Rubber product and method for producing same

By using a filler to absorb and control ionic liquid concentration in fluororubber compositions, the method addresses crosslinking inhibition and stability issues, achieving effective antistatic performance and consistent properties in rubber products.

WO2024236871A1PCT designated stage expired Publication Date: 2024-11-21MITSUBISHI CABLE INDUSTRIES LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/004753
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-02-13
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The incorporation of ionic liquids in crosslinked rubber compositions, particularly with fluororubber, often inhibits crosslinking, and results in uneven distribution and potential bleed-out of ionic liquids, affecting the stability of antistatic performance in rubber products.

Method used

A method involving a filler that absorbs a higher concentration of ionic liquid than the fluororubber, allowing for localized ionic liquid distribution, which suppresses crosslinking inhibition and ensures stable antistatic performance by controlling the ionic liquid concentration within the rubber product, utilizing a filler like PVDF powder and specific ionic liquid compositions, and employing a peroxide crosslinking system.

Benefits of technology

This approach enables stable antistatic performance with suppressed crosslinking inhibition and reduced ionic liquid bleed-out, ensuring consistent properties across the rubber product, as demonstrated by increased maximum torque values and localized ionic liquid distribution analysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

This rubber product is formed of a crosslinked rubber composition containing a fluororubber, an ionic liquid, and a filler dispersed in the fluororubber and capable of absorbing the ionic liquid. The concentration of the ionic liquid in the filler is higher than the concentration of the ionic liquid in the fluororubber.
Need to check novelty before this filing date? Find Prior Art

Description

Rubber products and their manufacturing methods

[0001] The present invention relates to a rubber product and a method for producing the same.

[0002] A technique for controlling electrical properties by incorporating an ionic liquid into a cross-linked rubber composition that forms a rubber product is known. For example, Patent Document 1 discloses a sealing material formed from a cross-linked rubber composition in which an ionic liquid is blended with fluororubber.

[0003] Japanese Patent Application Laid-Open No. 2022-1642

[0004] The present invention provides a rubber product formed from a crosslinked rubber composition containing a fluororubber, an ionic liquid, and a filler that is dispersed in the fluororubber and can absorb the ionic liquid, wherein the concentration of the ionic liquid in the filler is higher than the concentration of the ionic liquid in the fluororubber.

[0005] The present invention is a method for producing a rubber product, which comprises allowing a filler to absorb an ionic liquid, kneading the filler that has absorbed the ionic liquid with a fluororubber to prepare an uncrosslinked rubber composition, and crosslinking the uncrosslinked rubber composition.

[0006] The embodiments will be described in detail below.

[0007] The rubber product according to the embodiment is formed from a crosslinked rubber composition X containing a fluororubber, an ionic liquid, and a filler. The fluororubber is the main component of the base rubber. The filler is dispersed in the fluororubber. The filler is capable of absorbing the ionic liquid. The concentration of the ionic liquid in the filler is higher than the concentration of the ionic liquid in the fluororubber.

[0008] According to the rubber product of the embodiment, firstly, the inclusion of an ionic liquid allows stable antistatic performance to be obtained. In addition, when an ionic liquid is compounded with a fluororubber, there is a problem that crosslinking inhibition by the ionic liquid occurs when an uncrosslinked rubber composition is crosslinked to obtain a crosslinked rubber composition. However, since the concentration of the ionic liquid in the filler dispersed in the fluororubber is higher than the concentration of the ionic liquid in the fluororubber, crosslinking inhibition by the ionic liquid can be suppressed. This is thought to be because the ionic liquid is localized around the filler, thereby reducing the effect of the ionic liquid on the fluororubber, which is the main subject of direct crosslinking. The distribution state of the ionic liquid in the crosslinked rubber composition X can be analyzed by energy dispersive X-ray spectroscopy (EDS).

[0009] According to the rubber product of the embodiment, the filler absorbs the ionic liquid, thereby suppressing the bleeding out of the ionic liquid. However, in order to obtain stable antistatic performance, it is preferable that the concentration of the ionic liquid increases from the inside to the surface in the surface layer of the crosslinked rubber composition X that forms the rubber product. The distribution of the ionic liquid in the depth direction of the surface layer of the crosslinked rubber composition X can be analyzed by time-of-flight secondary ion mass spectrometry (TOF-SIMS).

[0010] Examples of fluororubbers include tetrafluoroethylene (TFE) polymer (PTFE), vinylidene fluoride (VDF) polymer (PVDF), copolymer of vinylidene fluoride (VDF) and hexafluoropropylene (HFP) (binary FKM), copolymer of vinylidene fluoride (VDF), hexafluoropropylene (HFP) and tetrafluoroethylene (TFE) (ternary FKM), copolymer of tetrafluoroethylene (TFE) and propylene (Pr) (FEP), copolymer of vinylidene fluoride (VDF), propylene (Pr) and tetrafluoroethylene (TFE ), a copolymer of ethylene (E) and tetrafluoroethylene (TFE) (ETFE), a copolymer of ethylene (E), tetrafluoroethylene (TFE) and perfluoromethyl vinyl ether (PMVE), a copolymer of vinylidene fluoride (VDF), tetrafluoroethylene (TFE) and perfluoromethyl vinyl ether (PMVE), a copolymer of tetrafluoroethylene (TFE) and perfluoromethyl vinyl ether (PMVE) (FFKM), a copolymer of vinylidene fluoride (VDF) and perfluoromethyl vinyl ether (PMVE), etc. The fluororubber preferably contains one or more of these, and from the viewpoint of obtaining a high suppression effect against crosslinking inhibition by ionic liquids, it is more preferable to contain a ternary FKM.

[0011] In the present application, the term "ionic liquid" refers to a salt composed of a cation component and an anion component, and has a melting point of 100°C or lower.

[0012] Examples of cationic components of ionic liquids include imidazolium-based cations, pyridinium-based cations, aliphatic amine-based cations, and pyrazolium-based cations. Examples of imidazolium-based cations include 1-ethyl-3-methylimidazolium, 1-methyl-3-methylimidazolium, 1-butyl-3-methylimidazolium, 1-hexyl-3-methylimidazolium, 1-octyl-3-methylimidazolium, 1-methyl-2,3-dimethylimidazolium, 1-butyl-2,3-dimethylimidazolium, 1-hexyl-2,3-dimethylimidazolium, and 1-octyl-2,3-dimethylimidazolium. Examples of pyridinium-based cations include 1-octyl-4-methyl-pyridinium, 1-methyl-pyridinium, 1-butyl-pyridinium, and 1-hexyl-pyridinium. Examples of the aliphatic amine cation include tributylmethylammonium.

[0013] Examples of the anion component include bisfluorosulfonylimide anions, fluorinated sulfonic acid anions, fluorinated carboxylic acid anions, thiocyanate anions, dicyanamide anions, and tetracyanoborate anions. Examples of the bisfluorosulfonylimide anions include bisfluorosulfonylimide, bistrifluoromethanesulfonylimide, and bistrifluorobutanesulfonylimide. Examples of the fluorinated sulfonic acid anions include tetrafluoroborate, hexafluoroborate, and trifluoromethanesulfonate. Examples of the fluorinated carboxylic acid anions include trifluoroacetic acid.

[0014] The ionic liquid preferably contains one or more of these cationic components and one or more anionic components. From the viewpoint of obtaining a high suppression effect against crosslinking inhibition by the ionic liquid, the cationic component of the ionic liquid preferably contains an imidazolium-based cation or an aliphatic amine-based cation. From the same viewpoint, the cationic component of the ionic liquid preferably contains 1-butyl-3-methylimidazolium as an imidazolium-based cation, and preferably contains tributylmethylammonium as an aliphatic amine-based cation. From the same viewpoint, the anionic component of the ionic liquid preferably contains a bisfluorosulfonylimide-based anion, and more preferably contains bistrifluoromethanesulfonylimide.

[0015] The content of the ionic liquid in the crosslinked rubber composition X is preferably 0.01 parts by mass or more and 5 parts by mass or less, more preferably 0.1 parts by mass or more and 1 part by mass or less, relative to 100 parts by mass of the fluororubber, from the viewpoint of obtaining a high effect of suppressing the inhibition of crosslinking by the ionic liquid.

[0016] Examples of fillers include resin powders and porous powders capable of absorbing ionic liquids. Examples of resin powders capable of absorbing ionic liquids include fluororesin powders, phenolic resin powders, polyether ether ketone resin (PEEK) powders, and polyimide resin (PI) powders. Examples of fluororesin powders include polyvinylidene fluoride resin (PVDF) powders. Examples of porous powders include carbon black, silica, and zeolite. The filler preferably contains one or more of these. From the viewpoint of obtaining a high suppression effect against crosslinking inhibition by ionic liquids, it is more preferable to contain a resin powder, even more preferable to contain a fluororesin powder, and even more preferable to contain a PVDF powder. Examples of commercially available PVDF powders include the Kynar series manufactured by Arkema.

[0017] The density of the filler is preferably 1 g / cm from the viewpoint of obtaining a high effect of suppressing the inhibition of crosslinking by the ionic liquid. 3 3g / cm or more 3or less, more preferably 1.5 g / cm 3 2g / cm or more 3 The density of this filler is measured in accordance with ISO 1183.

[0018] From the viewpoint of obtaining a high effect of suppressing inhibition of crosslinking by the ionic liquid, the content of the filler in the crosslinked rubber composition X is preferably 1 part by mass or more and 15 parts by mass or less, more preferably 3 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the fluororubber. From the same viewpoint, the ratio of the content of the filler to the content of the ionic liquid in the crosslinked rubber composition X (filler content / ionic liquid content) is preferably 3 or more and 20 or less, more preferably 5 or more and 15 or less.

[0019] Examples of the crosslinking system of the crosslinked rubber composition X include a peroxide crosslinking system, a polyol crosslinking system, and an amine crosslinking system. Of these, the peroxide crosslinking system is preferred as the crosslinking system of the crosslinked rubber composition X from the viewpoint of obtaining a high suppression effect against crosslinking inhibition by the ionic liquid. In the case of a peroxide crosslinking system, a peroxide crosslinking agent is blended into the uncrosslinked rubber composition X' before crosslinking with the crosslinked rubber composition X.

[0020] Examples of peroxides used as crosslinking agents include 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, 2,5-dimethylhexane-2,5-dihydroperoxide, di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, α,α-bis(t-butylperoxy)-p-diisopropylbenzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)-hexyne-3, benzoyl peroxide, t-butylperoxybenzene, t-butylperoxymaleic acid, t-butylperoxyisopropyl carbonate, and t-butylperoxybenzoate. The peroxide used as crosslinking agent preferably contains one or more of these compounds, and more preferably contains 2,5-dimethyl-2,5-di(t-butylperoxy)hexane from the viewpoint of achieving a high inhibitory effect against crosslinking inhibition by the ionic liquid.

[0021] The amount of peroxide crosslinking agent blended into the uncrosslinked rubber composition X' is preferably 0.5 parts by mass or more and 5 parts by mass or less, more preferably 1 part by mass or more and 3 parts by mass or less, per 100 parts by mass of fluororubber, from the viewpoint of obtaining a high inhibitory effect against crosslinking inhibition by the ionic liquid.

[0022] The degree of crosslinking of the crosslinked rubber composition X may be further increased by a crosslinking aid. Examples of the crosslinking aid include triallyl cyanurate, trimethallyl isocyanurate, triallyl isocyanurate, triacryl formal, triallyl trimellitate, N,N'-m-phenylene bismaleimide, dipropargyl terephthalate, diallyl phthalate, tetraallyl terephthalate amide, triallyl phosphate, bismaleimide, fluorinated triallyl isocyanurate (1,3,5-tris(2,3,3-trifluoro-2-propenyl)-1,3,5-triazine), and the like. Examples of suitable crosslinking aids include 5-norbornene-2-methylene trimethylsiloxane, 5-norbornene-2-methyltri ...

[0023] The crosslinked rubber composition X may contain silicone rubber or the like as a base rubber component other than the fluororubber. The crosslinked rubber composition X may also contain rubber compounding agents such as processing aids, plasticizers, processing aids, vulcanization accelerators, and antioxidants.

[0024] The volume resistivity of the crosslinked rubber composition X is preferably 1.0×1012 Ω cm or less, more preferably 1.0 × 10 11 The volume resistivity is Ω·cm or less. This volume resistivity is measured based on JIS K6271-1:2015.

[0025] Specific examples of rubber products according to the embodiment include sealing materials such as O-rings.

[0026] Next, a method for manufacturing a rubber product according to an embodiment will be described.

[0027] In the method for producing a rubber product according to the embodiment, first, a filler and an ionic liquid are mixed together, and the ionic liquid is absorbed into the filler.

[0028] Next, the fluororubber is masticated using a rubber kneader, and rubber compounding ingredients containing a filler that has absorbed an ionic liquid and a crosslinking agent are added thereto. Thus, the filler that has absorbed the ionic liquid and the like are kneaded with the fluororubber to prepare an uncrosslinked rubber composition X'. At this time, in the resulting uncrosslinked rubber composition X', a portion of the ionic liquid absorbed in the filler flows out and diffuses into the fluororubber.

[0029] The maximum torque value of the uncrosslinked rubber composition X′ is preferably 0.5 N m or more, more preferably 1 N m or more, and is determined in accordance with JIS K6300-2:2001 based on a vulcanization curve obtained from a Curelastometer (registered trademark).

[0030] The uncrosslinked rubber composition X' is then molded into a predetermined shape and held at a predetermined temperature and pressure for a predetermined time to crosslink, thereby obtaining a rubber product according to the embodiment formed from the crosslinked rubber composition X. The obtained rubber product may be subjected to a secondary crosslinking treatment in which it is held in an atmosphere at a predetermined temperature for a predetermined time and / or a radiation crosslinking treatment in which it is irradiated with radiation.

[0031] (O-ring) The O-rings of Examples 1 and 2 and a comparative example were prepared as follows. The constitution of the crosslinked rubber composition forming each is shown in Table 1.

[0032] Example 1 A fluorine-containing ternary FKM (Technoflon P459 manufactured by Solvay) was used as a base rubber. First, 5 parts by mass of a filler PVDF powder (Kynar MG15 manufactured by Arkema, density: 1.78 g / cm) was added to 100 parts by mass of this ternary FKM. 3 ) and 0.5 parts by mass of ionic liquid A, 1-butyl-3-methylimidazolium bistrifluoromethanesulfonylimide (BMI-N111, manufactured by Mitsubishi Materials Corporation), were mixed, and ionic liquid A was absorbed into the PVDF powder. Next, 100 parts by mass of ternary FKM was mixed with the PVDF powder having absorbed ionic liquid A, along with 1.5 parts by mass of the crosslinking agent, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (Perhexa 25B, manufactured by NOF Corporation), and 3 parts by mass of the crosslinking coagent, triallyl isocyanurate (TAIC, manufactured by Nippon Kasei Chemical Co., Ltd.), and kneaded to prepare an uncrosslinked rubber composition. This uncrosslinked rubber composition was then crosslinked by press molding to produce an O-ring formed from the crosslinked rubber composition. This O-ring was designated Example 1.

[0033] Example 2 An O-ring having the same configuration as in Example 1 was produced, except that ionic liquid B, tributylmethylammonium bistrifluoromethanesulfonylimide (FC-4400, manufactured by 3M Japan Ltd.), was used instead of ionic liquid A. This was designated Example 2.

[0034] Comparative Example An O-ring having the same configuration as in Example 2 was produced as a comparative example, except that ionic liquid B was directly blended with the ternary FKM without blending PVDF powder.

[0035]

[0036] (Test Method and Results) <Maximum Torque Value> For the uncrosslinked rubber compositions used to prepare the O-rings of Examples 1 and 2 and the Comparative Example, vulcanization curves were obtained using a curastometer. Then, the maximum torque values ​​were calculated based on the vulcanization curves in accordance with JIS K6300-2:2001. The results are shown in Table 2.

[0037]

[0038] Table 2 shows that Example 1, in which ionic liquid A was absorbed into PVDF powder, and Example 2, in which ionic liquid B was absorbed into PVDF powder, had high maximum torque values, whereas the Comparative Example, in which no PVDF powder was used, had a very low maximum torque value. This is thought to be because crosslinking inhibition by the ionic liquid occurred in the Comparative Example, whereas crosslinking inhibition by the ionic liquid was suppressed in Examples 1 and 2 by absorbing the ionic liquid into the PVDF powder.

[0039] <SEM Observation and EDS Analysis> For each of the O-rings of Examples 1 and 2 and the Comparative Example, a circular sample of a thin film of the cross-linked rubber composition having a thickness of approximately 1 μm was cut out, and the center portion, the surface layer portion, and the intermediate portion between them were observed by SEM and analyzed by EDS.

[0040] Observation and analysis revealed that in Examples 1 and 2, a sea-island structure was observed, in which PVDF powder islands were dispersed in a sea of ​​ternary FKM. Furthermore, analysis revealed that the oxygen and sulfur concentrations were higher in the PVDF powder islands than in the sea of ​​ternary FKM. This is due to bistrifluoromethanesulfonylimide, the anionic component of the ionic liquid. This indicates that the ionic liquid is localized, and the concentration of the ionic liquid in the PVDF powder is higher than that in the ternary FKM. Furthermore, analysis revealed that the fluorine concentration was lower in the PVDF powder islands than in the sea of ​​ternary FKM. This is consistent with the fluorine content of the ternary FKM being 68% by mass, compared with 59.4% by mass in PVDF. In contrast, the comparative example did not exhibit the sea-island structure seen in Examples 1 and 2, nor was the localization of oxygen and sulfur concentrations analyzed.

[0041] <TOF-SIMS Analysis> For the O-ring of Example 1, a depth direction analysis of the surface layer of the crosslinked rubber composition was carried out by TOF-SIMS.

[0042] According to the depth profile of the analysis results, in the surface layer from the surface of the crosslinked rubber composition to a depth of 18 nm, the concentration of the ionic liquid increases from the inside to the surface, with the maximum concentration difference being about 10 times.

[0043] The present invention is useful in the technical field of rubber products and their manufacturing methods.

Claims

1. A rubber product formed from a crosslinked rubber composition containing a fluororubber, an ionic liquid, and a filler that is dispersible in the fluororubber and can absorb the ionic liquid, wherein the concentration of the ionic liquid in the filler is higher than the concentration of the ionic liquid in the fluororubber.

2. A rubber product according to claim 1, wherein the concentration of the ionic liquid in the surface layer of the crosslinked rubber composition increases from the inside to the surface.

3. A rubber product according to claim 1 or 2, wherein the fluororubber contains a copolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene.

4. A rubber product according to any one of claims 1 to 3, wherein the cationic component of the ionic liquid contains an imidazolium-based cation or an aliphatic amine-based cation.

5. The rubber product according to claim 4, wherein the cationic component of the ionic liquid comprises 1-butyl-3-methylimidazolium.

6. The rubber product according to claim 4, wherein the cationic component of the ionic liquid comprises tributylmethylammonium.

7. A rubber product according to any one of claims 1 to 6, wherein the anion component of the ionic liquid contains a bisfluorosulfonylimide-based anion.

8. The rubber product according to claim 7, wherein the anion component of the ionic liquid comprises bistrifluoromethanesulfonylimide.

9. A rubber product according to any one of claims 1 to 8, wherein the content of the ionic liquid in the crosslinked rubber composition is 0.01 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the fluororubber.

10. A rubber product according to any one of claims 1 to 9, wherein the filler contains polyvinylidene fluoride resin powder.

11. A rubber product according to any one of claims 1 to 10, wherein the content of the filler in the crosslinked rubber composition is 1 part by mass or more and 15 parts by mass or less per 100 parts by mass of the fluororubber.

12. A rubber product according to any one of claims 1 to 11, wherein the ratio of the content of the filler to the content of the ionic liquid in the crosslinked rubber composition is 3 or more and 20 or less.

13. A rubber product according to any one of claims 1 to 12, wherein the crosslinking system of the crosslinked rubber composition is a peroxide crosslinking system, and the peroxide of the crosslinking agent contains 2,5-dimethyl-2,5-di(t-butylperoxy)hexane.

14. The rubber product according to any one of claims 1 to 13, wherein the rubber product is a sealing material.

15. A method for producing a rubber product, comprising the steps of: causing a filler to absorb an ionic liquid; kneading the filler soaked in the ionic liquid with a fluororubber to prepare an uncrosslinked rubber composition; and crosslinking the uncrosslinked rubber composition.

Citation Information

Patent Citations

  • Sealant, and production method thereof

    JP2022001642A

  • Semiconductive member for image formation, image forming apparatus and method, and process cartridge

    JP2008129481A

  • Partially fluorinated elastomers, a method for producing the same, and a method for using the same

    JP2016516880A

  • Resin particle, composition containing resin particle, panel containing the composition, and electrophoresis display device containing the panel

    JP2018072614A

  • Sealant rubber material and sealant including the same

    JP2019085475A