Quantum dot, method for manufacturing quantum dot, photosensitive resin composition thereof, and electronic device
By employing a core/shell structure with specific ligands for quantum dots containing Ag, In, Ga, and S, the issues of surface defects and stability are addressed, resulting in enhanced quantum efficiency and luminous performance for quantum dots in electronic devices.
Patent Information
- Application Number
- PCT/KR2024/003692
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2024-03-25
- Publication Date
- 2024-11-14
AI Technical Summary
Quantum dots with core/shell structures face challenges in maintaining high quantum efficiency due to surface defects caused by interactions with other atoms or molecules, leading to reduced dispersibility and stability, which affects their optical and electrical properties.
The development of quantum dots with a core containing Ag, In, Ga, and S, and a shell with a ligand that interacts with the metal surface, using L-type, X-type, and Z-type ligands as electron donors and acceptors, to improve dispersibility and stability, and a method involving core manufacturing, shell formation, and ligand binding to achieve optimal weight ratios for enhanced performance.
The approach results in quantum dots with improved luminous efficiency, increased quantum efficiency, and enhanced stability, as demonstrated by the binding of suitable ligands to the core/shell components, leading to uniform growth and reduced surface defects, thereby improving the overall performance of quantum dots in electronic devices.
Smart Images

Figure KR2024003692_14112024_PF_FP_ABST
Abstract
Description
Quantum dots, methods for producing quantum dots, photosensitive resin compositions and electronic devices thereof
[0001] The present disclosure relates to quantum dots, a method for producing the quantum dots, a photosensitive resin composition thereof, and an electronic device.
[0002] Quantum dots (QDs) are nano-sized semiconductor particles that exhibit superior optical and electrical properties that bulk semiconductor materials do not have. For example, quantum dots have the characteristic of emitting light through photoluminescence (PL), in which electrons excited by external light move from the conduction band to the valence band and emit light, or electroluminescence (EL), in which light is emitted by an external charge. Even if they are composed of the same material, the color of the light emitted varies depending on the size of the quantum dot. Due to these characteristics, quantum dots are attracting attention as next-generation high-brightness light-emitting diodes (LEDs), biosensors, lasers, solar cell nanomaterials, etc.
[0003] Meanwhile, the core surface of a quantum dot can easily form chemical bonds with other atoms or molecules when approached, causing surface defects and potentially reducing quantum efficiency. To prevent this reduction in core quantum efficiency, quantum dots with a core / shell structure, in which a shell is formed on the core surface, have been developed.
[0004] Quantum dots with a core / shell structure can be manufactured in the form of colloidal quantum dots, which are quantum dots dispersed in an organic solvent and are also referred to as quantum dot solutions. To ensure that colloidal quantum dots remain well dispersed in the solvent, the quantum dots may include ligands bound to the shell surface.
[0005] However, the dispersibility and stability of quantum dots may vary depending on the type of ligand combined with the core / shell component. Therefore, it is necessary to develop quantum dots with improved dispersibility and stability by combining ligands suitable for the core / shell component.
[0006] Embodiments of the present disclosure can provide a quantum dot having excellent luminous efficiency, a method for producing the quantum dot, a photosensitive resin composition thereof, and an electronic device.
[0007] Embodiments of the present disclosure can provide a quantum dot capable of improving quantum efficiency, a method for manufacturing the quantum dot, and an electronic device, comprising a nanostructure including a core comprising Ag, In, Ga, and S and a shell disposed on the core, a ligand interacting with a metal bonded to the surface of the nanostructure, wherein the ligand is at least one selected from an L-type ligand which is a two-electron donor, an X-type ligand which is a one-electron donor, and a Z-type ligand which is an electron acceptor.
[0008] In one aspect, embodiments of the present disclosure provide a quantum dot comprising a core comprising Ag, In, Ga, and S, a nanostructure comprising a shell disposed on the core, and a ligand interacting with a metal bound to a surface of the nanostructure, wherein the ligand is at least one selected from an L-type ligand which is a two-electron donor, an X-type ligand which is a one-electron donor, and a Z-type ligand which is an electron acceptor, and wherein a weight ratio of the ligand to the sum of the nanostructure and the ligand is greater than 5 wt% and less than or equal to 50 wt%.
[0009] In another aspect, embodiments of the present disclosure provide a method for manufacturing quantum dots.
[0010] The quantum dot manufacturing method includes a core manufacturing step, a shell manufacturing step, and a ligand binding step.
[0011] The core manufacturing step is a step of manufacturing a core. The core manufacturing step is a step of manufacturing a core by injecting a silver precursor, an indium precursor, a gallium precursor, a sulfur precursor, and a solvent into a first reactor and reacting them.
[0012] The shell manufacturing step is a step of manufacturing a shell by injecting the manufactured core into a second reactor equipped with a precursor containing a specific element and reacting the core.
[0013] The ligand binding step is a step of binding a ligand that interacts with a metal to the manufactured shell. The ligand may be one or more selected from the aforementioned L-type ligand, X-type ligand, and Z-type ligand.
[0014] The weight ratio of the above-mentioned ligand may be greater than 5 wt% and less than 50 wt% compared to the sum of the nanostructure and the ligand.
[0015] In another aspect, embodiments of the present disclosure provide a photosensitive resin composition comprising quantum dots.
[0016] In another aspect, embodiments of the present disclosure provide an electronic device including a display device including a light-emitting diode including a photosensitive resin composition including quantum dots and a control unit for driving the display device.
[0017] Quantum dots, methods for producing quantum dots, photosensitive resin compositions, and electronic devices according to embodiments of the present disclosure may have excellent luminous efficiency.
[0018] The quantum dots, the method for manufacturing the quantum dots, the photosensitive resin compositions and the electronic devices according to the embodiments of the present disclosure can improve quantum efficiency by improving dispersibility and stability by combining at least one ligand selected from among an L-type ligand which is a two-electron donor suitable for the core / shell, an X-type ligand which is a one-electron donor and a Z-type ligand which is an electron acceptor.
[0019] FIG. 1 is a cross-sectional view of a quantum dot according to one embodiment.
[0020] Figure 2 is a cross-sectional view of a quantum dot according to another embodiment.
[0021] Figure 3 is a cross-sectional view of a quantum dot according to another embodiment.
[0022] Figure 4 is a flowchart of a method for manufacturing quantum dots according to another embodiment.
[0023] Figure 5 is a flow chart of a method for manufacturing quantum dots according to another embodiment.
[0024] Figure 6 is a cross-sectional view of an electronic device according to another embodiment.
[0025] Figure 7 is a cross-sectional view of a light emitting diode according to another embodiment.
[0026] Hereinafter, some embodiments of the present disclosure will be described in detail. In describing the present disclosure, detailed descriptions of related known configurations or functions may be omitted if they are deemed to obscure the gist of the present disclosure.
[0027] Additionally, when describing components of the present disclosure, when "includes," "has," "consists of," etc. are used, other parts may be added unless "only" is used. When a component is expressed in the singular, it may include cases where the plural is included unless there is a special explicit description.
[0028] Additionally, terms such as first, second, A, B, (a), (b), etc. may be used to describe the components of the present disclosure. These terms are only intended to distinguish the components from other components, and the nature, order, sequence, or number of the components are not limited by the terms.
[0029] In a description of the positional relationship of components, when it is described that two or more components are "connected," "combined," or "connected," it should be understood that the two or more components may be directly "connected," "combined," or "connected," but that the two or more components may also be further "interposed" with another component to be "connected," "combined," or "connected." Here, the other component may be included in one or more of the two or more components that are "connected," "combined," or "connected" to each other.
[0030] Furthermore, when a component is said to be "on" or "over" another component, it should be understood that this includes not only cases where it is "directly over" the other component, but also cases where there are other components in between. Conversely, when a component is said to be "directly over" another part, it should be understood that there are no other parts in between. Furthermore, when a component is said to be "on" or "over" a reference part, it means that it is located above or below the reference part, and does not necessarily mean that it is located "over" or "over" in the opposite direction of gravity.
[0031] In the description of the temporal flow relationship related to components, operation methods, or manufacturing methods, for example, when the temporal or flow relationship is described as “after”, “following”, “next to”, “before”, etc., it may also include cases where it is not continuous, unless “immediately” or “directly” is used.
[0032] Meanwhile, when numerical values or corresponding information for components are mentioned, even without separate explicit description, the numerical values or corresponding information may be interpreted as including an error range that may occur due to various factors (e.g., process factors, internal or external impact, noise, etc.).
[0033] The "diameter" of a nanostructure refers to the diameter of a cross-section perpendicular to the first axis of the nanostructure, where the first axis has the greatest difference in length with respect to the second and third axes (the second and third axes being the two axes that are most closely equal in length). The first axis is not necessarily the longest axis of the nanostructure; for example, for a disk-shaped nanostructure, the cross-section will be a substantially circular cross-section perpendicular to the short longitudinal axis of the disk. If the cross-section is not circular, the diameter is the average of the major and minor axes of the cross-section. For elongated or high aspect ratio nanostructures, such as nanowires, the diameter is measured across a cross-section perpendicular to the longest axis of the nanowire. For spherical nanostructures, the diameter is measured through the center of the sphere from one side to the other.
[0034] The term "quantum dot" (or "dot") refers to a nanocrystal that exhibits quantum confinement or exciton confinement. A quantum dot may be substantially homogeneous in its material properties, or in certain embodiments, may be heterogeneous, for example comprising a core and at least one shell. The optical properties of a quantum dot may be influenced by its particle size, chemical composition, and / or surface composition, and can be determined by suitable optical testing available in the art. The ability to tailor the nanocrystal size, for example, to a range of about 1 nm to about 15 nm, allows for light emission coverage across the entire optical spectrum, providing great versatility in color rendering.
[0035] As used herein, the term "shell" refers to material that is deposited onto a core or onto a previously deposited shell of the same or different composition, and that results from a single act of deposition of shell material. The exact shell thickness depends on the material as well as the precursor input and conversion and may be reported in nanometers or single layers. "Target shell thickness" refers to the intended shell thickness used to calculate the required precursor amount, and "actual shell thickness" refers to the actual deposited amount of shell material after synthesis and can be measured by methods known in the art. For example, the actual shell thickness can be measured by comparing particle diameters determined from transmission electron microscope (TEM) images of nanocrystals before and after shell synthesis.
[0036] Additionally, in describing embodiments of the present disclosure, "group" refers to a group of the periodic table of elements. Additionally, in describing embodiments of the present disclosure, "cycle" refers to a period of the periodic table of elements.
[0037] Here, “Group I” may include Group IA (or 1A) and Group IB (or 1B), and Group I elements may include, but are not limited to, Li, Na, K, Rb, Cs Cu, Ag, and Au.
[0038] “Group II” may include Group IIA (or 2A) and Group IIB (or 2B), and Group II elements may include, but are not limited to, Be, Mg, Ca, Sr, Zn, Cd, and Hg.
[0039] “Group III” may include Group IIIA (or 3A) and Group IIIB (or 3B), and Group III elements may include, but are not limited to, In, Ga, Al, and Tl.
[0040] “Group V” may include Group VA (or 5A), and Group V elements may include, but are not limited to, P, As, Sb, Bi, and N.
[0041] “Group VI” may include Group VIA (or 6A), and Group VI elements may include, but are not limited to, S, Se, and Te.
[0042] In describing embodiments of the present disclosure, a precursor is a chemical substance prepared in advance to react quantum dots, and is a concept referring to all compounds including metals, ions, elements, compounds, complexes, composites, and clusters, and is not limited to the final material of the reaction, and may refer to a material that can be obtained at an arbitrarily determined stage.
[0043] Quantum dots according to embodiments of the present disclosure will be described in detail with reference to the drawings below.
[0044] FIG. 1 is a cross-sectional view of a quantum dot according to one embodiment.
[0045] Referring to FIG. 1, a quantum dot (10) according to the present disclosure includes a nanostructure (13) including a quantum dot core (12) including Ag, In, and S or including Ag, In, Ga, and S. The nanostructure (13) may include a shell disposed on the surface of the core. That is, the nanostructure (13) may have a core / shell structure.
[0046] The core (12) may be purified prior to deposition of the shell (14). The core (12) may be filtered to remove precipitates from the core solution.
[0047] Shell(14) is AIS, AISe, AITe, AISeS, AISeTe, AITeS, GaS, GaSe, GaTe, GaSeS, GaSeTe, GaTeS, InS, InSe, InTe, InSeS, InSeTe, InTeS, TiS, TiSe, TiTe, TiSeS, TiSeTe, TiTeS, LiGaS, LiGaSe, LiGaTe, NaGaS, NaGaSe, NaGaTe, KGaS, KGaSe, KGaTe, CuAlS, CuAlSe, CuAlTe, CuGaS, CuGaSe, CuGaTe, CuInS, CuInSe, CuInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe, AgAlTe, AgGaS, AgGaSe, AgGaTe, AuGaS, AuGaSe, AuGaTe, AgInTe, CuTiS, CuTiSe, CuTiTe, AgAlS AgTiTe, AuAlS, AuAlSe, AuAlTe, AuInS, AuInSe, AuInTe, AuTiS, AuTiSe, AuTiTe, LiNaGaS, LiNaGaSe, LiNaGaTe, NaGaSeTe, NaGaSSe, NaGaSTe, LiGaSeTe, LiGaSSe, LiGaSTe, KLiGaS, KLiGaSe, KLiGaTe, KNaGaS, KNaGaSe, KNaGaTe, KGaSeTe, KGaSSe. KGaSTe, CuLiGaS, CuLiGaSe, CuLiGaTe, CuNaGaS, CuNaGaSe, CuNaGaTe, CuKGaS, CuKGaSe, CuKGaTe, CuGaSeTe, CuGaSSe, CuGaSTe, AgLiGaS, AgLiGaSe, AgLiGaTe, AgNaAlS, AgNaAlSe, AgNaAlTe, AgNaGaS, AgNaInS, AgNaInSe, AgNaInTe, AgNaTiS, AgNaTiSe, AgNaTiTe, AgKGaS, AgKGaSe, AgKGaTe, AgGaSeTe, AgGaSSe, AgGaSTe, AgCuGaS, AgCuGaSe,It may include one or more of AgCuGaTe, AgAuGaS, AgAuGaSe, AgAuGaTe, AuLiGaS, AuLiGaSe, AuLiGaTe, AuNaGaS, AuNaGaSe, AuNaGaTe, AuKGaS, AuKGaSe, AuKGaTe, AuGaSeTe, AuGaSSe, AuGaSTe, AuCuGaS, AuCuGaSe or AuCuGaTe.
[0048] The quantum dot (10) includes a ligand (15) that interacts with a metal bonded to the surface of the nanostructure (13), and the ligand (15) may be at least one selected from an L-type ligand which is a two-electron donor, an X-type ligand which is a one-electron donor, and a Z-type ligand which is an electron acceptor. The L-type ligand may be suitable for synthesis because it is compatible with amines or fatty acids. The size of the quantum dot (10) may increase due to the increase in amines and the compatibility of the X-type ligands during synthesis, thereby increasing the quantum efficiency. In addition, the halide-based precursor used in the synthesis of the quantum dot is very effective in suppressing surface defects with the X-type ligand (see Examples 1 and 11 and Table 1 described below).
[0049] An L-type ligand is a ligand that interacts with a metal (M) as a 2-electron donor, and as can be seen in the metal (M)-L-type ligand (L) molecular orbital diagram below, both electrons placed in the HOMO (Highest occupied molecular orbital) are provided by the L-type ligand.
[0050] [Metal (M)-L type ligand (L) molecular orbital diagram]
[0051]
[0052] The L-type ligand may be one or more selected from, but is not limited to, oleylamine, N,N,N',N'-tetramethylethylene-1,2-diamine, pyridine tri-n-butylphosphine oxide, tri-n-octylphosphine oxide, and 5,8-Dimethyl-4,7,10-trioxatridecane-2,12-diamine.
[0053] An X-type ligand is a ligand that interacts with a metal (M) as a 1-electron donor. As can be seen in the metal (M)-X-type ligand (X) molecular orbital diagram below, one of the two electrons placed in the HOMO (Highest occupied molecular orbital) is provided by the metal and the other by the X-type ligand.
[0054] [Metal (M)-X type ligand (X) molecular orbital diagram]
[0055]
[0056] The X-type ligand may be at least one selected from oleic acid, tetradecanol, a thiol group, a halide group, an O2CR group, and a phosphine group, but is not limited thereto.
[0057] In the O2CR group, R may be selected from the group consisting of a substituted or unsubstituted alkyl group, an alkenyl group, a cycloalkyl group, a cycloalkenyl group, a heterocyclyl group, an amino group, an alkylamino group, a dialkylamino group, an arylalkyl group, a silyl group, an aryl group, a heteroaryl group, or a combination thereof, and R may be further substituted with a substituted or unsubstituted alkyl, aryl, or heteroaryl, but is not limited thereto.
[0058] The thiol group may be at least one selected from, but is not limited to, a dodecanethiol group, an adamantanethiol group, an octanethiol group, a 6-mercapto-1-hexanol group, and a 6-amino-1-hexanol group.
[0059] The halide group may be one or more selected from, but is not limited to, -F, -Cl, -I, and -Br.
[0060] The O2CR group may be at least one selected from, but is not limited to, a carboxylate group, an octanoate group, a crotonate group, a dimethylacrylate group, a benzoate group, a p-toluate group, and an oxo group.
[0061] The phosphine group may be at least one selected from, but is not limited to, a tris methyl silyl phosphine group, a tris dimethylamino phosphine group, a tris diethylamino phosphine group, a tris carboxyethyl phosphine hydrochloride group, a tris (hydroxypropyl) phosphine group, and a 2-diphenylphosphinobenzaldehyde group.
[0062] A Z-type ligand is a ligand that interacts with a metal (M) as an electron acceptor (or 0-electron donor), and as can be seen in the metal (M)-Z-type ligand (Z) molecular orbital diagram below, both electrons placed in the HOMO (Highest occupied molecular orbital) are provided by the metal.
[0063] [Metal (M)-Z type ligand (Z) molecular orbital diagram]
[0064]
[0065] The metal may be one or more selected from, but is not limited to, In, P, Ga, Ag, Cd, Zn, Se, S, Al, Cu, Li, Au, K, Na, Pb, and Cs.
[0066] The alkyl group may be one or more selected from a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a Sec-butyl group, an n-pentyl group, an isopentyl group, a hexyl group, a heptyl group, and an octyl group, but is not limited thereto.
[0067] Quantum dots (10) include nanostructures (13) and ligands (15) bound to the surface of the nanostructures (13), and the weight ratio of the ligands (15) to the sum of the nanostructures (13) and the ligands (15) is greater than 5 wt% and less than or equal to 50 wt%. The ligands interacting with metals are exemplarily described as being 10 wt%, 20 wt%, 30 wt%, 40 wt%, and 50 wt% relative to the total quantum dots (nanostructures and ligands). However, when the weight ratio of the ligands (15) exceeds 50 wt%, it may be helpful in forming quantum dots, but the half-width may increase or the quantum efficiency may decrease due to uneven growth of the quantum dots.
[0068] As can be seen from the examples and comparative examples described below, when the weight ratio of the ligand (15) interacting with the metal to the sum of the nanostructure (13) and the ligand (15) is more than 5 wt% and less than 50 wt%, it not only helps in forming quantum dots, but also reduces the half-width and increases the quantum efficiency through uniform growth of the quantum dots.
[0069] In one embodiment, the shell (14) disposed on the core (12) may include at least one selected from a group I element or a group III element and a group VI element.
[0070] The group I element used in the shell (14) may include group IA and group IB, and may be one selected from the group consisting of Li, Na, K, Rb, Cs, Cu, Ag, and Au or a combination thereof, but is not limited thereto.
[0071] The group III element used in the shell (14) may include group IIIA and group IIIB, and may be one selected from the group consisting of In, Ga, Al, and Tl or a combination thereof, but is not limited thereto.
[0072] The group VI element used in the shell (14) may be one selected from the group consisting of S, Se, and Te or a combination thereof, but is not limited thereto.
[0073] The shell (14) may be doped with a metal or non-metal. The core (12) / shell (14) may be purified after deposition of the shell (14). The core (12) / shell (14) may be filtered to remove precipitates from the core solution.
[0074] Shell(14) is AIS, AISe, AITe, AISeS, AISeTe, AITeS, GaS, GaSe, GaTe, GaSeS, GaSeTe, GaTeS, InS, InSe, InTe, InSeS, InSeTe, InTeS, TiS, TiSe, TiTe, TiSeS, TiSeTe, TiTeS, LiGaS, LiGaSe, LiGaTe, NaGaS, NaGaSe, NaGaTe, KGaS, KGaSe, KGaTe, CuAlS, CuAlSe, CuAlTe, CuGaS, CuGaSe, CuGaTe, CuInS, CuInSe, CuInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe, AgAlTe, AgGaS, AgGaSe, AgGaTe, AuGaS, AuGaSe, AuGaTe, AgInTe, CuTiS, CuTiSe, CuTiTe, AgAlS AgTiTe, AuAlS, AuAlSe, AuAlTe, AuInS, AuInSe, AuInTe, AuTiS, AuTiSe, AuTiTe, LiNaGaS, LiNaGaSe, LiNaGaTe, NaGaSeTe, NaGaSSe, NaGaSTe, LiGaSeTe, LiGaSSe, LiGaSTe, KLiGaS, KLiGaSe, KLiGaTe, KNaGaS, KNaGaSe, KNaGaTe, KGaSeTe, KGaSSe. KGaSTe, CuLiGaS, CuLiGaSe, CuLiGaTe, CuNaGaS, CuNaGaSe, CuNaGaTe, CuKGaS, CuKGaSe, CuKGaTe, CuGaSeTe, CuGaSSe, CuGaSTe, AgLiGaS, AgLiGaSe, AgLiGaTe, AgNaAlS, AgNaAlSe, AgNaAlTe, AgNaGaS, AgNaInS, AgNaInSe, AgNaInTe, AgNaTiS, AgNaTiSe, AgNaTiTe, AgKGaS, AgKGaSe, AgKGaTe, AgGaSeTe, AgGaSSe, AgGaSTe, AgCuGaS, AgCuGaSe,It may include, but is not limited to, one or more of AgCuGaTe, AgAuGaS, AgAuGaSe, AgAuGaTe, AuLiGaS, AuLiGaSe, AuLiGaTe, AuNaGaS, AuNaGaSe, AuNaGaTe, AuKGaS, AuKGaSe, AuKGaTe, AuGaSeTe, AuGaSSe, AuGaSTe, AuCuGaS, AuCuGaSe or AuCuGaTe.
[0075] According to one embodiment, the diameter of the quantum dot (10) may be 2 nm to 20 nm. The diameter of the quantum dot (10) may be 2 nm or more and 10 nm or less.
[0076] Quantum dots (10) have a full width at half maximum (FWHM) of between 10 nm and 50 nm and can exhibit a photoluminescence quantum efficiency of between 60 and 99%.
[0077] The shape of the quantum dot (10) is not particularly limited to a shape commonly used in the field, but more specifically, a shape such as a spherical, pyramidal, multi-arm, or cubic nanoparticle, nanotube, nanowire, nanofiber, or nanoplatelet particle can be used.
[0078] Quantum dots (10) can control the color of light they emit depending on their particle size, and accordingly, quantum dots (10) can have various light-emitting colors such as blue, red, and green.
[0079] Figure 2 is a cross-sectional view of a quantum dot according to another embodiment.
[0080] Figure 3 is a cross-sectional view of a quantum dot according to another embodiment.
[0081] Referring to FIG. 2, in one embodiment, the quantum dot (10) may include a core-multilayer shell structured nanostructure (13) having a core (12) including Ag, In, Ga, and S, a first shell (14) including, for example, at least one of a Group I element and a Group III element and a Group VI element, disposed on (or directly above) the core (12), and a second shell (16) including at least one selected from a Group I element and a Group III element and a Group VI element, disposed on (or directly above) the first shell.
[0082] According to other embodiments, a quantum dot (10) may include a core (12) including Ag, In, Ga, and S, a first shell (14), a second shell (16), as shown in FIG. 3, and may additionally include another shell (18) on the outer surface than the second shell (16), or may additionally include another intermediate shell between the shell (14) and the second shell (16), although not shown.
[0083] According to other embodiments, the quantum dot (10) may have a core (12) and a first shell (14) that are substantially identical to the core (12) and shell (14) described with reference to FIG. 1. In other words, the quantum dot (10) including the core (12) and shell (14) illustrated in FIG. 1 may be equally applied to the quantum dot (10) having a core / multilayer shell structure illustrated in FIGS. 2 and 3.
[0084] The second shell (16) surrounds the first shell (14) on the first shell (14) and includes at least one group I element and at least one group III element selected from among group VI elements. The group I element included in the second shell (16) may be the same as Ag included in the core (12), but may not be the same. The group III element included in the second shell (16) may be the same as In and Ga included in the core (12), but may not be the same. In addition, the group VI element included in the second shell (16) may be the same as S included in the core (12), but may not be the same.
[0085] At least one group I element included in the first shell (14) and the second shell (16) may include one or more selected from Li, Na, K, Rb, Cs, Cu, Ag, and Au. At least one group III element included in the first shell (14) and at least one group I element included in the second shell (16) may be the same or different.
[0086] At least one group III element included in the first shell (14) and the second shell (16) may include one or more selected from Al, Ga, In, and Tl. At least one group III element included in the first shell (14) and at least one group III element included in the second shell (16) may be the same or different.
[0087] At least one group VI element included in the first shell (14) and the second shell (16) may include one or more selected from S, Se, and Te. At least one group VI element included in the first shell (14) and at least one group VI element included in the second shell may be the same or different.
[0088] The second shell (16) may additionally include other doped group I elements or group III elements.
[0089] Also, 제2shell(16) is AIS, AISe, AITe, AISeS, AISeTe, AITeS, GaS, GaSe, GaTe, GaSeS, GaSeTe, GaTeS, InS, InSe, InTe, InSeS, InSeTe, InTeS, TiS, TiSe, TiTe, TiSeS, TiSeTe, TiTeS, LiGaS, LiGaSe, LiGaTe, NaGaS, NaGaSe, NaGaTe. KGaS, KGaSe, KGaTe, CuAlS, CuAlSe, CuAlTe, CuGaS, CuGaSe, CuGaTe, CuInS, CuInSe, CuInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe, AgAlTe, AgGaS, AgGaSe, AgGaTe, AuGaS, AuGaSe, AuGaTe, AgInTe, CuTiS, CuTiSe, CuTiTe, AgAlS AgTiTe, AuAlS, AuAlSe, AuAlTe, AuInS, AuInSe, AuInTe, AuTiS, AuTiSe, AuTiTe, LiNaGaS, LiNaGaSe, LiNaGaTe, NaGaSeTe, NaGaSSe, NaGaSTe, LiGaSeTe, LiGaSSe, LiGaSTe, KLiGaS, KLiGaSe, KLiGaTe, KNaGaS, KNaGaSe, KNaGaTe, KGaSeTe, KGaSSe. KGaSTe, CuLiGaS, CuLiGaSe, CuLiGaTe, CuNaGaS, CuNaGaSe, CuNaGaTe, CuKGaS, CuKGaSe, CuKGaTe, CuGaSeTe, CuGaSSe, CuGaSTe, AgLiGaS, AgLiGaSe, AgLiGaTe, AgNaAlS, AgNaAlSe, AgNaAlTe, AgNaGaS, AgNaInS, AgNaInSe, AgNaInTe, AgNaTiS, AgNaTiSe, AgNaTiTe, AgKGaS, AgKGaSe, AgKGaTe, AgGaSeTe, AgGaSSe, AgGaSTe, AgCuGaS,It may include one or more of AgCuGaSe, AgCuGaTe, AgAuGaS, AgAuGaSe, AgAuGaTe, AuLiGaS, AuLiGaSe, AuLiGaTe, AuNaGaS, AuNaGaSe, AuNaGaTe, AuKGaS, AuKGaSe, AuKGaTe, AuGaSeTe, AuGaSSe, AuGaSTe, AuCuGaS, AuCuGaSe or AuCuGaTe.
[0090] The quantum dot (10) illustrated in FIGS. 2 and 3 includes a ligand (15) that interacts with a metal bound to the surface of the nanostructure (13).
[0091] As described above, in the quantum dot (10) according to the embodiment of the present disclosure, the details regarding the ligand (15) are the same as those described for the quantum dot (10) according to the embodiment described above.
[0092] According to one embodiment, the diameter of the quantum dot (10) may be 2 nm to 20 nm. The diameter of the quantum dot (10) may be 2 nm or more and 10 nm or less.
[0093] In another aspect, embodiments of the present disclosure may provide a method for manufacturing quantum dots.
[0094] Figure 4 is a flowchart of a method for manufacturing quantum dots according to another embodiment.
[0095] Referring to FIG. 4, the quantum dot manufacturing method (20) according to embodiments of the present disclosure includes a core manufacturing step (S22), a shell manufacturing step (S24), and a ligand binding step (S26).
[0096] In the quantum dot manufacturing method (20) according to the embodiments of the present disclosure, details regarding the core and shell are the same as those regarding the core (12) and shell (14) described for the quantum dot (10) according to the above-described embodiment, unless specifically described otherwise.
[0097] The quantum dot manufacturing method (20) can be performed by manufacturing a core using a silver precursor, an indium precursor, a gallium precursor, and a sulfur precursor in a heated reactor, and then manufacturing the core together with a precursor from which a shell is manufactured using a hot-injection method and a heating up method. In addition, the hot-injection method and the heating up method can be performed in each of the core manufacturing step (S22) and the shell manufacturing steps (S24).
[0098] The core manufacturing step (S22) is a step of manufacturing a core by injecting a silver precursor, an indium precursor, a gallium precursor, a sulfur precursor, and a solvent into a first reactor and reacting them.
[0099] As described above, the shell (14) disposed on the core (12) may include at least one selected from a group I element or a group III element and a group VI element.
[0100] The shell manufacturing step (S24) is a step of manufacturing a shell by injecting and reacting a core manufactured in a first reactor equipped with a precursor containing a specific element.
[0101] As described above, the shell (14) placed on the core (12) may include at least one selected from among Group I elements or Group III elements and a Group VI element. In this case, the shell manufacturing step (S24) may manufacture the shell by injecting and reacting the manufactured core into a first reactor equipped with a precursor including at least one selected from among Group I elements or Group III elements and a precursor including a Group VI element.
[0102] The core manufacturing step (S22) is a step for manufacturing a core, and may include step 1-1 and step 1-2.
[0103] Step 1-1 may be a step of preparing a core solution by injecting a silver precursor, an indium precursor, a gallium precursor, a sulfur precursor, and a solvent into a first reactor and heating them.
[0104] The silver precursor injected in step 1-1 may be, for example, one or more selected from the group consisting of silver (I) acetylacetonate, silver (I) chloride, silver (I) bromide, silver (I) iodide, silver (I) acetate, silver (I) nitrate, and silver (I) myristate.
[0105] The indium precursor injected in step 1-1 may be, for example, one or more selected from the group consisting of indium(III) acetylacetonate, indium(III) chloride, indium(III) acetate, trimethyl indium, alkyl indium, aryl indium, indium(III) myristate, and indium(III) myristate acetate.
[0106] The gallium precursor injected in step 1-1 may be, for example, one or more selected from the group consisting of gallium (III) acetylacetonate, gallium (III) chloride, gallium (III) iodide, gallium (III) bromide, gallium (III) acetate, and gallium (III) nitrate.
[0107] The sulfur precursor injected in step 1-1 may be, for example, one or more selected from the group consisting of alkylthiols such as n-butanethiol, isobutanethiol, n-hexanethiol, 1-octanethiol, decanethiol, 1-dodecanethiol, hexadecanethiol, octadecanethiol, sulfur chloride, elemental sulfur (S), S-TOP, S-ODE, S-toluene, S-oleylamine, and N,N-dimethylthiourea.
[0108] The solvent injected in step 1-1 may be one or more selected from oleylamine, octadecene, and trioctylamine, but is not limited thereto.
[0109] Each of the silver precursor, indium precursor, gallium precursor, and sulfur precursor injected in step 1-1 may be a precursor solution mixed with a solvent.
[0110] Through step 1-1, a core solution including a core formed by reacting a silver precursor, an indium precursor, a gallium precursor, and a sulfur precursor in a second reactor can be manufactured.
[0111] Steps 1 and 2 may be steps of adding a purification solvent to the core solution, centrifuging, and dispersing the precipitate separated through centrifugation in a dispersion solvent.
[0112] For example, steps 1 and 2 may be steps of adding a purification solvent such as methanol, ethanol, acetone, or isopropyl alcohol (2-propanol, IPA) to the core solution, centrifuging the solution, and then dispersing the precipitate separated through centrifugation in a dispersion solvent such as hexane, toluene, octadecane, heptane, oleylamine, or 1-octadecene.
[0113] A purified core solution can be manufactured through steps 1 and 2.
[0114] The shell manufacturing step (S24) may include step 2-1 and step 2-2.
[0115] Step 2-1 may be a step of injecting a precursor containing at least one selected from a group element or a group III element into a second reactor equipped with oleyamine.
[0116] Step 2-2 may be a step of injecting and reacting a VI precursor containing a purified core solution and another Group VI element into the first reactor.
[0117] The group III precursor and group VI precursor injected in steps 2-1 and 2-2 may be, for example, one selected from the group consisting of compounds chemically bonded with group III elements, such as acetate, acetylacetone, oxide, bromide, chloride, and iodide.
[0118] For example, if the group III precursor injected in step 2-1 is a gallium precursor, it may be one selected from the group consisting of compounds such as gallium acetate, gallium acetylacetone, gallium oxide, gallium bromide, gallium chloride, and gallium iodide.
[0119] In the case of the indium precursor injected in step 2-1, the indium precursor has already been described in step 1-1, so the description thereof is omitted.
[0120] If the group VI precursor injected in step 2-2 is a sulfur precursor, the sulfur precursor has already been described in step 1-1, so its description is omitted.
[0121] When the group VI precursor injected in step 2-2 is a selenium precursor, the selenium precursor may be at least one selected from the group consisting of compounds such as selenium chloride, elemental selenium (Se), Se-TOP, Se-DPP, Se-ODE, organic selenium compounds, for example, Dibenzyl Diselenide, Diphenyl Diselenide, or selenium hydride.
[0122] When the group VI precursor injected in step 2-2 is a tellurium precursor, the tellurium precursor may be, for example, one or more selected from the group consisting of tellurium chloride, elemental tellurium (Te), or tellurium hydride.
[0123] A shell (14) is manufactured by a shell manufacturing step (S24) on a core (12) manufactured by a core manufacturing step (S22), thereby completing the manufacturing of a nanostructure (13) including a core (12) and a shell (14).
[0124] The ligand binding step (S26) is a step of binding the terminal functional group of a ligand (15) that interacts with a metal to the surface of a nanostructure (13).
[0125] As described above, in the quantum dot manufacturing method (20) according to the embodiments of the present disclosure, the details regarding the ligand (15) are the same as those regarding the ligand (15) according to the embodiment described above.
[0126] The ligand binding step (S26) prepares a ligand that interacts with a metal in a round flask, injects an AgInGaS core solution, and injects shell precursors, as specifically described in the examples and comparative examples described below, so that a ligand that interacts with a metal can be bound to the surface of a nanostructure including a core and a shell.
[0127] Hereinafter, a quantum dot (10) including a core (12) and first and second shells (14, 16) as shown in FIG. 2 and a quantum dot (10) including a core (12) and three shells (14, 16, 18) as shown in FIG. 3 can be manufactured by repeating the process of manufacturing the shell (14) described above two or three times using precursors used for each shell (14, 16, 18).
[0128] The shape of the quantum dot (10) is not particularly limited to a shape commonly used in the field, but more specifically, a shape such as a spherical, pyramidal, multi-arm, or cubic nanoparticle, nanotube, nanowire, nanofiber, or nanoplatelet particle can be used.
[0129] Referring to FIG. 4, a method for manufacturing a quantum dot (10) including a core (12) and a first cell (14) as shown in FIG. 1 has been described. Hereinafter, a method for manufacturing a quantum dot (10) including a core (12) and first and second shells (14, 16) as shown in FIG. 2 will be described with reference to FIG. 5. A quantum dot (10) including a core (12) and three shells (14, 16, 18) as shown in FIG. 3 can be manufactured by adding an outermost shell (18) to the method for manufacturing a quantum dot (10) described with reference to FIG. 5.
[0130] Figure 5 is a flow chart of a method for manufacturing quantum dots according to another embodiment.
[0131] Referring to FIG. 5, the quantum dot manufacturing method (30) according to the embodiments of the present disclosure includes a core manufacturing step (S32), a first shell manufacturing step (S34), a second shell manufacturing step (S36), and a ligand binding step (S38).
[0132] In the quantum dot manufacturing method (30) according to the embodiments of the present disclosure, details regarding the core, the first shell, and the second shell are the same as those regarding the core (12), the first shell (14), and the second shell (16) described for the quantum dot (10) according to the above-described embodiment, unless otherwise specifically described.
[0133] The core manufacturing step (S32) and the first shell manufacturing step (S34) may be substantially the same as the core manufacturing step (S22) and the first shell manufacturing step (S24) described with reference to FIG. 4.
[0134] The second shell manufacturing step (S36) injects and reacts the core / first shell manufactured into a second reactor equipped with at least one precursor selected from a group I precursor including at least one group I element and a group III precursor including at least one group III element and a group VI precursor including at least one group VI element to manufacture a second shell that surrounds the first shell.
[0135] The group I elements included in the second shell may include, but are not limited to, one or more selected from Li, Na, K, Rb, Cs, Cu, Ag, and Au.
[0136] The group III element included in the second shell may include, but is not limited to, one or more selected from In, Ga, Al, and Tl. The group VI element included in the second shell may include, but is not limited to, one or more selected from S, Se, and Te. The group VI element included in the second shell may or may not be the same as S included in the core.
[0137] At least one precursor selected from among a group I precursor including at least one group I element and a group III precursor including at least one group III element used in the second shell manufacturing step (S36) and a group VI precursor including at least one group VI element may be the group I precursor, group III precursor and group VI precursor described in the first shell manufacturing step (S34).
[0138] In another aspect, in the quantum dots manufactured in another embodiment, the thickness of the first shell (14) formed in the first shell manufacturing step (S34) may be relatively thicker than the thickness of the second shell formed in the second shell manufacturing step (S36).
[0139] The 1st shell formed in the 1st shell manufacturing step (S34) is AIS, AISe, AITe, AISeS, AISeTe, AITeS, GaS, GaSe, GaTe, GaSeS, GaSeTe, GaTeS, InS, InSe, InTe, InSeS, InSeTe, InTeS, TiS, TiSe, TiTe, TiSeS, TiSeTe, TiTeS, LiGaS, LiGaSe, LiGaTe, NaGaS. NaGaSe, NaGaTe, KGaS, KGaSe, KGaTe, CuAlS, CuAlSe, CuAlTe, CuGaS, CuGaSe, CuGaTe, CuInS, CuInSe, CuInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe, AgAlTe, AuGaS, AuGaSe, AuGaTe, AgInS, AgInSe, AgGaTe, AgTiS, AgTiSe, AgTiTe, AuAlS, AuAlSe, AuAlTe, AuInS, AuInSe, AuInTe, AuTiS, AuTiSe, AuTiTe, LiNaGaS, LiNaGaSe, LiNaGaTe, NaGaSeTe, NaGaSSe, NaGaSTe, LiGaSeTe, LiGaSSe, LiGaSTe, KLiGaS, KLiGaSe, KLiGaTe, KNaGaS, KNaGaSe, KNaGaTe, KGaSeTe, KGaSSe, KGaSTe, CuLiGaS, CuLiGaSe, CuLiGaTe, CuNaGaS, CuNaGaSe, CuNaGaTe, CuKGaS, CuKGaSe, CuKGaTe, CuGaSeTe, CuGaSSe, CuGaSTe, AgLiGaS, AgLiGaSe, AgLiGaTe, AgNaAlS, AgNaAlSe, AgNaAlTe, AgNaGaS, AgNaGaTe, AgNaGaTe AgNaInS, AgNaInSe, AgNaInTe, AgNaTiS, AgNaTiSe, AgNaTiTe, AgKGaS, AgKGaSe, AgKGaTe, AgGaSeTe, AgGaSSe, AgGaSTe,It may include one or more of AgCuGaS, AgCuGaSe, AgCuGaTe, AgAuGaS, AgAuGaSe, AgAuGaTe, AuLiGaS, AuLiGaSe, AuLiGaTe, AuNaGaS, AuNaGaSe, AuNaGaTe, AuKGaS, AuKGaSe, AuKGaTe, AuGaSeTe, AuGaSSe, AuGaSTe, AuCuGaS, AuCuGaSe or AuCuGaTe.
[0140] Also, the 제2shell formed in the 제2shell manufacturing step (S36) is AIS, AISe, AITe, AISeS, AISeTe, AITeS, GaS, GaSe, GaTe, GaSeS, GaSeTe, GaTeS, InS, InSe, InTe, InSeS, InSeTe, InTeS, TiS, TiSe, TiTe, TiSeS, TiSeTe, TiTeS, LiGaS, LiGaSe, LiGaTe. NaGaS, NaGaSe, NaGaTe, KGaS, KGaSe, KGaTe, CuAlS, CuAlSe, CuAlTe, CuGaS, CuGaSe, CuGaTe, CuInS, CuInSe, CuInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe, AgAlTe, AuGaS, AuGaSe, AuGaTe, AgInS, AgInSe, AgInTe, AgGaS, AgGaSe, AgGaTe, AgTiS, AgTiSe, AgTiTe, AuAlS, AuAlSe, AuAlTe, AuInS, AuInSe, AuInTe, AuTiS, AuTiSe, AuTiTe, LiNaGaS, LiNaGaSe, LiNaGaTe, NaGaSeTe, NaGaSSe, NaGaSTe, LiGaSeTe, LiGaSSe, LiGaSTe, KLiGaS, KLiGaSe, KLiGaTe, KNaGaS, KNaGaTe, KNaGaTe. KGaSeTe, KGaSSe, KGaSTe, CuLiGaS, CuLiGaSe, CuLiGaTe, CuNaGaS, CuNaGaSe, CuNaGaTe, CuKGaS, CuKGaSe, CuKGaTe, CuGaSeTe, CuGaSSe, CuGaSTe, AgLiGaS, AgLiGaSe, AgLiGaTe, AgNaAlS, AgNaAlSe, AgNaAlTe, AgNaGaS, AgNaGaSe, AgNaGaTe, AgNaInS, AgNaInSe, AgNaInTe, AgNaTiS, AgNaTiSe, AgNaTiTe, AgKGaS, AgKGaSe, AgKGaTe, AgGaSeTe, AgGaSSe, AgGaSTe,It may include one or more of AgCuGaS, AgCuGaSe, AgCuGaTe, AgAuGaS, AgAuGaSe, AgAuGaTe, AuLiGaS, AuLiGaSe, AuLiGaTe, AuNaGaS, AuNaGaSe, AuNaGaTe, AuKGaS, AuKGaSe, AuKGaTe, AuGaSeTe, AuGaSSe, AuGaSTe, AuCuGaS, AuCuGaSe or AuCuGaTe.
[0141] The ligand binding step (S38) may also be substantially the same as the ligand binding step (S26) described with reference to FIG. 4, except that the ligand interacting with the aforementioned metal is bound to the surface of the second shell manufactured by the second shell manufacturing step (S36).
[0142] For example, in the ligand binding step (S38), as specifically described in the examples and comparative examples described below, a ligand that interacts with a metal is prepared in a round flask, an AgInGaS core solution is injected, and first shell precursors and second precursors are injected, so that a ligand that interacts with a metal can be bound to the surface of a nanostructure including a core, a first shell, and a second shell.
[0143] In another aspect, according to embodiments of the present disclosure, a quantum dot composition including a quantum dot (10) described with reference to FIG. 1 or a quantum dot manufactured by a manufacturing method (20) described with reference to FIGS. 2 and 3 can be provided. In the photosensitive resin composition or ink composition according to embodiments of the present disclosure, details regarding the quantum dot are the same as those regarding the quantum dot (10) according to embodiments of the present disclosure, unless otherwise described.
[0144] In addition to the quantum dot (10) bound to a ligand (15) that interacts with a metal, the quantum dot may contain various other compounds, such as capping agents, solvents, and other additives. These additional compounds can affect the properties of the quantum dot (10), such as stability, size, and optical properties.
[0145] In another aspect, according to embodiments of the present disclosure, a photosensitive resin composition or ink composition including quantum dots (10) described with reference to FIGS. 1 to 3 or quantum dots manufactured by the quantum dot manufacturing method (20, 30) described with reference to FIGS. 4 and 5 can be provided. In the photosensitive resin composition according to embodiments of the present disclosure, details regarding the quantum dots are the same as those for the quantum dots (10) according to embodiments of the present disclosure, unless otherwise described.
[0146] The photosensitive resin composition according to the present embodiments may be a photoconversion ink composition including quantum dots (10), a photocurable monomer, a photoinitiator, and a light diffuser.
[0147] Photocrosslinkable monomers include, for example, monofunctional esters such as ethylene glycol methacrylate, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, N-butyl methacrylate, T-butyl methacrylate, hexyl methacrylate, ethylhexyl methacrylate, lauryl methacrylate, octyl methacrylate, cyclohexyl methacrylate, benzyl methacrylate, tetracyclodecyl methacrylate, N-phenylmaleimide, N-cyclohexyl maleimide, methacrylic acid, isobornyl methacrylate, styrene, vinyl acetate, and vinyl pyrrolidone, and multifunctional esters such as ethylene glycol diacrylate, ethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, and triethylene glycol dimethacrylate. Examples thereof include 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, propylene glycol diacrylate, propylene glycol dimethacrylate, dipropylene glycol diacrylate, dipropylene glycol dimethacrylate, tripropylene glycol diacrylate, tripropylene glycol, dimethacrylate pentaerythritol triacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, bisphenol A epoxy acrylate, ethylene glycol monomethyl ether acrylate, trimethylolpropane triacrylate, and the like, and multi-acrylates having ethyleneoxy groups or γ or ε-lactone chains linked thereto, but are not limited thereto.
[0148] The photoinitiator may be one or more of a photopolymerization initiator and a thermal polymerization initiator.
[0149] The photopolymerization initiator may be, for example, one or more of an acetophenone-based compound, a benzophenone-based compound, a thioxanthone-based compound, a benzoin-based compound, an oxime ester-based compound, a phosphorus-based compound, and a triazine-based compound.
[0150] Thermal polymerization initiators that can be used include, for example, peroxide compounds, azobis compounds, etc.
[0151] Initiators can also be used with photosensitizers, which cause a chemical reaction by absorbing light, becoming excited, and then transferring that energy.
[0152] Examples of photosensitizers include tetraethylene glycol bis-3-mercaptopropionate, pentaerythritol tetrakis-3-mercaptopropionate, and dipentaerythritol tetrakis-3-mercaptopropionate.
[0153] According to one embodiment, the content of the quantum dots (10) may be 20 parts by weight to 60 parts by weight, for example, 25 parts by weight to 50 parts by weight, or 30 parts by weight to 45 parts by weight, based on 100 parts by weight of the total content of the quantum dot ink composition. According to one embodiment, the ink composition may not include a solvent. That is, the ink composition may be a solvent-free quantum dot ink composition. According to one embodiment, the ink composition may have a viscosity of 10 cP to 25 cP. According to one embodiment, the ink composition may have a surface tension of 30 mN / m or more at 25°C. When the above-described viscosity and / or surface tension ranges are satisfied, the ink composition may be suitably used as a solvent-free quantum dot ink composition for various components such as a color conversion member or a light-emitting layer of a light-emitting device in a solution process such as an inkjet.
[0154] In another aspect, embodiments of the present disclosure provide an optical film comprising a photosensitive resin composition.
[0155] In describing the optical film according to the embodiments of the present disclosure, details regarding the photosensitive resin composition are the same as those described for the photosensitive resin composition according to the embodiments of the present disclosure described above, unless specifically described otherwise, and thus will be omitted.
[0156] An optical film may be, for example, a wavelength conversion film that converts light of a specific wavelength into light of another specific wavelength, or a color filter. For example, an optical film according to embodiments of the present disclosure may be used as a color filter that converts the wavelength of light emitted from a backlight including a light-emitting diode, but an optical film according to embodiments of the present disclosure is not limited to a color filter or a wavelength conversion film.
[0157] An optical film can be used, for example, as a layer positioned between the cathode and anode electrodes of an electroluminescent diode, and in which light is emitted by electrons and holes arriving from the cathode and anode electrodes.
[0158] In another aspect, embodiments of the present disclosure provide an electronic device including an optical film.
[0159] According to one embodiment, an optical member formed using a photosensitive resin composition may be provided. For example, the optical member may be a color conversion member.
[0160] According to another aspect, referring to FIG. 6, an electronic device (100) according to one embodiment includes a substrate (130), a light source (120) disposed on the substrate (130), and a color conversion member (110) disposed in a path of light emitted from the light source (120), and the color conversion member (110) can be formed using the ink composition described above.
[0161] According to one implementation example, the light source (120) may be a light-emitting element. For example, the light source (120) may be an organic light-emitting diode (OLED) or an inorganic light-emitting diode (QLED or ILED).
[0162] In another aspect, referring to FIG. 7, a light emitting diode (200) according to another embodiment may include quantum dots (10). The light emitting diode (200) may include an optical film manufactured from a photosensitive resin composition including the quantum dots (10) described above.
[0163] A light emitting diode (200) according to other embodiments includes an anode (210), a cathode (230), and an intermediate layer (220) positioned therebetween. The intermediate layer (220) may include a light emitting layer comprising a photosensitive resin composition including the quantum dots (10) described above.
[0164] In addition, another aspect of the present disclosure can provide an electronic device including a display device including the aforementioned light-emitting diode and a control unit for driving the display device.
[0165] Electronic devices may include, for example, display devices, lighting devices, solar cells, portable or mobile terminals (e.g., smart phones, tablets, PDAs, electronic dictionaries, PMPs, etc.), navigation terminals, game consoles, various TVs, various computer monitors, etc., but are not limited thereto, and any form of device may be included as long as it includes the above-mentioned component(s).
[0166] Since the application of quantum dots (10) to various electronic components and devices can be easily applied by those with ordinary knowledge in the art, a detailed description thereof is omitted.
[0167] The quantum dots, methods for manufacturing quantum dots, and electronic devices according to the embodiments of the present disclosure can cause a change in the solubility of the quantum dots (10) by binding a ligand that interacts with a metal suitable for the core / shell component, thereby increasing the affinity with the photosensitive resin composition.
[0168] Furthermore, in terms of the stability of quantum dot optical films, if the quantum dot (10) includes a ligand that interacts with a metal, stability can be improved before and after heat treatment. As can be seen from the examples and comparative examples described below, this can effectively protect the surface of the quantum dot from oxygen and moisture due to the steric effect enhanced by the ligand that interacts with the metal.
[0169] The quantum dots, methods for manufacturing quantum dots, and electronic devices according to the embodiments of the present disclosure can provide quantum dots, methods for manufacturing quantum dots, and electronic devices capable of improving quantum efficiency by improving dispersibility and stability through the combination of ligands that interact with metals suitable for the components of the core / shell.
[0170] Hereinafter, embodiments according to the present disclosure will be specifically described as experimental examples, but the present disclosure is not limited to the following embodiments.
[0171] The examples below exemplarily describe a method for manufacturing a quantum dot (10) including a core (12) and first and second shells (14, 16) described with reference to FIG. 2.
[0172] At this time, Ga is exemplarily described as a group III element used in the first shell (14) and the second shell (16), and S is exemplarily described as a group VI element. In other words, an example of manufacturing AgInGaS / GaS / GaS quantum dots is exemplarily described. In addition, although oleinamine, which is an L-type ligand that interacts with a metal, is exemplarily described as a ligand that interacts with a metal, an X-type ligand or a Z-type ligand can also synthesize quantum dots by binding a ligand that interacts with a metal to the surface of a nanostructure in the same manner as the ligand binding step (S26, S38) described above, and other compounds among the L-type ligands can also synthesize quantum dots in the same manner by binding a ligand that interacts with a metal to the surface of a nanostructure in the same manner as the ligand binding step (S26, S38) described above.
[0173] Manufacturing the core (12) and the first and second shells (14, 16) using the elements described in the above-described examples in the same manner as in the examples below corresponds to a conventional technique, so a specific description thereof is omitted.
[0174] [Example]
[0175] 1. Precursor manufacturing example
[0176] (1) Precursor manufacturing example 1 (manufacturing of silver iodide-oleylamine precursor solution)
[0177] 0.56 g (2.4 mmol) of silver (I) iodide and 10 mL (30 mmol) of oleylamine were placed in a 50 mL flask, depressurized at room temperature (RT) for 1 hour, heated to 120°C for 10 minutes under reduced pressure, and reacted for 1 hour. The mixed solution was then made into an argon (Ar) atmosphere and cooled to room temperature to prepare a silver (Ag) precursor solution. The silver (Ag) concentration of the precursor solution is 0.24 M.
[0178] (2) Precursor manufacturing example 2 (manufacturing of indium chloride-ethanol precursor solution)
[0179] An indium (In) precursor solution was prepared by adding 0.11 g (0.5 mmol) of indium (III) chloride and 5 mL of ethanol to a 10 mL vial. The indium (In) concentration of the precursor solution was 0.10 M.
[0180] (3) Precursor manufacturing example 3 (manufacturing of gallium chloride-toluene precursor solution)
[0181] A gallium (Ga) precursor solution was prepared by adding 0.80 g (4.54 mmol) of gallium (III) chloride and 0.8 mL of toluene to a 10 mL vial. The gallium (Ga) concentration of the precursor solution was 5.68 M.
[0182] (4) Precursor manufacturing example 4 (manufacturing of gallium acetylacetonate-toluene precursor solution)
[0183] A gallium (Ga) precursor solution was prepared by adding 1.67 g (4.54 mmol) of gallium (III) acetylacetonate and 16 mL of toluene to a 20 mL vial. The gallium (Ga) concentration of the precursor solution was 0.28 M.
[0184] (5) Precursor manufacturing example 5 (manufacturing of sulfur-oleylamine precursor solution)
[0185] 0.305 g (9.5 mmol) of sulfur (S) and 9.5 mL (28.5 mmol) of oleylamine were placed in a 50 mL flask, depressurized at room temperature (RT) for 30 minutes, heated to 120 °C for 10 minutes under reduced pressure, and reacted for 1 hour. The mixed solution was then made into an argon (Ar) atmosphere and cooled to room temperature to prepare a sulfur (S) precursor solution. The sulfur (S) concentration of the precursor solution is 1 M.
[0186] 2. Comparative example of AgInGaS nanostructure-L type ligand
[0187] (1) Comparative Example 1 (AgInGaS / AgGaS nanostructure with L-type ligand (5 wt%))
[0188] 1) Prepare 16 ml of octadecene in a 50 mL three-necked round flask with a reflux, heat to 120 °C, and maintain the pressure at approximately 0.005 torr using a vacuum pump for 30 minutes. After replacing the atmosphere with a nitrogen (N2) at 120 °C, inject the AgInGaS core / AgGaS shell solution of Example 1 (1-2) and inject 6.2 mmol of gallium (III) acetylacetonate-toluene and 4.2 mmol of sulfur-oleylamine, and then remove toluene using a vacuum pump. After replacing the atmosphere with a nitrogen (N2), the reaction is performed at 310 °C for 100 minutes.
[0189] 2) After injecting 5 ml of a mixed solution of tris dimethylamino phosphine ((PDEA)3) + trioctylphosphine (TOP) at a temperature of 280 °C, the temperature is reduced to room temperature, and then an AgInGaS / AgGaS / GaS quantum dot composition solution is obtained.
[0190] 3) The synthesized quantum dot composition solution was dispersed in toluene at a ratio of 1:1. The solution dispersed in toluene was mixed with ethanol at a ratio of 1:3, centrifuged at 5000 RPM for 1 minute, and dried in a vacuum oven for 24 hours to obtain 0.1 g of quantum dots. Through thermogravimetric analysis (TGA), it was confirmed that the weight ratio of the ligand to the sum of the nanostructure and ligand was 5 wt%.
[0191] (2) Comparative Example 2 (AgInGaS / AgGaS / GaS nanostructure with L-type ligand (5 wt%))
[0192] 1) Prepare 16 ml of octadecene in a 50 mL three-necked round flask with a reflux, heat to 120 °C, and maintain the pressure at approximately 0.005 torr using a vacuum pump for 30 minutes. After replacing the atmosphere with nitrogen (N2) at 120 °C, inject the AgInGaS core / AgGaS shell solution of Example 1 (1-2), inject 6.2 mmol of gallium (III) acetylacetonate-toluene, and 4.2 mmol of sulfur-oleylamine, and then remove toluene using a vacuum pump. Afterwards, the reaction is performed at 310 °C for 100 minutes after replacing with a nitrogen (N2) atmosphere, and then 0.5 ml of dodecanethiol, a thiol ligand, is injected at 260 °C to cool the reaction.
[0193] 2) After injecting 5 ml of a mixed solution of tris dimethylamino phosphine ((PDEA)3) + trioctylphosphine (TOP) at a temperature of 280 °C, the temperature is reduced to room temperature, and then an AgInGaS / AgGaS / GaS quantum dot composition solution is obtained.
[0194] 3) The synthesized quantum dot composition solution was dispersed in toluene at a ratio of 1:1. The solution dispersed in toluene was mixed with ethanol at a ratio of 1:3, centrifuged at 5000 RPM for 1 minute, and dried in a vacuum oven for 24 hours to obtain 0.1 g of quantum dots. Through thermogravimetric analysis (TGA), it was confirmed that the weight ratio of the ligand to the sum of the nanostructure and ligand was 5 wt%.
[0195] (3) Comparative Example 3 (AgInGaS / AgGaS / GaS nanostructure with L-type ligand (55 wt%))
[0196] Quantum dots (0.1 g) were obtained by manufacturing in the same manner as in Comparative Example 2, except that 60 ml of octadecene was used in process 1) of Comparative Example 2, and it was confirmed through thermogravimetric analysis (TGA) that the organic ligand ratio of the manufactured quantum dots to 0.1 g of the quantum dots containing inorganic and organic substances was 55 wt%.
[0197] 3. AgInGaS nanostructures - Comparative examples of L, X, and Z type ligands
[0198] (1) Comparative Example 4 (AgInGaS / AgGaS / GaS nanostructure with L, X, Z type ligands (5 wt%))
[0199] 1) Prepare 16 ml of oleylamine in a 50 mL three-necked round flask with a reflux device, heat to 120 °C, and maintain the pressure at approximately 0.005 torr using a vacuum pump for 30 minutes. After replacing the atmosphere with nitrogen (N2) at 120 °C, inject the AgInGaS core / AgGaS shell solution of Comparative Example 1, then inject 6.2 mmol of gallium (Ⅲ) acetylacetonate-toluene and 4.2 mmol of sulfur-oleylamine, and then remove toluene using a vacuum pump. Afterwards, the reaction is performed at 310 °C for 100 minutes after replacing with a nitrogen (N2) atmosphere, and then 0.5 ml of dodecanethiol, a thiol ligand, is injected at 260 °C to cool the reaction.
[0200] 2) After injecting 5 ml of a mixed solution of tris dimethylamino phosphine ((PDEA)3) + trioctylphosphine (TOP) at a temperature of 280 °C, the temperature is reduced to room temperature, and then an AgInGaS / AgGaS / GaS quantum dot composition solution is obtained.
[0201] 3) The synthesized quantum dot composition solution was dispersed in toluene at a ratio of 1:1. The solution dispersed in toluene was mixed with ethanol at a ratio of 1:3, centrifuged at 5000 RPM for 1 minute, and dispersed in 5 ml of hexane.
[0202] 4) The AgInGaS / AgGaS / GaS quantum dot composition dispersed in hexane was mixed with ethanol in a 1:3 ratio and centrifuged at 5000 RPM for 1 minute. The same process was repeated 3 times and dried in a vacuum oven for 24 hours to obtain 0.1 g of quantum dots. Thermogravimetric analysis (TGA) measurement confirmed that the weight ratio of the ligand to the sum of the nanostructure and ligand was 5 wt%.
[0203] 4. AgInGaS nanostructures - L-type, X-type, and Z-type ligand examples
[0204] (1) Example 1 (AgInGaS / AgGaS nanostructure with L-type ligand (10 wt%))
[0205] (1-1) AgInGaS core manufacturing
[0206] 1) In a 50 mL three-necked round flask with a reflux device, 0.3 g of gallium(III) acetylacetonate-toluene and trioctylphosphine oxide (TOPO) prepared in Precursor Preparation Example 4, 5 ml of silver(I) iodide-oleylamine prepared in Precursor Preparation Example 1, and indium(III) chloride-ethanol and 1-octadecene prepared in Precursor Preparation Example 2 are added, heated to 120 °C, and maintained at approximately 0.005 torr for 30 minutes using a vacuum pump.
[0207] 2) Then, after replacing the atmosphere with nitrogen (N2), 1 ml (0.03 g, 1 mmol) of the sulfur-oleylamine (S-oleylamine) solution prepared in the precursor preparation example 5 and 0.5 ml of 1-dodecanethiol are injected at 120 °C.
[0208] 3) After adding the above sulfur-oleylamine (S-oleylamine) solution, maintain the temperature at approximately 0.005 torr using a vacuum pump at 120 °C for 30 minutes. Then, stir at 190 °C for 10 minutes to complete the reaction.
[0209] 4) Inject 5 ml of a mixed solution of tris dimethylamino phosphine (PDEA)3 and trioctylphosphine (TOP) at 280 °C and then cool to room temperature.
[0210] 5) Prepare 50 ml of AgInGaS core-ethanol solution by adding 42.5 ml of ethanol to the manufactured AgInGaS nanostructure core solution.
[0211] 6) The above solution is centrifuged at 5000 RPM for 5 minutes and then dispersed in 1.2 ml of toluene. The dispersed AgInGaS core-toluene solution is centrifuged at 5000 RPM for 1 minute to remove impurities, and a AgInGaS core nanostructure solution is obtained.
[0212] (1-2) Fabrication of AgInGaS core / AgGaS shell with ligand interacting with metal
[0213] 1) Prepare 2 ml of oleylamine and 15 ml of octadecene in a 50 mL three-necked round flask with a reflux device, heat to 120 °C, and maintain the temperature at approximately 0.005 torr for 30 minutes using a vacuum pump. After replacing the atmosphere with nitrogen (N2) at 120 °C, inject the AgInGaS core solution, then inject 0.13 mmol of silver(I) iodide, 7 mmol of gallium(III) acetylacetonate prepared in Precursor Preparation Example 4, and 6 mmol of sulfur-oleylamine prepared in Precursor Preparation Example 5, and then remove toluene using a vacuum pump. Afterwards, the reaction is performed at 310 °C for 100 minutes after replacing with a nitrogen (N2) atmosphere, and then 0.5 ml of dodecanethiol, a thiol ligand, is injected at 260 °C to cool the reaction.
[0214] 2) After injecting 5 ml of a mixed solution of tris dimethylamino phosphine ((PDEA)3) and trioctylphosphine (TOP) at 280 °C, the temperature is reduced to room temperature to obtain an AgInGaS core / AgGaS shell solution.
[0215] 3) The synthesized quantum dot composition solution was dispersed in toluene at a ratio of 1:1. The solution dispersed in toluene was mixed with ethanol at a ratio of 1:3, centrifuged at 5000 RPM for 1 minute, and dried in a vacuum oven for 24 hours to obtain 0.1 g of quantum dots. It was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and ligand was 10 wt%.
[0216] (2) Example 2 (AgInGaS / AgGaS nanostructure with L-type ligand (20 wt%))
[0217] Quantum dots (0.1 g) were obtained by manufacturing in the same manner as in Example 1, except that 4 ml of oleylamine and 13 ml of octadecene were used in (1-2) of the above Example 1, and it was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and the ligand was 20 wt%.
[0218] (3) Example 3 (AgInGaS / AgGaS nanostructure with L-type ligand (30 wt%))
[0219] Quantum dots (0.1 g) were obtained by manufacturing in the same manner as in Example 1, except that 6 ml of oleylamine and 10 ml of octadecene were used in (1-2) of the above Example 1, and it was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and the ligand was 30 wt%.
[0220] (4) Example 4 (AgInGaS / AgGaS nanostructure with L-type ligand (40 wt%))
[0221] Quantum dots (0.1 g) were obtained by manufacturing in the same manner as in Example 1, except that 10 ml of oleylamine and 6 ml of octadecene were used in (1-2) of the above Example 1, and it was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and the ligand was 40 wt%.
[0222] (5) Example 5 (AgInGaS / AgGaS nanostructure with L-type ligand (50 wt%))
[0223] Quantum dots (0.1 g) were obtained by manufacturing in the same manner as in Example 1, except that 16 ml of oleylamine was used in (1-2) of the above Example 1 and octadecene was not used. It was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and the ligand was 50 wt%.
[0224] (6) Example 6 (AgInGaS / AgGaS / GaS nanostructure with L-type ligand (10 wt%))
[0225] 1) Prepare 2 ml of oleylamine and 15 ml of octadecene in a 50 mL three-necked round flask with a reflux device, heat to 120 °C, and maintain the temperature at approximately 0.005 torr using a vacuum pump for 30 minutes. After replacing the atmosphere with nitrogen (N2) at 120 °C, inject the AgInGaS core / AgGaS shell solution of Example 5, then inject 6.2 mmol of gallium (III) acetylacetonate-toluene and 4.2 mmol of sulfur-oleylamine, and then remove toluene using a vacuum pump. Afterwards, the reaction is performed at 310 °C for 100 minutes after replacing with a nitrogen (N2) atmosphere, and then 0.5 ml of dodecanethiol, a thiol ligand, is injected at 260 °C to cool the reaction.
[0226] 2) After injecting 5 ml of a mixed solution of tris dimethylamino phosphine ((PDEA)3) + trioctylphosphine (TOP) at a temperature of 280 °C, the temperature is reduced to room temperature, and then an AgInGaS / AgGaS / GaS quantum dot composition solution is obtained.
[0227] 3) The synthesized quantum dot composition solution was dispersed in toluene at a ratio of 1:1. The solution dispersed in toluene was mixed with ethanol at a ratio of 1:3, centrifuged at 5000 RPM for 1 minute, and dried in a vacuum oven for 24 hours to obtain 0.1 g of quantum dots. The weight ratio of the ligand to the sum of the nanostructure and ligand was confirmed to be 10 wt% through thermogravimetric analysis (TGA).
[0228] (7) Example 7 (AgInGaS / AgGaS / GaS nanostructure with L-type ligand (20 wt%))
[0229] Quantum dots (0.1 g) were obtained by manufacturing in the same manner as in Example 6, except that 4 ml of oleylamine and 13 ml of octadecene were used in step 1) of Example 6, and it was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and the ligand was 20 wt%.
[0230] (8) Example 8 (AgInGaS / AgGaS / GaS nanostructure with L-type ligand (30 wt%))
[0231] Quantum dots (0.1 g) were obtained by manufacturing in the same manner as in Example 6, except that 6 ml of oleylamine and 10 ml of octadecene were used in step 1) of Example 6, and it was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and the ligand was 30 wt%.
[0232] (9) Example 9 (AgInGaS / AgGaS / GaS nanostructure with L-type ligand (40 wt%))
[0233] Quantum dots (0.1 g) were obtained by manufacturing in the same manner as in Example 6, except that 10 ml of oleylamine and 6 ml of octadecene were used in step 1) of Example 6, and it was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and the ligand was 40 wt%.
[0234] (10) Example 10 (AgInGaS / AgGaS / GaS nanostructure with L-type ligand (50 wt%))
[0235] Quantum dots (0.1 g) were obtained by manufacturing in the same manner as in Example 6, except that 16 ml of oleylamine was used and octadecene was not used in step 1) of Example 6, and it was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and the ligand was 50 wt%.
[0236] (11) Example 11 (AgInGaS / AgGaS / GaS nanostructure with X-type ligand (40 wt%))
[0237] In the process 1) of the above Example 6, 10 ml of tris diethylamino phosphine was used instead of oleylamine to produce 0.1 g of quantum dots using the same method as Example 6, and it was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and the ligand was 40 wt%.
[0238] (12) Example 12 (AgInGaS / AgGaS / GaS nanostructure with X-type ligand (50 wt%))
[0239] In the process 1) of the above Example 6, 13 ml of tris diethylamino phosphine was used instead of oleylamine to produce 0.1 g of quantum dots using the same method as Example 6, and it was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and the ligand was 50 wt%.
[0240] (13) Example 13 (AgInGaS / AgGaS / GaS nanostructure with Z-type ligand (40 wt%))
[0241] In the process 1) of the above Example 6, 16 mmol of gallium (III) acetylacetonate-toluene was used instead of 6.2 mmol of gallium (III) acetylacetonate-toluene, and 0.1 g of quantum dots were obtained by the same method as Example 6, and it was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and the ligand was 50 wt%.
[0242] (14) Example 14 (AgInGaS / AgGaS / GaS nanostructure with Z-type ligand (50 wt%))
[0243] In the process 1) of the above Example 6, 20 mmol of gallium (III) acetylacetonate-toluene was used instead of 6.2 mmol of gallium (III) acetylacetonate-toluene, and 0.1 g of quantum dots were obtained by the same method as Example 6, and it was confirmed through thermogravimetric analysis (TGA) that the weight ratio of the ligand to the sum of the nanostructure and the ligand was 50 wt%.
[0244] 5. AgInGaS nanostructures - L, X, Z type ligand examples
[0245] (1) Example 15 (AgInGaS / AgGaS / GaS nanostructures with L, X, and Z type ligands (50 wt%))
[0246] 1) Prepare 16 ml of oleylamine in a 50 mL three-necked round flask with a reflux device, heat to 120 °C, and maintain the temperature at approximately 0.005 torr using a vacuum pump for 30 minutes. After replacing the atmosphere with nitrogen (N2) at 120 °C, inject the AgInGaS core / AgGaS shell solution of Example 5, then inject 6.2 mmol of gallium(Ⅲ) acetylacetonate-toluene and 4.2 mmol of sulfur-oleylamine, and then remove toluene using a vacuum pump. Afterwards, the reaction is performed at 310 °C for 100 minutes after replacing with a nitrogen (N2) atmosphere, and then 0.5 ml of dodecanethiol, a thiol ligand, is injected at 260 °C to cool the reaction.
[0247] 2) After injecting 5 ml of a mixed solution of tris dimethylamino phosphine ((PDEA)3) + trioctylphosphine (TOP) at a temperature of 280 °C, the temperature is reduced to room temperature, and then an AgInGaS / AgGaS / GaS quantum dot composition solution is obtained.
[0248] 3) The synthesized quantum dot composition solution was dispersed in toluene at a ratio of 1:1. The solution dispersed in toluene was mixed with ethanol at a ratio of 1:3, centrifuged at 5000 RPM for 1 minute, and dispersed in 5 ml of hexane.
[0249] 4) The AgInGaS / AgGaS / GaS quantum dot composition dispersed in hexane was mixed with ethanol in a 1:3 ratio and centrifuged at 5000 RPM for 1 minute. The same process was repeated 3 times and dried in a vacuum oven for 24 hours to obtain 0.1 g of quantum dots. Thermogravimetric analysis (TGA) measurement confirmed that the weight ratio of the ligand to the sum of the nanostructure and ligand was 50 wt%.
[0250] [Experimental Example]
[0251] The optical properties of the quantum dots manufactured by the examples and comparative examples as described above were measured using a QE-2000 device from Otsuka Electronics and a Q50 THERMOGRAVIMETRIC ANALYZER device from TA INSTRUMENTS.
[0252] Table 1 shows the results measured using the QE-2000 equipment from Otsuka Electronics and the Q50 THERMOGRAVIMETRIC ANALYZER equipment from TA INSTRUMENTS. The optical properties and thermal stability of quantum dots were measured by dispersing them in octadecene. The results confirming the optical properties [emission peak wavelength, quantum yield, full width at half maximum (FWHM)] and thermal stability of quantum dots are presented.
[0253]
[0254] [Table 1]
[0255]
[0256]
[0257]
[0258] Referring to Table 1, comparing Comparative Examples 1 to 4 and Examples 1 to 11 in Table 1, it can be confirmed that Examples 1 to 11 are superior to Comparative Examples 1 to 2 in terms of half-maximum width, quantum efficiency, and thermal stability.
[0259] When the weight ratio of the ligand exceeds 50 wt%, the half-width increases or the quantum efficiency decreases due to uneven growth of the quantum dots. (See Comparative Examples 1, 2, and 4)
[0260] In addition, when the weight ratio of the ligand is less than 5 wt%, the amount of ligand that eliminates dangling bonds and provides dispersibility decreases, resulting in decreased dispersibility and stability, which in turn lowers quantum efficiency. (See Comparative Example 4)
[0261] Quantum dots are composed of nanostructures and ligands. Generally, the inorganic substances contained in the nanostructures act as quantum dots that enable light emission, and the organic substances contained in the ligands strengthen the binding energy of the quantum dots or act as ligands to eliminate dangling bonds and provide dispersibility. Quantum dots, which are nanoparticles containing such nanostructures and ligands, contain ligands that interact with metals along with cationic sites and anionic sites, and the ligands are composed of L-type ligands, X-type ligands, Z-type ligands, or a combination thereof.
[0262] X-type ligands, such as thiol groups, halide groups, and phosphine groups, have very strong binding energies and are very effective in improving stability. They are also excellent in suppressing surface defects, resulting in high quantum efficiency. (See Examples 11 and 12)
[0263] On the other hand, referring to comparative examples 1 and 2, in the case of materials such as octadecane, the contribution to quantum dot synthesis is low, resulting in small size and low quantum efficiency.
[0264] In the case of synthesizing quantum dots composed of nanostructures and ligands, the change in luminescence characteristics according to the content of the nanoprecursor forming the quantum dot is important, but the type and ratio of the ligand used in the synthesis are important factors in determining the optical and physical properties of the quantum dot.
[0265] In the above-described examples, AgInGaS / AgGaS / GaS quantum dots in which Ag is used as the Group I element in the first shell and the second shell, Ga is used as the Group III element, and S is used as the Group VI element have been representatively described. However, the Group III element included in the first and second shells (14, 16) is one of Al, In, and Tl in addition to Ga, the Group VI element is one of Se and Te in addition to S, and even if Group I elements (Li, Na, K, Rb, Cs, Cu, Ag, and Au) are additionally included, the AgInGaS / first shell / second shell quantum dots can also improve the luminescence efficiency for the same reasons as described above.
[0266] The embodiments of the present disclosure described above are briefly described below.
[0267] In one aspect, embodiments of the present disclosure provide a quantum dot comprising a core comprising Ag, In, Ga, and S, a nanostructure comprising a shell disposed on the core, and a ligand interacting with a metal bound to a surface of the nanostructure, wherein the ligand is at least one selected from an L-type ligand which is a two-electron donor, an X-type ligand which is a one-electron donor, and a Z-type ligand which is an electron acceptor, and wherein a weight ratio of the ligand to the sum of the nanostructure and the ligand is greater than 5 wt% and less than or equal to 50 wt%.
[0268] The L-type ligand may be at least one selected from oleylamine, N,N,N',N'-tetramethylethylene-1,2-diamine, pyridine tri-n-butylphosphine oxide, tri-n-octylphosphine oxide, and 5,8-Dimethyl-4,7,10-trioxatridecane-2,12-diamine.
[0269] The X-type ligand may be at least one selected from oleic acid, tetradecanol, a thiol group, a halide group, an O2CR group, and a phosphine group, and in the O2CR group, R is selected from the group consisting of a substituted or unsubstituted alkyl group, an alkenyl group, a cycloalkyl group, a cycloalkenyl group, a heterocyclyl group, an amino group, an alkylamino group, a dialkylamino group, an arylalkyl group, a silyl group, an aryl group, a heteroaryl group, or a combination thereof.
[0270] The thiol group may be at least one selected from a dodecanethiol group, an adamantanethiol group, an octanethiol group, a 6-mercapto-1-hexanol group, and a 6-amino-1-hexanol group.
[0271] The halide group may be one or more selected from -F, -Cl, -I, and -Br.
[0272] The O2CR group may be at least one selected from a carboxylate group, an octanoate group, a crotonate group, a dimethylacrylate group, a benzoate group, a p-toluate group, and an oxo (OXO) group.
[0273] The phosphine group may be at least one selected from a tris methyl silyl phosphine group, a tris dimethylamino phosphine group, a tris diethylamino phosphine group, a tris carboxyethyl phosphine hydrochloride group, a tris (hydroxypropyl) phosphine group, and a 2-diphenylphosphinobenzaldehyde group.
[0274] The Z-type ligand may be one or more selected from a metal and an alkyl group.
[0275] The metal may be one or more selected from In, P, Ga, Ag, Cd, Zn, Se, S, Al, Cu, Li, Au, K, Na, Pb and Cs.
[0276] The alkyl group may be at least one selected from a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a Sec-butyl group, an n-pentyl group, an isopentyl group, a hexyl group, a heptyl group, and an octyl group.
[0277] The shell may include at least one selected from a Group I element or a Group III element and a Group VI element. The Group I element may include one or more selected from Li, Na, K, Rb, Cs, Cu, Ag, and Au, the Group III element may include one or more selected from Al, Ga, In, and Tl, and the Group VI element may include one or more selected from S, Se, and Te.
[0278] The shell includes a first shell disposed on the core and including at least one selected from a group I element and a group III element and a group VI element, a second shell disposed on the first shell and including at least one selected from a group I element and a group III element and a group VI element, wherein the group I element includes at least one selected from Li, Na, K, Rb, Cs, Cu, Ag, and Au, the group III element includes at least one selected from Al, Ga, In, and Tl, and the group VI element may include at least one selected from S, Se, and Te.
[0279] 제1은 AIS, AISe, AITe, AISeS, AISeTe, AITeS, GaS, GaSe, GaTe, GaSeS, GaSeTe, GaTeS, InS, InSe, InTe, InSeS, InSeTe, InTeS, TiS, TiSe, TiTe, TiSeS, TiSeTe, TiTeS, LiGaS, LiGaSe, LiGaTe, NaGaS, NaGaSe, NaGaTe, KGaS, KGaSe, KGaTe, CuAlS, CuAlSe, CuAlTe, CuGaS, CuGaSe, CuGaTe, CuInS, CuInSe, CuInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe, AgAlTe, AgGaS, AgGaSe, AgGaTe, AuGaS, AuGaSe, AuGaTe, AgInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe. AuAlS, AuAlSe, AuAlTe, AuInS, AuInSe, AuInTe, AuTiS, AuTiSe, AuTiTe, LiNaGaS, LiNaGaSe, LiNaGaTe, NaGaSeTe, NaGaSSe, NaGaSTe, LiGaSeTe, LiGaSSe, LiGaSTe, KLiGaS, KLiGaSe, KLiGaTe, KNaGaS, KNaGaSe, KNaGaTe, KGaSeTe, KGaSSe, KGaSTe. CuLiGaS, CuLiGaSe, CuLiGaTe, CuNaGaS, CuNaGaSe, CuNaGaTe, CuKGaS, CuKGaSe, CuKGaTe, CuGaSeTe, CuGaSSe, CuGaSTe, AgLiGaS, AgLiGaSe, AgLiGaTe, AgNaAlS, AgNaAlSe, AgNaAlTe, AgNaGaS, AgNaGaSe, AgNaInSe, AgNaInTe, AgNaTiS, AgNaTiSe, AgNaTiTe, AgKGaS, AgKGaSe, AgKGaTe, AgGaSeTe, AgGaSSe, AgGaSTe, AgCuGaS, AgCuGaSe,It may include one or more of AgCuGaTe, AgAuGaS, AgAuGaSe, AgAuGaTe, AuLiGaS, AuLiGaSe, AuLiGaTe, AuNaGaS, AuNaGaSe, AuNaGaTe, AuKGaS, AuKGaSe, AuKGaTe, AuGaSeTe, AuGaSSe, AuGaSTe, AuCuGaS, AuCuGaSe or AuCuGaTe.
[0280] 제2은 AIS, AISe, AITe, AISeS, AISeTe, AITeS, GaS, GaSe, GaTe, GaSeS, GaSeTe, GaTeS, InS, InSe, InTe, InSeS, InSeTe, InTeS, TiS, TiSe, TiTe, TiSeS, TiSeTe, TiTeS, LiGaS, LiGaSe, LiGaTe, NaGaS, NaGaSe, NaGaTe, KGaS, KGaSe, KGaTe, CuAlS, CuAlSe, CuAlTe, CuGaS, CuGaSe, CuGaTe, CuInS, CuInSe, CuInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe, AgAlTe, AgGaS, AgGaSe, AgGaTe, AuGaS, AuGaSe, AuGaTe, AgInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe. AuAlS, AuAlSe, AuAlTe, AuInS, AuInSe, AuInTe, AuTiS, AuTiSe, AuTiTe, LiNaGaS, LiNaGaSe, LiNaGaTe, NaGaSeTe, NaGaSSe, NaGaSTe, LiGaSeTe, LiGaSSe, LiGaSTe, KLiGaS, KLiGaSe, KLiGaTe, KNaGaS, KNaGaSe, KNaGaTe, KGaSeTe, KGaSSe, KGaSTe. CuLiGaS, CuLiGaSe, CuLiGaTe, CuNaGaS, CuNaGaSe, CuNaGaTe, CuKGaS, CuKGaSe, CuKGaTe, CuGaSeTe, CuGaSSe, CuGaSTe, AgLiGaS, AgLiGaSe, AgLiGaTe, AgNaAlS, AgNaAlSe, AgNaAlTe, AgNaGaS, AgNaGaSe, AgNaInSe, AgNaInTe, AgNaTiS, AgNaTiSe, AgNaTiTe, AgKGaS, AgKGaSe, AgKGaTe, AgGaSeTe, AgGaSSe, AgGaSTe, AgCuGaS, AgCuGaSe,It may include one or more of AgCuGaTe, AgAuGaS, AgAuGaSe, AgAuGaTe, AuLiGaS, AuLiGaSe, AuLiGaTe, AuNaGaS, AuNaGaSe, AuNaGaTe, AuKGaS, AuKGaSe, AuKGaTe, AuGaSeTe, AuGaSSe, AuGaSTe, AuCuGaS, AuCuGaSe or AuCuGaTe.
[0281] In another aspect, embodiments of the present disclosure provide a method for manufacturing quantum dots.
[0282] The quantum dot manufacturing method includes a core manufacturing step, a shell manufacturing step, and a ligand binding step.
[0283] The core manufacturing step is a step of manufacturing a core. The core manufacturing step is a step of manufacturing a core by injecting a silver precursor, an indium precursor, a gallium precursor, a sulfur precursor, and a solvent into a first reactor and reacting them.
[0284] The shell manufacturing step is a step of manufacturing a shell by injecting the manufactured core into a second reactor equipped with a precursor containing a specific element and reacting the core.
[0285] The ligand binding step is a step of binding a ligand that interacts with a metal to the manufactured shell. The ligand may be one or more selected from the aforementioned L-type ligand, X-type ligand, and Z-type ligand.
[0286] The weight ratio of the above-mentioned ligand may be greater than 5 wt% and less than 50 wt% compared to the sum of the nanostructure and the ligand.
[0287] The quantum dot manufacturing method further includes a second shell manufacturing step of manufacturing a second shell on the shell, in addition to the core manufacturing step and the shell manufacturing step. In other words, the shell manufacturing step may include a first shell manufacturing step and a second shell manufacturing step.
[0288] The first shell and the second shell may independently contain at least one selected from a group I element or a group III element and a group VI element.
[0289] The second shell manufacturing step is a step of manufacturing a second shell placed on the first shell.
[0290] The core manufacturing steps may include Step 1-1 and Step 1-2.
[0291] Step 1-1 may be a step of preparing a core solution by injecting a silver precursor, an indium precursor, a gallium precursor, a sulfur precursor, and a solvent into a first reactor and heating them.
[0292] Steps 1 and 2 may be steps of adding a purification solvent to the core solution, centrifuging, and dispersing the precipitate separated through centrifugation in a dispersion solvent.
[0293] The L-type ligand may be at least one selected from oleylamine, N,N,N',N'-tetramethylethylene-1,2-diamine, pyridine tri-n-butylphosphine oxide, tri-n-octylphosphine oxide, and 5,8-Dimethyl-4,7,10-trioxatridecane-2,12-diamine.
[0294] The X-type ligand may be at least one selected from oleic acid, tetradecanol, a thiol group, a halide group, an O2CR group, and a phosphine group.
[0295] In the O2CR group, R is selected from the group consisting of a substituted or unsubstituted alkyl group, an alkenyl group, a cycloalkyl group, a cycloalkenyl group, a heterocyclyl group, an amino group, an alkylamino group, a dialkylamino group, an arylalkyl group, a silyl group, an aryl group, a heteroaryl group, or a combination thereof.
[0296] The phosphine group may be at least one selected from a tris methyl silyl phosphine group, a tris dimethylamino phosphine group, a tris diethylamino phosphine group, a tris carboxyethyl phosphine hydrochloride group, a tris (hydroxypropyl) phosphine group, and a 2-diphenylphosphinobenzaldehyde group.
[0297] The Z-type ligand may be one or more selected from a metal and an alkyl group.
[0298] The metal may be one or more selected from In, P, Ga, Ag, Cd, Zn, Se, S, Al, Cu, Li, Au, K, Na, Pb and Cs.
[0299] The alkyl group may be at least one selected from a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a Sec-butyl group, an n-pentyl group, an isopentyl group, a hexyl group, a heptyl group, and an octyl group.
[0300] The shell may include at least one selected from a Group I element or a Group III element and a Group VI element. The Group I element may include one or more selected from Li, Na, K, Rb, Cs, Cu, Ag, and Au, the Group III element may include one or more selected from Al, Ga, In, and Tl, and the Group VI element may include one or more selected from S, Se, and Te.
[0301] The shell includes a first shell disposed on the core and including at least one selected from a group I element and a group III element and a group VI element, a second shell disposed on the first shell and including at least one selected from a group I element and a group III element and a group VI element, wherein the group I element includes at least one selected from Li, Na, K, Rb, Cs, Cu, Ag, and Au, the group III element includes at least one selected from Al, Ga, In, and Tl, and the group VI element may include at least one selected from S, Se, and Te.
[0302] 제1은 AIS, AISe, AITe, AISeS, AISeTe, AITeS, GaS, GaSe, GaTe, GaSeS, GaSeTe, GaTeS, InS, InSe, InTe, InSeS, InSeTe, InTeS, TiS, TiSe, TiTe, TiSeS, TiSeTe, TiTeS, LiGaS, LiGaSe, LiGaTe, NaGaS, NaGaSe, NaGaTe, KGaS, KGaSe, KGaTe, CuAlS, CuAlSe, CuAlTe, CuGaS, CuGaSe, CuGaTe, CuInS, CuInSe, CuInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe, AgAlTe, AgGaS, AgGaSe, AgGaTe, AuGaS, AuGaSe, AuGaTe, AgInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe. AuAlS, AuAlSe, AuAlTe, AuInS, AuInSe, AuInTe, AuTiS, AuTiSe, AuTiTe, LiNaGaS, LiNaGaSe, LiNaGaTe, NaGaSeTe, NaGaSSe, NaGaSTe, LiGaSeTe, LiGaSSe, LiGaSTe, KLiGaS, KLiGaSe, KLiGaTe, KNaGaS, KNaGaSe, KNaGaTe, KGaSeTe, KGaSSe, KGaSTe. CuLiGaS, CuLiGaSe, CuLiGaTe, CuNaGaS, CuNaGaSe, CuNaGaTe, CuKGaS, CuKGaSe, CuKGaTe, CuGaSeTe, CuGaSSe, CuGaSTe, AgLiGaS, AgLiGaSe, AgLiGaTe, AgNaAlS, AgNaAlSe, AgNaAlTe, AgNaGaS, AgNaGaSe, AgNaInSe, AgNaInTe, AgNaTiS, AgNaTiSe, AgNaTiTe, AgKGaS, AgKGaSe, AgKGaTe, AgGaSeTe, AgGaSSe, AgGaSTe, AgCuGaS, AgCuGaSe,It may include one or more of AgCuGaTe, AgAuGaS, AgAuGaSe, AgAuGaTe, AuLiGaS, AuLiGaSe, AuLiGaTe, AuNaGaS, AuNaGaSe, AuNaGaTe, AuKGaS, AuKGaSe, AuKGaTe, AuGaSeTe, AuGaSSe, AuGaSTe, AuCuGaS, AuCuGaSe or AuCuGaTe.
[0303] 제2은 AIS, AISe, AITe, AISeS, AISeTe, AITeS, GaS, GaSe, GaTe, GaSeS, GaSeTe, GaTeS, InS, InSe, InTe, InSeS, InSeTe, InTeS, TiS, TiSe, TiTe, TiSeS, TiSeTe, TiTeS, LiGaS, LiGaSe, LiGaTe, NaGaS, NaGaSe, NaGaTe, KGaS, KGaSe, KGaTe, CuAlS, CuAlSe, CuAlTe, CuGaS, CuGaSe, CuGaTe, CuInS, CuInSe, CuInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe, AgAlTe, AgGaS, AgGaSe, AgGaTe, AuGaS, AuGaSe, AuGaTe, AgInTe, CuTiS, CuTiSe, CuTiTe, AgAlS, AgAlSe. AuAlS, AuAlSe, AuAlTe, AuInS, AuInSe, AuInTe, AuTiS, AuTiSe, AuTiTe, LiNaGaS, LiNaGaSe, LiNaGaTe, NaGaSeTe, NaGaSSe, NaGaSTe, LiGaSeTe, LiGaSSe, LiGaSTe, KLiGaS, KLiGaSe, KLiGaTe, KNaGaS, KNaGaSe, KNaGaTe, KGaSeTe, KGaSSe, KGaSTe. CuLiGaS, CuLiGaSe, CuLiGaTe, CuNaGaS, CuNaGaSe, CuNaGaTe, CuKGaS, CuKGaSe, CuKGaTe, CuGaSeTe, CuGaSSe, CuGaSTe, AgLiGaS, AgLiGaSe, AgLiGaTe, AgNaAlS, AgNaAlSe, AgNaAlTe, AgNaGaS, AgNaGaSe, AgNaInSe, AgNaInTe, AgNaTiS, AgNaTiSe, AgNaTiTe, AgKGaS, AgKGaSe, AgKGaTe, AgGaSeTe, AgGaSSe, AgGaSTe, AgCuGaS, AgCuGaSe,It may include one or more of AgCuGaTe, AgAuGaS, AgAuGaSe, AgAuGaTe, AuLiGaS, AuLiGaSe, AuLiGaTe, AuNaGaS, AuNaGaSe, AuNaGaTe, AuKGaS, AuKGaSe, AuKGaTe, AuGaSeTe, AuGaSSe, AuGaSTe, AuCuGaS, AuCuGaSe or AuCuGaTe.
[0304] In another aspect, embodiments of the present disclosure provide a photosensitive resin composition comprising quantum dots.
[0305] In another aspect, embodiments of the present disclosure provide an electronic device including a display device including a light-emitting diode including a photosensitive resin composition including quantum dots and a control unit for driving the display device.
[0306] The above description is merely an example of the present disclosure, and those skilled in the art will appreciate that various modifications may be made without departing from the essential characteristics of the present disclosure. Accordingly, the embodiments disclosed in this specification are intended to illustrate rather than limit the present disclosure, and the spirit and scope of the present disclosure are not limited by these embodiments. The scope of protection of the present disclosure should be interpreted by the claims below, and all technologies within a scope equivalent thereto should be interpreted as being included within the scope of the rights of the present disclosure.
[0307]
[0308] CROSS-REFERENCE TO RELATED APPLICATION
[0309] This patent application claims priority under 35 USC §119(a) to Korean Patent Application No. 10-2023-0061079, filed May 11, 2023, the entire contents of which are incorporated herein by reference. Furthermore, this patent application claims priority in countries other than the United States for the same reasons, the entire contents of which are incorporated herein by reference.
Claims
1. Core containing Ag, In, Ga and S; A nanostructure comprising a shell disposed on the core; and Contains a ligand that interacts with a metal bound to the surface of the nanostructure, The above ligand is at least one selected from an L-type ligand which is a 2-electron donor, an X-type ligand which is a 1-electron donor, and a Z-type ligand which is an electron acceptor. A quantum dot in which the weight ratio of the ligand to the sum of the nanostructure and the ligand is greater than 5 wt% and less than or equal to 50 wt%.
2. In paragraph 1, A quantum dot wherein the L-type ligand is at least one selected from oleylamine, N,N,N',N'-tetramethylethylene-1,2-diamine, pyridine tri-n-butylphosphine oxide, tri-n-octylphosphine oxide, and 5,8-Dimethyl-4,7,10-trioxatridecane-2,12-diamine.
3. In paragraph 1, The above X-type ligand is at least one selected from oleic acid, tetradecanol, a thiol group, a halide group, an O2CR group, and a phosphine group, A quantum dot in which R in the above O2CR group is selected from the group consisting of a substituted or unsubstituted alkyl group, an alkenyl group, a cycloalkyl group, a cycloalkenyl group, a heterocyclyl group, an amino group, an alkylamino group, a dialkylamino group, an arylalkyl group, a silyl group, an aryl group, a heteroaryl group, or a combination thereof.
4. In paragraph 3, A quantum dot wherein the above thiol group is at least one selected from a dodecanethiol group, an adamantanethiol group, an octanethiol group, a 6-mercapto-1-hexanol group, and a 6-amino-1-hexanol group.
5. In paragraph 3, A quantum dot wherein the O2CR group is at least one selected from a carboxylate group, an octanoate group, a crotonate group, a dimethylacrylate group, a benzoate group, a p-toluate group, and an oxo (OXO) group.
6. In paragraph 3, A quantum dot wherein the phosphine group is at least one selected from a tris methyl silyl phosphine group, a tris dimethylamino phosphine group, a tris diethylamino phosphine group, a tris carboxyethyl phosphine hydrochloride group, a tris (hydroxypropyl) phosphine group, and a 2-diphenylphosphinobenzaldehyde group.
7. In paragraph 1, The above Z-type ligand is at least one selected from a metal and an alkyl group, The above metal is a quantum dot selected from at least one of In, P, Ga, Ag, Cd, Zn, Se, S, Al, Cu, Li, Au, K, Na, Pb and Cs.
8. In paragraph 1, The above shell is, A first shell disposed on the core and including at least one selected from group I elements and group III elements and group VI elements; and A second shell is disposed in the first shell and includes at least one selected from a group I element and a group III element and a group VI element, The above group I element includes at least one selected from Li, Na, K, Rb, Cs, Cu, Ag, and Au, The above group III element includes at least one selected from Al, Ga, In and Tl, A quantum dot comprising at least one element of Group VI selected from S, Se, and Te.
9. A core manufacturing step of manufacturing a core by injecting a silver precursor, an indium precursor, a gallium precursor, a sulfur precursor and a solvent into a first reactor and reacting them; A shell manufacturing step of manufacturing a shell by injecting and reacting the manufactured core into a second reactor equipped with a precursor containing a specific element; and A ligand binding step is included in the manufactured shell, wherein a ligand that interacts with one or more metals is selected from among an L-type ligand that is a two-electron donor, an X-type ligand that is a one-electron donor, and a Z-type ligand that is an electron acceptor. A method for manufacturing a quantum dot, wherein the weight ratio of the ligand to the sum of the nanostructure and the ligand is greater than 5 wt% and less than or equal to 50 wt%.
10. In paragraph 9, A method for manufacturing a quantum dot, wherein the L-type ligand is at least one selected from oleylamine, N,N,N',N'-tetramethylethylene-1,2-diamine, pyridine tri-n-butylphosphine oxide, tri-n-octylphosphine oxide, and 5,8-dimethyl-4,7,10-trioxatridecane-2,12-diamine.
11. In paragraph 9, The above X-type ligand is at least one selected from oleic acid, tetradecanol, a thiol group, a halide group, an O2CR group, and a phosphine group, A method for manufacturing a quantum dot, wherein in the above O2CR group, R is selected from the group consisting of a substituted or unsubstituted alkyl group, an alkenyl group, a cycloalkyl group, a cycloalkenyl group, a heterocyclyl group, an amino group, an alkylamino group, a dialkylamino group, an arylalkyl group, a silyl group, an aryl group, a heteroaryl group, or a combination thereof.
12. In paragraph 11, A method for manufacturing a quantum dot, wherein the above thiol group is at least one selected from a dodecanethiol group, an adamantanethiol group, an octanethiol group, a 6-mercapto-1-hexanol group, and a 6-amino-1-hexanol group.
13. In paragraph 11, A method for manufacturing a quantum dot, wherein the O2CR group is at least one selected from a carboxylate group, an octanoate group, a crotonate group, a dimethylacrylate group, a benzoate group, a p-toluate group, and an oxo (OXO) group.
14. In paragraph 11, A method for manufacturing a quantum dot, wherein the phosphine group is at least one selected from a tris methyl silyl phosphine group, a tris dimethylamino phosphine group, a tris diethylamino phosphine group, a tris carboxyethyl phosphine hydrochloride group, a tris (hydroxypropyl) phosphine group, and a 2-diphenylphosphinobenzaldehyde group.
15. In paragraph 9, The above Z-type ligand is at least one selected from a metal and an alkyl group, A method for manufacturing a quantum dot, wherein the metal is at least one selected from In, P, Ga, Ag, Cd, Zn, Se, S, Al, Cu, Li, Au, K, Na, Pb, and Cs.
16. In paragraph 9, The above shell is, A first shell disposed on the core and including at least one selected from group I elements and group III elements and group VI elements; and A second shell is disposed in the first shell and includes at least one selected from a group I element and a group III element and a group VI element, The above group I element includes at least one selected from Li, Na, K, Rb, Cs, Cu, Ag, and Au, The above group III element includes at least one selected from Al, Ga, In and Tl, A method for manufacturing a quantum dot, wherein the above group VI element includes at least one selected from S, Se, and Te.
17. A photosensitive resin composition comprising the quantum dot of paragraph 1.
18. A display device including a light-emitting diode including an optical film manufactured with a photosensitive resin composition including the quantum dot of paragraph 1; and An electronic device comprising a control unit for driving the display device.
Citation Information
Patent Citations
Core-shell structured quantum dots, preparation method thereof and polarizing film
CN109233802A
Origami type self-assembly walking robot with improved running structure
KR1020210035960A
Apparatus and method for beamforming in wireless communication system
KR1020230073369A
Insect breeding system
KR102313778B1
Quantum dot and method for producing the same
US20210363422A1