Method for manufacturing flexible copper clad laminate having PTFE substrate

The method of using atomic sputtering epitaxy in a controlled vacuum environment for depositing copper thin films on PTFE substrates addresses the challenge of uniform deposition and adhesion, resulting in improved electrical and mechanical properties for flexible copper clad laminate films, suitable for advanced industrial applications.

WO2024232574A1PCT designated stage expired Publication Date: 2024-11-14CIT CO LTD

Patent Information

Application Number
PCT/KR2024/005684
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-22
Filing Date
2024-04-26
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Conventional methods for manufacturing flexible copper clad laminate films with PTFE substrates face challenges in achieving uniform metal thin film deposition, leading to poor adhesion and deterioration of PTFE substrate properties, which affects electrical performance and signal transmission speeds.

Method used

A method involving a vacuum chamber with controlled temperature and argon gas injection, using high-frequency power to deposit copper thin films on PTFE substrates via atomic sputtering epitaxy (ASE) to improve adhesion and maintain substrate integrity, ensuring uniform deposition and enhanced electrical performance.

Benefits of technology

This approach enhances the adhesion between the PTFE substrate and metal thin film, improving electrical performance, mechanical properties, and heat resistance, making it suitable for high-tech applications like communications, semiconductors, and secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005684_14112024_PF_FP_ABST
    Figure KR2024005684_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a flexible copper clad laminate (FCCL) having a PTFE substrate. More specifically, the present invention relates to a method for manufacturing an FCCL having a PTFE substrate, the method, in order to manufacture an FCCL, uniformly depositing a metal thin film on a PTFE substrate so that the electrical performance of the FCCL can be improved and deterioration of the physical properties of the PTFE substrate can be prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing a flexible copper-clad laminate film having a PTFE substrate

[0001] The present invention relates to a method for manufacturing a flexible copper clad laminate (FCCL) having a PTFE substrate. More specifically, the present invention relates to a method for manufacturing a flexible copper clad laminate (FCCL) having a PTFE substrate, which can improve the electrical performance of the FCCL and prevent deterioration of the physical properties of the PTFE substrate by uniformly depositing a metal thin film on the PTFE substrate to manufacture the FCCL.

[0002] Flexible copper clad laminate (FCCL) is a key material for flexible printed circuit boards (FPCBs) that are mainly used in smartphones, PCs, semiconductors, automotive electronics, displays, mobility, and secondary batteries. Generally, FCCL is a product in which a metal film is laminated on one or both sides of a polymer substrate.

[0003] The substrate constituting the flexible copper clad laminate (FCCL) can be made of various insulating materials such as polyimide (PI) resin, thermoplastic resin, glass, epoxy resin, and liquid crystal polymer (LCP), but preferably, polytetrafluoroethylene (PTFE) material with excellent mechanical properties and electrical performance can be used.

[0004] Polytetrafluoroethylene (hereinafter referred to as 'PTFE') material has excellent mechanical properties such as chemical resistance, heat resistance, and dimensional stability, and has lower permittivity and dielectric loss than other insulating materials. Therefore, when applied to a printed circuit board (PCB), it has the advantage of increasing signal and data transmission speed in the same antenna circuit. However, PTFE has poor metal bonding strength compared to other insulating materials, so a method to improve the bonding strength between the PTFE substrate and the metal is required.

[0005] Figure 1 illustrates various manufacturing methods of conventional flexible copper clad laminate (FCCL).

[0006] Among the various manufacturing processes for bonding a substrate and a copper film during the manufacture of a flexible copper clad laminate (FCCL), the laminating process illustrated in FIG. 1(a) is a method of bonding a copper film (20) by applying an adhesive (30) to one or both sides of a PTFE substrate (10), the casting process illustrated in FIG. 1(b) is a method of bonding a copper film (20) to a substrate made of an insulating resin (40) by casting a solution of an insulating resin (40) mixed with polyimide (PI) and PTFE onto a copper film (20), and the coating process illustrated in FIG. 1(c) is a method of bonding a copper film (20) to a PTFE substrate (10) by impregnating the PTFE substrate (10) with polyimide (PI) and then plating or coating a copper melt (50) on the impregnated PTFE substrate (10).

[0007] As shown in Fig. 1, the conventional method of manufacturing a flexible copper clad laminate (FCCL) uses an adhesive or polyimide (PI), so there was a problem that the dielectric constant of the flexible copper clad laminate (FCCL) increased compared to the case where a PTFE substrate (10) was used alone, resulting in a slow signal and data transmission speed.

[0008] Accordingly, a sputtering process has been proposed that can prevent problems such as a decrease in the transmission speed of a flexible copper clad laminate (FCCL) due to the use of adhesive or PI as in the past by directly depositing a copper thin film on a PTFE substrate (10).

[0009] Sputtering is a type of vacuum deposition method primarily used in direct circuit production. It involves accelerating an ionized gas under a relatively low vacuum, colliding it with a target, and ejecting the atoms to form a thin film on the substrate. In this sputtering process, it is crucial to control the uniform deposition of metal particles forming the thin film on the substrate to eliminate electrical noise and physical vibration.

[0010] Among related prior arts, Korean Patent Publication No. 10-2022-0049366 discloses a sputtering device for evenly growing a metal thin film on a substrate by controlling particles emitted from a target at the atomic layer level.

[0011] Meanwhile, as a result of forming a metal thin film on a substrate to which various materials are applied using a sputtering device according to the above prior art, the metal thin film was uniformly formed on a substrate having a crystal structure such as sapphire (aluminum oxide), but on a substrate made of PTFE material, it was not easy to control the atomic layer, so the metal thin film could not be uniformly formed. In addition, there was a problem that the properties of the PTFE substrate were damaged or deformed during the deposition process, resulting in a deterioration in the quality of the flexible copper clad laminate (FCCL).

[0012] Recently, with the development of cutting-edge industries such as communications, displays, semiconductors, and secondary batteries, the demand for flexible copper clad laminates (FCCLs) has been rapidly increasing. However, there is virtually no technology that can uniformly deposit a metal film on a PTFE substrate, which is widely used as a substrate material for FCCLs.

[0013] Accordingly, in order to manufacture a flexible copper clad laminate (FCCL), there is an urgent need for a method for manufacturing a flexible copper clad laminate having a PTFE substrate that can improve the electrical performance of the FCCL and prevent deterioration of the physical properties of the PTFE substrate by uniformly depositing a metal thin film on the PTFE substrate while omitting the use of an adhesive or a resin such as polyimide (PI) as in the past.

[0014] The present invention aims to provide a method for manufacturing a flexible copper clad laminate (FCCL) having a PTFE substrate, which can improve the electrical performance of a flexible copper clad laminate (FCCL) and prevent deterioration of the physical properties of the PTFE substrate by uniformly depositing a metal film on a PTFE substrate in order to manufacture the FCCL.

[0015] In order to solve the above problem, the present invention can provide a method for manufacturing a PTFE-based flexible copper clad laminate substrate, characterized by including a PTFE substrate preparation step of preparing a substrate made of PTFE (Polytetrafluoroethylene) material in a chamber space of a vacuum chamber; a reaction gas injection step of injecting a reaction gas after the chamber space of the vacuum chamber is evacuated for a sputtering process; a high-frequency power application step of applying high-frequency power to a target mounted on the upper part of the interior of the vacuum chamber and made of single-crystal metal particles; and a metal thin film lamination step of depositing metal particles separated from the target by the applied high-frequency power on the PTFE substrate to form a metal thin film.

[0016] Additionally, in the PTFE substrate preparation step, the chamber space temperature of the vacuum chamber in which the PTFE substrate is prepared can be formed in the range of 140 degrees (℃) to 200 degrees (℃).

[0017] And, in the reaction gas injection step, the gas injected into the chamber space of the vacuum chamber may include argon (Ar).

[0018] In this case, in the high-frequency power application step, the high-frequency power can be transmitted to the target mounted on the inner upper part of the vacuum chamber through a power supply line composed of a single-crystal copper wire.

[0019] In this case, the metal thin film deposition step may be performed by depositing the metal thin film on the PTFE substrate through an atomic sputtering epitaxy (ASE) process that deposits atomic-level metal particles on the PTFE.

[0020] Additionally, in the metal thin film lamination step, the metal thin film can be laminated on top of the PTFE substrate in a thickness range of 100 to 300 nm.

[0021] And, in the metal thin film lamination step, the metal particles may include copper (Cu).

[0022] Here, during the metal film lamination step, vibrations transmitted to the vacuum chamber while the metal particles separated from the target are deposited on the PTFE substrate can be absorbed or blocked.

[0023] In addition, a metal film pattern forming step of forming a pattern having a specific shape on the surface of the metal film that has been laminated on the PTFE substrate may be further performed.

[0024] And, the pattern formed in the metal thin film pattern forming step may be a hexagonal honeycomb shape with a line width of 5 μm to 14 μm.

[0025] According to the method for manufacturing a flexible copper clad laminate having a PTFE substrate according to the present invention, the bonding strength between the PTFE substrate and the metal thin film is improved by using an atomic sputtering epitaxy (ASE) process, and the metal thin film is uniformly deposited on the PTFE substrate, thereby improving the electrical performance of the flexible copper clad laminate, and since it has excellent heat resistance and mechanical properties, it can be applied as an advanced material used in various industrial fields such as communications, semiconductors, displays, and secondary batteries.

[0026] Figure 1 illustrates various manufacturing methods of conventional flexible copper clad laminate (FCCL).

[0027] Figure 2 shows the initial growth mechanism of a metal thin film deposited on a sapphire substrate through an atomic sputtering epitaxy (ASE) process.

[0028] Figure 3 is a flow chart of a method for manufacturing a flexible copper foil laminate film having a PTFE substrate according to the present invention.

[0029] Figure 4 is an image of each PTFE substrate before and after copper deposition, observed using a scanning electron microscope (SEM).

[0030] Figure 5 is an image of a copper surface deposited on PTFE observed using electron beam scatter diffraction (EBSD).

[0031] FIG. 6 is a photograph of a mesh and circuit image of a copper thin film patterned on a PTFE substrate using a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention.

[0032] FIG. 7 shows an image of the results of an x-ray diffraction experiment of a Cu / e-PTFE thin film manufactured using a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention.

[0033] FIG. 8 shows an AFM surface image of a Cu / e-PTFE thin film manufactured using a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention.

[0034] FIG. 9 illustrates another example of an AFM surface image of a Cu / e-PTFE thin film manufactured using a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention.

[0035] FIG. 10 illustrates another example of an AFM surface image of a Cu / e-PTFE thin film manufactured using a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention.

[0036] Figure 11 shows an SEM image of a Cu / e-PTFE thin film manufactured using a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention.

[0037] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings. However, the present invention is not limited to the embodiments described herein and may be embodied in other forms. Rather, the embodiments introduced herein are provided to ensure that the disclosure is thorough and complete, and to sufficiently convey the spirit of the invention to those skilled in the art. Like reference numbers designate like elements throughout the specification.

[0038] According to the method for manufacturing a flexible copper-clad laminate having a PTFE substrate according to the present invention, the method is characterized in that the bonding strength between the PTFE substrate and the metal thin film is improved and the metal thin film is uniformly deposited on the PTFE substrate by using an atomic sputtering epitaxy (ASE) process. The atomic sputtering epitaxy (ASE) process used in the present invention will be described with reference to FIG. 2.

[0039] Figure 2 shows the initial growth mechanism of a metal thin film (20) deposited on a sapphire (Al2O3) substrate (10s) through an atomic sputtering epitaxy (ASE) process.

[0040] As illustrated in FIG. 2, the initial growth mechanism of the metal thin film (20) largely consists of three stages (I) to (III), and specifically, stage (a) is a stage in which the ejected metal particles (21) grow into nanodroplets, stage (II) is a stage in which the nanodroplet-shaped metal particles (21) are integrated with each other, and stage (III) is a stage in which the metal particles (21) grow into multiple layers.

[0041] A typical sputtering process deposits a polycrystalline metal thin film (20) on a sapphire substrate (10s) to form a grain boundary in the polycrystalline metal thin film (20). A grain boundary is a thin transition layer that forms a boundary between crystals. During the crystal growth process, this area is finally solidified, and impurities are included or oxygen atoms combine to generate copper oxide. Therefore, a typical sputtering process has a problem in that a copper thin film (20) cannot grow epitaxially on top of a sapphire substrate (10s).

[0042] Accordingly, by performing an atomic sputtering epitaxy (ASE) process, an ultra-flat copper thin film (20) at the single-atomic layer level can be formed on top of a sapphire substrate (10s), thereby preventing copper oxidation.

[0043] Meanwhile, while the general sputtering process ejects metal particles (21) from the target material in bulk and deposits them on the substrate, the atomic sputtering epitaxy (ASE) process is a thin film growth method that stacks atoms one by one on the substrate like building bricks. Hereinafter, the atomic sputtering epitaxy (ASE) process will be described in more detail.

[0044] Copper (Cu) is generally the most widely used conductor in electrical civilization. However, its critical weakness, oxidation, has limited its use. Therefore, for ultra-precision materials or circuits requiring high reliability, gold, a precious metal with poorer electrical conductivity than copper, has been used instead. While extensive research has been conducted on copper oxidation, only phenomenological descriptions or theoretical predictions have been reported. As materials become smaller and more integrated, securing sufficient operating time and miniaturizing power supplies become increasingly important, necessitating materials with high conductivity. Against this backdrop, the atomic sputtering epitaxy (ASE) process can be used to address copper oxidation on sapphire substrates (10s).

[0045] Since it is empirically known that oxidation begins at the roughest portions of copper, the creation of a thin film with the best possible surface condition is paramount. Therefore, using the atomic sputtering epitaxy (ASE) process, a thin film with an ultra-flat surface at the atomic layer level can be grown on a sapphire substrate (10s).

[0046] A metal thin film (20) manufactured on a sapphire substrate (10s) is in a single crystal state and has an ultra-flat surface with an RMS roughness of 0.2 nm or less, and does not oxidize even when exposed to air for a long time. High-resolution transmission electron microscopy observation shows that if the surface is maintained with a roughness of less than a single atomic layer, phase transition due to oxidation does not occur. As a result of calculating the oxygen penetration energy according to the surface state through first-principle calculations, when the surface is maintained with a roughness of less than a single atomic layer, energy must be supplied from the outside for oxygen to penetrate into the metal thin film (20), so oxidation does not occur easily. In addition, if the oxygen occupancy of the surface physically adsorbed without chemical bonding exceeds 50%, a repulsive force is generated, which has a self-regulating function that suppresses oxidation by itself.

[0047] The atomic sputtering epitaxy (ASE) process, thus, has a significant impact on the materials industry, enabling copper to replace gold (Au) in numerous applications. With the advancement of nanotechnology, circuit line widths have shrunk and integration has increased, making oxidation of thin conductive lines a more serious problem. However, ultra-flat single-crystal thin films eliminate oxidation concerns, broadening their scope of application. Economically, copper thin films could potentially replace gold in nanocircuits. Copper's electrical conductivity is approximately 40% higher than gold, and a single-crystal copper film with an ultra-flat surface can further increase its conductivity by more than 15%. This translates into significant added economic value, including reduced power consumption and energy consumption, extended operating life, and miniaturization of equipment.

[0048] Meanwhile, a technology has been introduced for depositing a metal film (20), such as a copper film, on a sapphire (aluminum oxide, Al2O3) substrate (10s) by performing an atomic sputtering epitaxy (ASE) process, but a technology for uniformly depositing a copper film on a PTFE substrate (10) by applying an atomic sputtering epitaxy (ASE) process has not been introduced.

[0049] Polytetrafluoroethylene (PTFE) is one of the materials that has recently been in the spotlight because it has sufficient mechanical properties and excellent low-dielectric properties, and in particular, PTFE material can reduce data loss and improve transmission speed when applied to the substrate of flexible copper clad laminate (FCCL).

[0050] However, when a copper thin film is deposited on a PTFE substrate (10) by performing an atomic sputtering epitaxy (ASE) process, unlike a crystalline substrate made of aluminum oxide (Al2O3), etc., the PTFE material is a polymer material that is relatively vulnerable to environmental variables such as temperature and pressure, so there were difficulties in the process such as the physical properties easily changing during the deposition process, resulting in a deterioration in the quality of the FCCL.

[0051] In addition, when a copper thin film is deposited on a PTFE substrate (10) by performing an atomic sputtering epitaxy (ASE) process, unlike a crystalline substrate such as a sapphire substrate (10s), the adsorption energy between the PTFE substrate (10) and the copper thin film is insufficient, so the copper thin film is easily detached from the PTFE substrate (10) and the electrical conductivity is reduced.

[0052] Accordingly, the present invention applies the conventionally introduced atomic sputtering epitaxy (ASE) process and improves the deposition conditions to suit the substrate material, thereby facilitating the deposition of a uniform metal thin film (20) even on a PTFE substrate (10), thereby improving the electrical performance of a flexible copper clad laminate (FCCL) and improving the adsorption property at the interface between the PTFE substrate (10) and the metal thin film (20).

[0053] Figure 3 is a process flow diagram of a method for manufacturing a flexible copper foil laminate film having a PTFE substrate according to the present invention.

[0054] As illustrated in FIG. 3, a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention may include a PTFE substrate preparation step (S100) of preparing a substrate made of a PTFE (Polytetrafluoroethylene) material in a chamber space of a vacuum chamber; a reaction gas injection step (S200) of injecting a reaction gas into the chamber space of the vacuum chamber after a vacuum is formed for a sputtering process; a high-frequency power application step (S300) of applying high-frequency power to a target mounted on the inner upper portion of the vacuum chamber and made of single-crystal metal particles; and a metal thin film lamination step (S400) of depositing metal particles separated from the target by the applied high-frequency power on the upper portion of the PTFE substrate (10) to form a metal thin film (20).

[0055] The present invention provides a method for manufacturing a flexible copper clad laminate (FCCL) based on PTFE, which can control a high-quality metal film (20) by controlling the crystal structure of a metal film (20) on a PTFE substrate (10) forming the flexible copper clad laminate (FCCL) at the atomic layer level by applying an atomic sputtering epitaxy (ASE) process in manufacturing the FCCL.

[0056] The sputtering device used in the method for manufacturing a PTFE-based flexible copper-clad laminate substrate according to the present invention, as illustrated in FIG. 3, is a device that removes noise, electrical noise, and mechanical noise of a target material from a general sputtering device, and can perform the atomic sputtering epitaxy (ASE) process described above.

[0057] The method for manufacturing a PTFE-based flexible copper-clad laminate substrate according to the present invention can be performed by a sputtering device including a vacuum chamber, an RF generation unit, a vacuum pump unit, a gas supply unit, and a vibration isolation unit.

[0058] First, a PTFE substrate preparation step (S100) can be performed to prepare a substrate made of PTFE (Polytetrafluoroethylene) material in the chamber space of a vacuum chamber.

[0059] Here, the vacuum chamber is a space where a sputtering process for depositing a metal thin film (20) on a PTFE substrate (10) is performed, and the vacuum chamber is composed of a PTFE substrate, a target, and a chamber space. The PTFE substrate (10) is an anode portion of the sputtering process and may be made of a polytetrafluoroethylene (PTFE) material. A target is positioned on the cathode portion facing the PTFE substrate (10), and the target is formed of a metal material of a thin film to be deposited on the PTFE substrate (10). The PTFE substrate (10) and the target are positioned inside the chamber space, so that particles falling from the target in a subsequent sputtering process are separated and deposited on the PTFE substrate (10), thereby manufacturing a metal thin film (20).

[0060] In the PTFE substrate preparation step (S100), the chamber space temperature of the vacuum chamber in which the PTFE substrate (10) is prepared can be formed and maintained in the range of 140 degrees (°C) to 200 degrees (°C), preferably in the range of 150 degrees (°C) to 170 degrees (°C). If the temperature inside the chamber space is less than 140 degrees (°C), the metal thin film (20) deposited on the PTFE substrate (10) is not uniformly formed, whereas if it exceeds 200 degrees (°C), there is a problem in that the physical properties of the PTFE substrate (10) change.

[0061] In addition, the method for manufacturing a PTFE-based flexible copper-clad laminate substrate according to the present invention can be optimized through repeated experiments so that the pressure conditions or vacuum conditions inside the chamber space can uniformly grow crystals of a metal thin film (20) on a PTFE substrate (10). Furthermore, the PTFE substrate (10) is pretreated so that the metal thin film (20) can grow with high adsorption at the interface of the PTFE substrate (10).

[0062] Next, the reaction gas injection step (S200) and the high-frequency power application step (S300) of the present invention can be performed sequentially.

[0063] The above reaction gas injection step (S200) is a step in which reaction gas is injected after the chamber space of the vacuum chamber is formed into a vacuum for the sputtering process, and the high-frequency power application step (S300) is a step in which high-frequency power is applied to a target made of single-crystal metal particles and is mounted on the upper part of the inside of the vacuum chamber.

[0064] The above reaction gas injection step (S200) and high-frequency power application step (S300) can be performed by a gas supply unit and an RF generator, respectively, constituting a sputtering device.

[0065] The RF generator for performing the high-frequency power application step (S300) is configured to apply high-frequency power, RF power, to the target in the vacuum chamber for the sputtering process, and is connected to the target by a connection wire.

[0066] Meanwhile, for the sputtering process, the chamber space must form a vacuum state, and the vacuum pump unit constituting the sputtering device is configured to suck in a fluid inside the chamber space to form a vacuum inside the chamber space of the vacuum chamber, and may be a commonly used rotary pump.

[0067] To this end, a gas supply unit that supplies a reaction gas for a sputtering process inside a vacuum chamber space is connected to the chamber space of the vacuum chamber, and the reaction gas supplied by the gas supply unit may be argon (Ar) gas. The higher the purity of the argon gas, the more uniformly the deposition particles can be separated from the target over the entire surface of the target, so that the metal thin film deposition step (S400) can be performed.

[0068] The above metal thin film deposition step (S400) is a configuration of the above-described sputtering device, in which RF power is applied to a target in a chamber space supplied with a reaction gas in a vacuum state through an RF generator, the reaction gas is ionized by glow discharge, a plasma discharge is generated between the PTFE substrate (10) and the target, and the positive ions present in the discharge region strike the surface of the target by electrical power, so that the deposition particles falling off the target surface are deposited on the facing PTFE substrate (10), thereby manufacturing a metal thin film (20).

[0069] Meanwhile, in performing the high-frequency power application step (S300) of the present invention, the power cable that supplies power to the RF generator is formed of a single-crystal copper wire, which prevents noise and signal distortion from being mixed in the signal transmitted through the power cable, and increases the stability of the RF power applied to the target, so that the deposition particles can be uniformly separated from the entire surface of the target, thereby improving the quality of the metal thin film (20) deposited on the PTFE substrate (10).

[0070] And, the homogeneity of the deposition particles falling from the target is connected to the crystallinity of the target in that the deposition particles are separated from the target. Therefore, the target included in the vacuum chamber can be formed of a single crystal metal. In this way, when the target is formed of a single crystal metal, the metal particles are evenly formed with a certain directionality on the entire surface of the target, and the deposition particles separated therefrom are also homogeneous, so that the deposited metal thin film (20) can be manufactured with high quality. The type of the single crystal metal forming the target is determined according to the type of the metal thin film (20) to be deposited on the PTFE substrate (10), and may be copper, silver, or a metal of a single element.

[0071] In addition, when performing the high-frequency power application step (S300), the connecting wire for transmitting the RF power of the RF generator to the target of the vacuum chamber can be formed of a single crystal copper wire. Accordingly, electrical noise in the RF power applied to the target can be removed and the stability of the power can be increased, and the homogeneity of the plasma discharge formed between the PTFE substrate (10) and the target can be increased, so that the deposition particles can be uniformly dropped from the entire surface of the target.

[0072] The outdoor grounding section, which is formed to ground the RF generator, can be formed from a single-crystal copper bulk. The single-crystal copper constituting the outdoor grounding section can be manufactured in the same manner as the target, if the target metal type is copper. Thus, forming the outdoor grounding section from a single-crystal copper bulk can enhance the stability of RF power and enable the uniform deposition of deposition particles.

[0073] In addition, the present invention can prevent mechanical noise, such as vibration, from being applied during the process of depositing particles away from the target on the PTFE substrate (10) in the metal thin film lamination step (S400), thereby allowing the metal thin film (20) to grow with high adsorption at the interface with the PTFE thin film.

[0074] To this end, the vacuum chamber may be supported at each corner of its bottom by vibration isolation members to prevent vibrations from being transmitted from the floor. The vibration isolation members have a mechanically irreversible structure that prevents vibrations from being transmitted from the floor to the vacuum chamber and, conversely, cancels out vibrations generated in the vacuum chamber by discharging them to the outside (floor).

[0075] Specifically, in the metal film lamination step (S400), a vibration isolation unit for blocking vibration transmitted to the vacuum chamber is configured to include a spike and a damping mat. The spike is attached to the bottom of the vacuum chamber to support the vacuum chamber, and has a sharp horn shape that becomes sharper as it goes toward the bottom. The damping mat is configured to be placed on the bottom and receive the spike on its upper surface, and an insertion groove for receiving the tip of the spike is formed on the upper surface of the damping mat, and the spike is received in the insertion groove of the damping mat to fix the planar position of the spike.

[0076] By means of the vibration isolation part including the spike and the damping mat, the vibration generated from the floor only shakes the damping mat and cannot exert force on the spike, and is not transmitted to the vacuum chamber supported by the spike. As a result, the vacuum chamber is not affected by the vibration of the floor, and no physical external force is transmitted in the process of the deposition particles separated from the target being deposited on the PTFE substrate (10), so that the metal thin film (20) can be uniformly deposited on the PTFE substrate (10) and improve its quality. Meanwhile, the spike may be formed in various shapes such as a cone, a triangular pyramid, a square pyramid, etc., although a cone shape is sufficient.

[0077] And, in order to further block physical vibration in the vacuum chamber, the sputtering device used for the method for manufacturing the PTFE-based flexible copper-clad laminate substrate of the present invention can physically separate the vacuum chamber and the vacuum pump unit.

[0078] A rotary pump, which is an example of a vacuum pump unit, generates a lot of vibrations due to the operation of the pump in the process of sucking in a fluid to create a vacuum in the chamber space of a vacuum chamber. If the vacuum chamber and the vacuum pump unit are physically configured together, the vibrations generated during the operation of the vacuum pump unit are transmitted to the vacuum chamber as is, so that the deposition particles deposited on the PTFE substrate (10) are not formed evenly.

[0079] Accordingly, the vacuum pump unit is physically separated from the vacuum chamber, and the connection to the chamber space is connected by a rubber pump line. In order to block vibrations of the pump line from being transmitted to the vacuum chamber, the center of the pump line can be fixed to a wall surface connected to the floor.

[0080] Meanwhile, in cases where the vacuum pump unit is physically separated from the vacuum chamber, the vacuum pump unit itself also needs to be isolated from vibrations. To prevent vibrations from being transmitted from the floor, such as the vacuum chamber, each corner of the bottom surface can be supported by a vibration isolation unit.

[0081] Fig. 4(a) is an image of a pure PTFE substrate without copper laminate observed using a scanning electron microscope (SEM), and Fig. 4(b) is an image of a PTFE substrate with copper laminate observed using a SEM.

[0082] Meanwhile, as shown in Fig. 4(a), it is not easy to observe the surface of the PTFE substrate (10) using a scanning electron microscope (SEM) due to the charging of electrons, but it was confirmed that the surface appeared rough and bumpy when observed at magnifications of 500 and 5000 times. As shown in Fig. 4(b), when a copper thin film was deposited with a thickness of 200 nm on the PTFE substrate (10) using the aforementioned sputtering device through an atomic sputtering epitaxy (ASE) process, it was found that the copper thin film was deposited very evenly while maintaining the original shape of the pTFE.

[0083] Figure 5 is an image of a copper surface deposited on PTFE observed using electron beam scatter diffraction (EBSD).

[0084] As shown in Fig. 5, when observing a map using electron beam scatter diffraction (EBSD) of a copper surface deposited on PTFE with a thickness of 200 nm, it can be seen that all copper crystal grains are arranged in different directions.

[0085] Figures 5(b) and 5(c) show the inverse pole figure (IPF) and pole figure (IPF) of the grain faces measured in different axial directions of the crystal, respectively, and it can be seen that the crystal orientations are scattered in a wide variety of directions.

[0086] Figure 5(d) shows an IQ image of a misorientation map indicating the boundaries between grains. The misorientation lines appear in a very blue color, almost invisible. Here, red indicates lines that exactly satisfy the twin boundary condition, while blue indicates grain boundaries with arbitrary orientations that do not satisfy the specific conditions. The absence of red lines and the presence of only blue lines indicates that grains are scattered in a wide variety of directions.

[0087] When the image shown in Fig. 5(d) is enlarged, grains are visible as in Fig. 5(e) (scale bar: 100 nm), and it can be seen that the sizes are very uniform and densely arranged overall, and the maximum size of the grains is approximately 10 nm. This small grain size minimizes the atomic spacing at the grain boundaries and minimizes the gaps, thereby creating less space for oxygen or external impurities to enter despite being a polycrystal, thereby minimizing oxidation and preventing the formation of copper oxide.

[0088] The method for manufacturing a flexible copper foil laminate film having a PTFE substrate according to the present invention may further include a metal film pattern forming step (S500) of forming a pattern (p) having a specific shape on the surface of a metal film (20) laminated on the PTFE substrate (10).

[0089] FIG. 6 is a photograph of a mesh and circuit image of a copper thin film patterned on a PTFE substrate using a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention.

[0090] FIG. 6(b) and FIG. 6(c) are enlarged images of a hexagonal honeycomb mesh patterned through a photolithography process of a copper thin film deposited on a PTFE substrate (10) in a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention. The images shown in FIG. 6(b) and FIG. 6(c) were photographed at 40x and 250x magnifications, respectively, using a transmission polarizing microscope.

[0091] FIG. 6(d) shows a circuit image in which a copper thin film deposited on a PTFE substrate (10) is patterned through a photolithography process in a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention.

[0092] As illustrated in Fig. 6(a), a hexagonal honeycomb mesh pattern (p) can be formed on a copper film deposited on an e-PTFE substrate. The mesh pattern (p) can be used to perform electrical connections using a copper film in products such as electronic devices or solar cells, and can enhance durability by reinforcing the surface of the copper film. The mesh pattern (p) can be formed by drilling holes at regular intervals on the surface of the copper film and connecting copper wires therein.

[0093] The line width of the mesh pattern (p) formed through the metal film pattern formation step (S500) is determined by the spacing between the holes drilled in the copper film, and as the line width decreases, the electrical resistance decreases. The open area of ​​the mesh pattern refers to the ratio of the area occupied by the holes in the mesh pattern, and the larger the open area, the easier the current flow, allowing for effective electrical connection.

[0094] The line width and open area of ​​such a mesh pattern (p) can be appropriately selected depending on the electrical performance and manufacturing cost required for flexible copper clad laminate (FCCL), etc. In the example shown in Fig. 6(a), it was confirmed that the mesh pattern (p) of the copper film deposited on the e-PTFE substrate had a line width of approximately 10 μm and an open area of ​​approximately 50 μm.

[0095] The mesh pattern of the above copper film is a type of PCB (Printed Circuit Board) used in electronic circuits, and can form a desired circuit pattern as shown in Fig. 6(b) by using a PTFE substrate (10) on which a copper film is deposited for electrical connection.

[0096] In this way, the method for manufacturing a flexible copper-clad laminate film having a PTFE substrate according to the present invention controls environmental variables, such as temperature, pressure, and vacuum level within the chamber space, during the sputtering process, details deposition conditions optimized for the PTFE substrate (10), and performs a pretreatment process for the PTFE substrate (10), thereby confirming that a metal thin film (20) can be uniformly deposited by performing an atomic sputtering epitaxy (ASE) process even on a PTFE substrate (10) that is not a conventional crystalline substrate.

[0097] Specifically, as a method for manufacturing a flexible copper foil laminate having a PTFE substrate according to the present invention, an atomic sputtering epitaxy (ASE) process was performed, and as a result, it was confirmed that the crystal growth rate of the copper foil was about 10 nm / min or more, the grain size was very uniform at the level of 10 to 15 nm, vacancies or staking defects due to grain boundaries were minimized, and the surface roughness was about 0.5 nm.

[0098] FIG. 7 shows an image of an X-ray diffraction experiment result of a Cu / e-PTFE thin film on which 300 nm of Cu is deposited using a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention.

[0099] As shown in Fig. 7, the X-ray diffraction experiment result image of the Cu / e-PTFE thin film shows multiple e-PTFE diffraction peaks (▽) and copper diffraction peaks. In addition, it can be seen that diffraction peaks in various directions exist in the image, and it can be seen that both materials (e-PTFE, Cu) exist in a polycrystalline state. Meanwhile, it was confirmed that grains corresponding to (100) and (110) orientations exist, but the orientation in the Cu (111) direction is the most well developed.

[0100] Fig. 8 illustrates an AFM surface image of a Cu / e-PTFE thin film manufactured using a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention. In the AFM surface image of the Cu / e-PTFE thin film illustrated in Fig. 8, it was confirmed that the root mean square (RMS) roughness was approximately 90.4 nm.

[0101] FIG. 9 illustrates another example of an AFM surface image of a Cu / e-PTFE thin film manufactured using a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention.

[0102] Specifically, the AFM surface image of the Cu / e-PTFE thin film shown in Fig. 9 has a measurement range of 10 μm in Fig. 8. 2 This is the result of measurement by reducing it to (10 μm X 10 μm). In the AFM surface image of the Cu / e-PTFE thin film shown in Fig. 9, it was confirmed that the RMS roughness was reduced to approximately 29.2 nm when the defective part of the e-PTFE was excluded from the measurement.

[0103] FIG. 10 illustrates another example of an AFM surface image of a Cu / e-PTFE thin film manufactured using a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention.

[0104] Specifically, the AFM surface image of the Cu / e-PTFE thin film shown in Fig. 10 has a measurement range of 1 μm in Fig. 8. 2 This is the result of measurement by reducing it to (1 μm X 1 μm). In the AFM surface image of the Cu / e-PTFE thin film shown in Fig. 10, it was confirmed that most of the defective parts of the e-PTFE were removed, and the RMS roughness was reduced to about 5 nm. In addition, it was confirmed that copper (Cu) particles existed in the form of fine grains in the copper thin film deposited on the e-PTFE substrate.

[0105] FIG. 11 shows SEM images at various magnifications of a Cu / e-PTFE thin film on which 300 nm of Cu is deposited using a method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention.

[0106] The SEM image of the Cu / e-PTFE thin film at low magnification can confirm the state of the e-PTFE substrate, and the SEM image of the Cu / e-PTFE thin film at high magnification can observe the shape of the deposited copper, and it can be confirmed that the copper (Cu) particles exist in the form of granules, as observed in Fig. 10.

[0107] The method for manufacturing a flexible copper-clad laminate film having a PTFE substrate according to the present invention can realize excellent high-temperature oxidation resistance characteristics when a PTFE substrate (10) on which a metal thin film (20) is deposited is used in a semiconductor PCB by applying an atomic sputtering epitaxy (ASE) process. Therefore, it has the effect of solving the problem of circuit performance degradation due to server heat generation in ICT in the semiconductor industry.

[0108] In addition, the method for manufacturing a flexible copper clad laminate having a PTFE substrate according to the present invention can evenly control the copper oxide layer on the PTFE substrate (10) by applying an atomic sputtering epitaxy (ASE) process. In the existing manufacturing method, since a polycrystalline metal thin film (20) is formed on the substrate, oxygen atoms are adsorbed on the grain boundaries inside the metal thin film (20), causing an irregular oxidation process. On the other hand, in the method for manufacturing a flexible copper clad laminate using a PTFE substrate (10) according to the present invention, the metal thin film (20) deposited on the PTFE substrate (10) is a flat and dense thin film, so that oxidation can evenly proceed on the surface, thereby implementing a material capable of ensuring reliable 5G communication quality. In the existing communication industry, there was an issue of communication quality degradation and attenuation due to the formation of a copper oxide layer by the content of atmospheric moisture (rain, resonance absorption of oxygen or water molecules in the air), but the method for manufacturing a flexible copper clad laminate film having a PTFE substrate according to the present invention can control the copper oxide layer in the copper thin film on the PTFE substrate (10), so that communication quality reliability can be secured in a high-frequency environment.

[0109] Furthermore, the method for manufacturing a flexible copper-clad laminate film having a PTFE substrate according to the present invention has an extremely high thermal conductivity when a graphene thin film is grown on a copper thin film deposited on a PTFE substrate using an atomic sputtering epitaxy (ASE) process, so that it can be used as a heat dissipation material for various electronic components such as OLEDs.

[0110] While this specification has described preferred embodiments of the present invention, those skilled in the art will appreciate that various modifications and variations can be made to the present invention without departing from the spirit and scope of the invention as defined in the claims below. Therefore, any modified implementation that fundamentally includes the elements of the claims should be considered within the technical scope of the present invention.

Claims

1. PTFE substrate preparation step of preparing a substrate made of PTFE (Polytetrafluoroethylene) material in the chamber space of a vacuum chamber; A reaction gas injection step in which a reaction gas is injected after the chamber space of the vacuum chamber is evacuated for a sputtering process; A high-frequency power application step for applying high-frequency power to a target made of single-crystal metal particles and mounted on the inner upper part of the vacuum chamber; and A method for manufacturing a PTFE-based flexible copper-clad laminate substrate, characterized in that it includes a metal film lamination step in which metal particles separated from the target by applied high-frequency power are deposited on the PTFE substrate to form a metal film.

2. In paragraph 1, A method for manufacturing a PTFE-based flexible copper-clad laminate substrate, characterized in that in the above PTFE substrate preparation step, the chamber space temperature of the vacuum chamber in which the PTFE substrate is prepared is formed in a range of 140 degrees (℃) to 200 degrees (℃).

3. In paragraph 1, A method for manufacturing a PTFE-based flexible copper-clad laminate substrate, characterized in that the gas injected into the chamber space of the vacuum chamber in the above reaction gas injection step contains argon (Ar).

4. In paragraph 1, A method for manufacturing a PTFE-based flexible copper-clad laminate substrate, characterized in that in the high-frequency power application step, the high-frequency power is transmitted to the target mounted on the inner upper part of the vacuum chamber through a power supply line composed of a single-crystal copper wire.

5. In paragraph 1, A method for manufacturing a flexible copper foil laminate having a PTFE substrate, characterized in that the metal film is deposited on the PTFE substrate through an atomic sputtering epitaxy (ASE) process that deposits metal particles of atomic units on the PTFE.

6. In paragraph 1, A method for manufacturing a flexible copper foil laminate film having a PTFE substrate, characterized in that in the metal film laminating step, the metal film is laminated on top of the PTFE substrate in a thickness range of 100 to 300 nm.

7. In paragraph 1, A method for manufacturing a flexible copper foil laminate film having a PTFE substrate, characterized in that the metal particles in the above metal film lamination step include copper (Cu).

8. In paragraph 1, A method for manufacturing a flexible copper foil laminate film having a PTFE substrate, characterized in that vibration transmitted to the vacuum chamber is absorbed or blocked while metal particles separated from the target are deposited on the PTFE substrate in the metal film lamination step.

9. In paragraph 1, A method for manufacturing a flexible copper foil laminate film having a PTFE substrate, characterized in that a metal film pattern forming step of forming a pattern having a specific shape on the surface of a metal film laminated on top of the PTFE substrate is further performed.

10. In paragraph 9, A method for manufacturing a flexible copper foil laminate film having a PTFE substrate, characterized in that the pattern formed in the above metal film pattern forming step is a hexagonal honeycomb shape with a line width of 5 μm to 14 μm.

Citation Information

Patent Citations

  • Lamination device, unit cell manufacturing method and unit cell

    KR1020230149983A

  • Polymer coated particulate compositions and related methods and applications

    KR1020230150200A

  • Package substrate having copper alloy sputter seed layer and high density interconnects

    US20190259631A1

Cited By

  • Method for depositing copper thin film in through glass via using atomic sputtering epitaxy

    EP4800151A1