Fluorine-containing polymer, conductive paste, negative pole piece, secondary battery, and electronic apparatus
By using fluoropolymers in secondary batteries to improve the dispersion of conductive paste and the cohesion of the electrode sheet, the problems of cold press rebound of the electrode sheet and conductive paste gel are solved, and the dynamic performance and stability of the battery are improved .
Patent Information
- Application Number
- PCT/CN2023/136748
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2023-12-06
- Publication Date
- 2024-11-21
AI Technical Summary
The existing secondary battery pole plates are prone to rebound during cold pressing, which affects the battery assembly process and electrochemical performance. The conductive paste is prone to gel during storage, resulting in a decrease in the battery dynamics performance.
Using fluoropolymer as dispersant, a conductive paste with high thermal stability is prepared through polymerization, which improves the cohesion and dispersion of the electrode sheet, reduces the diaphragm resistance of the electrode sheet and the DC internal resistance of the battery, and reduces the Rebound rate after cold pressing.
The cohesion force of the electrode sheet and the dynamic performance of the battery are significantly improved, the rebound rate of the electrode sheet and the DC internal resistance of the battery are reduced, and the anti-gel and storage properties of the conductive paste are improved.
Smart Images

Figure CN2023136748_21112024_PF_FP_ABST
Abstract
Description
Fluoropolymer, conductive paste, negative electrode sheet, secondary battery and electrical device
[0001] Cross-references
[0002] This application refers to Chinese Patent Application No. 202310534845.8 filed on May 12, 2023, entitled “Fluoropolymer, Conductive Paste, Negative Electrode Sheet, Secondary Battery and Electrical Device,” which is incorporated herein by reference in its entirety. Technical Field
[0003] The present application relates to the technical field of secondary batteries, and in particular to a fluorine-containing polymer, a conductive paste, a negative electrode sheet, a secondary battery, and an electrical device. Background Art
[0004] Secondary batteries have many advantages such as high volume and mass energy density, long cycle life, high nominal voltage, low self-discharge rate, small size and light weight, and are widely used in the field of consumer electronics.
[0005] The production of secondary batteries involves multiple steps, including cold pressing, die-cutting, assembly, baking, and liquid injection. Pole sheet manufacturing is a crucial front-end process throughout the entire process. The quality of the pole sheet is crucial to the success of the secondary battery's mid-stage assembly process and also impacts the subsequent stages and the secondary battery's electrochemical performance.
[0006] Summary of the Invention
[0007] The present application is made in view of the above-mentioned problems, and its purpose is to provide a fluorine-containing polymer and a conductive paste containing the fluorine-containing polymer, which can improve the cohesion of the electrode, reduce the rebound rate of the electrode after cold pressing for 24 hours, and improve the quality of the electrode while improving the dispersibility of the conductive paste and slowing down the gelation of the conductive paste.
[0008] The first aspect of the present application provides a fluorine-containing polymer comprising at least one structural unit derived from a monomer represented by formula I and at least one structural unit derived from a monomer represented by formula II.
[0009] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, R4, R5, R6 and R7 contain at least two -COOM, M is selected from hydrogen, NH4 or alkali metal.
[0010] On the one hand, the fluorine-containing polymer provided in the present application can act as a dispersant, which can significantly alleviate the gelation of the conductive paste during storage, improve the anti-gelation and storage properties of the conductive paste, reduce the diaphragm resistance of the electrode, reduce the DC internal resistance of the battery, and thus improve the dynamic performance of the battery. On the other hand, the fluorine-containing polymer can increase the cohesion of the electrode, reduce the irreversible expansion of the electrode during the manufacturing process, reduce the rebound rate of the electrode after 24 hours of cold pressing, and improve the quality of the electrode.
[0011] In any embodiment, M comprises one or more of lithium, sodium, and potassium.
[0012] The lithium, sodium or potassium introduced into the fluorinated polymer can form ion exchange with the active ions during the charge and discharge process, further increasing the mobility of the active ions, reducing the DC internal resistance of the battery, and improving the battery's kinetic performance.
[0013] In any embodiment, R1 is fluorine, and R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl.
[0014] In any embodiment, the molar content of the structural unit derived from the monomer represented by formula I is 60% to 80%, based on the total moles of all structural units in the fluoropolymer.
[0015] By controlling the molar content of the structural unit derived from the monomer represented by Formula I within an appropriate range, the viscosity of the conductive paste, the cohesive force of the electrode, and the rebound rate of the electrode after cold pressing for 24 hours can be taken into account, thereby comprehensively improving the processing performance and performance of the conductive paste.
[0016] In any embodiment, the molar content of the structural unit derived from the monomer represented by formula II is 20% to 40%, based on the total moles of all structural units in the fluoropolymer.
[0017] By controlling the molar content of the structural unit derived from the monomer represented by Formula II within an appropriate range, the viscosity of the conductive paste, the cohesive force of the electrode, and the rebound rate of the electrode after cold pressing for 24 hours can be taken into account, thereby comprehensively improving the processing performance and performance of the conductive paste.
[0018] In any embodiment, the weight average molecular weight of the fluorinated polymer is 80,000 to 120,000.
[0019] By controlling the weight-average molecular weight of the fluoropolymer within an appropriate range, the viscosity of the conductive paste, the cohesive force of the electrode, and the rebound rate of the electrode after 24 hours of cold pressing can be taken into account, thereby comprehensively improving the processing performance and performance of the conductive paste.
[0020] In any embodiment, the monomer represented by formula I is selected from one or more of vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.
[0021] In any embodiment, the monomer represented by formula II is selected from one or more of allylmalonic acid, 2-pentaconedioic acid, lithium 2-pentaconedioate, lithium allylmalonic acid, lithium methylenemalonic acid, lithium vinylmalonic acid, lithium butylmalonic acid, lithium glutaconedioate, lithium maleate, lithium trans-glutaconedioate, lithium hexamethylenediamine, lithium heptamethylenediamine, lithium octamethylenediamine, sodium allylmalonic acid, sodium methylenemalonic acid, sodium vinylmalonic acid, sodium allylmalonic acid, sodium 2-(4-pentene)malonic acid, sodium maleate, sodium trans-glutaconedioate, sodium hexamethylenediamine, sodium heptamethylenediamine, sodium octamethylenediamine, potassium allylmalonic acid, potassium methylenemalonic acid, potassium vinylmalonic acid, and potassium heptamethylenediamine.
[0022] In any embodiment, the fluorine-containing polymer includes one or more of vinylidene fluoride-allyl lithium propylene copolymer, vinylidene fluoride-allyl malonic acid copolymer, vinylidene fluoride-sodium butylmalonate copolymer, vinylidene fluoride-lithium 2-pentenedioate copolymer, vinylidene fluoride-chlorotrifluoroethylene-allyl lithium malonate copolymer, tetrafluoroethylene-allyl lithium propylene copolymer, and vinylidene fluoride-hexafluoropropylene-allyl lithium propylene copolymer.
[0023] A second aspect of the present application provides a method for preparing a fluorinated polymer, comprising the following steps:
[0024] Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized to form a polymer product,
[0025] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, R4, R5, R6 and R7 contain at least two -COOH groups,
[0026] Optionally, the polymer product is subjected to a neutralization reaction with a neutralizing agent, and the neutralization reaction converts at least part of -COOH in the polymer product into -COOM, where M is selected from NH4 or an alkali metal.
[0027] Compared with traditional dispersants, the fluorine-containing polymer prepared by this method can not only improve the dispersibility of the conductive slurry, alleviate the gelation of the conductive slurry during storage, improve the anti-gelation and storage properties of the conductive slurry, reduce the diaphragm resistance of the electrode, reduce the DC internal resistance of the battery, and improve the dynamic performance of the battery, but also the fluorine-containing polymer can improve the cohesion of the electrode, reduce the irreversible expansion of the electrode during the manufacturing process, reduce the rebound rate of the electrode after 24 hours of cold pressing, and improve the quality of the electrode.
[0028] In any embodiment, M comprises one or more of lithium, sodium, and potassium.
[0029] In any embodiment, R1 is fluorine, and R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl.
[0030] In any embodiment, the molar content of the monomer represented by formula I is 60%-80%, based on the total moles of the monomer represented by formula I and the monomer represented by formula II.
[0031] In any embodiment, the molar content of the monomer represented by formula II is 20% to 40%, based on the total moles of the monomer represented by formula I and the monomer represented by formula II.
[0032] In any embodiment, the polymerization reaction specifically comprises:
[0033] First stage polymerization: providing an initiator, an emulsifier, at least one monomer represented by formula I, and a solvent to carry out the first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure;
[0034] Second stage polymerization: After a period of reaction, the monomer represented by formula I and the monomer represented by formula II are fed into the reaction vessel to carry out the second stage polymerization, and the monomer represented by formula I is continuously fed into the second stage polymerization;
[0035] Optionally, after the second stage polymerization reaction is completed, a neutralizing agent is added into the reactor to carry out a neutralization reaction.
[0036] The method provided by the present application is to form a fluorine-containing segment by first continuously feeding the monomer shown in formula I, so that the fluorine-containing polymer has high thermal stability; and then the monomer shown in formula II is introduced to reduce the contact between the fluorine-containing segment and the external environment, effectively alleviating the gel phenomenon caused by the fluorine element. The fluorine-containing polymer prepared by this method can effectively improve the stability of the conductive paste, improve the dispersibility of the paste, reduce the diaphragm resistance of the pole piece and the DC internal resistance of the battery, and improve the dynamic performance of the battery compared to the fluorine-containing polymer prepared by simultaneously feeding all the monomers into the reaction vessel. In addition, when the monomer shown in formula II is fed into the reaction vessel for the second stage of polymerization, the monomer shown in formula I is continued to be fed into the reaction vessel, which helps to improve the compatibility of the segment generated by the first stage of polymerization and the segment generated by the second stage of polymerization, thereby improving the stability of the fluorine-containing polymer.
[0037] In any embodiment, the mass of the monomer of formula I introduced in the first stage polymerization is 30%-70% of the total mass of the monomer of formula I supplied in the polymerization reaction, and the mass of the monomer of formula I introduced in the second stage polymerization reaction is 30%-70% of the total mass of the monomer of formula I supplied in the polymerization reaction.
[0038] In any embodiment, the neutralizing agent includes one or more of lithium carbonate, sodium carbonate, potassium carbonate, lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, lithium hydroxide, sodium hydroxide, potassium hydroxide, and aqueous ammonia.
[0039] The third aspect of the present application provides use of the fluorine-containing polymer of the first aspect in a secondary battery.
[0040] In a fourth aspect of the present application, a conductive paste is provided, comprising a conductive agent, an aqueous medium and the fluorine-containing polymer provided in the first aspect.
[0041] Compared with the prior art of directly adding a conductive agent during the preparation of the negative electrode slurry, the conductive slurry provided in the present application can reduce the rebound rate of the electrode after cold pressing for 24 hours, thereby improving the quality of the electrode. At the same time, by improving the dispersibility of the conductive agent in the negative electrode slurry, the conductive effect of the conductive agent in the electrode is improved, thereby effectively reducing the conductive agent content in the electrode, which is conducive to further increasing the load of the negative electrode active material in the electrode and improving the battery power performance.
[0042] In any embodiment, the mass fraction of the conductive agent is 1.5% to 4.5%, based on the total mass of the conductive paste.
[0043] By controlling the mass fraction of the conductive agent within an appropriate range, the slurry has an appropriate viscosity based on the total mass of the conductive slurry. At the same time, the electrode has a low rebound rate after cold pressing for 24 hours, which comprehensively improves the processing performance and usage performance of the slurry.
[0044] In any embodiment, the mass fraction of the fluorine-containing polymer is 0.5% to 1.5%, based on the total mass of the conductive paste.
[0045] By controlling the mass fraction of the fluoropolymer within a suitable range, the slurry has a suitable viscosity based on the total mass of the conductive slurry, and the electrode has a low rebound rate after cold pressing for 24 hours, thereby comprehensively improving the processing performance and performance of the slurry.
[0046] In any embodiment, the solid content of the conductive paste is 1%-10%, and the viscosity of the conductive paste is 500 mPa·s-5000 mPa·s.
[0047] The solid content is 1%-10%, and the viscosity is 500mPa·s-5000mPa·s. It can be directly mixed and stirred with active materials and binders to prepare negative electrode slurry without adding additional additives, which is beneficial to improving production efficiency and reducing production costs.
[0048] The fifth aspect of the present application provides a negative electrode plate, comprising a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, the negative electrode film layer comprising a negative electrode active material, a conductive agent and a binder, and the conductive agent comprises a deposit of the conductive slurry of the fourth aspect.
[0049] Compared with the negative electrode sheets prepared by directly adding conductive agent powder in the prior art, the conductive agent in the negative electrode sheets disclosed in the present application exists in the form of conductive slurry deposits in the negative electrode sheets. On the one hand, it can improve the cohesion of the sheets, reduce the rebound rate of the sheets after cold pressing for 24 hours, and improve the quality of the sheets. On the other hand, adding in the form of conductive slurry can improve the dispersion performance of the conductive material, so that the negative electrode sheets can have low membrane resistance when the conductive agent is added in a low amount, which provides the possibility of further increasing the loading amount of the negative electrode active material in the sheets.
[0050] In any embodiment, the compacted density of the negative electrode sheet is 1.5 g / cm 3 -1.8g / cm 3 When the negative electrode is cold pressed for 24 hours, the rebound rate of the negative electrode is not higher than 7.0%.
[0051] In any embodiment, the cohesive force of the negative electrode sheet is not less than 73 N / m, and can be optionally not less than 80 N / m.
[0052] In any embodiment, based on the total mass of the negative electrode film layer, the mass content of the conductive agent is 0.2%-2%, and the sheet resistance of the negative electrode film layer is not higher than 0.15Ω.
[0053] A sixth aspect of the present application provides a secondary battery, characterized in that it includes the negative electrode sheet of the fifth aspect.
[0054] In any embodiment, the secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.
[0055] A seventh aspect of the present application provides an electrical device comprising the secondary battery of the sixth aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] FIG1 is a schematic diagram of a secondary battery according to an embodiment of the present application;
[0057] FIG2 is an exploded view of the secondary battery according to one embodiment of the present application shown in FIG1 ;
[0058] FIG3 is a schematic diagram of a battery module according to an embodiment of the present application;
[0059] FIG4 is a schematic diagram of a battery pack according to an embodiment of the present application;
[0060] FIG5 is an exploded view of the battery pack according to an embodiment of the present application shown in FIG4 ;
[0061] FIG6 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.
[0062] Description of reference numerals:
[0063] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 secondary battery; 51 shell; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION
[0064] Below, the embodiments of the fluoropolymer, conductive paste, negative electrode sheet, secondary battery and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0065] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0066] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0067] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0068] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0069] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0070] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0071] As the energy density of secondary batteries gradually increases, battery manufacturers are increasing the compaction density of pole pieces to fit more pole pieces into the limited housing volume, thereby achieving the goal of increasing the energy density of the battery cell. However, in the actual production process of pole pieces, as the compaction density of the pole pieces increases, the cold pressing process will cause damage to the active material. There is insufficient space between the particles, and the internal repulsive force is too strong. The pole pieces are prone to increase in thickness after cold pressing, and the pole pieces may rebound, affecting the subsequent battery assembly process.
[0072] [Fluoropolymer]
[0073] Based on this, the present application proposes a fluorine-containing polymer comprising at least one structural unit derived from a monomer represented by formula I and at least one structural unit derived from a monomer represented by formula II.
[0074] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15Alkyl, R4, R5, R6 and R7 contain at least two -COOM, M is selected from hydrogen, NH4 or alkali metal.
[0075] As used herein, the term "fluoropolymer" refers to a polymer containing fluorine in its structural units.
[0076] As used herein, the term "polymer" includes, on the one hand, a collection of chemically homogeneous macromolecules prepared by polymerization, but differing in degree of polymerization, molar mass, and chain length. The term also includes derivatives of such collections of macromolecules formed by polymerization, i.e., products that can be obtained by reaction of functional groups in the aforementioned macromolecules, such as addition or substitution, and can be chemically homogeneous or chemically heterogeneous.
[0077] In this article, the term “C 1-3 "Alkyl" refers to both branched and straight-chain saturated aliphatic monovalent hydrocarbon radicals having the specified number of carbon atoms, with no unsaturation present in the radical, having from one to three carbon atoms, and attached to the rest of the molecule by a single bond.
[0078] In this context, the term "C 1-3 "Alkyl" refers to an alkyl group containing 1-3 C in which at least one H atom is replaced by a F atom. In some embodiments, a C 1‐3 Alkyl groups include -CF3 groups and -C2F6 groups.
[0079] In this article, the term “C 1-15 "Alkyl" refers to both branched and straight-chain saturated aliphatic monovalent hydrocarbon radicals having the specified number of carbon atoms, with no unsaturation present in the radical, having from one to fifteen carbon atoms, and attached to the rest of the molecule by a single bond.
[0080] As used herein, the term "substituted" refers to a compound or chemical moiety in which at least one hydrogen atom is replaced by another chemical moiety, wherein the substituents are each independently selected from the group consisting of hydroxyl, thiol, amino, cyano, nitro, aldehyde, halogen, alkenyl, alkynyl, aryl, heteroaryl, C 1-6 Alkyl, C 1-6 Alkoxy.
[0081] In some embodiments, R1 is fluorine, and R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl.
[0082] As used herein, the term "alkali metals" refers to the six metal elements in Group IA of the periodic table except hydrogen (H), namely lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), and francium (Fr).
[0083] In some embodiments, -COOM includes any one of -COOH, -COONH4, -COOLi, -COONa, and -COOK.
[0084] In some embodiments, R4, R5, R6 and R7 contain at least two -COOH groups.
[0085] In some embodiments, R4, R5, R6 and R7 contain at least two -COO NH4 groups.
[0086] In some embodiments, R4, R5, R6, and R7 contain at least two -COOLi.
[0087] In some embodiments, R4, R5, R6 and R7 contain at least two -COONa groups.
[0088] In some embodiments, R4, R5, R6 and R7 contain at least two -COOK groups.
[0089] In some embodiments, R4, R5, R6 and R7 independently comprise any two or more of -COOH, -COONH4, -COOLi, -COONa, and -COOK.
[0090] In some embodiments, R4 and R5 are independently selected from any one of -COOH, -COONH4, -COOLi, -COONa, and -COOK.
[0091] In some embodiments, in some embodiments, R6 and R7 are independently selected from any one of -COOH, -COONH4, -COOLi, -COONa, and -COOK.
[0092] In some embodiments, R4 and R6 are independently selected from any one of -COOH, -COONH4, -COOLi, -COONa, and -COOK.
[0093] In some embodiments, R4 comprises two or more -COOH, -COONH4, -COOLi, -COONa, or -COOK.
[0094] In some embodiments, the monomer represented by formula I is selected from one or more of vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.
[0095] In some embodiments, the monomer represented by Formula II is selected from one or more of allylmalonic acid, 2-pentaconedioic acid, lithium 2-pentaconedioate, lithium allylmalonic acid, lithium methylenemalonic acid, lithium vinylmalonic acid, lithium butylmalonic acid, lithium glutaconedioate, lithium maleic acid, trans-glutaconedioate, lithium hexamethylenediamine, lithium heptamethylenediamine, lithium octenedioate, sodium allylmalonic acid, sodium methylenemalonic acid, sodium vinylmalonic acid, sodium allylmalonic acid, sodium 2-(4-pentene)malonic acid, sodium maleic acid, trans-glutaconedioate, sodium hexamethylenediamine, sodium heptamethylenediamine, sodium octenedioate, potassium allylmalonic acid, potassium methylenemalonic acid, potassium vinylmalonic acid, and potassium heptamethylenediamine.
[0096] In this article, the term "process window" refers to the process range that can ensure product quality, including but not limited to temperature range, pressure range, storage time length, etc. It can be understood that the wider the process window, the lower the requirement for process accuracy.
[0097] As used herein, the term "carboxylate group" refers to -COONH4, -COOLi, -COONa, -COOK, -COORb, -COOCs, -COOFr.
[0098] In some embodiments, the polymer comprises one or more structural units derived from the monomers of formula I. In some embodiments, the polymer comprises one or more structural units derived from the monomers of formula II. In some embodiments, the polymer includes but is not limited to fluoropolymers including vinylidene fluoride-allyl dilithium propylene copolymer, vinylidene fluoride-allyl malonic acid copolymer, vinylidene fluoride-sodium butyl malonate copolymer, vinylidene fluoride-lithium 2-pentenedioate copolymer, vinylidene fluoride-chlorotrifluoroethylene-lithium allyl malonate copolymer, and hexafluoropropylene-sodium vinyl malonate copolymer.
[0099] The fluorine element in the structural unit derived from the monomer shown in formula I can form hydrogen bonds with the hydroxyl group or / and carboxyl group on the surface of the active substance. In addition, the carboxyl group and / or carboxylate group contained in the structural unit derived from the monomer shown in formula II can form hydrogen bonds with the hydroxyl group or / and carboxyl group on the surface of the active substance. The two work together to improve the cohesion of the electrode, reduce the irreversible expansion of the electrode during the manufacturing process, reduce the rebound rate of the electrode after 24 hours of cold pressing, and improve the quality of the electrode. In addition, the structural unit derived from the monomer shown in formula II can effectively reduce the fluorine content of the fluorine-containing polymer and improve the slurry gel phenomenon caused by the fluorine element. Moreover, the structural unit derived from the monomer shown in formula II can further increase the steric hindrance of the fluorine-containing polymer, reduce the aggregation of the fluorine-containing units, reduce the viscosity of the slurry, alleviate the gelation of the slurry, and effectively improve the filterability of the slurry. The structural unit derived from the monomer represented by Formula II contains at least two carboxyl groups and / or carboxylate groups, which can further improve the cohesion of the electrode and reduce the rebound rate of the electrode after cold pressing. In addition, it can also reduce the viscosity of the conductive paste and improve the filterability of the conductive paste, making it less likely for the conductive paste to gel during storage, thereby improving the anti-gelling and storage properties of the conductive paste and further reducing the DC impedance of the battery.
[0100] In summary, the fluorine-containing polymer provided in the present application can, on the one hand, act as a dispersant, which can significantly alleviate the gelation of the conductive paste during storage, improve the anti-gelation and storage properties of the conductive paste, reduce the diaphragm resistance of the electrode, reduce the DC internal resistance of the battery, and thus improve the dynamic performance of the battery. On the other hand, the fluorine-containing polymer can increase the cohesion of the electrode, reduce the irreversible expansion of the electrode during the manufacturing process, reduce the rebound rate of the electrode after cold pressing for 24 hours, and improve the quality of the electrode.
[0101] In some embodiments, M is selected from one or more of lithium, sodium, and potassium.
[0102] In some embodiments, -COOM is any one of -COOLi, -COONa, and -COOK.
[0103] The lithium, sodium or potassium introduced into the fluorinated polymer can form ion exchange with the active ions during the charge and discharge process, further increasing the mobility of the active ions, reducing the DC internal resistance of the battery, and improving the battery's kinetic performance.
[0104] In some embodiments, the molar content of the structural unit derived from the monomer represented by Formula I is 60% to 80%, based on the total moles of all structural units in the fluoropolymer.
[0105] In some embodiments, the molar content of the structural unit derived from the monomer represented by Formula I can be selected from any value of 60%, 70%, 80%, or a range consisting of any two values thereof, based on the total molar number of all structural units in the fluoropolymer.
[0106] By controlling the molar content of the structural unit derived from the monomer represented by Formula I within an appropriate range, the viscosity of the conductive paste, the cohesive force of the electrode, and the rebound rate of the electrode after cold pressing for 24 hours can be taken into account, thereby comprehensively improving the processing performance and performance of the conductive paste.
[0107] In some embodiments, the molar content of the structural units derived from the monomer of Formula II is 20% to 40%, based on the total moles of all structural units in the fluoropolymer. In some embodiments, the molar content of the structural units derived from the monomer of Formula II can be any value selected from 20%, 30%, or 40%, or a range consisting of any two values thereof, based on the total moles of all structural units in the fluoropolymer.
[0108] By controlling the molar content of the structural unit derived from the monomer represented by Formula II within an appropriate range, the viscosity of the conductive paste, the cohesion of the electrode, and the rebound rate of the electrode after cold pressing for 24 hours can be taken into account, thereby comprehensively improving the processing performance and performance of the conductive paste.
[0109] In some embodiments, the weight average molecular weight of the fluorinated polymer is 80,000 to 120,000. In some embodiments, the weight average molecular weight of the fluorinated polymer can be any value selected from 80,000, 90,000, 100,000, 110,000, and 120,000, or a range consisting of any two of these values.
[0110] As used herein, the term "weight average molecular weight" refers to the sum of the weight fractions of molecules of different molecular weights in a polymer multiplied by their corresponding molecular weights.
[0111] In the present application, the weight-average molecular weight of the polymer can be tested using methods known in the art, such as gel chromatography, such as using a Waters 2695 Isocratic HPLC gel chromatograph (differential refractive index detector 2141). In some embodiments, the testing method is to use a polystyrene solution sample with a mass fraction of 3.0% as a reference and select a matching chromatographic column (oily: Styragel HT5DMF7.8×300mm+Styragel HT4). Use purified N-methylpyrrolidone (NMP) solvent to prepare a 3.0% fluoropolymer glue, and let the prepared solution stand for one day for use. During the test, first use a syringe to draw tetrahydrofuran, rinse, and repeat several times. Then draw 5 ml of the experimental solution, expel the air in the syringe, and wipe the needle tip dry. Finally, slowly inject the sample solution into the injection port. After the reading stabilizes, obtain the data and read the weight-average molecular weight.
[0112] Controlling the weight average molecular weight of the fluoropolymer within an appropriate range allows the slurry to have an appropriate viscosity, which is beneficial for the subsequent preparation of the negative electrode slurry. At the same time, the fluoropolymer with an appropriate weight average molecular weight is conducive to the formation of a three-dimensional network bonding structure, which allows the electrode to have good cohesion. The electrode has a low rebound rate after cold pressing for 24 hours, which can take into account the viscosity of the conductive slurry, the cohesion of the electrode and the rebound rate of the electrode after cold pressing for 24 hours, and comprehensively improve the processing performance and use performance of the conductive slurry.
[0113] In one embodiment of the present application, a method for preparing a fluorinated polymer is provided, comprising the following steps:
[0114] Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized to form a polymer product,
[0115] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, said R4, R5, R6 and R7 contain at least two -COOH,
[0116] Optionally, the polymer product is subjected to a neutralization reaction with a neutralizing agent, wherein the neutralization reaction converts at least part of -COOH in the polymer product into -COOM, where M comprises NH4 or an alkali metal.
[0117] In some embodiments, the method for preparing a fluoropolymer comprises the following steps:
[0118] Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized to form a polymer product,
[0119] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, wherein R4, R5, R6 and R7 contain at least two -COOH groups.
[0120] In some embodiments, the method for preparing a fluoropolymer comprises the following steps:
[0121] Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized to form a polymer product,
[0122] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, said R4, R5, R6 and R7 contain at least two -COOH,
[0123] The polymer product is subjected to a neutralization reaction with a neutralizing agent, wherein the neutralization reaction converts at least a portion of -COOH in the polymer product into -COOM, where M comprises NH4 or an alkali metal.
[0124] In some embodiments, the neutralizing agent includes one or more of lithium carbonate, sodium carbonate, potassium carbonate, lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, lithium hydroxide, sodium hydroxide, potassium hydroxide, and aqueous ammonia.
[0125] Compared with traditional dispersants, the fluorine-containing polymer prepared by this method can improve the dispersibility of the conductive paste, alleviate the gelation of the conductive paste during storage, improve the anti-gelation and storage properties of the conductive paste, reduce the diaphragm resistance of the electrode, reduce the DC internal resistance of the battery, and improve the dynamic performance of the battery. At the same time, the fluorine-containing polymer can also improve the cohesion of the electrode, reduce the irreversible expansion of the electrode during the production process, reduce the rebound rate of the electrode after 24 hours of cold pressing, and improve the quality of the electrode.
[0126] In some embodiments, M comprises one or more of lithium, sodium, and potassium.
[0127] In some embodiments, R1 is fluorine, and R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl.
[0128] In some embodiments, the molar content of the monomer represented by formula I is 60%-80%, based on the total moles of the monomer represented by formula I and the monomer represented by formula II.
[0129] In some embodiments, the molar content of the monomer represented by formula II is 20%-40%, based on the total moles of the monomer represented by formula I and the monomer represented by formula II.
[0130] In some embodiments, the polymerization reaction specifically comprises:
[0131] First stage polymerization: providing an initiator, an emulsifier, at least one monomer represented by formula I, and a solvent to carry out the first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure;
[0132] Second stage polymerization: After a period of reaction, the monomer represented by formula I and the monomer represented by formula II are fed into the reaction vessel to carry out the second stage polymerization, and the monomer represented by formula I is continuously fed into the second stage polymerization;
[0133] Optionally, after the second stage polymerization reaction is completed, the neutralizing agent is added into the reactor to carry out a neutralization reaction.
[0134] In some embodiments, the polymerization reaction specifically comprises:
[0135] First stage polymerization: providing an initiator, an emulsifier, at least one monomer represented by formula I, and a solvent to carry out the first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure;
[0136] Second stage polymerization: After a period of reaction, the monomer represented by formula I and the monomer represented by formula II are fed into the reaction vessel for second stage polymerization, and the monomer represented by formula I is continuously fed into the second stage polymerization.
[0137] In some embodiments, the polymerization reaction specifically comprises:
[0138] First stage polymerization: providing an initiator, an emulsifier, at least one monomer represented by formula I, and a solvent to carry out the first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure;
[0139] Second stage polymerization: After a period of reaction, the monomer represented by formula I and the monomer represented by formula II are fed into the reaction vessel to carry out the second stage polymerization, and the monomer represented by formula I is continuously fed into the second stage polymerization;
[0140] After the second stage polymerization reaction is completed, the neutralizing agent is added into the reactor to carry out a neutralization reaction.
[0141] The method provided in the present application is to form a fluorine-containing segment by continuously feeding the monomer shown in formula I first, so that the fluorine-containing polymer has high thermal stability; and then the monomer shown in formula II is introduced to reduce the contact of the fluorine-containing segment with the external environment, effectively alleviating the gel phenomenon caused by the fluorine element. The fluorine-containing polymer prepared by this method can effectively improve the stability of the conductive paste, improve the dispersibility of the slurry, improve the cohesion of the pole piece, reduce the pole piece rebound rate after 24 hours of cold pressing of the pole piece, reduce the diaphragm resistance of the pole piece and the DC internal resistance of the battery, and improve the dynamic performance of the battery. In addition, when the monomer shown in formula II is fed into the reaction vessel for the second stage of polymerization, the monomer shown in formula I is continued to be fed into the reaction vessel, which helps to improve the compatibility of the segment generated by the first stage of polymerization and the segment generated by the second stage of polymerization, thereby improving the stability of the fluorine-containing polymer.
[0142] In some embodiments, the mass of the monomer of formula I introduced in the first stage of polymerization is 30%-70% of the total mass of the monomer of formula I supplied in the polymerization reaction, and the mass of the monomer of formula I introduced in the second stage of polymerization is 30%-70% of the total mass of the monomer of formula I supplied in the polymerization reaction.
[0143] In some embodiments, the weight percentage of the initiator is 0.5%-1.5%, based on the total weight of the monomer represented by Formula I and the monomer represented by Formula II.
[0144] In some embodiments, the mass percentage of the emulsifier is 0.1%-0.5%, based on the total mass of the monomer represented by Formula I and the monomer represented by Formula II.
[0145] In some embodiments, the mass percentage of the aqueous medium provided in the polymerization reaction is 400% to 600%, based on the total mass of the monomer represented by Formula I and the monomer represented by Formula II.
[0146] In some embodiments, the reaction pressure of the polymerization reaction is 7 MPa-9 MPa, and the reaction temperature of the polymerization reaction is 80° C.-120° C.
[0147] In some embodiments, the initiator is one or both of N,N-dimethylbenzylamine and N-methylamphetamine.
[0148] In some embodiments, the emulsifier is at least one of alkali metal perfluorooctanoate, polyoxyethylene-4-phenol ether ammonium sulfate, and nonylphenol polyoxyethylene ether ammonium sulfate.
[0149] In one embodiment of the present application, there is provided an application of the fluorine-containing polymer in any embodiment in a secondary battery. Optionally, the secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.
[0150] [Conductive paste]
[0151] In one embodiment of the present application, a conductive paste is provided, comprising a conductive agent, an aqueous medium, and the fluorine-containing polymer described in any embodiment.
[0152] Compared to the prior art method of directly adding a conductive agent to the negative electrode slurry during preparation, the conductive slurry provided in this application can improve the dispersibility of the conductive agent in the negative electrode slurry, enhance the conductive effect of the conductive agent in the electrode sheet, and thus effectively reduce the conductive agent content in the electrode sheet, which is conducive to further increasing the load of the electrode sheet and improving the power performance of the battery. In addition, the fluoropolymer in the conductive slurry can simultaneously act as a binder and a dispersant. On the premise of improving the dispersibility of the conductive slurry, increasing the dispersibility of the conductive agent in the electrode sheet, and reducing the DC impedance of the battery, it can also increase the cohesion of the electrode sheet, reduce the rebound rate after cold pressing, and improve the quality of the electrode sheet.
[0153] In some embodiments, the aqueous medium comprises deionized water.
[0154] In some embodiments, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0155] In some embodiments, the conductive agent comprises carbon nanotubes.
[0156] The one-dimensional linear carbon nanotubes form a long-range conductive network in the electrode. This conductive network can connect the active material particles together, so that the particles maintain electrical contact, and the battery has a small DC impedance. At the same time, this conductive network can play a certain limiting role in the mutual repulsion between the active material particles after cold pressing, reduce the rebound rate of the electrode after cold pressing, and improve the quality of the electrode.
[0157] In some embodiments, the mass fraction of the conductive agent is 1.5%-4.5%, based on the total mass of the conductive paste.
[0158] In some embodiments, the mass fraction of the conductive agent can be selected as any value of 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or a range consisting of any two values thereof, based on the total mass of the conductive paste.
[0159] By controlling the mass fraction of the conductive agent within an appropriate range, the slurry has an appropriate viscosity based on the total mass of the conductive slurry, and the electrode has a low rebound rate after cold pressing for 24 hours, thereby comprehensively improving the processing performance and performance of the slurry.
[0160] In some embodiments, the mass fraction of the fluoropolymer is 0.5%-1.5%, based on the total mass of the conductive paste. In some embodiments, the mass fraction of the fluoropolymer is any value selected from the group consisting of 0.5%, 0.75%, 1%, 1.25%, and 1.5%, or a range consisting of any two of these values, based on the total mass of the conductive paste.
[0161] By controlling the mass fraction of the fluoropolymer within a suitable range, the slurry has a suitable viscosity based on the total mass of the conductive slurry, and the electrode has a low rebound rate after cold pressing for 24 hours, thereby comprehensively improving the processing performance and performance of the slurry.
[0162] In any embodiment, the solid content of the conductive paste is 1%-10%, and the viscosity of the conductive paste is 500 mPa·s-5000 mPa·s.
[0163] In some embodiments, the solid content of the conductive paste may be any value selected from 1%, 3%, 5%, 6%, 10%, or a range consisting of any two values thereof.
[0164] In some embodiments, the viscosity of the conductive paste can be selected as any value of 500mPa·s, 600mPa·s, 700mPa·s, 800mPa·s, 900mPa·s, 1000mPa·s, 1100mPa·s, 1200mPa·s, 1300mPa·s, 1400mPa·s, 1500mPa·s, 2000mPa·s, 2500mPa·s, 3000mPa·s, 3500mPa·s, 4000mPa·s, 4500mPa·s, 5000mPa·s, or a range consisting of any two values therein.
[0165] The solid content is 1%-10%, and the viscosity is 500mPa·s-5000mPa·s. It can be directly mixed and stirred with active materials and binders to prepare negative electrode slurry without adding additional additives, which is beneficial to improving production efficiency and reducing production costs.
[0166] [Negative electrode]
[0167] The fifth aspect of the present application provides a negative electrode plate, comprising a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, wherein the negative electrode film layer comprises a negative electrode active material, a conductive agent and a binder, and the conductive agent comprises a deposit of the conductive slurry of the fourth aspect.
[0168] As used herein, the term "binder" refers to a chemical compound, polymer, or mixture that forms a colloidal solution or colloidal dispersion in a dispersion medium.
[0169] Compared with the negative electrode sheets prepared by directly adding conductive agent powder in the prior art, the conductive agent in the negative electrode sheets disclosed in the present application exists in the form of conductive slurry deposits in the negative electrode sheets. On the one hand, it can improve the cohesion of the sheets, reduce the rebound rate of the sheets after cold pressing for 24 hours, and improve the quality of the sheets. On the other hand, adding in the form of conductive slurry can improve the dispersion performance of the conductive material, so that the negative electrode sheets can have low membrane resistance when the conductive agent is added in a low amount, which provides the possibility of further increasing the loading amount of the negative electrode active material in the sheets.
[0170] In some embodiments, the compacted density of the negative electrode sheet is 1.5 g / cm 3 -1.8g / cm 3 When the negative electrode is cold pressed for 24 hours, the rebound rate of the negative electrode is not higher than 7.0%.
[0171] In this article, the rebound rate of the negative electrode after cold pressing for 24 hours is a well-known meaning in the art and can be measured using instruments and methods known in the art. As an example, the coated negative electrode is cold pressed to a fixed compaction density (1.5g / cm 3 ), test the thickness of the negative electrode sheet, recorded as h1; after the cold pressed electrode sheet is left to stand for 24 hours, test the thickness of the negative electrode sheet, recorded as h2,
[0172] Rebound rate of the electrode after 24 hours of cold pressing (%) = (h2-h1) / h1×100%.
[0173] On the premise of meeting the high compaction density of the negative electrode plate and improving the energy density of the battery, the negative electrode plate of the present application has a low rebound rate after 24 hours of cold pressing, which improves the use quality of the plate, improves the quality of the plate, and is beneficial to the subsequent assembly process of the battery.
[0174] In some embodiments, the compacted density of the pole piece can be selected to be 1.3 g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 Any value in , or a range of any two values in .
[0175] In some embodiments, the rebound rate of the negative electrode plate after cold pressing for 24 hours can be selected to be any one of no higher than 7.0%, no higher than 6.0%, and no higher than 5.0%.
[0176] In some embodiments, the cohesive force of the negative electrode sheet is not less than 73 N / m, and can be optionally not less than 80 N / m.
[0177] In this article, the cohesion of the negative electrode sheet has a meaning well known in the art and can be measured using instruments and methods well known in the art. As an example, double-sided tape is used to stick on a steel plate, and the negative electrode sheet is cut into a 20 cm long and 20 mm wide strip on the double-sided tape. A single-sided adhesive tape (width × length = 20 mm × 80 mm) for testing the cohesion of the negative electrode sheet is centered on and covers the strip. A white paper strip with a width × length = 20 mm × 60 mm is cut and inserted between the steel plate and the single-sided adhesive tape, with an overlap length of about 15 mm. A roller is used to roll back and forth on the strip four times. The white paper is clamped in the tensile testing machine fixture, and the tensile testing machine is turned on to separate the single-sided adhesive tape adhering to the negative electrode film layer of the strip from the strip. The cohesion value is obtained after the test is completed.
[0178] In some embodiments, based on the total mass of the negative electrode film layer, the mass content of the conductive agent is 0.2%-2%, and the sheet resistance of the negative electrode film layer is not higher than 0.15Ω.
[0179] In some embodiments, based on the total mass of the negative electrode film layer, the mass content of the conductive agent can be any value of 0.2%, 0.5%, 1%, 1.5%, 2%, or a range consisting of any two values thereof.
[0180] In some embodiments, the sheet resistance of the negative electrode film layer may be selected to be no higher than any one of 0.15Ω, 0.1Ω, and 0.05Ω.
[0181] In this article, the sheet resistance of the negative electrode film layer has a meaning well known in the art and can be measured using instruments and methods well known in the art. As an example, cut the dried electrode sheet at the left, center, and right sides of the electrode sheet into small discs with a diameter of 10 mm. Turn on the Yuanneng Technology electrode sheet resistance meter power supply, place it in the appropriate position of the electrode sheet resistance meter "probe", click the "Start" button, wait for the reading to stabilize, and then read it. Test two positions on each small disc, and finally calculate the average of the six measurements, which is the membrane resistance of the electrode sheet.
[0182] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0183] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0184] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0185] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0186] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0187] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0188] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the fluoropolymer, the conductive agent, and the deionized water are first stirred to prepare a conductive slurry, and the negative electrode active material, the binder, the conductive slurry and any other components are dispersed in the deionized water to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0189] [Positive electrode]
[0190] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.
[0191] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0192] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0193] In some embodiments, the positive electrode active material may adopt the positive electrode active material for batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0194] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0195] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0196] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0197] [Electrolytes]
[0198] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0199] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0200] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0201] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0202] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0203] [Isolation film]
[0204] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0205] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0206] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0207] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0208] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0209] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG1 shows a secondary battery 5 with a square structure as an example.
[0210] In some embodiments, referring to Figure 2, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0211] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.
[0212] Figure 3 shows an example battery module 4. Referring to Figure 3 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.
[0213] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0214] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.
[0215] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 5 and 6 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0216] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.
[0217] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.
[0218] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.
[0219] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0220] Example
[0221] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0222] Example 1
[0223] 1) Preparation of fluorinated polymers
[0224] First stage polymerization: Add 30 kg of deionized water (conductivity less than or equal to 2 μs / cm), 15 g of sodium perfluorooctanoate, and 54 g of N,N-dimethylbenzylamine into a 50 L reactor and close the reactor;
[0225] The reactor was vacuumed and filled with nitrogen, and the operation was repeated until the oxygen concentration in the reactor was less than 100 ppm;
[0226] Add vinylidene fluoride monomer into the reactor until the pressure inside the reactor reaches 8.0 MPa;
[0227] The temperature in the kettle was raised to 100°C to start the reaction. During the reaction, vinylidene fluoride monomer was continuously introduced to maintain the reaction pressure in the kettle constant.
[0228] Second stage polymerization: When the mass of the introduced vinylidene fluoride monomer reached 1411.1 g, the reaction pressure was maintained at 8.0 MPa and the temperature was 100°C. 1411.1 g of vinylidene fluoride monomer and 3177.8 g of allylmalonic acid monomer were introduced into the reactor and the reaction was continued for 8 hours.
[0229] When the reaction is completed, the pressure in the autoclave drops to 0.2 MPa, and the unreacted vinylidene fluoride monomer is recovered;
[0230] The reaction product was coagulated, washed, neutralized by adding 1625.58 g of lithium carbonate, and stirred for 2 h; then separated and concentrated to obtain a vinylidene fluoride-allyl lithium malonate copolymer emulsion with a solid content of 25%, wherein the vinylidene fluoride-allyl lithium malonate copolymer had a weight average molecular weight of 100,000.
[0231] 2) Preparation of conductive paste
[0232] 18400 g of deionized water and 800 g of vinylidene fluoride-lithium allyl malonate copolymer emulsion were added to a 35 L stirring tank and stirred at a stirring speed of 800 rpm for 30 min to obtain a precast glue solution;
[0233] Then, 800 g of carbon nanotubes were added to the prefabricated glue solution and stirred at a speed of 800 rpm for 180 min, and cooling water circulation was started to obtain a conductive paste having a solid content of 5%.
[0234] 3) Preparation of negative electrode sheet
[0235] Active material artificial graphite, active material SiO2, binder styrene butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC), and the above conductive slurry are added to deionized water and mixed evenly to prepare a negative electrode slurry; the negative electrode slurry is evenly coated on a negative electrode current collector copper foil once or multiple times, and the negative electrode sheet is obtained after drying, cold pressing, and slitting. In the negative electrode film layer, the weight ratio of the deposits of active material artificial graphite, active material SiO2, binder styrene butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC), and conductive slurry is 90.8%:5%:3%:1%:0.2%.
[0236] 4) Preparation of positive electrode sheet
[0237] Lithium nickel cobalt manganese (NCM) material, conductive agent carbon black, polyvinylidene fluoride binder, and N-methylpyrrolidone (NMP) are stirred and mixed in a weight ratio of 96.9:2.1:1:21 to obtain a positive electrode slurry with a solid content of 73%. The positive electrode slurry is then evenly coated on the positive electrode current collector aluminum foil, and then dried, cold pressed, and cut to obtain a positive electrode sheet.
[0238] 5) Isolation film
[0239] Polypropylene film is used as the isolation film.
[0240] 6) Preparation of electrolyte
[0241] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), the organic solvent ethylene carbonate (EC) / ethyl methyl carbonate (EMC) was mixed uniformly in a volume ratio of 3 / 7, 12.5% LiPF6 lithium salt was added and dissolved in the organic solvent, and stirred uniformly to obtain the electrolyte of Example 1.
[0242] 7) Preparation of batteries
[0243] The positive electrode sheet, separator, and negative electrode sheet of Example 1 were stacked in order, with the separator positioned between the positive and negative electrode sheets to provide insulation. The cells were then wound to form a bare cell. The tabs were welded to the bare cell and placed in an aluminum casing. The cells were then baked at 80°C to remove moisture. Electrolyte was then injected and sealed to produce an uncharged battery. The uncharged battery then underwent a series of steps, including resting, hot and cold pressing, formation, shaping, and capacity testing, to produce the lithium-ion battery product of Example 1.
[0244] In Examples 2 to 5, the molar ratio of each monomer in the fluorine-containing polymer was adjusted, and other parameters remained the same as in Example 1. Specific parameters are shown in Table 1.
[0245] In Examples 6 to 9, the experimental parameters of the preparation method of the fluoropolymer were adjusted so that the fluoropolymer had different weight-average molecular weights. Other parameters remained the same as in Example 1. Specific parameters are shown in Tables 1 and 2.
[0246] Specifically, the preparation method of the fluorine-containing polymer with a weight-average molecular weight of 60,000 in Example 6 is basically the same as the steps in Example 1, except that the amount of N,N-dimethylbenzylamine added is adjusted to 59.4 g and the reaction temperature is adjusted to 105°C.
[0247] The preparation method of the fluorinated polymer with a weight-average molecular weight of 80,000 in Example 7 is basically the same as that in Example 1, except that the amount of N,N-dimethylbenzylamine added is adjusted to 56.7 g and the reaction temperature is adjusted to 105°C.
[0248] The preparation method of the fluorine-containing polymer with a weight-average molecular weight of 120,000 in Example 8 is basically the same as the steps in Example 1, except that the reaction temperature is adjusted to 95° C. and the amount of N,N-dimethylbenzylamine added is adjusted to 51.3 g.
[0249] The preparation method of the fluorine-containing polymer with a weight-average molecular weight of 150,000 in Example 9 is basically the same as the steps in Example 1, except that the reaction temperature is adjusted to 95° C. and the amount of N,N-dimethylbenzylamine added is adjusted to 48.6 g.
[0250] In Examples 10 to 13, the mass fraction of the fluorine-containing polymer in the conductive paste was adjusted, and other parameters remained the same as in Example 1. Specific parameters are shown in Table 1.
[0251] In Examples 14 to 17, the mass fraction of the conductive agent in the conductive primer slurry was adjusted, and other parameters remained the same as in Example 1. Specific parameters are shown in Table 1.
[0252] In Example 18, the allylmalonic acid monomer was replaced with a 2-pentaconedioic acid monomer, and the other parameters were the same as in Example 1. For specific parameters, see Table 1.
[0253] In Example 19, 1411.1 g of vinylidene fluoride monomer in the first stage polymerization and 1411.1 g in the second stage polymerization were replaced by 960.5 g of vinylidene fluoride and 815.3 g of chlorotrifluoroethylene monomer, respectively. Other parameters were the same as in Example 1. For specific parameters, see Table 1.
[0254] In Example 20, lithium carbonate was not added for neutralization after the polymerization was completed, and other parameters were the same as in Example 1. For specific parameters, see Table 1.
[0255] In Comparative Example 1, the fluorine-containing polymer in the conductive paste was replaced with a dispersant polyvinylpyrrolidone (PVP), and other parameters were the same as those in Example 1. For specific parameters, see Table 1.
[0256] In Comparative Example 2, polyvinylidene fluoride emulsion was used as the fluorine-containing polymer, and other parameters were the same as those in Example 1. For specific parameters, see Table 1.
[0257] In Comparative Example 3, polyallyl lithium malonate emulsion was used as the fluorine-containing polymer, and other parameters were the same as those in Example 1. For specific parameters, see Table 1.
[0258] In Comparative Example 4, the allylmalonic acid monomer was replaced with 4-pentenoic acid monomer, and other parameters were the same as those in Example 1. For specific parameters, see Table 1.
[0259] In Comparative Example 5, conductive carbon black was used instead of conductive paste to directly prepare the negative electrode sheet. Other parameters were the same as those in Example 1. For specific parameters, see Table 1.
[0260] In Comparative Example 6, the mass content of the conductive carbon black was adjusted to 2.0%, based on the total mass of the negative electrode film layer. Other parameters were substantially the same as those in Comparative Example 5. For specific parameters, see Table 1.
[0261] 2. Test Method
[0262] 1. Characterization of Fluoropolymer Properties
[0263] (1) Measurement of weight average molecular weight of fluoropolymer
[0264] A Waters 2695 Isocratic HPLC gel chromatograph (differential refractive index detector 2141) was used. A polystyrene solution sample with a mass fraction of 3.0% was used as a reference, and a matching chromatographic column was selected (oily: Styragel HT5 DMF 7.8×300 mm + Styragel HT4). A 3.0% fluoropolymer solution was prepared using purified N-methylpyrrolidone (NMP) solvent. The prepared solution was allowed to stand for one day for later use. During the test, tetrahydrofuran was first drawn into a syringe and rinsed, and repeated several times. Then 5 ml of the experimental solution was drawn, the air in the syringe was expelled, and the needle tip was wiped dry. Finally, the sample solution was slowly injected into the injection port. After the display stabilized, the data was acquired and the weight-average molecular weight was read.
[0265] 2. Property test of conductive paste
[0266] (1) Viscosity test of conductive paste
[0267] Use a rotating viscometer to measure the viscosity of the primer slurry. Select a suitable rotor, secure the viscometer rotor, and place the primer slurry under the viscometer rotor, so that the slurry just covers the rotor scale line. Instrument model: Shanghai Fangrui NDJ-5S, rotor #62, speed 30 rpm, measurable slurry viscosity range 0-1000mPa·s; rotor #63, speed 30 rpm, measurable slurry viscosity range 0-2000mPa·s); rotor #63, speed 12 rpm, measurable slurry viscosity range 2000-10000mPa·s. Test temperature: 25°C, test time 5 minutes, wait for the display to stabilize before reading the data.
[0268] (2) Filtration performance test of conductive slurry
[0269] Take a 500ml beaker and place it at the lower end of a 200-mesh filter stand. Take 500ml of the conductive slurry and place it in the filter to filter. Record the time when the volume of the slurry in the beaker reaches 300ml. This time is used to judge the filtration performance of the slurry. If the filtration time is less than 120s, it indicates that the filtration performance of the slurry is good, which is recorded as "Y". If the slurry cannot pass through the filter, it indicates that the filtration performance of the slurry is poor, which is judged as "N".
[0270] (3) Solid content of conductive paste and the difference in solid content of upper and lower layers after standing for 24 hours
[0271] Take the copper foil and weigh it in the weight loss rate measuring instrument, record it as M0, and reset it to zero;
[0272] Take a small amount of conductive paste and apply it on the copper foil, then put it into the moisture meter and weigh it, record it as M1;
[0273] Close the device and start drying;
[0274] After the end, record the weighing data, record it as M2, and calculate the solid content, the solid content is (M2-M0) / (M1-M0);
[0275] The solid content of the upper and lower conductive pastes was measured in the same way after standing for 24 hours, and the solid content of the lower conductive paste minus the solid content of the upper conductive paste was taken as the difference in solid content of the upper / lower layers after standing for 24 hours.
[0276] (4) Gel state test after the conductive paste has been left standing for 60 days
[0277] Use a steel ruler to lift the slurry in the beaker and judge whether the slurry is gelled based on the flow state of the slurry. If the slurry does not gel, record it as "No", if the slurry has gelled, record it as "Yes";
[0278] There is gel: The slurry clumps or does not flow naturally and continuously.
[0279] No gel: The slurry flows naturally and continuously, and the slurry flows flat on the surface of the steel ruler without lumps.
[0280] 3. Pole performance test
[0281] (1) Cohesion of the electrode
[0282] Use double-sided tape to stick on the steel plate, cut the negative electrode sheet into a strip with a length of 20 cm and a width of 20 mm and stick it on the double-sided tape, stick the single-sided tape (width × length = 20 mm × 80 mm) for testing the cohesion of the negative electrode sheet in the center and cover the strip, cut a white paper strip with a width × length = 20 mm × 60 mm and insert it between the steel plate and the single-sided tape, with an overlapping length of about 15 mm, roll the strip back and forth on the strip with a roller 4 times, clamp the white paper on the tensile testing machine fixture, turn on the tensile testing machine test, so that the single-sided tape sticking to the negative electrode film layer of the strip is separated from the strip, and the cohesion value is obtained after the test is completed.
[0283] (2) Electrode rebound rate after 24 hours of cold pressing
[0284] The coated negative electrode sheet is cold pressed to a fixed compaction density (1.65g / cm 3 ), test the thickness of the negative electrode sheet, recorded as h1; after the cold pressed electrode sheet is left to stand for 24 hours, test the thickness of the negative electrode sheet, recorded as h2,
[0285] The rebound rate of the electrode after 24 hours of cold pressing (%) = (h2-h1) / h1×100%.
[0286] (3) Diaphragm resistance of the electrode
[0287] Cut the dried electrode sheet at the left, center, and right sides of the electrode into small discs with a diameter of 10mm. Turn on the Yuanneng Technology electrode resistance meter, place it in the appropriate position on the "probe" of the electrode resistance meter, click the "Start" button, and wait for the reading to stabilize before reading. Test two positions on each small disc, and calculate the average of the six measurements to obtain the film resistance of the electrode.
[0288] 4. Battery performance test
[0289] (1) Battery DC impedance test
[0290] At 25°C, the secondary battery was charged at a constant current rate of 1 / 3C to 4.2V, then charged at a constant voltage of 4.2V to a current of 0.05C, and left for 5 minutes. It was then discharged at a rate of 1 / 3C for 90 minutes, with the electrode assembly adjusted to 50% SOC. The battery was left standing for 60 minutes, and then discharged at a rate of 4C for 30 seconds. The 50% SOC discharge DCR was calculated based on the test data.
[0291] 3. Analysis of test results of various embodiments and comparative examples
[0292] The fluorine-containing polymer, conductive paste, negative electrode sheet and secondary battery of each embodiment and comparative example were prepared according to the above method, and various parameters were measured. The results are shown in Tables 1 and 2 below.
[0293] Table 1 Preparation parameters and results of fluorinated polymers of Example and Comparative Example 1
[0294] Table 2 Preparation parameters and test results of Example 2 and Comparative Example 1
[0295] As can be seen from Tables 1 and 2, the fluorine-containing polymers of Examples 1 to 20 include structural units derived from vinylidene fluoride or chlorotrifluoroethylene, and further include structural units derived from allyl dilithium, allyl diacid, or lithium 2-pentenedioate.
[0296] From the comparison of Examples 1-9, Examples 18-20 and Comparative Example 1, it can be seen that compared with the traditional polyvinyl pyrrolidone dispersant, the fluorine-containing polymer disclosed in the present application can improve the cohesion of the electrode, reduce the rebound rate of the electrode after 24 hours of cold pressing, and improve the quality of the electrode. At the same time, it can also significantly alleviate the gelation of the conductive paste during storage, improve the anti-gelation and storage properties of the conductive paste, reduce the diaphragm resistance of the electrode, reduce the DC internal resistance of the battery, and thus improve the dynamic performance of the battery.
[0297] Comparisons of Examples 1-9 and 18-20 with Comparative Example 2 demonstrate that, compared to polyvinylidene fluoride, the fluoropolymers provided herein can reduce the viscosity of the conductive paste, improve its filterability, and reduce the likelihood of gelation during storage, thereby enhancing its anti-gelling properties and storage properties. This improved dispersion of the conductive paste further reduces the DC impedance of the battery.
[0298] From the comparison of Examples 1-5 and Example 19 with Comparative Example 3, it can be seen that compared to polyallyl lithium malonate, the vinylidene fluoride-allyl lithium propylene copolymer, vinylidene fluoride-2-pentenedioic acid lithium copolymer, vinylidene fluoride-trifluorochloroethylene-allyl lithium malonate copolymer, and vinylidene fluoride-allyl malonic acid copolymer disclosed in the present application can improve the cohesion of the pole piece, reduce the rebound rate of the pole piece after 24 hours of cold pressing, and improve the quality of the pole piece. At the same time, it can also improve the anti-settling property of the conductive paste, improve the adhesion of the pole piece, and reduce the DC internal resistance of the battery. From the comparison of Examples 1-5 and Comparative Example 4, it can be seen that the vinylidene fluoride-allyl lithium propylene copolymer disclosed in the present application can improve the cohesion of the pole piece, reduce the rebound rate of the pole piece after 24 hours of cold pressing, and improve the quality of the pole piece. At the same time, it can also reduce the viscosity of the conductive paste, improve the filterability of the conductive paste, make the conductive paste less likely to gel during storage, and improve the anti-gel and storage properties of the conductive paste. Due to the improvement of the dispersion performance of the conductive slurry, the DC impedance of the battery is further reduced.
[0299] From the comparison between Example 1 and Example 20, it can be seen that compared with the structural unit derived from allylmalonic acid, the fluorine-containing polymer containing lithium 2-allyl propylene can reduce the DC internal resistance of the battery and improve the dynamic performance of the battery.
[0300] From the comparison between Examples 1-3 and 4-5, it can be seen that the molar content of the structural units derived from vinylidene fluoride is 60%-80%, which is based on the total molar number of all structural units in the fluoropolymer. This can take into account the viscosity of the conductive paste, the cohesion of the electrode and the rebound rate of the electrode after cold pressing for 24 hours, thereby comprehensively improving the processing performance and usage performance of the conductive paste.
[0301] From the comparison of Examples 1-3 and 4-5, it can be seen that the molar content of the structural unit derived from allyl dilithium propylene is 20%-40%, based on the total molar number of all structural units in the fluoropolymer, which can take into account the viscosity of the conductive paste, the cohesion of the electrode and the rebound rate of the electrode after cold pressing for 24 hours, thereby comprehensively improving the processing performance and performance of the conductive paste.
[0302] From the comparison between Examples 1, 7-8 and Examples 6 and 9, it can be seen that the weight average molecular weight of the fluorine-containing polymer is 80,000-120,000, which can take into account the viscosity of the conductive paste, the cohesion of the electrode and the rebound rate of the electrode after cold pressing for 24 hours, and comprehensively improve the processing performance and use performance of the conductive paste.
[0303] The conductive pastes in Examples 1-20 all include carbon nanotubes, deionized water, and vinylidene fluoride-allyl dilithium propylene copolymer, vinylidene fluoride-lithium 2-pentenedioate copolymer, vinylidene fluoride-chlorotrifluoroethylene-lithium allyl malonate copolymer, and vinylidene fluoride-allyl malonic acid copolymer.
[0304] As can be seen from Examples 1, 10-13, the mass fraction of the fluoropolymer is 0.5%-1.5% based on the total mass of the conductive paste. The paste has a suitable viscosity and the electrode has a low rebound rate after cold pressing for 24 hours, which comprehensively improves the processing and performance of the paste.
[0305] As can be seen from Examples 1, 14-17, the mass fraction of the conductive agent is 1.5%-4.5% based on the total mass of the conductive paste. The paste has a suitable viscosity, and the electrode has a low rebound rate after cold pressing for 24 hours, which comprehensively improves the processing and performance of the paste.
[0306] As can be seen from Examples 1-20, the solid content of the conductive paste is 1%-10%, and the viscosity of the conductive paste is 500mPa·s-5000mPa·s. The conductive paste prepared from the fluoropolymer does not require the addition of additional dispersants or thickeners to improve processing performance, which helps to improve production efficiency and optimize the production process.
[0307] The negative electrode sheets in Examples 1-20 all include a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector. The negative electrode film layer includes a negative electrode active material, a conductive agent, and a binder. The conductive agent includes a deposit of a conductive slurry.
[0308] From the comparison between Examples 1-20 and Comparative Example 5, it can be seen that compared with the negative electrode plates prepared by directly adding conductive agent powder commonly used in the prior art, the negative electrode plates of the present application contain a conductive agent in the form of a deposit of conductive slurry, which is beneficial to reducing the rebound rate of the plates after cold pressing for 24 hours, improving the cohesion of the plates, and improving the quality of the plates. At the same time, it can also reduce the diaphragm resistance of the plates and the DC internal resistance of the battery, and improve the dynamic performance of the battery.
[0309] Comparison of Examples 1-20 with Comparative Example 6 demonstrates that, compared to prior art methods of directly adding conductive agent powder to negative electrode sheets, the negative electrode sheets disclosed herein contain a conductive agent in the form of a conductive slurry deposit, effectively reducing the rebound rate of the sheet after 24 hours of cold pressing, thereby improving the sheet's quality. Furthermore, the amount of conductive agent required in the negative electrode sheet can be reduced, contributing to an increase in the battery's energy density.
[0310] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A fluorine-containing polymer, It is characterized in that It comprises at least one structural unit derived from a monomer represented by formula I and at least one structural unit derived from a monomer represented by formula II, Among them, R 1 , R 2 , R 3 Each independently selected from hydrogen, fluorine, chlorine or C containing at least one fluorine atom 1-3 Alkyl, R 4 , R 5 , R 6 , R 7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, R 4 , R 5 , R 6 and R 7 Contains at least two -COOM, M is selected from hydrogen, NH 4 or alkali metals.
2. The fluorine-containing polymer according to claim 1, It is characterized in that The M comprises one or more of lithium, sodium and potassium.
3. The fluorine-containing polymer according to claim 1 or 2, It is characterized in that The R 1 is fluorine, R 2 , R 3 Each is independently selected from hydrogen, fluorine, chlorine or trifluoromethyl.
4. The fluorine-containing polymer according to any one of claims 1 to 3, It is characterized in that The molar content of the structural unit derived from the monomer represented by formula I is 60% to 80%, based on the total molar number of all structural units in the fluorine-containing polymer.
5. The fluorine-containing polymer according to any one of claims 1 to 4, It is characterized in that The molar content of the structural unit derived from the monomer represented by formula II is 20% to 40%, based on the total molar number of all structural units in the fluorine-containing polymer.
6. The fluorine-containing polymer according to any one of claims 1 to 5, It is characterized in that The weight average molecular weight of the fluorine-containing polymer is 80,000-120,000.
7. The fluorine-containing polymer according to any one of claims 1 to 6, It is characterized in that The monomer represented by formula I comprises one or more of vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene and hexafluoropropylene.
8. The fluorine-containing polymer according to any one of claims 1 to 7, It is characterized in that The monomer represented by formula II comprises one or more of allylmalonic acid, 2-pentaconedioic acid, lithium 2-pentaconedioate, lithium allylmalonic acid, lithium methylenemalonic acid, lithium vinylmalonic acid, lithium butylmalonic acid, lithium glutaconedioate, lithium maleic acid, trans-glutaconedioate, lithium hexamethylenediamine, lithium heptamethylenediamine, lithium octaconedioate, sodium allylmalonic acid, sodium methylenemalonic acid, sodium vinylmalonic acid, sodium allylmalonic acid, sodium 2-(4-pentene)malonic acid, sodium maleic acid, trans-glutaconedioate, sodium hexamethylenediamine, sodium heptamethylenediamine, sodium octaconedioate, potassium allylmalonic acid, potassium methylenemalonic acid, potassium vinylmalonic acid, and potassium heptamethylenediamine.
9. The fluorine-containing polymer according to any one of claims 1 to 8, It is characterized in that The fluorine-containing polymer includes one or more of vinylidene fluoride-allyl lithium propylene copolymer, vinylidene fluoride-allyl malonic acid copolymer, vinylidene fluoride-sodium butylmalonate copolymer, vinylidene fluoride-2-pentenedioic acid lithium copolymer, vinylidene fluoride-chlorotrifluoroethylene-allyl lithium malonate copolymer, tetrafluoroethylene-allyl lithium propylene copolymer, and vinylidene fluoride-hexafluoropropylene-allyl lithium propylene copolymer.
10. A method for preparing a fluorine-containing polymer, It is characterized in that The following steps are involved: Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized to form a polymer product, Among them, R 1 , R 2 , R 3 Each independently selected from hydrogen, fluorine, chlorine or C containing at least one fluorine atom 1-3 Alkyl, R 4 , R 5 , R 6 , R 7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, R 4 , R 5 , R 6 and R 7 Contains at least two -COOH groups, Optionally, the polymer product is subjected to a neutralization reaction with a neutralizing agent, wherein the neutralization reaction converts at least part of the -COOH in the polymer product into -COOM, where M is selected from NH 4 or alkali Metal.
11. The preparation method according to claim 10, It is characterized in that The M comprises one or more of lithium, sodium and potassium.
12. The preparation method according to claim 10 or 11, It is characterized in that R 1 is fluorine, R 2 , R 3 Each is independently selected from hydrogen, fluorine, chlorine or trifluoromethyl.
13. The preparation method according to any one of claims 10 to 12, It is characterized in that The molar content of the monomer represented by formula I is 60%-80%, based on the total molar number of the monomer represented by formula I and the monomer represented by formula II.
14. The preparation method according to any one of claims 10 to 13, It is characterized in that The molar content of the monomer represented by formula II is 20%-40%, based on the total molar number of the monomer represented by formula I and the monomer represented by formula II.
15. The preparation method according to any one of claims 10 to 14, It is characterized in that The polymerization reaction specifically includes: First stage polymerization: providing an initiator, an emulsifier, at least one monomer represented by formula I and a solvent to carry out first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure; Second stage polymerization: after a period of reaction, the monomer represented by formula I and the monomer represented by formula II are introduced into the reaction container for second stage polymerization, and the monomer represented by formula I is continuously introduced in the second stage polymerization; Optionally, after the second stage polymerization reaction is completed, the neutralizing agent is added into the reactor to carry out a neutralization reaction.
16. The preparation method according to claim 15, It is characterized in that The mass of the monomer of formula I introduced in the first stage polymerization is 30%-70% of the total mass of the monomer of formula I supplied in the polymerization reaction, and the mass of the monomer of formula I introduced in the second stage polymerization reaction is 30%-70% of the total mass of the monomer of formula I supplied in the polymerization reaction.
17. The preparation method according to any one of claims 10 to 16, It is characterized in that The neutralizing agent includes one or more of lithium carbonate, sodium carbonate, potassium carbonate, lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, lithium hydroxide, sodium hydroxide, potassium hydroxide, and ammonia water.
18. Use of the fluorine-containing polymer according to any one of claims 1 to 9 in a secondary battery.
19. A conductive paste, It is characterized in that The conductive paste comprises a conductive agent, an aqueous medium and the fluorine-containing polymer according to any one of claims 1 to 9.
20. The conductive paste according to claim 19, It is characterized in that The mass fraction of the conductive agent is 1.5%-4.5%, based on the total mass of the conductive paste.
21. The conductive paste according to claim 19 or 20, It is characterized in that The mass fraction of the fluorine-containing polymer is 0.5%-1.5%, based on the total mass of the conductive paste.
22. The conductive paste according to any one of claims 19 to 21, It is characterized in that The solid content of the conductive paste is 1%-10%, and the viscosity of the conductive paste is 500mPa·s-5000mPa·s.
23. A negative electrode sheet, comprising a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, wherein the negative electrode film layer comprises a negative electrode active material, a conductive agent and a binder, and the conductive agent comprises a deposit of the conductive slurry according to any one of claims 19 to 22.
24. The negative electrode sheet according to claim 23, It is characterized in that The compaction density of the negative electrode sheet is 1.5 g / cm 3 -1.8g / cm 3 When the negative electrode plate is cold pressed for 24 hours, the plate rebound rate is not higher than 7.0%.
25. The negative electrode sheet according to claim 23 or 24, It is characterized in that The cohesive force of the negative electrode plate is not less than 73 N / m, and can be optionally not less than 80 N / m.
26. The negative electrode sheet according to any one of claims 23 to 25, It is characterized in that Based on the total mass of the negative electrode film layer, the mass content of the conductive agent is 0.2%-2%, and the film resistance of the negative electrode film layer is not higher than 0.15Ω.
27. A secondary battery, It is characterized in that A negative electrode sheet comprising the negative electrode sheet described in any one of claims 23 to 26.
28. The secondary battery according to claim 27, It is characterized in that The secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.
29. An electrical device, It is characterized in that The invention comprises a secondary battery selected from the group consisting of:
Citation Information
Patent Citations
Binder for secondary battery, electrode mixture for secondary battery, electrode for secondary battery and secondary battery
CN111194495A
Binder, preparation method, positive pole piece, secondary battery and electric device
CN115286728A
Polymer, conductive paste, positive electrode sheet, secondary battery, and electric device
CN115340624A
Polymer film layer, preparation method thereof and LED product
CN115889118A
Method for the preparation of styrenic fluoropolymers
US20130211025A1