Signal enhancement in immunoassays through cellulose substrate contraction
The method of coating polydopamine on a cellulose substrate and inducing a Malaprade reaction to shrink the substrate enhances the immunoassay signal, addressing the instability and cost issues of conventional methods, achieving stable and reproducible signal amplification for gold nanoparticle-based assays in on-site diagnostics.
Patent Information
- Application Number
- PCT/KR2023/007959
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-08
- Filing Date
- 2023-06-09
- Publication Date
- 2024-11-14
AI Technical Summary
Conventional post-analysis signal enhancement methods for gold nanoparticle-based immunoassays are unstable and costly, limiting their applicability and reproducibility in on-site diagnostics.
A method involving coating a conjugate with polydopamine on a cellulose substrate followed by a Malaprade reaction to shrink the substrate, enhancing the colorimetric signal by increasing the density of gold nanoparticles without increasing particle size, thus stabilizing and amplifying the signal.
The method provides a stable and cost-effective signal enhancement for immunoassays, maintaining reproducibility and amplifying the colorimetric signal, suitable for on-site diagnostics even in resource-limited environments.
Smart Images

Figure KR2023007959_14112024_PF_FP_ABST
Abstract
Description
Signal enhancement in immunoassays through shrinkage of cellulose substrates
[0001] The present invention relates to a method for increasing the signal of all kinds of immunoassays using a cellulose substrate, and more particularly, to a method for enhancing the signal by coating a conjugate in which a label is conjugated to a detector after an immunoassay with polydopamine and increasing the density of a colorimetric signal by shrinking the cellulose substrate by a malafrade reaction.
[0002] Cellulose- and gold nanoparticle-based immunoassays, such as lateral flow assays, are widely commercialized, planned, and developed worldwide. These gold nanoparticle-based immunoassays utilize the colorimetric signals generated on the surface of precious metals using nanoparticles. Their exceptional sensitivity and selectivity allow them to detect a wide range of analytes, making them highly useful for point-of-care diagnostics. Furthermore, their low cost and rapid response times have led to their widespread application in diverse fields, and they have become a dominant technology for point-of-care diagnostics, particularly in rural healthcare settings.
[0003] Paper cellulose substrate ELISA is a technique for detecting the presence of a specific substance by immobilizing an antigen or antibody of interest on a paper substrate instead of a conventional solid substrate. This technique is versatile and relatively inexpensive, making it particularly useful in resource-limited environments. Paper matrices offer several advantages, including a high surface-to-volume ratio, capillary action, and ease of use.
[0004] In recent years, the industry has focused on combining gold nanoparticle-based immunoassays with paper-cellulose-based ELISA to create next-generation point-of-care diagnostic methods. Research is also actively underway to enhance the performance of these hybrid systems by enhancing the colorimetric signal generated by gold nanoparticles. In particular, according to the National Institutes of Health (NIH), research and funding related to this area have increased rapidly since the COVID-19 pandemic.
[0005] Signal enhancement methods for gold nanoparticle-based immunoassays can be divided into two categories: pre-analytical enhancement and post-analytical enhancement. Pre-analytical enhancement includes nanoparticle expansion through enzymatic metal deposition, polymer coating, and other signal-enhancing methods. While simple in procedure, its application is significantly limited.
[0006] On the other hand, post-analytical enhancement has the advantage of being applicable to all types of biological assays that use antibodies conjugated with gold nanoparticles for staining. However, there are currently only a few post-analytical enhancement methods available (i.e., silver enhancement and gold enhancement). Furthermore, the two post-analytical signal enhancement methods mentioned above involve adsorption of precious metal ions onto gold nanoparticles used in immunoassays, thereby increasing their size. However, due to the nature of colloids, they are unstable in the surrounding environment, making it difficult to obtain reproducible results. Furthermore, they are expensive for use in point-of-care diagnostic devices.
[0007] Against this backdrop, the inventors of the present invention have completed the present invention by confirming that a signal is strengthened when a conjugate in which a label is conjugated to a detector is coated with polydopamine and a Malaprade reaction is induced to shrink a cellulose substrate, as a post-analysis signal strengthening method that is stable in the surrounding environment, inexpensive, and can be used in various ways for field diagnosis.
[0008]
[0009] [Prior Art Literature]
[0010] [Patent Document]
[0011] (Non-patent Document 1) Muhammad Sajid et al, Journal of Saudi Chemical Society, Volume 19, Issue 6, November 2015, Pages 689-705
[0012] The purpose of the present invention is to provide a method for increasing the signal of an immunoassay using a cellulose substrate. In particular, the present invention overcomes the limitations of conventional methods for increasing the signal after immunoassay, such as instability and high costs, and provides an analytical method that can effectively increase the immunoassay signal while being stable in the surrounding environment and at low cost.
[0013] In order to achieve the above purpose, the present invention provides an immunoassay method including a conjugate in which a labeling substance is conjugated to a detector,
[0014] A step of coating the detector on a cellulose substrate with polydopamine using a dopamine polymerization reaction; and
[0015] A method for enhancing an immunoassay signal is provided, characterized by including a shrinkage step of a cellulose substrate by a Malaprade reaction.
[0016] In the present invention, the Malaprade reaction is performed not for the purpose of miniaturizing the substrate, but to enhance the signal generated as a result of the immunoassay analysis. In the present invention, the step of coating the gold nanoparticles with polydopamine is not to increase the particle size as in the prior art, but rather to reduce signal loss that may occur after the Malaprade reaction, protect the gold nanoparticles, and prevent their detachment.
[0017] In the present invention, the polydopamine coating step and the shrinking step of the cellulose substrate may be performed after the immunoassay analysis results are obtained. Conventional post-analysis signal enhancement methods involve adsorbing precious metal ions onto gold nanoparticles to increase their size, which is unstable in the surrounding environment and requires high costs. Therefore, the present invention has demonstrated that signals can be enhanced and maintained reproducibly without requiring significant costs.
[0018] In the present invention, the detector may be an antibody, an aptamer, or an antibody-aptamer.
[0019] In the present invention, the labeling material may be a nanoparticle made of a material that is not easily etched by oxidation. For example, the labeling material may be a nanoparticle made of a material such as gold (Au), platinum (Pt), cerium oxide (CeO2), zinc sulfide (ZnS), or silicon oxide (SiO). Preferably, the labeling material may be a gold nanoparticle.
[0020] In the present invention, the immunoassay method may be a lateral flow assay, a vertical flow assay, or an ELISA.
[0021] In the present invention, the immunoassay method may be direct, indirect, sandwich, or competitive.
[0022] In the present invention, the cellulose substrate may be chromatography paper, cellulose acetate film, cellulose nanocrystals, cellulose-based hydrogels, bacterial cellulose, or microcrystalline cellulose.
[0023] In the present invention, the labeling material may be fixed on a cellulose substrate at a density of 0.013 to 271.152 amol / mm2.
[0024] In the present invention, shrinkage of the cellulose substrate may be achieved through cross-linking between cellulose molecules.
[0025] In the present invention, the signal enhancement of the immunoassay method may be achieved by increasing the density of the colorimetric signal of the gold nanoparticles through shrinkage of the cellulose substrate, and / or maintaining or enhancing the color development derived from the analysis result of the immunoassay method.
[0026] In the present invention, the signal enhancement of the immunoassay method may be performed for 0 to 6 hours. Preferably, it may be performed for 2 to 4 hours.
[0027] The present invention is a method for increasing a colorimetric signal after an immunoassay, and, compared to conventional post-analysis signal enhancement methods (silver enhancement, gold enhancement, etc.), uses inexpensive reagents and can stably amplify signals even under contamination and general reaction conditions.
[0028] Therefore, it can be applied in the field of on-site diagnostic devices where it is difficult to have an environment that can be created in a laboratory (e.g., precise devices such as micropipettes and an uncontaminated environment).
[0029] In particular, since anyone can easily implement the present invention, it can be implemented in tertiary medical institutions and research facilities, as well as primary medical institutions and general homes.
[0030] Figure 1 shows the chemical change of cellulose by malaprade reaction (A) and the protective coating of gold nanoparticles using internal cross-linking and polymerization of dopamine (B).
[0031] Figure 2 shows the shrinkage of the substrate due to the Malafrade reaction (A), the signal intensity enhancement of the insoluble color ink (B), the density change of the substrate using paraffin-wax microdots (C, D), the dopamine-doped gold nanoparticles on the substrate before and after the reaction (E), and the UV-visible spectral change (F) and the particle density change of the gold nanoparticles per unit surface area during the reaction time (0 to 6 hours) (G).
[0032] Figure 3 shows the results of Raman spectra (B) and FTIR spectra (C) showing the morphological changes of the fibers (A; top, normal cellulose fiber; bottom, gold-cellulose fiber) and chemical modifications observed with a scanning electron microscope during the reaction time.
[0033] Figure 4 shows polydopamine-coated nanoparticles (A), XPS spectra demonstrating the presence of Au and organic element species and the heterogeneity of AuNP distribution (B), XPS spectra of Au 4d and Au 3d shells showing peak heights attenuated by polydopamine coating (C), high-resolution XPS spectra of Au 4f shells showing reduction of gold oxide by polydopamine (D), scanning electron microscope images of gold nanoparticles immobilized on a substrate before and after the shrinkage reaction (E), and SE and BSE images contrasting gold nanoparticles immobilized under polydopamine coating (F).
[0034] Figure 5 shows the area reduction according to reaction time and temperature (A), consistency evaluation for gold nanoparticle-doped cellulose substrates with various gold nanoparticle particle numbers (B), and quantification using Boltzmann sigmoid curve (C).
[0035] Figure 6 shows the results of colorimetric analysis under different conditions of shrinkage time and particle density (A), the shrinkage pattern when the density of nanoparticles is high, medium, and low (B), the change in reliability according to various particle densities (C), and the results of colorimetric analysis according to various particle densities and shrinkage times (D).
[0036] Figure 7 shows the results of direct ELISA of human IgG and the images of the results after contraction reaction at 2 and 4 hours.
[0037] Figure 8 shows the signal enhancement mechanism based on gold nanoparticles using polydopamine coating in direct ELISA (A), a visual comparison of the direct ELISA signal in the negative control and low concentration human IgG before and after contraction (B), and graphs quantified by the red scale index (C, D, E).
[0038] The present invention relates to an immunoassay method comprising a conjugate in which a labeling substance is conjugated to a detector,
[0039] A step of coating the conjugate on a cellulose substrate with polydopamine using a dopamine polymerization reaction; and
[0040] A method for enhancing signal in an immunoassay, comprising a step of shrinking a cellulose substrate by a Malaprade reaction; more specifically, the present invention provides a method for enhancing signal after analysis in an immunoassay.
[0041] The malaprade reaction refers to a glycolysis reaction in which adjacent diols are oxidized by periodic acid or periodate to provide the corresponding carbonyl functional group. In the present invention, the malaprade reaction oxidizes cellulose fibers and cross-links them with other fibers through hemiacetal formation, thereby reducing crystallinity, resulting in fiber coiling and shrinkage of the entire substrate (see A in Fig. 1).
[0042] The above-mentioned labeling material refers to a material that emits a colorimetric signal after binding to a substance to be detected in an immunoassay. The labeling material of the present invention may be a nanoparticle made of a material that is not easily etched by oxidation. Examples of materials that are not easily etched by oxidation include gold (Au), platinum (Pt), cerium oxide (CeO2), zinc sulfide (ZnS), silicon oxide (SiO), etc., and in the examples of the present invention, gold nanoparticles (AuNP) were used.
[0043] The above labeling material can be fixed to cellulose through non-covalent bonds to the ester and hydroxyl groups of cellulose.
[0044] Cellulose substrates that can be used include chromatography paper, cellulose acetate film, cellulose nanocrystals, cellulose-based hydrogels, bacterial cellulose, or microcrystalline cellulose.
[0045] The coating of the conjugate with polydopamine of the present invention is performed prior to shrinkage of the cellulose substrate, to prevent aggregation of the conjugate due to substrate shrinkage (see B in Fig. 1). In particular, metal nanoparticles can be easily destroyed as colloids when exposed to physical and chemical changes, and since the cellulose substrate shrinkage step of the present invention includes an oxidation step using a high concentration of periodate, a fixing agent for coating the conjugate is required. Dopamine is a small hydrophilic molecule with two hydroxyl groups and one amine group, and has the property of being easily absorbed onto the surface of gold nanoparticles and cellulose fibers, so it can be used as a fixing agent and protective coating. In addition, periodate initiates not only the Malafrade reaction but also the polymerization reaction of dopamine, thereby reducing the overall steps and efficiently enhancing the signal.
[0046] Hereinafter, one or more specific examples will be described in more detail through examples. However, these examples are provided for illustrative purposes only and the scope of the present invention is not limited to these examples.
[0047]
[0048] Example 1 Preparation of materials and reagents
[0049]
[0050] Whatman filter paper No. 1 was purchased from GE Healthcare's Life Science (USA). Gold(III) chloride, bovine serum albumin, Tween 20, sodium periodate, and human IgG were all purchased from Sigma-Aldrich (USA). Sodium citrate was purchased from Daejung (South Korea), phosphate-buffered saline (PBS) tablets were purchased from Thermo Fisher Scientific (USA), and gold nanoparticle conjugate (anti-human IgG monoclonal antibody; conjugated to 40 nm gold nanoparticles; OD ~ 10) was purchased from MIRIMEDIX, Inc. (South Korea).
[0051]
[0052] Example 2 Doping of gold nanoparticles on a cellulose substrate
[0053]
[0054] Gold nanoparticles (approximately 40 nm) were synthesized using the Turkevich Method (J. Kimling et al. J. Phys. Chem. B 2006, 110, 32, 15700-15707). 200 mL of a 0.3 mM HAuCl3 solution in deionized water was heated to 90°C with strong magnetic stirring in a three-necked flask. Then, 1.7 mL of a 38.75 mM trisodium citrate aqueous solution was added, and the mixture was heated at 90°C for 30 min. After the resulting solution was cooled to room temperature, 0.6 g of filter paper (equivalent to 70 mm X 100 mm) was precisely cut and immersed in the synthesized gold nanoparticle solution. The volume of the solution was adjusted to the desired particle density (mm) on the cellulose surface. 2 1.63 X 10 per 8 - 2.61 X 10 9 The paper doped with gold nanoparticles was then dried in a racking incubator and stored in the dark at 4°C until use in the next step.
[0055]
[0056] Example 3 Shrinkage of cellulose substrate by malafrade reaction
[0057]
[0058] The cellulose substrate doped with gold nanoparticles obtained in Example 2 was immersed in a dopamine solution (50 mM dopamine chloride) and incubated at 37°C for 10 min. Afterwards, excess dopamine was washed away with deionized water, and the sample was gently wiped with a wiper. Next, it was immersed in a preheated 0.133 M sodium periodate solution at the desired temperatures (2, 30, 50, 60, and 70°C) for various times up to 6 h. The volume of the reagent was minimized depending on the size of the sample, and in the case of dopamine treatment, it was 0.25 μL / mm. 2 Less than 5 μL / mm for oxidation by sodium periodate 2 Less than. When used in direct ELISA, 5 μL of dopamine solution and 40 mL of sodium periodate solution were used on a paper plate. After the reaction, the sample was wiped again with a wiper and dried.
[0059] As a result, when an appropriate amount of heat and a high-concentration periodate solution were applied to the cellulose substrate, the area of the substrate shrank to approximately one-tenth (see A in Fig. 2). Here, when the cellulose substrate was colored with insoluble color inks (cyan, magenta, yellow, and black) and then shrunk for 6 hours, it was confirmed that the color intensity was amplified up to 6 times (see B in Fig. 2).
[0060]
[0061] Example 4 Confirmation of signal enhancement by increasing particle density
[0062]
[0063] To confirm that the mechanism of signal enhancement is due to the increase in the density of colored particles, paraffin wax microdots (diameter 142.57 ± 16.80 μm) were printed at wide intervals on a paper cellulose substrate, and the paper cellulose substrate was subjected to a shrinkage reaction by the Malaprade reaction. As a result, the density of the microdots increased from 4.7 ± 1.4 to 35.0 ± 4.7 particles / mm. 2 It was confirmed that there was a significant increase (see C and D in Fig. 2).
[0064] We investigated whether the particle density increased even when the paper cellulose substrate doped with gold nanoparticles was shrunk. The gold nanoparticles were pre-coated with polydopamine to prevent aggregation and then oxidized. The increase in particle density was quantified according to Beer's law using UV-visible spectroscopy. UV-visible spectroscopy was performed using a Nano-MD device (Sinco, South Korea), and the measurement of solid samples was performed using a special cuvette (Nano Stick-S; Sinco, South Korea) that can hold a single drop of liquid. The extinction coefficient of gold nanoparticles using an aqueous suspension was ε = 2.23 x 10 9 M -1 cm -1 , and then the particle density observed on the paper substrate was determined according to each shrinkage time.
[0065] As a result, it was confirmed that as the shrinkage of the substrate progressed, the color intensity of the gold nanoparticles increased, and the particle density per unit area increased (see E, F, and G of Fig. 2).
[0066]
[0067] Example 5 Morphological Characteristics Analysis According to Cellulose Substrate Shrinkage
[0068]
[0069] Example 5-1 Electron Microscope Observation
[0070] The synthesized gold nanoparticles were observed using scanning electron microscopy (SEM) and transmission electron microscopy (TEM). SEM was performed at 10 keV in both backscattering electron (BSE) and secondary electron (SE) modes using a Hitachi High Technologies Corporation (SU8010) instrument to evaluate morphological characteristics. TEM was performed using a JEOL (JEM-2010) instrument from JEOL Ltd., Japan to observe the shape and size of the gold nanoparticles. The size of the gold nanoparticles was measured manually using KLONK Image Measurement software from KLONK GmbH, Germany, and the size distribution was obtained through statistical analysis and plotting using Origin 2018 software from OriginLab Corporation, USA.
[0071] As a result of analyzing the morphological characteristics through SEM, it was observed that the fibers coiled and thickened according to the shrinkage reaction time, and it was confirmed that they showed an appearance consistent with the morphological changes of general cellulose fibers (see A in Fig. 3).
[0072]
[0073] Example 5-2 Spectroscopic analysis
[0074] To further investigate the morphological characteristics of the cellulose substrates as they shrank, spectroscopic analyses were performed. Fourier transform infrared (FTIR) spectroscopy and Raman spectroscopy were used for the analyses. FTIR spectroscopy was performed using a Varian 640-IR instrument (Varian, USA). Raman spectroscopy was performed 100 times using a C12710 Raman spectrometer (Hamamatsu, Japan) at a laser output of 50 mW, a laser source of 785 nm, and an acquisition time of 1,000 ms.
[0075] Raman spectroscopy results showed that 383 cm -1 (s) and 1096cm -1(vs), 1120cm -1 The peak at (vs) gradually decreases as the reaction time progresses, conversely at 1355 cm -1 (vs) and 906cm -1 It was confirmed that the peak at (vs) increases as the reaction time increases (see the left graph of Fig. 3B). This is 383 cm -1 (s) The peak corresponds to the cc aliphatic chain, at 1096 cm -1 (vs) and 1120cm -1 (vs) Since the peak corresponds to cellulose crystals, the decrease of this peak indicates that the polymer structure is destroyed as the reaction progresses due to the cleavage of the cellulose sugar rings. And 1355 cm -1 (vs) The peak corresponds to the C=O stretching vibration of aldehyde, at 906 cm -1 (vs) Since the peak corresponds to the CO stretching vibration, the increase of this peak indicates the formation of dialdehyde by cleavage of the sugar ring structure and the formation of intra-fiber / inter-fiber crosslinking via ester bonds.
[0076] FTIR spectroscopy results showed that as the reaction time progressed, 891 cm -1 (m), 994cm -1 (s), 1026cm -1 (vs), 1110cm -1 (m) and 1166cm -1 It can be confirmed that the peak at (m) increases (see the right graph B in Fig. 3). This is related to the CO stretching vibration of the ester bond, meaning that ester bonds are formed as the cellulose substrate shrinks.
[0077]
[0078] Example 6 Protection by polydopamine coating
[0079]
[0080] XPS analysis and morphological analysis were performed to determine the degree of protection of gold nanoparticles doped on cellulose by polydoping coating. XPS analysis was performed using Nexas (Thermo Fisher Scientific, USA) with a time of approximately 2 min for C, N, and O and approximately 15 min for Au, and the excitation source was 1486 eV aluminum X-ray.
[0081] The surface of the polydopamine coating was investigated by XPS analysis, and a measurement spectrum was obtained as shown in Fig. 4. The measurement spectrum showed Au 3d, Au 4d, and Au 4f peaks, and the Au 3d and Au 4d peaks that showed distinct peaks were normalized and displayed as a spectrum (see B and C in Fig. 4). The value when the polydopamine coating was present was lower than that when the polydopamine coating was not present, which means that polydopamine coated the gold nanoparticles and protected them from colloidal decomposition. In addition, a longer scanning time was performed to check the binding energy of the main peak, and the peaks of the spectrum shifted to the right and the intervals were the same when the polydopamine coating was present compared to when the polydopamine coating was not present (see D in Fig. 4). This indicates that the surface of the gold nanoparticles is associated with covalent bonds to the amine groups of the polydopamine coating.
[0082] Furthermore, the protective effect of the polydopamine coating was confirmed through morphological analysis using SEM, particularly by comparing BSE and SE images (see Fig. 4E and F). From the SEM images showing that gold nanoparticles remained evenly dispersed on the cellulose surface even after the shrinkage reaction, it was confirmed that the polydopamine coating effectively protected particles from loss or aggregation.
[0083]
[0084] Example 7 Controllability and reproducibility of the shrinkage reaction
[0085]
[0086] To determine whether the shrinkage rate of the cellulose substrate varies depending on the number of nanoparticles, we measured the area change according to the density of gold nanoparticles and shrinkage time using gold nanoparticles with a diameter of approximately 40 nm, which are commonly used in commercial immunosensors. The amount of gold nanoparticles was mm 2 1.63 x 10 per 8 - 2.61 x 10 9 Particle count (0.0132 - 271.152 amol / mm 2 ) range. The measurements were made using UV-visible spectroscopy, and curve fitting and statistical analysis were performed using SigmaPlot software (version 15.0, Systat Software Inc., USA). The Boltzmann sigmoid function of the reaction time (t) was used to characterize the shrinkage pattern, which is expressed by the following equation (1).
[0087] (1)
[0088] Here, A is the normalized % area of the shrunken cellulose paper at time t, and x 50 is the inflection point, and S is the slope coefficient. Pearson correlation coefficient (r t,x50 ) was calculated using SPSS 18 (IBM Corporation, USA).
[0089] As a result, very similar results were observed in all samples (see Fig. 5B), indicating that the shrinkage reaction can be utilized in a controlled manner to enhance the colorimetric signal regardless of the number of gold nanoparticles.
[0090] In Boltzmann sigmoid curves, all curves are R 2=0.990 or higher, and the inflection point values useful for comparing the swelling ratios of different polymer matrices ranged from 2.273 to 2.645, and the Pearson correlation coefficient was lower than 0.1 (see C in Fig. 5). This means that there is no significant correlation between the number of nanoparticles and the shrinkage response, which means that the shrinkage response is sufficiently reproducible to be used for colorimetric signal enhancement.
[0091]
[0092] Example 8 Colorimetric signal analysis according to nanoparticle density and shrinkage time
[0093]
[0094] To evaluate the extent to which the colorimetric signal is enhanced depending on the density of nanoparticles, gold nanoparticles of various densities were set (3.0 x 10 8 - 2.0 x 10 9 ) The colorimetric signal was measured according to the shrinkage time. Colorimetric analysis was performed by extracting RGB channels and grayscale values using GIMP (ver. 2.10, USA) in 1200-DPI mode (Epson, Perfection V37, Epson, Japan) and quantifying the signal from gold nanoparticles in cellulose.
[0095] As a result mm 2 2.0 x 10 per 9 At high nanoparticle densities exceeding the number of particles, no correlation was observed between the colorimetric signal and the shrinkage time, confirming that the signal enhancement effect due to shrinkage did not occur. mm 2 3.0 x 10 per 8 At low nanoparticle densities less than the particle number, a linear correlation was observed between the shrinkage time and the colorimetric signal, confirming that the signal enhancement effect due to shrinkage was well demonstrated (see A, B, and C in Fig. 6).
[0096] Subsequently, quantitative analysis was performed using serially diluted gold nanoparticle samples to quantify the concentration of nanoparticles and evaluate the signal enhancement performance of the present invention. Specifically, gold nanoparticle-doped cellulose samples were prepared by diluting the gold nanoparticle solution by two times, and the nanoparticle concentration range per test area (the upper surface area is 153.86 mm 2 ) was set from 41.72 to 0.02 fmol. As a result, it was confirmed that 40 fmol / zone, which is a concentration commonly used in studies on immunoassays, is included within the range as the maximum value of the effective analysis range of the present invention (see D of Fig. 6). In addition, it was confirmed that the colorimetric signal increases to a higher value as the contraction occurs during the contraction time of 0 to 4 hours, but no significant difference in the colorimetric signal value appears from 4 hours or more.
[0097]
[0098] Example 9 Application to direct ELISA for detecting human IgG
[0099]
[0100] Next, we attempted to determine whether the colorimetric signal could be increased when using direct ELISA, an actual immunoassay technique. ELISA was performed with some modifications based on Cheng's method (Cheng et al. 2010). To produce a 96-well paper substrate, a wax pattern was printed on filter paper using Xerox 8880 and baked at 120°C for 2 minutes to obtain a 5-mm diameter test area. Then, to perform direct ELISA, the sample was suspended in 10 mL of PBS and aliquoted into a 1-mL tube for immunoassay. 5 μL of a 2-fold diluted sample was immobilized on the test area, and PBS was used as a negative control. Afterwards, the test area was blocked with blocking buffer (1 μL of a PBS solution containing 0.05% Tween-20 and 1% (w / v) BPS) and dried for 10 minutes. Next, 5 μL of gold nanoparticle conjugate solution was added and incubated for 2 minutes. The test area was washed twice with 50 μL of PBS solution, and the positive control area was not subjected to this washing step.
[0101] After performing a direct ELISA to detect human IgG (0-20 pmol / zone), the signal enhancement method of the present invention was applied. The shrinkage time was set to 2 or 4 hours, respectively. As a result, a weak signal that was difficult to distinguish with the naked eye was observed at low concentrations of human IgG. After the shrinkage reaction, it was confirmed that the signal intensity increased significantly (see Figure 7).
[0102] To quantify the signal, we designed the redscale index, a proportional contrast index between two color channels in RGB space, to effectively demonstrate the signal difference between the negative and positive controls compared to the grayscale index. Its value is calculated as follows.
[0103]
[0104]
[0105] R and G represent the red and green channels, respectively, and R0 and G0 represent the red and green channels of the negative control, respectively.
[0106] The direct ELISA colorimetric signal for human IgG was calculated as a normalized red scale index and converted to a Hill curve for quantitative evaluation and graphically represented.
[0107] As a result, it was confirmed that the colorimetric signal increased overall, and the maximum signal increased more than twice after 2 hours of contraction (see D in Fig. 8). Before the contraction reaction, the signal was not well distinguished from the negative control group, but after 2 and 4 hours of contraction reaction, the signal was clearly distinguished (see E in Fig. 8).
[0108]
[0109] The present invention has been described above, focusing on preferred embodiments thereof. Those skilled in the art will appreciate that the present invention can be implemented in modified forms without departing from its essential characteristics. Therefore, the disclosed embodiments should be considered illustrative rather than limiting. The scope of the present invention is set forth in the claims, not the foregoing description, and all differences within the scope equivalent thereto should be construed as being encompassed by the present invention.
[0110] The present invention is a method for increasing a colorimetric signal after an immunoassay, and, compared to conventional post-analysis signal enhancement methods (silver enhancement, gold enhancement, etc.), uses inexpensive reagents and can stably amplify signals even under contamination and general reaction conditions.
[0111] Therefore, it can be applied in the field of on-site diagnostic devices where it is difficult to have an environment that can be created in a laboratory (e.g., precise devices such as micropipettes and an uncontaminated environment).
[0112] In particular, since anyone can easily implement the present invention, it can be implemented in tertiary medical institutions and research facilities, as well as primary medical institutions and general homes.
Claims
1. In an immunoassay method including a conjugate in which a labeling substance is conjugated to a detector, A step of coating the above conjugate on a cellulose substrate with polydopamine using a polymerization reaction of dopamine; and A method for signal enhancement of an immunoassay comprising a shrinkage step of a cellulose substrate by a Malaprade reaction.
2. A method for enhancing a signal of an immunoassay method, wherein the polydopamine coating step and the shrinking step of the cellulose substrate are performed after deriving the analysis results of the immunoassay method.
3. A method for enhancing a signal in an immunoassay, wherein the detector is an antibody, an aptamer, or an antibody-aptamer in the first paragraph.
4. A method for enhancing a signal of an immunoassay, wherein the marker material is a nanoparticle made of a material selected from the group consisting of gold (Au), platinum (Pt), cerium oxide (CeO2), zinc sulfide (ZnS), or silicon oxide (SiO).
5. A method for enhancing the signal of an immunoassay, wherein the labeling material in paragraph 1 is a gold nanoparticle.
6. A method for enhancing the signal of an immunoassay, wherein the immunoassay is a lateral flow assay, a vertical flow assay, or an enzyme-linked immunosorbent assay (ELISA) in the first paragraph.
7. A method for enhancing the signal of an immunoassay, wherein the immunoassay is performed in a direct, indirect, sandwich or competitive manner in the first paragraph.
8. A method for enhancing a signal in an immunoassay, characterized in that the cellulose substrate in the first paragraph is chromatography paper, cellulose acetate film, cellulose nanocrystals, cellulose-based hydrogels, bacterial cellulose, or microcrystalline cellulose.
9. A method for enhancing the signal of an immunoassay, wherein the labeling material is fixed on a cellulose substrate before shrinkage at a density of 0.013 to 271.152 amol / mm2 in the first paragraph.
10. A method for enhancing the signal of an immunoassay, wherein the shrinkage of the cellulose substrate in the first paragraph is achieved through cross-linking between cellulose molecules.
11. A method for strengthening a signal of an immunoassay method in accordance with paragraph 1, wherein the signal strengthening of the immunoassay method is achieved by increasing the density of the colorimetric signal of the conjugate without loss of color development derived from the analysis result of the immunoassay method through shrinkage of the cellulose substrate.
12. A method for enhancing the signal of an immunoassay, wherein the signal enhancement of the immunoassay is performed for 2 to 4 hours in the first paragraph.
Citation Information
Patent Citations
Immunoassay method based on ultra-sensitive magnetic relaxation time sensor
CN113295869A
Pressing member comprising glass coating layer for reducing friction between fusing belt and pressing member