Material and method for forming a material

The method uses chitosan to separate and concentrate dye from wastewater, creating a biodegradable material that addresses environmental issues in the fashion industry by integrating dye removal and material production, achieving efficient dye removal and cost savings.

WO2024236274A1PCT designated stage expired Publication Date: 2024-11-21CQ STUDIO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/GB2024/051212
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-05-09
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The fashion industry faces environmental issues due to non-degradable petroleum-based plastics and inefficient dye removal from wastewater, leading to pollution and waste, with existing dye removal processes being costly and inefficient.

Method used

A method involving the use of chitosan to separate and concentrate dye from wastewater, forming a biodegradable material that can mimic synthetic plastics, utilizing waste dyeing liquids and integrating into existing supply chains, with optional additives like alginate and glycerol for improved properties.

Benefits of technology

This method effectively remediates dye-containing wastewater, producing a biodegradable material with similar performance to synthetic plastics, reducing environmental impact and offering cost savings through vertical integration and efficient dye removal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GB2024051212_21112024_PF_FP_ABST
    Figure GB2024051212_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A method for producing dyed materials for use in fashion and other industries. The method involves mixing chitosan with a dye-containing liquid, separating a liquid portion of the mixture to form a liquid having an enriched proportion of chitosan and subsequently drying the enriched portion to yield a dyed material. This provides a sustainable method of producing biodegradable dyed materials and recycling dye-containing wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Material and method for forming a material

[0002] Petroleum-based plastics are used in many industries. Their use causes environmental problems because these plastics do not degrade and cause pollution in waterways and landfill. Their use in the fashion industry is widespread, for example in the manufacture of embellishments such as sequins and glitter and in the manufacture of accessories such as buttons.

[0003] Fabrics used in the fashion industry are often dyed by contacting them with a liquid containing a dye. Uptake of the dye by the fabric is rarely complete and this leads to large volumes of waste liquid (usually wastewater) which is contaminated with dye. It is difficult to separate the dye from the waste liquid so that the liquid and dye can be safely disposed of or recycled. Often, up to 50% of industrial synthetic dyes and plant-sourced dyes will not be fixed onto fabric, resulting in large quantities of pigmented wastewater.

[0004] It is known to remove dye from wastewater using chitosan. However, known processes for doing this are inefficient, inconsistent, inconvenient and expensive. The existing processes also generate their own waste products.

[0005] It is amongst the objects of the invention to solve one or more of these problems.

[0006] In a first aspect the invention provides a method of manufacturing a material comprising the steps of; i) providing a liquid which comprises a dye, ii) mixing chitosan with the liquid, iii) separating a liquid portion from the mixture formed in step ii), to leave an enriched portion which has a higher proportion of chitosan and the dye than the mixture formed in step ii), and iv) drying the enriched portion to form the material.

[0007] In a second aspect the invention provides a material which is obtainable by a method as described herein or obtained by a method as described herein.

[0008] In a third aspect the invention provides an article comprising a material which is obtainable by a method as described herein or which is obtained by a method as described herein. The article may be a clothing article. The article may be a fashion or decorative article such as an embellishment, an ornament, a trim, a sequin, a decoration, a textile article, a clothing article, a button, glitter, a sheet or a film. The article may also be, or form part of, a household article such as a curtain, a table cloth, a blind or an upholstery article.

[0009] The method produces a material which may be classed as a bio-plastic. The material is biodegradable and is produced using chitosan, which is an abundant polymer. The method may use chitosan derivatives in the place of chitosan. The chitosan can be sourced from seafood shell waste (i.e. crustacean derived chitosan) or from fungal sources (fungal-derived chitosan). Preferably the liquid in step i) is water. Preferably the liquid in step i) comprises or consists of water. Preferably the liquid is a waste liquid from a dyeing process.

[0010] The method for producing the material also remediates dye-containing liquid (usually wastewater), which is usually difficult to clean. It does so by removing a liquid portion from the mixture formed in step ii). That liquid portion contains a reduced amount of dye relative to the starting liquid mentioned in step i). Preferably the mixture which is created in step ii) is allowed to settle before step iii) is carried out. Preferably the mixture is allowed to settle such that a floc comprising the dye and the chitosan forms a layer. Preferably the layer sits at the bottom of a vessel in which the mixture is located. Preferably a liquid (which is preferably an aqueous liquid), settles above the layer which comprises the dye and the chitosan. Preferably the mixture is allowed to settle for at least 4, 6, 12, 24 or at least 48 hours before step iii) is carried out. Preferably these settling periods are characterised by a lack of agitation.

[0011] The method therefore uses a waste product from the fashion industry as a resource for the production of petroleum plastic-free fashion items. The fact that the method utilises a readily available waste product from the same industry means that the method of manufacturing the material can be integrated into existing fashion supply chains, with minimal disruption, at the same time as alleviating the environmental problems discussed above.

[0012] The enriched portion is preferably a sludge. Preferably the liquid portion which is removed in step ii) comprises about 70%, 80%, 90%, 95%, 98% or more of the mixture formed in step ii), by mass. This provides an enriched portion which comprises a high proportion of dye and chitosan flocs. This provides an enriched portion (preferably a sludge) which has fast drying times to form the material. Preferably the liquid portion is separated from the enriched portion by filtration. This can be accomplished using a Buchner funnel, optionally using a reduced pressure to draw liquid out of the enriched portion.

[0013] The material can mimic a synthetic plastic, with similar performance qualities and properties such as being rigid and translucent. Preferably the liquid used is a waste liquid, and preferably wastewater from a dyeing process.

[0014] Preferably, the chitosan is derived from a fungal source. This means that when the chitosan is added to the liquid provided in step i), fewer bubbles are generated. This improves the appearance of the material formed. It also avoids or reduces a yellow / orange tint which may be formed with crustacean-derived chitosan. It also provides materials and enriched portions (which are preferably sludges) which dry in a consistently flat manner. It also provides a brighter colour to the material produced. It is also easier to pour the resulting enriched portion (which is preferably a sludge) into a mould. The colour of the material produced is more consistent and the chitosan is more easily dissolved, leading to a material which is lower in imperfections.

[0015] A fungal-derived chitosan is available from Xian Pincredit Bio-tech Co., Ltd.

[0016] Preferably the chitosan is in a powdered form. This increases the speed at which the chitosan dissolves and speeds up the process.

[0017] In some embodiments, the chitosan may be provided as a chitosan solution. This assists in the chitosan being dissolved and easily dispersed throughout the dye wastewater. The method may further include a step of adding chitosan to the enriched portion formed in step iii) of the method. The chitosan in this step may be in a powdered form or added as a chitosan solution. The other additives discussed herein, and the characteristics of the chitosan discussed herein, may also be applied to, or incorporated into, this step. The addition of further chitosan promotes the formation of flocs which efficiently bind to the dye in the liquid. The addition of more chitosan also provides a thicker enriched portion which is easier to work and / or pour and is easier to separate from the remaining liquid and is quicker to dry to form the material. Preferably, the method further comprises a step of adding an alginate to the liquid, the mixture or the enriched portion. This provides a high gloss finish to the final material which makes it particularly suitable for fashion articles. The addition of alginate also makes the material more flexible.

[0018] Preferably the alginate is added in an amount of 0.25-2 wt%, relative to the amount of liquid provided in step i).

[0019] Preferably the method further comprises a step of adding glycerol to the liquid, the mixture or the enriched portion. This increases the pouring properties of the enriched portion and the ability to work (e.g. cut or bend) the material formed.

[0020] Preferably about 0.25, 0.5, 0.75, 1 or 2 wt% of glycerol is added to the liquid, the mixture or the enriched portion, relative to the amount of liquid provided in step i). The glycerol values provided towards the lower end of this range provide a low viscosity enriched portion or mixture which is easy to spread on a mould.

[0021] The glycerol values towards the higher end of this range provide a more translucent material.

[0022] The glycerol is preferably in an amount of 0.25-2 wt% relative to the amount of liquid provided in step i).

[0023] An acid, and preferably acetic acid, may be added to the liquid, the mixture or the enriched portion. This can help to protonate any NH3groups in the chitosan and promote interaction between those protonated positively charged groups with negatively charged groups on an anionic dye. This helps to dissolve the chitosan and also provides an efficient binding between the chitosan and the dye.

[0024] The liquid provided in step i) may be diluted with non-distilled water. The non-distilled water, may be tap water. Non-distilled water contains sulphate ions, which are thought to associate with the chitosan molecules to effectively increase their molecular weight and lead to increased bridging, intermolecular interactions, and thereby increased flocculation of dye and chitosan. This increased flocculation speeds up the removal of the dye molecules from the liquid and provides a faster, more complete, and more efficient process.

[0025] Step i) may comprise the step of obtaining the liquid containing the dye from a dyeing process. This vertically integrates the dyeing process and the wastewater recycling process with the production of a useful material which may be used in conjunction with articles which are produced in the dyeing process itself. For example, the dyeing process may be a process to dye an item of clothing and the remainder of the method steps described herein may produce a fashion item such as a sequin, glitter or a button, which may be attached to the item of clothing which was the product of the dyeing process. This vertical integration of the dyeing process, the wastewater recycling process and the manufacture of a related fashion item, can lead to significant cost savings. These savings may result from, reduced costs associated with wastewater transport and the transport of clothing components from one factory to another.

[0026] The dye may be a reactive dye, a substantive dye, an acid dye, a basic dye, a plant- derived dye, a disperse dye, a direct dye, a natural dye, a synthetic dye, a bacterial dye, a vegetable dye, an anionic dye or a cationic dye. Anionic dyes are particularly preferred due to their strong ionic interaction with a protonated NH4+group in the chitosan. In some embodiments reactive protonated amine groups in chitosan bind to negatively charged sulfonic groups of the dye (coagulation) and bind the chitosan to the dye. This leads to improved flocculation and efficiency of dye removal from the wastewater.

[0027] Room temperature mixing in step ii) is preferred. This provides an effective balance between chitosan denaturing and the desirable high temperature removal of acetyl groups (which produces reactive chitosan by deacetylation).

[0028] The method may further comprise the step of adding starch, another biopolymer, or a mixture thereof to the liquid, the mixture or the enriched portion. This provides a more opaque colour to the material. When starch or another biopolymer is added, the mixture or enriched portion may be heated. This thickens the mixture or the enriched portion and improves the pouring ability of the mixture or the enriched portion.

[0029] Starch may be added to the liquid, the mixture or the enriched portion in an amount of 0.5-2 wt%, relative to the amount of liquid provided in step i). This provides a preferred level of thickening and opacity of the material produced.

[0030] The pH of the chitosan solution may be 6.5 or less, and is preferably between 3 and 4. This provides a material which, when formed as a sheet, is less prone to cracking whilst drying. Lower pH is preferred because the absorption of dye is dependent on the pH of the solution. This is because the electrostatic attraction between the anionic dye and the chitosan is stronger because chitosan will have a higher degree of deacetylation. This means that the dyes with lower pH will have a more successful uptake of the chitosan and binding ability to form a material than those which are alkaline or higher in pH. This is because chitosan has a pKa of around 6.5, meaning that a pH below 6.5 is preferred for the protonation of chitosan and for the creation of a good number available sites for chitosan to bind to the dye. As the pH increases, protonation of the chitosan molecule decreases so there are fewer binding sites for the dye and therefore a reduction in the reaction efficiency.

[0031] The pH of the liquid provided in step i) may be 7 or greater. This provides efficient coagulation.

[0032] The liquid provided in step i) preferably comprises a blue dye. This provides an efficient coagulation between the chitosan and the dye molecules. It also seems to result in fewer air bubbles being formed and an enriched portion which dries thick enough to form useful fashion articles.

[0033] The pH of the liquid containing the dye may be 6.5 or less, and is preferably between 3 and 4. This provides a material which, when in the sheet form, is less prone to cracking whilst drying. Lower pH is preferred because the absorption of dye is dependent on the pH of the solution. This is because the electrostatic attraction between the anionic dye and the chitosan is stronger because chitosan will have a higher degree of deacetylation. This means that the dyes with lower pH will have a more successful uptake of the chitosan and binding ability to form a material than those which are alkaline or higher in pH. This is because chitosan has a pKa of around 6.5, meaning that a pH below 6.5 is preferred for the protonation of chitosan and for the creation of a good number available sites for chitosan to bind to the dye. As the pH increases, protonation of the chitosan molecule decreases so there are fewer binding sites for the dye and therefore a reduction in the reaction efficiency.

[0034] Agitation may be provided in step ii). In step ii) agitation may be provided to the mixture at a first level for a first time period, and at a second level for a following second time period, wherein the first level of agitation is higher than the second level of agitation. Preferably a high agitation is provided for 3 minutes followed by a period of lower agitation for at least 15 minutes. Preferably a period of high agitation is provided by a stirrer at a speed of between around 1000 and 2000 rpm. Preferably the agitation at a lower level of agitation is between 50-200 rpm, and preferably around 100 rpm. The agitation may be provided by a stirrer, such as a magnetic stirrer. The two agitation periods of differing agitation strength ensure proper agitation of the mixture components whilst promoting gradual separation and settling of any flocculated material.

[0035] The enriched portion may be located in a mould before step iv) takes place. The mould may be formed from the container in which the liquid reaction is carried out. For example, liquid could just be removed from a breaker with a shaped bottom and the enriched portion could be left to dry in the container in which it was mixed.

[0036] The enriched portion may be transferred from a vessel in which step ii) occurs, to a mould. The mould may be a tray with raised edges. This is useful for forming the material into a desired shape during the drying process.

[0037] Step iv) may be carried out on a mould or a separate surface. The mould or the surface upon which the enriched portion is dried may be made of plastic or glass or metal or a combination thereof.

[0038] The enriched portion may be transferred to a mould. The surface of the mould or the surface upon which the enriched portion is dried may be coated with a solvent. The solvent may be brushed onto the mould or the surface so that an even and / or complete covering is obtained before the enriched portion is transferred to the mould or surface. This enables easy removal of the material once dried, and easy spreading of the enriched portion around the mould or surface upon which it is dried.

[0039] The solvent may be an organic solvent, such as an alcohol, such as ethanol.

[0040] The mould or a surface upon which the enriched portion is dried may be textured to provide a texture to the material. This can be used to provide desired reflective properties in fashion articles such as sequins or glitter. The mould or surface may be etched to create the texture. The mould or the surface may be laser etched.

[0041] A mould or surface upon which the enriched portion is dried may be heated. The mould or surface may be in contact with a heat source. The heat source may be adapted to hold the mould or surface at a temperature of between 25 degrees Celsius and 50 degrees Celsius. Preferably the mould or surface in these embodiments comprises a metal, and is preferably a metal tray. This provides an effective way of transferring heat to the enriched portion to speed up its drying time. Alternatively, or additionally, the mould or surface may be located in a heated environment.

[0042] The method may further comprise the step of stamping, embossing or cutting the material.

[0043] The material may be a fashion or decorative article such as an embellishment, an ornament, a trim, a sequin, a decoration, a textile article, a clothing article, a button, glitter, a sheet or a film. The material may also be, or form part of, a household article such as a curtain, a table cloth, a blind or an upholstery article.

[0044] Step iv) may be conducted at a temperature of between 25-50 degrees Celsius. In step iv) the enriched portion may be dried to constant weight. The degree of deacetylation of the chitosan may be above 50% and is preferably above 85%.

[0045] The method may further include a step of fully or partially coating an article in the enriched portion formed in step iii) before drying the enriched portion. This can be useful for forming articles such as buttons and other fashion articles which are partially coated or fully coated with the material. The article may be (fully or partially) dipped into the enriched portion when the enriched portion is located in a mould, before the drying of the enriched portion takes place. This allows the outer shape of the coating to be controlled, whilst still providing a fully or partially coated article, if necessary.

[0046] In a further aspect of the invention, there is provided a method of preparing an item comprising the steps of providing a first material formed as described herein and joining it to a second piece of material formed as described herein by heating the two pieces of material and pressing them together. Preferably the item is a 3-dimensional article such as a sequin or another fashion item.

[0047] The heat may be provided by a heat gun. The two pieces of material may be held together by a tool such as pliers or in a jig.

[0048] In some embodiments of articles according to the invention a material according to the invention may be combined with a fabric.

[0049] Preferred pH ranges

[0050] The reaction between dye and chitosan is dependent on the pH of the solution. Dye removal is generally higher when the solution is more acidic and pH is lower, because the electrostatic attraction between an anionic dye and the chitosan is stronger as a result of a higher degree of deacetylation of the chitosan. This means lower pH levels require less chitosan to remove the dye from the liquid and are therefore more effective. The pKa of chitosan is dependent on the degree of deacetylation and the neutralisation of amine groups. The pKa is around 6.5 and therefore a pH below 6.5 will result in the protonation of the majority of chitosan amine groups which is preferred for the attraction of chitosan to an anionic dye. If the pH increases, protonation of chitosan decreases along with the density of available binding sites for the anionic dye. Therefore it’s effectiveness at removing the dye from solution decreases. This means that the preferred range of pH for the liquid in step i) prior to addition of an anionic dyes is between 3-4.

[0051] The source of chitosan’s effect on function (crustacean or fungi derived)

[0052] The degree of acetylation, molecular weight and distribution of charged groups in chitosan from fungal sources are different from that of crustacean- derived chitosan. Fungal sources have enhanced bioactivity which enhances their functional properties.

[0053] Fungal chitin is also found to have a lower inorganic matter content when compared to crustacean shell wastes, meaning that demineralisation is not required before processing, making the extraction process simpler and cost of the process lower. The process of purification to remove inorganic matter also tends to depolymerise chitosan in a random manner, meaning that the physiochemical properties of the chitosan originating from crustaceans is less consistent than fungal-derived chitosan. This means that crustacean derived chitosan has a reduced consistency of function in methods according to the invention. Fungal derived chitosan is therefore preferred.

[0054] Effect of pH, temperature range and other parameters

[0055] Chitosan removes some dyes from wastewater as a result of its positive charge in acidic mediums and presence of reactive protonated amine groups that neutralise negatively charged sulfonic groups of certain dyes (coagulation). The neutralisation of these charges, along with the formation of inter- and intra-chain bridging enhanced by a high chitosan molecular weight, destabilises and causes flocs to form and aggregate (flocculation) leaving a sludge that has collected the dye. For some dyes, the pH is therefore a component of why the process works, because the net charge of certain dyes is affected by pH and the behaviour of the chitosan in solution is affected by pH which affects the coagulation-flocculation.

[0056] Varying the temperature during the chitosan deacetylation process changes the molecular weight and degree of deacetylation of chitosan, and therefore its function. An increase in temperature increases the removal of acetyl groups from chitosan and causes a higher degree of deacetylation which results in a more reactive chitosan / strength of attraction and coagulation. The reaction is exothermic with significant dependence on pH. However, an increase in temperature may also reduce the absorption capacity as it may destabilise the structure of chitosan. Room temperature has been found to be the most appropriate condition for methods according to the invention, and in particular the steps i) and ii).

[0057] Chitosan parameters affecting the uptake of dye

[0058] Several factors affect the uptake of dye, including the degree of deacetylation molecular weight, moisture content, contact time, associated liquid media and pH.

[0059] The degree of deacetylation (DD) affects physical, biological and chemical properties of chitosan which in turn affect its ability to remove dye from solution. When chitosan has a higher degree of deacetylation (increased removal of acetyl groups), more amino groups, which are very reactive, are available on the structure. With a degree of deacetylation above 50%, chitosan becomes soluble in water and anything lower results in insoluble chitosan. Chitosan with a DD above 85% is said to be of high DD, which increases the removal of dye as it increases its positive charge and therefore the strength of attraction for anionic dye and therefore its function as a coagulant.

[0060] The molecular weight of chitosan has also been suggested to affect the uptake of dye in wastewater. The higher the molecular weight, the increased flocculation and sludge production speed. Chitosan has been found to perform more efficiently in tap water, as less chitosan was needed for the coagulation and flocculation of an AB92 dye, than in demineralised water as the addition of sulfate increased the molecular weight of the chitosan and therefore its increased bridging and flocculation.

[0061] The contact time with chitosan also affects the uptake of dye, with absorption capacity increasing constantly with increasing contact time until a maximum point is reached. This is due to the limited availability of biosorption sites on chitosan surface. The optimal contact time may be around 48 hours, and is preferably between 12 hours and 48 hours. Type of water in which the dye is provided

[0062] The presence of salt in tap water, and other non-distilled water, (and therefore a higher iconic strength) increases the efficiency of the process by requiring lower amounts of chitosan to bind with a given amount of dye, when compared to demineralised water. This is thought to be a result of the increased molecular weight of the chitosan due to the presence of sulfate ions and / or other salt components in non-distilled water, which help to form larger aggregates which enhance flocculation.

[0063] Investigations removing kaolinite and bentonite with chitosan in tap water and distilled water have also shown similar patterns, suggesting that it is those components in tap water which increase the effectiveness of the coagulationflocculation process.

[0064] Dye types: plant based dyes

[0065] Studies have demonstrated the removal of several type of dyes; azo dyes (such as Brilliant blue FCF, Congo red) direct, mordant, reactive and disperse dyes from wastewater using chitosan.

[0066] Research has been conducted on natural dyes and chitosan. For example, Spirulina Blue is derived from phycocyanin made from stacks of chromophorylated proteins. These are highly water soluble and covalently attached to chromophores. This makes Spirulina pH 6.93 and (as with most microalgal cells) it has a negative charge on its surface. Therefore, the addition of the chitosan (a cationic polyelectrolyte) will neutralise its charge and destabilise it as part of a coagulation reaction and then form flocs and flocculate. The addition of salts, such as NaCI, increases the flotation of algal cultures, again suggesting that salt water is more effective than distilled water and has shown that Spirulina grown in sea water vs fresh water affects its iodine content and therefore its ionic properties.

[0067] Turmeric, a substantive dye, is also appropriate for the coagulation-flocculation using chitosan. This is because the structure of turmeric is rich in phenolic compounds and belongs to the diaroylmethane group. It has a bioactive component from the rhizome of Curcuma. L linn ((1 ,7-bis(4-hydroxyl-3-methoxyphenyl)1 ,6-heptadiene-3, 5-Dione). Curcumin degrades by acidic, alkaline hydrolysis, oxidation and photodecomposition, however it is relatively stable at pH <6.5. Curcumin is attracted to the N-acyl components of the chitosan at pH <6.5 as it is protonated and has a strong attraction to anionic groups on the Curcumin molecule. This therefore suggests that chitosan will be successful at removing turmeric dyes from wastewater via coagulationflocculation. At physiological pH, chitosan’s degree of deacetylation is reduced and therefore it’s electrostatic attraction to Curcumin, causing the chitosan to swell and release Curcumin. This suggests that recycling of chitosan from dye sludge could be achieved using an alkaline based wash.

[0068] Polygalacturonic acid from orange peels has also been shown to form polyelectrolyte complexes with chitosan due to the interaction of complimentary electrostatic charged components. Orange peel, other food waste dyes that contain carotenoids, and also chlorophyll-containing dyes are also expected to be removeable from water using chitosan. This is because carotenoids and chlorophyll have high electrostatic attraction between their active groups (carbonyl group of chlorophyll) and chitosan’s positive amino groups, forming a sludge with chitosan.

[0069] Preferred materials and articles according to the invention comprise the additives mentioned above (such as alginate, starch and / or glycol). In preferred embodiments, all of the additive which is added during the process steps is incorporated into the material. However, in other embodiments, it is the presence of the additive in the material which is important, rather than the amount of additive or its ration with respect to the other components. The skilled person could, given the disclosures herein provide materials and articles comprising appropriate amounts of the additives herein to achieve the technical effects associated with those additives.

[0070] Embodiments of the invention will now be described with reference to the figures of the drawings, in which;

[0071] Figure 1 shows the flocculation process used in example 1 at various time intervals throughout the process.

[0072] Figure 2 shows an embossed mould tray for drying a sludge in accordance with a step of a method according to any embodiments of the invention described herein.

[0073] Figure 3 shows a textured material formed by a method according to the invention.

[0074] Figure 4 shows a clothing article having sequins and embellishments formed from a material according to the present invention.

[0075] Figures 5 to 7 show microscope slides of the mixtures disclosed in example 2 below.

[0076] Figure 8 shows the results of example 5 below. That is, Petri dishes comprising the dried solutions containing 0, 0.25, 0.5, 0.75, 1 and 2% of glycerol. The dish at the top of the page contains 0 wt% glycerol as per its label and the sequence of dishes shows 0.25, 0.5, 0.75, 1 and 2 wt%.

[0077] Example 1

[0078] A method for creating a material according to the invention is as follows:

[0079] A 300 ml volume of dye-containing wastewater was provided in a beaker. The dye was Acid Violet 19.

[0080] A separate chitosan solution was prepared. The chitosan solution contained 6 ml chitosan and was a 1 % acetic acid chitosan solution. The pH of the chitosan solution was adjusted to 4.8.

[0081] Separate embodiments of the process were demonstrated in which the dye was either a reactive dye, an acid dye or a plant derived dye. However, mixtures of these dyes could also be used.

[0082] A 4.6 ml volume of the chitosan solution was added to the dye-containing wastewater.

[0083] The mixture was agitated using a magnetic stirrer at a high rate (2000 rpm) for 3 minutes, followed by agitation at a slower rate (100 rpm) for 15 minutes. The mixing causes the dye to bind to the chitosan to form flocs which clump together and settle at the bottom of the beaker in the form of a sludge layer.

[0084] The mixture was allowed to settle. The beaker was left for 4 hours. Photographs of the beaker are shown in figure 1 at various points throughout the process (1 minute, 10 minutes, 1 hour and 4 hours). The colour of the liquid in the beaker becomes weaker over time, which indicates that over time, the dye binds to the chitosan and is taken out of the liquid phase. The reaction reached a stable state after around 4 hours. The sludge formed by the flocculation of the chitosan and the dye was separated from the liquid in the beaker by filtration.

[0085] The sludge was then weighed. A further 2 wt% of dried Chitosan was added to the sludge along with 1 wt% acetic acid.

[0086] The resulting mixture was placed into glass or plastic containers and placed either in a drying oven at a low temperature of 30 degrees, or air-dried.

[0087] In some embodiments of the general process, the containers (which may be moulds) may have laser-etched designs on a sludge-contacting surface. These designs allow the sludge to dry and replicate the embossed features. One container, in the form of a tray is shown in figure 2. The resulting material which has been made from a sludge dried in the tray of figure 2 is shown in figure 3. The embossed pattern is shown on its surface.

[0088] When the sludge is fully dried (optionally to constant weight), shapes can be cut out of a material formed in the process. A die-cutting press can be used to cut the shapes from a larger piece of the material, for example a sheet or film. A die-cutting press can be adapted to provide a variety of shapes. Examples of these shapes are shown in figure 4.

[0089] These shapes can be used as fashion articles such as sequins, embellishments, glitter and accessories on clothing, as shown in figure 4. The shapes are attached to a fabric by thread.

[0090] Example 2

[0091] This example prepares mixtures according to a first step of the invention, which contain different dyes. The mixtures were prepared, observed in bulk and then studied under a microscope. Experiments were run using the following dyes, which had the following pHs values:

[0092] Purple 1 (P1) pH 2.47

[0093] Blue 1 (B1 ) pH 7.97

[0094] Brown 1 (BR1 ) pH 8.01

[0095] Purple 2 (P2) pH 8.46

[0096] Each of these dye mixtures comprised mixtures of acid dye (sold by Jacquard Products® - h;i0$: / ;w .-acquardrxodMCts.co ) and Dye More Synthetics Powder Liquid which is sold under the mark Rit® (https: / / www.ritdye.com / ) by the company Nakoma Products LLC.

[0097] Materials

[0098] 4.6 g of chitosan solution (from a batch of chitosan solution containing 2g dried chitosan, 296g water and 2g acetic acid)

[0099] 300mL dye water (dyes specified above).

[0100] Procedure for making mixtures

[0101] - Measure out 300mL of dye water and record the pH.

[0102] - Weigh 4.6g of chitosan solution, add to the dye water and mix.

[0103] Mix the mixture with a metal rod.

[0104] - Agitate the mixture with a magnetic spinner on a high speed (2000 rpm) for 3 minutes. - Then, for 15 mins agitate with the magnetic stirrer on a low speed of 100 rpm. Leave the mixture to settle for at least 48 hours.

[0105] Microscope slide Preparation Procedure

[0106] Remove 50mL of liquid from the surface / upper layer of the dye mixtures. Then rest the mixture for another 48 hours.

[0107] Pipette 1 -2g of solution onto the microscope slide and then cover.

[0108] View the slide under a microscope.

[0109] Results

[0110] - Microscope images were captured.

[0111] Figure 5 shows the microscope image for P1. It was expected that this dye would form flocs quicker and more effectively as acidic mediums tend to make the chitosan biopolymer more reactive due to its degree of deacetylation.

[0112] The flocs, which are visible as darker flecks, are very small and spread out. This shows that the coagulation / flocculation is taking place but at a sub-optimal / inefficient rate.

[0113] Figure 6 shows the corresponding image of experiment which uses B1 . The B1 dye seemed to coagulate the most efficiently of all the dye mixtures in this example 2 and the flocs seemed to be larger and settle quickly after the 15 minute period of magnetic spinning.

[0114] Figure 6 shows a high amount of flocs present within the top layer of mixture after 48 hours in comparison to the other dyes. This supports the initial visual observations and suggests that this dye type may react more efficiently than the others as a result of its chemical components, rather than just providing a reaction which is easier to see than the other dyes.

[0115] Figure 7 shows the corresponding image of an experiment which uses BR1 . The pH of BR1 was 8.01 , slightly alkaline. The pigment was very dark and it was hard to see floc formation during the reaction. Image 7 shows fewer flocs than the other dyes, however the flocs formed are much larger. This suggests that this dye may be more chemically reactive than the others, perhaps due to a stronger ionic attraction between the chitosan and the NH4+ions in the anionic dye.

[0116] In the experiment with the dye P2, the dye had an alkaline pH, which is a contrast to the P1 dye, which was highly acidic. The pigment of P2 was very dense and it was hard to observe the flocculation reaction taking place.

[0117] Example 3

[0118] In this set of experiments the same mixtures of dyes used in example 2 were diluted with tap water (in a 50 / 50 ratio by volume). Those mixtures were;

[0119] Purple 1 (P1) pH 2.47

[0120] Blue 1 (B1 ) pH 7.97 Brown 1 (BR1 ) pH 8.01 Purple 2 (P2) pH 8.46

[0121] The speed of the reaction with chitosan, the efficiency of the separation of the dye, and the effectiveness of the floc formation were observed. Materials

[0122] 2.3g of chitosan solution (taken from a bulk solution made up on 2 g chitosan, 296 g water and 2 g acetic acid).

[0123] 150mL dye water

[0124] 150mL tap water (pH 7.35)

[0125] Procedure

[0126] - Measure out 150mL of dye water.

[0127] - Add 150mL of tap water to the dye water to dilute it.

[0128] - Weigh 2.3g of chitosan solution and add to the dye.

[0129] - Measure 1 % chitosan solution and add to the mixture.

[0130] Mix with metal rod.

[0131] - Agitate with magnetic spinner on high speed (2000 rpm) for 3 minutes.

[0132] - Then, for 15 mins agitate on low speed of 100 rpm.

[0133] Leave to settle for at least 48 hours.

[0134] Observations

[0135] Each dye appeared to form flocs quicker and settle quicker than with the non-diluted mixtures used in example 2.

[0136] This may be due to the tap water making the molecular weight of the chitosan higher and therefore increasing the efficiency of the reaction.

[0137] It appears that the dilution provided a higher chitosan molecular weight, and increased flocculation and sludge production speed. This was demonstrated by finding that chitosan performed more efficiently in tap water, as less chitosan was needed for the coagulation and flocculation, than in non-diluted experiments. This is thought to be because the addition of sulfate ions increases the molecular weight of the chitosan and therefore increases its bridging and flocculation. This also shows the influence of associated liquid media on the uptake of dye, as the possibility of hydrogen bridge formation is dependent on competitive formation of associations with other substrates. Inter-intramolecular H-bridges which will affect uptake of dye.

[0138] In some embodiments, diluting the dye mixture is beneficial. It speeds up the reaction that takes place between the dye and the chitosan and also achieves an easier separation of water and dye sludge after 48 hours of settling.

[0139] This allows for more water to be cleaned and therefore recycled.

[0140] Example 4

[0141] This experiment was to observe any differences between dyes when forming the bioplastic. It was also intended to investigate which properties can be modified to adapt the properties of bio sequins consistently to produce desirable characteristics, despite variations in the dyes used.

[0142] Materials

[0143] - 200mL portions of sludge created in the experiments in example 2.

[0144] - 6 wt% (based on the amount of dye water) acetic acid

[0145] - 6 g dry chitosan

[0146] 1 wt% (based on the amount of dye water) glycerol

[0147] - Ethanol (70% aqueous solution) Procedure

[0148] In the materials section above, the 200mL portions of sludge used were the ones formed in the experiments of example 2 described above. There were four 200mL portions of sludge; one for each dye used in example 2.

[0149] - Using the sludge portions from example 2, check and measure that there is 200mL present in each case.

[0150] - Weigh 6g of dry chitosan and add to each of the 4 portions of sludge.

[0151] - Stir each mixture slowly with a metal rod, to avoid making too many bubbles.

[0152] - Pipette 6 wt% acetic acid and 1 wt% glycerol into the mix.

[0153] Stir slowly until the mixture becomes viscous and thick.

[0154] - A plastic tray was prepared by spraying it with ethanol (70%). The ethanol was then spread onto the tray to form an evenly distributed and complete covering. The ethanol was spread with a brush.

[0155] The viscous mixture was poured onto the trays and left to settle for 48 hours at room temperature. The trays were left to air dry for 72 hours.

[0156] In the R1 , P1 and BR1 mixtures, there were flocs visible in the trays once the mixtures had been poured. It is thought that increasing the amount of acid (acetic or otherwise) above 6 wt% would reduce the appearance of flocs in the sludge and form an improved pigmentation. The BR1 mixture, diluted as per example 3 was also poured. The pigment was less dense than in the undiluted BR1 experiment. The undiluted BR1 experiment therefore provided a bioplastic which is more suitable for bio sequins (i.e. a denser pigment). The diluted BR1 mixture also suffered from similar visible flocs in the tray. It is thought that increasing the amount of acid would reduce the appearance of flocs in the sludge and form an improved pigmentation. The BR1 mixture, diluted as per example 3 was also poured.

[0157] It was found that an acetic acid (or presumably any other acid) percentage of 6 wt% or preferably greater than 6 wt% is preferable to ensure that any chitosan is well dissolved.

[0158] Example 5

[0159] This example shows a process for creating a bio sequin without any dye in order to investigate the process parameters which affect the characteristics of the product. These process parameters may be applied to products which do comprise dye, in order to vary the characteristics of the corresponding dye-containing products. The primary object of this example is to demonstrate the effect of glycerol addition to the mixtures used in methods according to the invention.

[0160] The weight percentage of glycerol was varied. Experiments were run using 0, 0.25, 0.5, 0.75, 1 and 2g of glycerol in 100ml of a chitosan containing solution. The solution was water-based with a pH of around 8.

[0161] Procedure

[0162] 3g of chitosan powder was added to 100ml of tap water. The mixture was stirred until the chitosan dissolved. 3g of acetic acid was added to the mixture. The above was repeated to provide 6 different water and chitosan mixtures. Either 0, 0.25, 0.5, 0.75, 1 or 2g of glycerol were added to each mixture. This produced 6 test mixtures with varying proportions of glycerol. Each mixture was stirred until it became viscous. 50g of each mixture was poured into its own separate petri dish. The remaining mixture was poured into a mould tray. This mould tray had been sprayed and brushed with ethanol as described above. Each mixture was left to air dry.

[0163] Immediate observations of the liquid mixtures:

[0164] As glycerol percentage increased, the mixtures became easier to pour, work with and spread. On pouring the 0% glycerol mixture into a mould tray, the mixture separated very easily and moved away from centre of the tray. The mixtures with a higher glycerol percentage appear more translucent.

[0165] The mixtures in the petri dishes were allowed to air dry at room temperature for 48 hours. Pieces of material were cut from each of the sheets of biomaterial in each petri dish once the material had dried. To investigate the properties of the biomaterial formed from each mixture, a square piece of material was cut from the sheet using scissors and a sequin was formed using a sequin press.

[0166] The results are shown in figure 8. The amounts of glycerol are shown on the petri dishes shown in figure 8. The dishes are arranged with the lowest concentration (0g) of glycerol at the top of figure 8, through to the highest proportion of glycerol (2g) at the bottom of the figure. The results were as follows:

[0167] 0% glycerol: too rigid, hard to cut without cracking. A crinkled texture and irregular.

[0168] 0.25% glycerol: easier than 0% to cut, but still too rigid and irregular.

[0169] 0.5% glycerol: easier to cut, relatively flexible but still strong, dried flatter than the 0% and 0.25% mixtures but still quite crinkled.

[0170] 0.75% glycerol: thinner and easier to cut than the previous materials, highly flexible, Moro consistent colour and thickness.

[0171] 1% glycerol: evenly distributed, very flexible, perhaps too thin for sequins as it was retained / caught in the sequin press. Very strong.

[0172] 2% glycerol: very evenly distributed, very flexible but very thin, behaves like a very thin film but has very good strength.

[0173] Example 6

[0174] Various additives were incorporated into test mixtures to assess their impact on the properties of the materials produced. The mould trays were also varied to see whether they had an effect on the process.

[0175] Alginate

[0176] The effect of alginate on the bioplastic’s physical and mechanical properties was investigated by adding sodium alginate to the biomaterial (bio sequin) mixture (without dye) at concentrations of 0, 0.25, 0.5, 0.75, 1 and 2 wt%.

[0177] Procedure:

[0178] Six test mixtures were prepared. For each test mixture, 50mL water was mixed with 1.5g chitosan powder (crustacean-derived chitosan powder). The mixture was stirred until the chitosan dissolved. 1 .5g acetic and 0.5g glycerol were added to the mixture. To each mixture 0, 0.13, 0.25, 0.42, 0.5 or 1g of sodium alginate was added and mixed until the sodium alginate dissolved and the mixture became viscous. Each mixture was poured int a petri dish and left to air dry at room temperature.

[0179] Immediate observations on the mixture: As the alginate concentration increases, more bubbles / foam formed when pouring the mixture onto the Petri dish and accumulated as a top layer. When dried, alginate containing mixtures formed a higher gloss finish.

[0180] When dried, the alginate chitosan compositions are more flexible when compared to the mixture which contained chitosan alone.

[0181] Type of Chitosan

[0182] The aim of this experiment was to compare the properties of the materials produced using a fungi-derived chitosan with those produced using a crustacean-derived chitosan. The crustacean-derived chitosan was obtained from BIORIGINS®. The fungal-derived chitosan was obtained from Xian Pincredit Bio-tech Co., Ltd.

[0183] Procedure:

[0184] 1 .5g dry chitosan powder (either crustacean or fungi) was added to 50mL tap water. The mixture was mixed until the chitosan dissolved. 1 .5 g Acetic acid and 0.5 g glycerol were added to the mixture. Each of the two mixtures was poured into separate petri dishes. They were left to air dry at room temperature.

[0185] Immediate Observations:

[0186] The fungal chitosan appears to be finer and lighter. It appears to dissolve better in water and the mixture produced appears to have fewer bubbles and has no yellow / orange tint like crustacean-derived chitosan mixture.

[0187] When dried, the material formed using the fungi-derived chitosan is more consistently flat and even in appearance and no bubbles or imperfections appear in the material. Fungi-derived chitosan therefore appears to be preferable for making fashion articles such as sequins or other fashion materials.

[0188] Mould tray conditions

[0189] The same mixtures were poured into various mould trays to determine whether the mould tray had an impact on the properties of the biomaterial formed. Glass, plastic, metal (steel), silicon and all of these options sprayed with ethanol.

[0190] 1 .5g dry of chitosan powder were added to 50mL tap water and mixed until dissolved. Acetic acid and glycerol were added to the mixture. The mixture was poured into either a glass petri dish, a plastic petri dish or a petri dish sprayed with ethanol. The trays were left to air dry at room temperature. All of these tray materials produced acceptable biomaterials.

[0191] In some embodiments, heated moulds, for example trays, may be used to encourage drying of the enriched portions. Preferably in these embodiments a metal mould is used for its heat conduction properties. Preferably the mould is put in contact with a heat source. However, the tray may be left in a heated environment. Fungi-derived chitosan and dye mixtures

[0192] This example was aimed at investigating the outcome of using fungi-derived chitosan with the dye mixtures used in example 4. The effect of drying the mixtures in smaller petri dishes was also investigated to see whether material dries flat, shrinks or deforms and how colour is distributed.

[0193] Materials

[0194] - 50g dye water

[0195] - 1.5g of chitosan powder (fungi-derived)

[0196] - 1 .5g acetic acid

[0197] - 0.5g of glycerol

[0198] Procedure

[0199] - Measure 50mL dye water from the flocculated dye water from experiment 4

[0200] - Weigh 1 ,5g dry chitosan powder.

[0201] - Add powder to water and mix until dissolved.

[0202] - Add the acetic acid and glycerol to the mixture.

[0203] - Pour into a plastic Petri dish.

[0204] - Leave to air dry at room temperature.

[0205] Initial observations:

[0206] - The colour seems to be brighter than crustacean chitosan and more chitosan seems to be dissolved than in previous experiments. The mixture was easier to pour and had fewer bubbles.

[0207] -When dried the colour is more consistent and the material is flatter.

[0208] Starch

[0209] These experiments were aimed at investigating the effect of adding starch to mixtures at 0.5, 1 and 2 wt%, on the physical and mechanical properties of the biomaterials formed.

[0210] Procedure

[0211] Add 1 wt% chitosan solution to 200mL of dye water. Add 6 wt% acetic acid and 6 wt% chitosan to the mixture. Add 1 wt% glycerol to the mixture. The mixture was heated until it became thick.

[0212] Initial Observations;

[0213] - Mixture is thicker when heated to between 60-90 degrees Celsius as the starch is activated.

[0214] - Mixture appears cloudy.

[0215] - Colour seems to be more opaque during the drying process.

[0216] The addition of starch provides the benefit that the material holds its shape due to the thickness of the enriched portion formed. The enriched portion also has improved pouring properties due to the improvement in viscosity. These benefits (e.g. the viscosity) are also retained when the heated enriched portion cools down. An additional benefit is that the cooled mixture (and dried material formed therefrom) has an improved tensile strength.

[0217] Example 7

[0218] This example provides a method of forming 3-dimensional shapes from sheets of material produced according to the invention. 1 . Shapes are cut from sheets of the dye and chitosan containing material produced by the methods described herein.

[0219] 2. Pliers are used to hold parts of the material together where the join will form.

[0220] 3. The material is held over a heat gun for no longer than 5-8 seconds at a temperature range between 100 °C and 550 °C.

[0221] 4. When removed from the heat source, the section of material which the pliers were holding will have formed a join and melted the piece or pieces together.

[0222] Loops of material can be made by joining opposite ends of a length of material together using this method.

[0223] The pieces of material to be joined may be formed using a sequin punch or by cutting a sheet of material using scissors, a craft knife, or a similar cutting implement.

Claims

Claims1 . A method of manufacturing a material comprising the steps of; i) providing a liquid which comprises a dye, ii) mixing chitosan with the liquid, iii) separating a liquid portion from the mixture formed in step ii), to form an enriched portion which has a higher proportion of chitosan and the dye than the mixture formed in step ii), and iv) drying the enriched portion to form the material.

2. A method according to claim 1 wherein the chitosan is derived from a fungal source.

3. A method according to either preceding claim wherein the chitosan is in a powdered form.

4. A method according to either of claims 1 or 2 wherein the chitosan is provided as a chitosan solution.

5. A method according to any preceding claim further comprising a step of adding an alginate to the liquid, the mixture or the enriched portion.

6. A method according to claim 5 wherein the alginate is added in an amount of 0.25- 2 wt%, relative to the amount of liquid provided in step i).

7. A method according to any preceding claim further comprising a step of adding glycerol to the liquid, the mixture or the enriched portion.

8. A method according to claim 7 wherein the glycerol is in an amount of 0.25-2 wt% relative to the amount of liquid provided in step i).

9. A method according to any preceding claim wherein an acid, preferably acetic acid, is added to the liquid, the mixture or the enriched portion.

10. A method according to any preceding claim wherein the liquid provided in claim i) is diluted with non-distilled water.11 . A method according to any preceding claim wherein step i) comprises the step of obtaining the liquid containing the dye from a dyeing process.

12. A method according to any preceding claim wherein the dye is a reactive dye, a substantive dye, an acid dye, a basic dye, a plant-derived dye, a direct dye, a natural dye, a synthetic dye, a bacterial dye, a vegetable dye, an anionic dye or a cationic dye.

13. A method according to any preceding claim further comprising the step of adding starch, another biopolymer, or a mixture thereof to the liquid, the mixture or the enriched portion.

14. A method according to claim 13 wherein starch is added to the liquid, the mixture or the enriched portion and the starch is added in an amount of 0.5-2 wt%, relative to the amount of liquid provided in step i).

15. A method according to claim 4 wherein the pH of the chitosan solution is 6.5 or less, and is preferably between 3 and 4.

16. A method according to any preceding claim wherein the pH of the liquid provided in step i) is 7 or greater.

17. A method according to any preceding claim wherein the liquid provided in step i) comprises a blue dye.

18. A method according to any preceding claim wherein the pH of the liquid containing the dye is 6.5 or less, and is preferably between 3 and 4.

19. A method according to any preceding claim wherein in step ii) agitation is provided to the mixture at a first level for a first time period, and at a second level for a following second time period, wherein the first level of agitation is higher than the second level of agitation.

20. A method according to any preceding claim wherein the enriched portion is located in a mould before step iv) takes place.21 . A method according to claim 20 wherein the enriched portion is transferred to a mould, the surface of which is coated with a solvent.

22. A method according to claim 21 wherein the solvent is ethanol.

23. A method according to any preceding claim wherein a mould or a surface upon which the enriched portion is dried is textured to provide a texture to the material.

24. A method according to claim 23 in which the mould or surface is etched to create the texture.

25. A method according to any preceding claim further comprising the step of stamping, embossing or cutting the material.

26. A method according to any preceding claim wherein the material is a fashion or decorative article such as an embellishment, an ornament, a trim, a sequin, a decoration, a textile article, a clothing article, a button, glitter, a sheet or a film.

27. A method according to any preceding claim wherein step iv) is conducted at a temperature of between 25-50 degrees Celsius.

28. A method according to any preceding claim wherein the degree of deacetylisation of the chitosan is above 50% and is preferably above 85%.

29. A material obtainable by the method of any preceding claim.

30. An article comprising a material obtainable by the method of any of claims 1 -28.31 . A method of preparing an item comprising the steps of providing a first material formed according to claim 29 and joining it to a second piece of material formed according to claim 29 by heating the two pieces of material and pressing them together.

Citation Information

Patent Citations

  • Method for preparing heavy metal ion adsorbent by using floc produced by flocculation

    CN115121229A

  • Use of biopolymer chitosan for the removal of colour from wastewater using a combined coagulation-flocculation and adsorption process

    ES2350074A1