. The measurement was performed under the following conditions: mobile phase: tetrahydrofuran, measurement temperature: 40°C, flow rate: 1 mL / min, and detector: RI.

[0029] The glass transition temperature of the acrylic polyol (A) having an alkoxysilyl group is preferably within the range of -30°C to 50°C, more preferably -10°C to 40°C, from the viewpoints of stain removability, scratch resistance, smoothness, etc.

[0030] In the present invention, the glass transition temperature Tg is a value calculated by the following formula: 1 / Tg(K)=W1 / T1+W2 / T2+...Wn / Tn Tg(°C)=Tg(K)-273 In the formula, W1, W2,...Wn are the mass fractions of each monomer, and T1, T2,...Tn are the glass transition temperatures Tg(K) of the homopolymers of each monomer.

[0031] The glass transition temperatures of the homopolymers of each monomer are values ​​according to "POLYMER HANDBOOK Fourth Edition," edited by J. Brandrup, E. h. Immergut, and E. A. Grulke (1999). The glass transition temperatures of monomers not described in the literature are values ​​obtained by synthesizing a homopolymer of the monomer so that the weight-average molecular weight is 50,000 and measuring the glass transition temperature using a Seiko Instruments DSC220U (differential scanning calorimeter). The measurement was performed by weighing out a predetermined amount of 50 mg of sample onto a dedicated sample dish, drying it at 130°C for 3 hours, and then heating it in an inert gas atmosphere from -50°C to 150°C at a rate of 10°C / min, and reading the temperature at the inflection point of the obtained heat change curve.

[0032] [Polyisocyanate Compound (B)] The coating material kit of the present invention contains a polyisocyanate compound (B) as a curing agent component. The polyisocyanate compound (B) in the present invention is a compound having two or more isocyanate groups in one molecule. Examples of the polyisocyanate compound (B) include aliphatic polyisocyanates, alicyclic polyisocyanates, araliphatic polyisocyanates, aromatic polyisocyanates, and derivatives of these polyisocyanates.

[0033] Examples of the aliphatic polyisocyanate include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4 or 2,2,4-trimethylhexamethylene diisocyanate, dimer acid diisocyanate, methyl 2,6-diisocyanatohexanoate (common name: methyl 2,6-diisocyanatohexanoate), and the like. aliphatic diisocyanates such as 2-isocyanatoethyl 2,6-diisocyanatohexanoate, 1,6-diisocyanato-3-isocyanatomethylhexane, 1,4,8-triisocyanatooctane, 1,6,11-triisocyanatoundecane, 1,8-diisocyanato-4-isocyanatomethyloctane, 1,3,6-triisocyanatohexane, and 2,5,7-trimethyl-1,8-diisocyanato-5-isocyanatomethyloctane.

[0034] Examples of the alicyclic polyisocyanate include 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diisocyanate), 4-methyl-1,3-cyclohexylene diisocyanate (common name: hydrogenated TDI), 2-methyl-1,3-cyclohexylene diisocyanate, ... alicyclic diisocyanates such as 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane (common name: hydrogenated xylylene diisocyanate) or a mixture thereof, methylenebis(4,1-cyclohexanediyl)diisocyanate (common name: hydrogenated MDI), and norbornane diisocyanate; 1,3,5-triisocyanatocyclohexane, 1,3,5-trimethylisocyanatocyclohexane, 2-(3-isocyanatopropyl )-2,5-di(isocyanatomethyl)-bicyclo(2.2.1)heptane, 2-(3-isocyanatopropyl)-2,6-di(isocyanatomethyl)-bicyclo(2.2.1)heptane, 3-(3-isocyanatopropyl)-2,5-di(isocyanatomethyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-3-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 6-(2 alicyclic triisocyanates such as 2-isocyanatoethyl-2-isocyanatomethyl-3-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, and 6-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane.

[0035] Examples of the araliphatic polyisocyanate include araliphatic diisocyanates such as methylenebis(4,1-phenylene)diisocyanate (common name: MDI), 1,3- or 1,4-xylylene diisocyanate or a mixture thereof, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene (common name: tetramethylxylylene diisocyanate) or a mixture thereof; and araliphatic triisocyanates such as 1,3,5-triisocyanatomethylbenzene.

[0036] Examples of the aromatic polyisocyanate include aromatic diisocyanates such as m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 2,4-tolylene diisocyanate (common name: 2,4-TDI) or 2,6-tolylene diisocyanate (common name: 2,6-TDI) or mixtures thereof, 4,4'-toluidine diisocyanate, and 4,4'-diphenyl ether diisocyanate; aromatic triisocyanates such as triphenylmethane-4,4',4''-triisocyanate, 1,3,5-triisocyanatobenzene, and 2,4,6-triisocyanatotoluene; and aromatic tetraisocyanates such as 4,4'-diphenylmethane-2,2',5,5'-tetraisocyanate.

[0037] Furthermore, examples of derivatives of the polyisocyanates include dimers, trimers, biurets, allophanates, uretdione, uretimine, isocyanurates, oxadiazinetrione, polymethylene polyphenyl polyisocyanate (crude MDI, polymeric MDI), crude TDI, etc. The polyisocyanates and derivatives thereof may be used alone or in combination of two or more.

[0038] In the paint kit of the present invention, the polyisocyanate compound (B) contains an isocyanurate trimer. By containing the isocyanurate trimer in the polyisocyanate compound (B), the crosslink density of the paint film formed from the thermosetting paint composition is increased, resulting in good removability.

[0039] The polyisocyanate compound (B) may be a blocked polyisocyanate compound in which the isocyanate groups in the polyisocyanate compound are blocked. Blocking can be easily achieved by mixing an unblocked polyisocyanate compound with a blocking agent. Examples of the blocking agent that can be used include phenol compounds, lactam compounds, alcohol compounds, oxime compounds, mercaptan compounds, and active methylene compounds such as dimethyl malonate and diethyl malonate. The polyisocyanate compounds may be used alone or in combination of two or more, and an unblocked polyisocyanate compound and a blocked polyisocyanate compound may also be used in combination.

[0040] The coating kit of the present invention contains the polyisocyanate compound (B) in such an amount that the equivalent ratio (NCO / OH) of the isocyanate groups in the polyisocyanate compound (B) in the curing agent to the hydroxyl groups of the hydroxyl group-containing resin in the base resin is preferably within the range of 0.5 to 2.0, and more preferably 0.6 to 1.2, from the viewpoint of the stain removability, scratch resistance, curability, etc. of the resulting coating film.

[0041] The paint kit of the present invention contains the polyisocyanate compound (B) in an amount such that the solid content of the polyisocyanate compound (B) is preferably 0.1 to 50 mass%, more preferably 5 to 45 mass%, and even more preferably 10 to 40 mass%, based on the mass of the resin solid content in the thermosetting paint composition, from the viewpoint of the stain removability, scratch resistance, curability, etc. of the resulting paint film.

[0042] [Catalyst Compound (C)] From the viewpoint of low-temperature curing, the coating kit of the present invention preferably comprises at least one catalyst compound (C) selected from amidine compounds, guanidine compounds, phosphazene compounds, and imidazole compounds. Low-temperature curing is, for example, by heating the thermosetting coating composition at 80°C for 30 minutes.

[0043] Examples of the amidine compound include 1,5-diazabicyclo[4,3,0]-nonene-5 (DBN) and derivatives thereof, 1,5-diazabicyclo[4,4,0]-decene-5 and derivatives thereof, 1,8-diazabicyclo[5,4,0]-undecene-7 (DBU) and derivatives thereof, 5-hydroxypropyl-1,8-diazabicyclo[5,4,0]-undecene-7 and derivatives thereof, and 5-dibutylamino-1,8-diazabicyclo[5,4,0]-undecene-7 and derivatives thereof.

[0044] Examples of the guanidine compound include 1-phenylguanidine, 1,3-diphenylguanidine, 1,3-dimethylguanidine, and 1,1,3,3-tetramethylguanidine (TMG).

[0045] Examples of the phosphazene compound include tert-butylimino-tris(dimethylamino)phosphorane and derivatives thereof, tert-butylimino-tri(pyrrolidino)phosphorane and derivatives thereof, 1-tert-octyl-4,4,4-tris(dimethylamino)-2,2-bis[tris(dimethylamino)phosphoranylideneamino]-2λ5,4λ5-catenadi(phosphazene) and derivatives thereof, and the like.

[0046] Examples of the imidazole compound include 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, and 1-cyanoethyl-2-phenylimidazole.

[0047] The catalyst compound (C) may be used alone or in combination of two or more. The catalyst compound (C) preferably contains an amidine compound, and more preferably contains 1,8-diazabicyclo[5,4,0]-undecene-7-ene (DBU) and / or a derivative thereof.

[0048] The catalyst compound (C) is preferably contained in an amount of 0.01 to 10 mass %, more preferably 0.1 to 8 mass %, and even more preferably 0.2 to 6 mass %, based on the mass of the resin solid content contained in the base resin.

[0049] [Hydroxyl-containing resin-modified silicone (D)] The paint kit of the present invention preferably includes a hydroxyl-containing resin-modified silicone (D). A coating film obtained from a thermosetting paint composition containing the hydroxyl-containing resin-modified silicone (D) repels ink and makes it difficult for graffiti to adhere, improving so-called repellency.

[0050] When the coating material kit of the present invention contains a silicone (D) modified with a hydroxyl group-containing resin, the silicone (D) is contained in an amount of preferably 0.01 to 20 mass %, more preferably 0.1 to 15 mass %, and even more preferably 1 to 10 mass %, based on the mass of the resin solids contained in the main resin.

[0051] The hydroxyl value of the silicone (D) modified with the hydroxyl-containing resin is preferably from 10 to 200 mgKOH / g, and more preferably from 20 to 150 mgKOH / g.

[0052] The number average molecular weight of the silicone (D) modified with the hydroxyl group-containing resin is preferably in the range of 1,000 to 100,000, more preferably 3,000 to 50,000.

[0053] Commercially available products of the silicone (D) modified with the hydroxyl group-containing resin include "X-22-4952" and "KF-6123" (trade names, manufactured by Shin-Etsu Chemical Co., Ltd.), which contain a polyether structure in the polymer structure; "BYK-370," "BYK-375," "BYK-377," and "BYK-SILCLEAN 3720" (trade names, manufactured by BYK Japan), which contain a polyester structure in the polymer structure; and "BYK-SILCLEAN 3700" (trade name, manufactured by BYK Japan), "ZX-028-G" (trade name, manufactured by T&K TOKA), and "Simac US-270" (trade name, manufactured by Toagosei Co., Ltd.), which contain an acrylic structure in the polymer structure.

[0054] [Organic solvent-dispersed colloidal silica (E)] The coating kit of the present invention preferably comprises organic solvent-dispersed colloidal silica (E). When the thermosetting coating composition contains organic solvent-dispersed colloidal silica (E), the coating film forms a highly crosslinked phase in the surface layer, improving the contamination resistance against contaminating liquids and the abrasion resistance.

[0055] The organic solvent-dispersed colloidal silica (E) is a stably dispersed silica particle having a particle size of about 5 to 120 nm in an organic solvent such as an alcohol, glycol, or ether. Commercially available products of the organic solvent-dispersed colloidal silica (E) include "SNOWTEX MPA-ST," "SNOWTEX IPA-ST," "SNOWTEX IPA-ST-UP," "SNOWTEX IPA-ST-ZL," "SNOWTEX EG-ST," "SNOWTEX NPC-ST-30," "SNOWTEX DMAC-ST," "SNOWTEX MEK-ST," "SNOWTEX MEK-ST-UP," "SNOWTEX MEK-ST-L," "SNOWTEX MIBK-ST," "SNOWTEX XBA-ST," "SNOWTEX PMA-ST," and "SNOWTEX PGM-ST" (all of which are trade names, manufactured by Nissan Chemical Industries, Ltd.), "NANOBYK-3650," "NANOBYK-3651," and "NANOBYK-3652" (all of which are trade names, manufactured by BYK Japan), and the "OSCAL" series (trade names, manufactured by JGC Catalysts and Chemicals, Ltd.).

[0056] For stability in the paint kit, the organic solvent-dispersed colloidal silica (E) preferably has its silica surface modified with a resin. Examples of such modification methods include reacting the organic solvent-dispersed colloidal silica (E) with 3-methacryloyloxypropyltrimethoxysilane, 3-acryloyloxypropyltrimethoxysilane, 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate, 1,1-bis(acryloyloxymethyl)ethyl isocyanate, or the like. Colloidal silica coated with an acrylic resin having a polysiloxane structure, as described in WO 2021 / 131444, is particularly preferred. The organic solvent-dispersed colloidal silica (E) may be used alone or in combination of two or more types.

[0057] The average primary particle size of the organic solvent-dispersed colloidal silica (E) is preferably 5 to 100 nm, more preferably 5 to 50 nm, which makes it easier for the dispersion to exhibit improved mechanical properties and transparency when mixed with other organic materials.

[0058] In this specification, "average primary particle size" refers to the median diameter (d50) of a volume-based particle size distribution, and the volume-based particle size distribution is measured by a laser diffraction / scattering method. In the present invention, the volume-based particle size distribution of the dispersion is measured using a laser diffraction / scattering particle size distribution analyzer "Microtrac NT3300" (trade name, manufactured by Nikkiso Co., Ltd.). In this case, the sample concentration is adjusted so as to fall within a predetermined transmittance range set in the instrument.

[0059] When the coating kit of the present invention comprises the organic solvent-dispersed colloidal silica (E), the organic solvent-dispersed colloidal silica (E) is contained in the thermosetting coating composition in an amount of preferably 0.1 to 50 mass %, more preferably 0.5 to 40 mass %, and even more preferably 1 to 30 mass %, based on the mass of the resin solid content contained in the main component.

[0060] [Thermosetting coating composition] The coating kit of the present invention is a multi-component coating composition containing a base agent and a curing agent. In the coating kit, the base agent and the curing agent are separate, and a thermosetting coating composition is obtained by mixing the base agent and the curing agent. The base agent contains the aforementioned acrylic polyol (A) having an alkoxysilyl group. The curing agent contains the aforementioned polyisocyanate compound (B). The thermosetting coating composition contains the acrylic polyol (A) having an alkoxysilyl group derived from the base agent and the polyisocyanate compound (B) derived from the curing agent.

[0061] At least one of the base agent and / or curing agent may further contain an organic solvent. Examples of the organic solvent include ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; esters such as ethyl acetate, butyl acetate, methyl benzoate, ethyl ethoxypropionate, ethyl propionate, and methyl propionate; ethers such as tetrahydrofuran, dioxane, and dimethoxyethane; glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and 3-methoxybutyl acetate; aromatic hydrocarbons; and aliphatic hydrocarbons. These may be used alone or in combination of two or more. Furthermore, when organic solvents are used in both the base agent and the curing agent, the organic solvent for the base agent and the organic solvent for the curing agent may be the same or different. The organic solvents may be used in appropriate combinations depending on the purpose, such as adjusting the viscosity or the coatability.

[0062] When the coating material kit of the present invention includes the aforementioned catalyst compound (C), the aforementioned catalyst compound (C) may be contained in either the main agent or the curing agent, or in both the main agent and the curing agent, or may be contained in a third component different from the main agent and the curing agent, but from the viewpoint of storage stability and workability, it may also be contained in a third component different from the main agent and the curing agent.

[0063] When the paint kit of the present invention includes the aforementioned hydroxyl group-containing resin-modified silicone (D), the hydroxyl group-containing resin-modified silicone (D) is preferably contained in the main component or a third component different from the main component and the curing agent from the standpoint of storage stability, and more preferably contained in the main component from the standpoint of workability.

[0064] When the coating material kit of the present invention includes the above-mentioned organic solvent-dispersed colloidal silica (E), the organic solvent-dispersed colloidal silica (E) is preferably contained in the main component or a third component different from the main component and the curing agent from the viewpoint of storage stability, and more preferably contained in the main component from the viewpoint of workability.

[0065] The paint kit (base and / or curing agent) of the present invention may further comprise, either alone or in combination of two or more, conventional paint additives such as resins other than the acrylic polyol (A) having an alkoxysilyl group, pigments, ultraviolet absorbers (e.g., benzotriazole-based absorbers, triazine-based absorbers, salicylic acid derivative-based absorbers, benzophenone-based absorbers, etc.), light stabilizers (e.g., hindered piperidines, etc.), dehydrating agents, thickeners, antifoamers, plasticizers, surface conditioners, and anti-settling agents.

[0066] Examples of resins other than the acrylic polyol (A) having an alkoxysilyl group include acrylic resins (excluding those containing an alkoxysilyl group and a hydroxyl group), polyester resins, alkyd resins, urethane resins, fluororesins, epoxy resins, silicone resins, polyether resins, acrylic silicone resins, and vinyl acetate veova resins.

[0067] When the coating kit (main agent and / or curing agent) of the present invention contains the above-mentioned ultraviolet absorber, the blending amount of the ultraviolet absorber is preferably an amount within the range of 0.1 to 10 parts by mass, more preferably 0.2 to 5 parts by mass, and even more preferably 0.3 to 2 parts by mass, based on 100 parts by mass of the total resin solids in the thermosetting coating composition.

[0068] When the paint kit of the present invention contains the above-mentioned light stabilizer, the blending amount of the light stabilizer is preferably an amount within the range of 0.1 to 10 parts by mass, more preferably 0.2 to 5 parts by mass, and even more preferably 0.3 to 2 parts by mass, based on 100 parts by mass of the total resin solids in the thermosetting paint composition.

[0069] Examples of the dehydrating agent include metal alkoxides such as aluminum isopropylate, aluminum sec-butylate, tetraisopropyl titanate, tetra-normal butyl titanate, zirconium normal butylate, ethyl silicate, and vinyltrimethoxysilane; organic alkoxy compounds such as trimethyl orthoformate, triethyl orthoformate, trimethyl orthoacetate, triethyl orthoacetate, triisopropyl orthoacetate, and dimethoxypropane; and monofunctional isocyanates such as "Additive TI" (trade name, manufactured by Sumika Bayer Urethane Co., Ltd.), and these can be used alone or in combination of two or more.

[0070] When the coating kit (base agent and / or curing agent) of the present invention contains the dehydrating agent, the amount of the dehydrating agent blended is preferably 0.01 to 15 parts by mass, and more preferably 0.1 to 8 parts by mass, based on 100 parts by mass of the total resin solids in the thermosetting coating composition.

[0071] The solids content of the coating kit of the present invention and the thermosetting coating composition obtained from the coating kit is not particularly limited. For example, in terms of the smoothness of the cured coating film and the shortened drying time, it is preferable to adjust the solids content of the coating kit and the thermosetting coating composition appropriately using a solvent such as the organic solvent described above so that the viscosity of the thermosetting coating composition at 20°C according to Ford Cup No. 4 is in the range of 15 to 60 seconds.

[0072] In this specification, the term "solid content" refers to the residue remaining after removing volatile components, and the residue may be solid or liquid at room temperature. The solid content mass can be calculated by multiplying the sample mass before drying by the solid content percentage, which is the ratio of the amount of remaining material after drying to the mass before drying.

[0073] The paint kit of the present invention is a coating film formed by applying the thermosetting paint composition to a substrate, heating and curing the composition at 80°C for 30 minutes, and then leaving the coating film to stand for 1 hour. The minimum storage modulus E' of the coating film in the range of 40 to 200°C is min But 2.6 x 10 7 The minimum storage modulus E' of the coating film prepared under these conditions is 0.05 Pa or more. min is 2.6 x 10 7 When the storage modulus of the coating film is 100 Pa or more, the coating film has a high crosslink density even when cured at a low temperature, so that inks used for graffiti and the like do not easily penetrate into the coating film, and the coating film has high removability. min is 3.6 x 10 7 Pa or more, and 7 From the viewpoint of the cracking resistance of the coating film, the coating kit of the present invention is characterized in that the coating film formed by applying the thermosetting coating composition to an object to be coated, heating and curing at 80°C for 30 minutes, and then leaving to stand for 1 hour has a minimum storage modulus E' in the range of 40 to 200°C. min But 1.0 x 10 9 It is preferable that the pressure is 0.05 Pa or less.

[0074] In this specification, the method for preparing the coating film used to measure the storage modulus is as follows: 1. A thermosetting coating composition obtained from a coating kit is applied to a polypropylene plate (substrate) so that the cured film thickness is 40 μm, and the coating is dried at 80° C. for 30 minutes and left to stand for 1 hour to form a cured coating film. 2. The cured coating film is cut into strips 20 mm long and 5 mm wide, and peeled off from the polypropylene plate. The resulting strip-shaped free coating film is used as a sample.

[0075] In this specification, the storage modulus was measured using an FT rheology spectrometer "Rheogel E-400" (manufactured by UBM Co., Ltd.) The free coating film prepared by the above-mentioned preparation method was subjected to dynamic viscoelasticity measurement under conditions of a frequency of 11 Hz, a temperature rise rate of 4°C / min, and a temperature range of room temperature to 200°C, and the minimum value E' of the storage modulus in the range of 40 to 200°C was measured. min By leaving the coating film standing for a predetermined time, such as one hour, the crosslinking reaction is completed to a certain extent, and therefore further crosslinking reaction is unlikely to occur even when the measurement is performed under high temperature conditions.

[0076] [Method for forming a coating film using a thermosetting coating composition] The method for forming a coating film using a thermosetting coating composition obtained from the coating kit of the present invention comprises the following steps: A coating film forming step of applying the thermosetting coating composition to an object to be coated to form a wet coating film A step of heat-curing the wet coating film in a temperature range of 50°C or higher and 120°C or lower

[0077] The substrate to which the thermosetting coating composition is applied is not particularly limited. Examples of components constituting the substrate include cold-rolled steel sheets, galvanized steel sheets, zinc alloy-plated steel sheets, stainless steel sheets, tin-plated steel sheets, and other steel sheets, aluminum sheets, aluminum alloy sheets, and other metal substrates; and various plastic materials. The component constituting the substrate (particularly in the case of a car body) may be a metal substrate whose surface has been subjected to a surface treatment such as phosphate treatment, chromate treatment, or complex oxide treatment. Furthermore, the component constituting the substrate (particularly in the case of a car body) may be a metal substrate on which an undercoat coating film such as various electrodeposition paints has been formed, or a metal substrate on which the undercoat coating film and intermediate coating film have been formed, or a metal substrate on which an undercoat coating film, intermediate coating film, and basecoat coating film have been formed, or a metal substrate on which an undercoat coating film, intermediate coating film, basecoat coating film, and clearcoat coating film have been formed.

[0078] Specific examples of the substrate include those having the above-mentioned components, such as vehicle bodies (e.g., automobiles, trucks, motorcycles, buses, railroad vehicles, two-wheeled vehicles, etc.), industrial machinery, construction machinery, ship hulls, building materials, housing equipment, etc., and parts thereof. The thermosetting coating composition has sufficient removability even when cured at low temperatures, so it can be used even when the substrate is a railroad vehicle, building material, housing equipment, etc. By applying the thermosetting coating composition to the substrate, a coated article on which a coating film is formed can be obtained.

[0079] The application method of the thermosetting coating composition is not particularly limited, but examples include air spray coating, airless spray coating, rotary atomization coating, curtain coating, and the like, and a wet coating film can be formed by the above coating methods. In the above coating methods, electrostatic application may be performed as needed. Of these, air spray coating, airless spray coating, and rotary atomization coating are particularly preferred. The amount of the thermosetting coating composition applied is usually preferably an amount that results in a cured film thickness of 10 to 100 μm.

[0080] The wet coating film formed by applying the thermosetting coating composition to the substrate is cured by heating the wet coating film. Heating of the wet coating film can be carried out by known heating means, for example, a drying oven such as a hot air oven, an electric oven, or an infrared induction heating oven. The heating temperature is not particularly limited, but from the viewpoints of production efficiency and energy saving, heating is preferably performed at 50°C or higher and 120°C or lower, more preferably at 50°C or higher and 100°C or lower, and even more preferably at a low temperature of 50°C or higher and 80°C or lower. The heating time is not particularly limited, but from the viewpoints of production efficiency and energy saving, it is preferably within the range of 10 to 60 minutes, and more preferably 15 to 30 minutes.

[0081] Furthermore, the heat-cured coating film may be further subjected to room temperature curing or heat curing (after-cure) as necessary. When after-cure is performed, it is preferable to dry at room temperature for at least one day or at 30 to 50°C for at least 30 minutes, but from the viewpoint of production efficiency and energy saving, it is more preferable not to perform after-cure. The thermosetting coating composition of the present invention has sufficient removability even without after-cure. The thermosetting coating composition of the present invention can be used as a top clear coat coating composition.

[0082] The present invention will be explained in more detail below with reference to Production Examples, Examples, and Comparative Examples. However, the present invention is not limited to these Examples. In each Example, "parts" and "%" are by mass unless otherwise specified. Furthermore, the film thickness of the coating film is based on the cured coating film.

[0083] Production Example 1 (Production of Alkoxysilyl Group-Containing Acrylic Polyol) A reaction vessel equipped with a thermometer, a thermostat, a stirrer, a reflux condenser, a nitrogen inlet tube, and a dropping device was charged with 30 parts of "Swasol 1000" (trade name, aromatic organic solvent, manufactured by Cosmo Oil Co., Ltd.) and 10 parts of n-butanol. The charged liquid was stirred at 125°C while blowing nitrogen gas into the reaction vessel, and a monomer mixture consisting of 30 parts of γ-methacryloxypropyltrimethoxysilane, 35 parts of 2-hydroxypropyl acrylate, 20 parts of styrene, 15 parts of isobutyl methacrylate, and 3 parts of 2,2'-azobis(2-methylbutyronitrile) (polymerization initiator) was added dropwise to the charged liquid at a uniform rate over 4 hours. Next, the charge liquid was aged for 30 minutes at 125 ° C., and then a solution consisting of 0.5 parts of 2,2'-azobis(2-methylbutyronitrile) and 5.0 parts of "Swasol 1000" was added dropwise to the charge liquid at a uniform rate over 1 hour. Thereafter, the charge liquid was aged for 1 hour at 125 ° C., and then cooled. The charge liquid was further diluted with isobutyl acetate to obtain an alkoxysilyl group-containing acrylic polyol (A-1) solution with a solids concentration of 60% by mass. The alkoxysilyl group content of the obtained alkoxysilyl group-containing acrylic polyol (A-1) was 1.2 mmol / g, a hydroxyl value of 151 mg KOH / g, a weight average molecular weight of 7,000, and a glass transition temperature of 16.6 ° C.

[0084] [Production Example 2 (Production of Alkoxysilyl Group-Free Acrylic Polyol)] A reaction vessel equipped with a thermometer, thermostat, stirrer, reflux condenser, nitrogen inlet tube, and dropping device was charged with 30 parts of "Swasol 1000" (trade name, aromatic organic solvent, manufactured by Cosmo Oil Co., Ltd.) and 10 parts of n-butanol. The charge liquid was stirred at 125°C while nitrogen gas was blown into the reaction vessel, and a monomer mixture consisting of 35 parts of 2-hydroxypropyl acrylate, 20 parts of styrene, 45 parts of isobutyl methacrylate, and 3 parts of 2,2'-azobis(2-methylbutyronitrile) (polymerization initiator) was added dropwise to the charge liquid at a uniform rate over 4 hours. The charge liquid was then aged at 125°C for 30 minutes, after which a solution consisting of 0.5 parts of 2,2'-azobis(2-methylbutyronitrile) and 5.0 parts of "Swasol 1000" was added dropwise to the charge liquid at a uniform rate over 1 hour. The resulting solution was aged at 125°C for 1 hour, cooled, and diluted with additional isobutyl acetate to obtain an acrylic polyol (A-2) solution with a solids concentration of 60% by mass. The resulting hydroxyl-containing acrylic resin (A-2) had a hydroxyl value of 151 mgKOH / g, a weight-average molecular weight of 7,000, and a glass transition temperature of 36.4°C.

[0085] Production Example 3 (Production of Acrylic Resin-Coated Colloidal Silica) 333 parts (100 parts solids content) of "PGM-ST" (trade name, manufactured by Nissan Chemical Industries, Ltd., silica average primary particle size: 15 nm, silica concentration: 30% by mass, dispersion medium: propylene glycol monomethyl ether) and 10 parts of deionized water were placed in a separable flask equipped with a reflux condenser, a thermometer, and a stirrer, and then 10 parts of "KBM-503" (trade name, manufactured by Shin-Etsu Chemical Co., Ltd., γ-methacryloyloxypropyltrimethoxysilane) was added. The resulting mixture was stirred at 80°C for 2 hours to carry out a dehydration condensation reaction. Thereafter, 0.03 parts of tetra-n-butylammonium fluoride was added to the mixture, and the mixture was allowed to react for another 1 hour with stirring. After the reaction was completed, 30 parts of propylene glycol monomethyl ether was added to the charged liquid, and then volatile components were distilled off from the charged liquid under reduced pressure to obtain a polymerizable unsaturated group-containing colloidal silica dispersion having a solids content of 40% of surface-modified silica particles.

[0086] A separable flask equipped with a reflux condenser, a thermometer, a stirrer, and a nitrogen gas inlet was charged with 104.5 parts of propylene glycol monomethyl ether and 8.5 parts of trimethyl orthoacetate, and the charged liquid was heated to 100°C under nitrogen gas flow. After the charged liquid reached 100°C, 375 parts (solids content: 150 parts) of the polymerizable unsaturated group-containing colloidal silica dispersion and a monomer mixture consisting of 1 part of "X-22-174ASX" (trade name, manufactured by Shin-Etsu Silicones Co., Ltd.), 30 parts of γ-methacryloxypropyltrimethoxysilane, 35 parts of 2-hydroxypropyl acrylate, 20 parts of styrene, 14 parts of isobutyl methacrylate, 3 parts of 2,2'-azobis(2-methylbutyronitrile) (polymerization initiator), and 23.5 parts of trimethyl orthoacetate were added dropwise to the charged liquid over 2 hours. Next, the charge liquid was aged at 100°C for 1 hour, and then a mixed solution of 1 part of 2,2'-azobis(2-methylbutyronitrile) (polymerization initiator) and 19.5 parts of propylene glycol monomethyl ether was added to the charge liquid, and the charge liquid was further aged for 2 hours. The conversion rate calculated from the nonvolatile content was 99%. Thereafter, propylene glycol monomethyl ether was added to the charge liquid, and the solvent was replaced by azeotropic distillation under reduced pressure, yielding an acrylic resin-coated colloidal silica dispersion (E-1) with a measured nonvolatile content of 40%.

[0087] Example 1 A base material was prepared by blending 100 parts (solid content 60 parts) of the alkoxysilyl group-containing acrylic polyol (A-1) obtained in Production Example 1, 4.0 parts (solid content 1.0 part) of "BYK-SILCLEAN3700" (trade name, manufactured by BYK Japan KK, silicone (D) modified with a hydroxyl group-containing resin, active ingredient 25%), 25 parts (solid content 10 parts) of the acrylic resin-coated colloidal silica dispersion (E-1) obtained in Production Example 3, 5.0 parts of trimethyl orthoacetate (dehydrating agent), and 32 parts of butyl acetate (organic solvent). The mixture was stirred until uniform.

[0088] In a separate container, 35.5 parts of polyisocyanate compound (B) "Sumidur N3300" (trade name, manufactured by Sumika Covestro Urethane Co., Ltd., isocyanurate ring adduct of hexamethylene diisocyanate, solid content 100%) and 17.5 parts of diethylene glycol monoethyl ether acetate were blended and mixed until uniform, to prepare a curing agent.

[0089] 166 parts of the base agent, 53 parts of the curing agent, and 1.5 parts of catalyst (C) "U-CAT SA102" (trade name, manufactured by San-Apro Co., Ltd., curing catalyst, DBU-octylate salt, active ingredient 100%) were mixed, and butyl acetate was added thereto so that the paint solids content was 40%, followed by stirring, to obtain a thermosetting paint composition (X-1).

[0090] [Examples 2 to 12, Comparative Examples 1 to 4] Thermosetting coating compositions (X-2) to (X-16) were obtained in the same manner as in Example 1, except that the formulations shown in Tables 1 and 2 were used.

[0091]

[0092]

[0093] Note that (Note 1) to (Note 3) in Tables 1 and 2 are as follows: (Note 1) "NANOBYK-3652": Trade name, manufactured by BYK Japan, organic solvent-dispersed colloidal silica, solid content 31%, silica content 25% (Note 2) "NACURE 4167": Trade name, manufactured by KING INDUSTRIES, triethylamine salt of alkyl phosphate, curing catalyst, active ingredient 25% (Note 3) "CAT-AC": Trade name, manufactured by Shin-Etsu Silicones, aluminum chelate, curing catalyst, active ingredient 50%.

[0094] [Measurement of Storage Modulus] The storage modulus was measured according to the method described herein.

[0095] [Preparation of Test Plates for Evaluation Tests] The viscosity of each of the thermosetting coating compositions (X-1) to (X-16) was adjusted to 25 seconds at 20°C using a Ford Cup No. 4 by adding butyl acetate, and test plates were prepared for each of them as follows. Each of the thermosetting coating compositions (X-1) to (X-16) was applied to the following base coat within 10 minutes after mixing the base resin, curing agent, and catalyst (C).

[0096] On a 0.8 mm thick dull steel plate that had been subjected to a zinc phosphate conversion treatment, "Elecron GT-10" (trade name, manufactured by Kansai Paint Co., Ltd., a thermosetting epoxy resin-based cationic electrodeposition paint) was electrodeposited to a film thickness of 20 μm to form an uncured electrodeposition coating film, which was then heated and cured at 170°C for 30 minutes to form an electrodeposition coating film. A water-based base coat "WBC713T" (trade name, manufactured by Kansai Paint Co., Ltd., an acrylic-melamine resin-based automotive topcoat base coat paint, white color) was applied to the above electrodeposition coating film to a dry film thickness of 15 μm to form an uncured base coat coating film. The uncured base coat coating film was left at room temperature for 5 minutes, preheated at 80°C for 10 minutes, and then heat-cured at 140°C for 30 minutes to form a cured base coat coating film. The cured base coat film was then coated with each of the thermosetting coating compositions prepared and adjusted in the above Examples and Comparative Examples to a thickness of 35 μm to form an uncured coating film. The uncured coating film was then left at room temperature for 10 minutes, then heated to 80°C for 30 minutes to cure, and then left to stand for 1 hour to form a coating film, yielding a test panel. Each of the resulting test panels was left to stand at room temperature for 7 days before undergoing the following evaluation tests. The evaluation results are shown in Tables 1 and 2.

[0097] [Removability (marker)] Each test plate was stained by drawing a 10 mm × 10 mm square with an oil-based marker. Six types of oil-based markers were used for staining: "Edding 850 permanent marker-red" (product name, manufactured by Edding Co., Ltd., red marker), "Edding 750 paint marker-black" (product name, manufactured by Edding Co., Ltd., black marker), "Camlin Kokuyo Permanent Marker blue" (product name, manufactured by Camlin Co., Ltd., blue marker), "Camlin Kokuyo Permanent Marker red" (product name, manufactured by Camlin Co., Ltd., red marker), "Magic Ink Extra Thick Red" (product name, manufactured by Teranishi Chemical Industry Co., Ltd., red marker), and "Magic Ink Extra Thick Black" (product name, manufactured by Teranishi Chemical Industry Co., Ltd., black marker). After staining with each marker, the area was left to stand for 5 minutes, then "Strong Graffiti Remover Spray" (trade name, graffiti remover, manufactured by Asahipen Co., Ltd.) was sprayed evenly over the area, and the stained area was wiped off with a dry Kimwipe (trade name). This operation constituted one cycle, and the same operation was carried out for two more cycles on the same area stained in the first cycle. After three cycles were completed, the time left for the staining with the marker was increased to 24 hours, and one similar operation was carried out again.

[0098] After the above-mentioned staining / removal work (three 5-minute standing cycles and one 24-hour standing cycle), the stained / removed area was observed and evaluated according to the following criteria. A and B are acceptable levels, and it can be said that the marker stains were easily and cleanly removed. A: No color remains B: Slight color remains C: Significant color remains and / or the coating is dissolved by the graffiti remover

[0099] [Removability (other than marker)] A simulated stained liquid was prepared by mixing a calcined Kanto loam product (JIS test powder 1, type 7) specified in JIS Z8901:2006 with gear oil at a weight ratio of 1:1. A curry stained liquid was prepared by mixing Red Can Curry Powder (manufactured by S&B Foods Co., Ltd.) with Nissin Canola Oil (edible rapeseed oil, manufactured by The Nissin Oillio Group, Ltd.) at a weight ratio of 1:1. A coffee stained liquid was prepared by mixing Nescafé Gold Blend (regular soluble coffee powder, manufactured by Nestle Japan, Inc.) with water at a weight ratio of 1:5.

[0100] Three cotton pieces cut into 30 mm squares were placed on the test plate, and 5 ml of each staining solution was dropped onto each cotton piece, allowing sufficient contact between the cotton and the coating surface of the test plate. The entire contact surface was then covered with a 60 mm diameter polypropylene lid and secured in place with masking tape to prevent the staining solution from volatilizing. The covered test plate was left standing at 50°C for 24 hours, after which the lid and cotton were removed from the test plate, and the test surface was thoroughly washed with tap water and new cotton.

[0101] The stain resistance against each staining liquid was evaluated on a three-point scale based on the appearance of the coating surface after cleaning. A and B are acceptable levels, and it can be said that staining from each staining liquid was easily and cleanly removed. A: No color remains. B: Slight color remains. C: Significant color remains.

[0102] [Repellency] A 10 mm x 10 mm square was drawn on each test plate with "Edding 850 permanent marker-red" (product name, red marker, manufactured by Edding Co.) to stain it, and the ink repellency was evaluated. A and B are acceptable levels. A: The coated surface repels ink, and 50% or more of the coated surface is visible. B: The coated surface repels ink slightly, and 10-50% of the coated surface is visible. C: The ink is not repelled, and the coated surface is almost invisible.

[0103] [Examples 1A and 1B] The storage modulus, removability, and repellency were evaluated in the same manner as in Example 1, except that the drying conditions were changed as shown in Table 3. The results are shown in Table 3.

[0104]

Claims

1. A paint kit for a thermosetting paint composition, comprising a base agent containing an acrylic polyol (A) having an alkoxysilyl group and a curing agent containing a polyisocyanate compound (B) containing an isocyanurate trimer, wherein the thermosetting paint composition obtained from the paint kit is heat-cured at 80°C for 30 minutes and allowed to stand for 1 hour to form a coating film having a minimum storage modulus E' in the range of 40 to 200°C. min is 2.6 x 10 7 A paint kit having a viscosity of 100 Pa or more.

2. The paint kit according to claim 1, further comprising at least one catalyst compound (C) selected from the group consisting of amidine compounds, guanidine compounds, phosphazene compounds, and imidazole compounds.

3. A paint kit according to claim 1 or 2, further comprising a silicone (D) modified with a hydroxyl-containing resin.

4. The paint kit according to any one of claims 1 to 3, further comprising an organic solvent-dispersed colloidal silica (E).

5. The paint kit according to any one of claims 1 to 4, wherein the paint film has stain resistance.

6. A thermosetting coating composition comprising a base agent containing an acrylic polyol (A) having an alkoxysilyl group and a curing agent containing a polyisocyanate compound (B) containing an isocyanurate trimer, wherein the coating film formed by heating and curing at 80°C for 30 minutes and leaving to stand for 1 hour has a minimum storage modulus E' in the range of 40 to 200°C. min is 2.6 x 10 7 A thermosetting coating composition having a viscosity of 100 Pa or more.

7. A base material for a thermosetting coating composition comprising a base material containing an acrylic polyol (A) having an alkoxysilyl group and a curing agent containing a polyisocyanate compound (B) containing an isocyanurate trimer, wherein the thermosetting coating composition is heat-cured at 80°C for 30 minutes and allowed to stand for 1 hour to form a coating film having a minimum storage modulus E' in the range of 40 to 200°C. min is 2.6 x 10 7 The base material is Pa or higher.

8. A coating film forming method comprising a coating film forming step of coating a substrate with a thermosetting coating composition obtained from a coating kit according to any one of claims 1 to 5, a thermosetting coating composition according to claim 6, or a thermosetting coating composition obtained by mixing a base agent and a curing agent according to claim 7 to form a wet coating film.

9. The method for forming a coating film according to claim 8, further comprising a step of heat-curing the wet coating film at a temperature in the range of 50°C or more and 120°C or less.

10. The method for forming a coating film according to claim 8 or 9, wherein the substrate is at least one selected from the group consisting of automobiles, industrial machinery, construction machinery, railway vehicles, ship hulls, building materials, and housing equipment, and parts thereof.

11. A coated article obtained by applying to a substrate a thermosetting coating composition obtained from a coating kit according to any one of claims 1 to 5, a thermosetting coating composition according to claim 6, or a thermosetting coating composition obtained by mixing a base agent and a curing agent according to claim 7.

Citation Information

Patent Citations

  • Coating composition for automobile and method for forming coating film

    JP2003049116A

  • Polyurethane coating composition and method for preparing coated product

    WO2019049864A1

  • Coating composition and method for forming multilayer coating film

    WO2021131444A1