Method for producing fine particles, fine particles, fine particle dispersion, and composite particles
The method efficiently produces monodisperse fine particles with specific properties by hydrolyzing intermediate particles in a solvent with hydrolases, addressing the inefficiencies of existing methods and enabling applications in singlet oxygen generation and temperature sensing.
Patent Information
- Application Number
- PCT/JP2024/015035
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-04-15
- Publication Date
- 2024-11-21
AI Technical Summary
Current methods for producing mesoscopic particles are inefficient and lack the capability to produce monodisperse or nearly monodisperse fine particles with specific properties such as luminescent or magnetic materials, and often result in particles with larger sizes and polydispersity.
A method involving a solvent with an intermediate particle, a hydrolase, and water, containing hydrophobic core parts connected by a linking group with a hydrolyzable group, where the hydrolyzable group is hydrolyzed to form fine particles with average sizes of 500 nm or less, and optionally incorporating photosensitizing or luminescent materials, allowing for the production of monodisperse or nearly monodisperse particles with specific properties.
This method efficiently produces fine particles with controlled sizes and properties, such as semiconductor quantum dots and porphyrin skeletons, capable of generating singlet oxygen and functioning as temperature sensors or drug carriers, with improved polydispersity indices and functional group incorporation.
Smart Images

Figure JP2024015035_21112024_PF_FP_ABST
Abstract
Description
Method for producing microparticles, microparticles, microparticle dispersion, and composite particles
[0001] The present disclosure relates to a method for producing microparticles, microparticles, a microparticle dispersion, and composite particles.
[0002] Fine particles having a particle diameter of about several tens to several hundreds of nanometers are generally referred to as mesoscopic particles. As methods for producing mesoscopic particles, top-down approaches using physical milling or lithography, as well as bottom-up approaches using chemical synthesis or self-assembly of amphiphilic substances, have been proposed. For example, Non-Patent Document 1 discloses a chemical synthesis method for mesoscopic particles.
[0003] Trinh, T. Thuy, et al. ,Synthesis of mesoscopic particles of multi-component rare earth permanent magnet compounds,Science and Technology of Advanced Materials, 22.1 (2021): 37-54.
[0004] The present disclosure relates to a novel method for efficiently producing fine particles, such as mesoscopic particles.
[0005] The present disclosure generally includes the following means: [1] A method for producing microparticles, the method comprising: forming microparticles having an average particle size smaller than that of the intermediate particles and including one or more core portions by hydrolyzing the hydrolyzable groups in a reaction solution containing intermediate particles, the intermediate particles having two or more hydrophobic core portions and linking groups connecting the two or more core portions, the linking groups having hydrolyzable groups, a hydrolytic enzyme, and a solvent containing water. [2] The method according to [1], wherein the microparticles include two or more core portions. [3] The method according to [1] or [2], further comprising forming the intermediate particles comprising the linking group having a partial structure derived from the linking agent by a linking reaction including a reaction of bonding the core portion with a linking agent having a reactive group, wherein the linking agent may have a hydrolyzable group, the linking reaction may include a reaction of bonding the linking agents together, and the hydrolyzable group contained in the linking group is one or more selected from the group consisting of a group formed by a reaction of bonding the linking agent with the core portion, the hydrolyzable group possessed by the linking agent before bonding with the core portion, and a group formed by bonding between linking agents. [4] The method according to any one of [1] to [3], wherein the average particle size of the fine particles is 500 nm or less. [5] The method according to any one of [1] to [4], wherein the hydrolase is a protease and the hydrolyzable group is an amide group, the hydrolase is an esterase or lipase and the hydrolyzable group is a carboxylic acid ester group, the hydrolase is an amylase and the hydrolyzable group is a group containing a glycosidic bond, the hydrolase is a phosphodiesterase or nuclease and the hydrolyzable group is a group containing a phosphodiester bond, or the hydrolase is a phosphotriesterase and the hydrolyzable group is a group containing a phosphotriester bond. [6] Microparticles comprising one or more hydrophobic core moieties and having an average particle size of 500 nm or less. [6a] Microparticles comprising one or more hydrophobic core moieties and a compound having a hydrophilic group formed by hydrolysis of the hydrolyzable group, wherein the compound may be covalently bonded to the core moiety, and having an average particle size of 500 nm or less.[6b] The microparticle according to [6], further comprising a compound having a hydrophilic group, wherein the compound may be bonded to the core portion. [7] The microparticle according to [6], [6a], or [6b], comprising an aggregate comprising two or more of the core portions. [8] The microparticle according to [6], [6a], [6b], or [7], having a polydispersity index of 0.4 or less. [9] The microparticle according to [6], [6a], [6b], [7], or [8], wherein the core portion comprises a luminescent material.
[10] The microparticle according to any one of [6], [6a], [6b], and [7] to [9], wherein the core portion comprises a metallic material.
[11] The microparticle according to any one of [6], [6a], [6b], and [7] to
[10] , wherein the core portion comprises a magnetic material.
[12] The microparticle according to any one of [6], [6a], [6b], and [7] to
[11] , wherein the core portion comprises a photosensitizing group.
[13] A microparticle according to any one of [6], [6a], [6b], and [7] to
[11] , wherein the compound contains a photosensitizing group.
[14] A singlet oxygen generator comprising the microparticle according to
[12] or
[13] .
[15] A temperature sensor material comprising the microparticle according to [9],
[12] , or
[13] .
[16] A microparticle dispersion comprising the microparticle according to any one of [6], [6a], [6b], and [7] to
[13] , and a solvent, in which the microparticles are dispersed.
[17] A composite particle comprising two or more hydrophobic core portions and linking groups connecting the two or more core portions, the linking groups having a hydrolyzable group.
[0006] It is possible to efficiently produce fine particles such as mesoscopic particles. It is also possible to easily produce monodisperse or nearly monodisperse fine particles.
[0007] FIG. 1 is a schematic diagram showing an example of a method for producing microparticles. FIG. 2 is a schematic diagram showing an example of a method for producing microparticles containing semiconductor quantum dots. FIG. 3 is a graph showing the particle size distribution (volume distribution) of microparticles containing semiconductor quantum dots. FIG. 4 is a schematic diagram showing an example of a method for producing microparticles having a core portion containing a porphyrin skeleton. FIG. 5 is a graph showing the particle size distribution (volume distribution) of microparticles having a core portion containing a porphyrin skeleton. FIG. 6 is a graph showing the results of measuring the amount of singlet oxygen generated by microparticles. FIG. 7 is a schematic diagram showing an example of a method for producing microparticles containing a core portion containing semiconductor quantum dots and a porphyrin skeleton. FIG. 8 is a graph showing the particle size distribution (volume distribution) of microparticles containing a core portion containing semiconductor quantum dots and a porphyrin skeleton (Condition 1). FIG. 9 is a graph showing the particle size distribution (volume distribution) of microparticles containing a core portion containing semiconductor quantum dots and a porphyrin skeleton (Condition 2). FIG. 10 is a graph showing the results of measuring the amount of singlet oxygen generated by microparticles. FIG. 11 is a schematic diagram showing an example of a method for producing microparticles containing a bipyridine skeleton. FIG. 12 is a graph showing the particle size distribution (volume distribution) of microparticles containing a bipyridine skeleton. 2+ 1 is an absorption spectrum of a test solution containing microparticles having a core portion containing a porphyrin skeleton. 2 is a schematic diagram showing an example of a method for producing microparticles having a core portion containing a porphyrin skeleton. 3 is a graph showing the results of measuring the amount of singlet oxygen generated by microparticles having a core portion containing a porphyrin skeleton. 4 is an absorption spectrum of a test solution containing microparticles having a core portion containing a porphyrin skeleton and having a pH of 6.5 or less. 5 is an absorption spectrum of a test solution containing microparticles having a core portion containing a porphyrin skeleton and glycine and having a pH of 7.5 to 8.4. 6 is a schematic diagram showing an example of a method for producing microparticles containing graphene nanoparticles. 7 is a graph showing the particle size distribution (number distribution) of microparticles containing graphene nanoparticles. 8 is a photograph of a production process of microparticles containing graphene nanoparticles. 9 is an absorption spectrum of a test solution containing microparticles having a core portion containing graphene nanoparticles and doxorubicin. 10 is a schematic diagram showing an example of a method for producing microparticles having a core portion containing a porphyrin skeleton. 11 is a graph showing the particle size distribution (number distribution) of microparticles having a core portion containing a porphyrin skeleton.
[0008] The present invention is not limited to the following examples.
[0009] Fig. 1 is a schematic diagram showing an example of a method for producing microparticles according to the present disclosure. The method shown in Fig. 1 includes preparing a hydrophobic core 1, forming an intermediate particle 10 (composite particle) including two or more cores 1 and a linking group 21 that links the two or more cores 1 and has a hydrolyzable group by a linking reaction including a reaction of bonding the cores 1 with a linking agent having a reactive group, and forming microparticles 30 by hydrolyzing the hydrolyzable group in a reaction solution that includes the intermediate particle 10, a hydrolytic enzyme, and a solvent containing water.
[0010] By hydrolyzing some of the hydrolyzable groups contained in the linking group 21 of the intermediate particle 10 with a hydrolytic enzyme, the intermediate particle 10 is decomposed to a certain extent, and it is possible to form fine particles 30 that have an average particle size smaller than that of the intermediate particle 10 and that include one or more core portions 1. The mechanism behind this is not entirely clear, but it is presumed that, for example, the hydrophobic core portion in the fine particle 30 surrounds the linking group, thereby inhibiting the interaction between the hydrolyzable group and the hydrolytic enzyme, and that the multiple core portions 1 aggregate with each other due to hydrophobic interactions.
[0011] The core part 1 may be a hydrophobic particle, a hydrophobic compound, or a hydrophobic partial structure of a compound. The hydrophobic particle serving as the core part 1 may be a particle that can maintain its particle shape in water at 20°C. The hydrophobic compound serving as the core part 1 may be, for example, a heteroaromatic compound, an aromatic hydrocarbon compound, or an aliphatic hydrocarbon compound. When the core part 1 is a partial structure of a compound, the core part 1 is a hydrophobic group. The hydrophobic group serving as the core part 1 is a group that is more hydrophobic than a hydrolyzable group, and examples thereof include a heteroaromatic group, an aromatic hydrocarbon group, and an aliphatic hydrocarbon group.
[0012] The average particle size of the particles used as the core portion 1 may be, for example, 0.7 nm or more and 50 nm or less. The average particle size of the particles used as the core portion 1 may be 5 nm or more, or 40 nm or less, 30 nm or less, or 20 nm or less. In this specification, the average particle size of the particles means a value determined by dynamic light scattering.
[0013] The hydrophobic particles serving as the core portion 1 may be inorganic particles. The core portion 1 may be one type of inorganic particle or a combination of two or more types of inorganic particles. The inorganic particles serving as the core portion 1 may be particles containing a metal material, particles containing nanocarbon, or a combination thereof. The particles containing a metal material serving as the core portion 1 may be metal particles or particles containing a metal compound.
[0014] The metal particles serving as the core portion 1 may be, for example, gold particles, silver particles, copper particles, platinum particles, or a combination thereof.
[0015] The metal compound constituting the particle of the core portion 1 may be a luminescent material that emits fluorescence and / or phosphorescence. The particle (core portion 1) containing the metal compound as a luminescent material may be a quantum dot (particularly, a semiconductor quantum dot). Examples of the metal compound constituting the quantum dot include CdSe, CdS, and ZnS.
[0016] The particle containing nanocarbon as the core portion 1 may be, for example, a quantum dot. Examples of nanocarbon constituting a quantum dot include carbon nanodots and carbon nanotubes. Examples of nanocarbon also include graphene nanoparticles.
[0017] The metal compound constituting the particle of the core portion 1 may be a magnetic material. That is, the core portion 1 may be a magnetic particle containing a metal compound. Examples of the metal compound that is a magnetic material include iron oxide, Nd 2 Fe 14 B, and multi-element R (rare earth)-T (transition metal) intermetallic compounds. The magnetic particles comprising iron oxide may be iron oxide nanoparticles.
[0018] The core 1 may be a coated particle having an inner particle containing a metal or a metal compound and a coating covering a part or the whole surface of the inner particle. The coating may be a film containing silica.
[0019] The hydrophobic group of the core portion 1 can be a partial structure constituting an organic compound and may include a functional group having various functions. Alternatively, a functional group may be bonded to the hydrophobic group of the core portion 1. The functional group may be, for example, a group capable of forming a coordinate bond with a metal ion or a photosensitizing group. The functional group may also be a luminescent group that imparts the organic compound with the function of a luminescent material that emits fluorescence and / or phosphorescence.
[0020] The hydrophobic group serving as the core portion 1 may be, for example, a group containing a porphyrin skeleton or a bipyridine skeleton. The porphyrin skeleton may be, for example, a group obtained by removing one or more hydrogen atoms from a porphyrin compound represented by the following formula (1A) or (1B). M in formula (1B) represents a metal ion. The bipyridine skeleton may be, for example, a group obtained by removing one or more hydrogen atoms from a bipyridine represented by the following formula (2).
[0021] The porphyrin skeleton is a functional group that functions as a photosensitizing group. Other examples of hydrophobic groups that include a photosensitizing group include a 4,4-difluoro-1,3-dimethyl-4-bora-3a,4a-diaza-s-indacene (BODIPY) skeleton, a halogenated xanthene skeleton, a flavin skeleton, and a bipyrrole skeleton. The porphyrin skeleton can also function as a luminescent group that imparts the functionality of an organic compound as a luminescent material that emits fluorescence and / or phosphorescence.
[0022] The porphyrin and bipyridine skeletons are functional groups that also function as ligands that form coordinate bonds with metal ions. Other examples of hydrophobic groups that can function as ligands include bipyrrole skeletons, crown ether skeletons, and peptide skeletons.
[0023] An arbitrary modifying group may be bonded to the core part 1 that is subjected to the reaction with the linking agent. The modifying group may contain a reactive group, in which case a linking group bonded to the core part 1 can be formed by reaction between the reactive group of the modifying group and the reactive group of the linking agent. In the example of Figure 1, a modified core part 1A is used that has a core part 1 and a modifying group 2 that contains a carboxy group bonded to the core part 1. The modified core part may have multiple reactive groups.
[0024] When the core part 1 is an inorganic particle, a modifying group may be bonded to the surface thereof to form a particle of the modified core part 1A. The inorganic particle and the modifying group may be bonded by a covalent bond or a coordinate bond. When the core part 1 is a partial structure of a compound (particularly an organic compound), the modified core part 1A may be formed by bonding a modifying group containing a reactive group to the partial structure as the core part. The modifying group may further include a group interposed between the core part and the reactive group. When the modified core part 1A is an organic compound having a core part (hydrophobic group) and a modifying group, the molecular weight thereof may be, for example, 50 to 10,000,000 or 100 to 5,000,000.
[0025] The reactive group possessed by the modified core part 1A can be a group capable of reacting with the reactive group of the linking agent to form a linking chain. Examples of the reactive group that the modified core part 1A can possess include a carboxy group, a carboxylate group, a hydroxy group, an amino group, a phosphate group, a thiol group, and a halogenated alkyl group. Here, the carboxylate group is —COO - and may form a salt with any cation.
[0026] The modifying group bonded to the particle as the core portion 1 can be, for example, a group represented by the following formula (3a) or (3b). In formula (3a), X represents a reactive group, and R 1 In formula (3b), X represents a reactive group, and R 2 represents a divalent organic group, and R 3 and R 4 R each independently represents an alkyl group. 3 and R 4 It may be bonded to the core particle at the position R1 and R 2 may be, for example, an alkanediyl group, an oxyalkylene group, or a polyoxyalkylene group.
[0027] The method for producing the microparticles 30 may further include bonding a modifying group containing a reactive group to the core portion 1. For example, the modifying group represented by formula (3a) or (3b) can be introduced by reacting a compound having a thiol group or trialkoxysilyl group and a reactive group X with the particles serving as the core portion.
[0028] A linking reaction including a reaction of bonding the linking agent and the core portion 1 forms an intermediate particle 10 including an aggregate including a large number of core portions 1 linked via linking groups 21. The linking groups 21 include a partial structure derived from the linking agent. The intermediate particle 10 is a composite particle having a relatively large particle size, and when the linking reaction proceeds in a reaction solution, a precipitate including the intermediate particle 10 is often formed. The linking reaction may include a reaction of bonding the linking agents together, particularly a polymerization reaction of the linking agent. When the linking agent polymerizes, a linking group including a polymer chain of the linking agent may be formed.
[0029] The linking agent is a compound having one or more reactive groups that react directly with the core 1 or react with the reactive group of the modified core 1A to form a bond. The linking agent may have two or more types of reactive groups, or may have two or more of the same type of reactive group. Examples of reactive groups of the linking agent include a carboxy group, a carboxylate group, a hydroxy group, an amino group, a phosphate group, a thiol group, and a halogenated alkyl group. When the linking agent has two or more reactive groups, the reactive groups may contain two or more reactive groups selected to bond the linking agents together, in other words, to polymerize the linking agents. For example, when the linking agent is a compound having an amino group and a carboxy group, polymerization of the linking agent can form a linking group containing a polymer chain containing an amide group. For example, the modifying group of the modified core 1A may have a carboxy group, and the linking agent may be a compound having an amino group and a carboxy group. The linking agent may have a hydrolyzable group. The linking agent may be a compound having one or more reactive groups that react directly with the core portion 1 or react with a reactive group of the modified core portion 1A to form a bond, and two or more reactive groups selected separately so that the linking agent polymerizes.
[0030] The linking agent can be, for example, an amino acid, a sugar, a nucleic acid, or a derivative thereof. Examples of amino acids include lysine, trilysine (a trimer of lysine), glutamic acid, tetraglutamic acid (a tetramer of glutamic acid), and arginine. Examples of sugars include hyaluronic acid, glucose, ribose, N-acetylglucosamine, and D-glucuronic acid. The nucleic acid can be a deoxyribonucleic acid or a ribonucleic acid.
[0031] The linking agent may contain a compound further having various functional groups. In this case, a linking group 21 further containing a functional functional group may be formed. The linking agent may contain a compound without a functional functional group and a compound with a functional functional group. In this case, at least one of these compounds has a reactive group capable of binding to the core portion 1 or the modified core portion 1A. The functional functional group may be, for example, a photosensitizing group or a luminescent group. For example, a compound having a porphyrin skeleton and a reactive group can be used as the linking agent.
[0032] The linking reaction to form the intermediate particle 10 can be carried out in a reaction solution containing, for example, the core part 1 or the modified core part 1A, a linking agent, and a reaction solvent. The reaction solution for the linking reaction may contain other components such as a condensing agent and a catalyst. Conditions such as the reaction solvent, reaction temperature, and reaction time are appropriately set so that the linking reaction proceeds appropriately. When the linking reaction includes a polymerization reaction of the linking agent, a stoichiometric excess of the linking agent relative to the core part 1 or the modified core part 1A is usually used. For example, the amount of the linking agent relative to the reactive group of the modified core part 1A may be 2 equivalents or more and 500 equivalents or less.
[0033] The intermediate particle 10 formed by the linking reaction is bonded to two or more core portions 1 and has a linking group 21 containing a hydrolyzable group. The linking group 21 contains a partial structure derived from the linking agent (residue of the linking agent). When a modified core portion 1A is used, the linking group 21 also contains a partial structure derived from the modifying group 2 of the modified core portion 1A (residue of the modifying group 2). The linking group 21 may be bonded to the core portion 1 by a covalent bond or a coordinate bond.
[0034] The intermediate particles 10 have an average particle size larger than the average particle size of the target fine particles 30. The average particle size of the intermediate particles 10 may be, for example, more than 200 nm, 500 nm or more, 1 μm or more, or 10 μm or more. The average particle size of the intermediate particles 10 may be 100 μm or less.
[0035] The hydrolyzable group contained in the linking group 21 may be a group formed by a reaction that bonds the core part 1 with the linking agent (for example, a reaction between a reactive group of the modified core part 1A and a reactive group of the linking agent), a group that the linking agent had before bonding with the core part, a group formed by bonding between linking agents, or a combination of these.
[0036] The hydrolyzable group contained in linking group 21 can be a group that is cleaved by a hydrolysis reaction involving a hydrolase. The hydrolyzable group may be, for example, an amide group, a carboxylic acid ester group (-C(=O)-O-), a group containing a glycosidic bond, a group containing a phosphodiester bond, a group containing a phosphotriester bond, a thioester group, a phosphate monoester group, a sulfate ester group, a diphosphate monoester group, a triphosphate monoester group, an ether group, a thioether group, a trialkylsulfonium group, a group containing an amidine, an acid anhydride, or a group containing a ketone. Linking group 21 may further contain a hydrolyzable group that is different from the hydrolyzable group hydrolyzed by the hydrolase used to form microparticles 30.
[0037] The formed intermediate particles 10 are purified as necessary and then subjected to a hydrolysis reaction to form microparticles 30. The hydrolysis reaction is carried out in a reaction solution containing intermediate particles 10, a hydrolytic enzyme, and a solvent containing water. The intermediate particles 10 may be dispersed or precipitated in the reaction solution. The hydrolysis reaction decomposes the intermediate particles 10 to a certain extent, forming microparticles 30 having a smaller particle size. The intermediate particles 10 dispersed or precipitated in the reaction solution may disappear as the hydrolysis reaction progresses. The disappearance of visible intermediate particles 10 suggests that microparticles 30 having a smaller particle size have been formed.
[0038] The hydrolase is selected from those capable of hydrolyzing the hydrolyzable group contained in the linking group 21. When the hydrolyzable group is an amide group, the hydrolase can be, for example, a protease (trypsin, etc.). When the hydrolyzable group is a carboxylic acid ester group, the hydrolase can be, for example, an esterase or a lipase. When the hydrolyzable group is a group containing a glycosidic bond, the hydrolase can be, for example, an amylase. When the hydrolyzable group is a group containing a phosphodiester bond, the hydrolase can be, for example, a phosphodiesterase or a nuclease. When the hydrolyzable group is a group containing a phosphotriester bond, the hydrolase can be, for example, a phosphotriesterase.
[0039] The solvent for the reaction solution may be water alone or a mixed solvent containing water and another hydrophilic solvent. The hydrophilic solvent may be, for example, alcohol, acetone, tetrahydrofuran, dimethylformamide, or dimethyl sulfoxide. The proportion of water relative to the total amount of solvent in the reaction solution may be, for example, 0.01% by mass or more and 100% by mass or less.
[0040] Conditions such as the concentrations of the intermediate particles and hydrolase in the reaction solution, the reaction temperature, and the reaction time can be adjusted so that the hydrolysis reaction proceeds appropriately. The reaction temperature may be, for example, 20°C or higher and 50°C or lower. The reaction time may be, for example, 30 minutes or higher and 24 hours or lower. The concentration of the hydrolase may be, for example, 0.05 w / v% or higher and 0.5 w / v% or lower. The formed microparticles 30 may be purified as necessary.
[0041] The reaction solution for the hydrolysis reaction may contain other components as necessary. For example, the reaction solution may contain a ligand compound such as ethylenediaminetetraacetic acid and glycol ether diaminetetraacetic acid, or may contain a compound having a buffering effect such as 4-(2-hydroxyethyl)-1-piperazineethanesulfonic acid (HEPES). The particle size of the resulting microparticles can be adjusted by the type and concentration of these other components.
[0042] The microparticles 30 may contain one or more core moieties 1 and compounds 22 formed by hydrolysis of the linking group. The microparticles 30 may also contain aggregates formed by two or more core moieties 1. The aggregates here are collections of two or more hydrophobic core moieties that have aggregated together. For example, the fact that the microparticles 30 have a particle diameter larger than the size of the core moieties 1 suggests that aggregates containing multiple core moieties 1 have been formed. When the core moieties 1 are particles, the aggregates can be secondary particles containing multiple core moieties 1 as primary particles. It is thought that the two or more core moieties form aggregates, for example, by bonding via compounds 22, hydrophobic interactions between the core moieties, or a combination of these.
[0043] The compound 22 forms the microparticle 30 together with the core portion 1 or an aggregate of the core portion 1. The compound 22 may be covalently bonded to one or more core portions 1, or may not be bonded to the core portion 1 at all. The compound 22 typically contains a hydrophilic group generated by hydrolysis of the hydrolyzable group of the linking group. For example, the compound 22 may have at least one of an amino group or a carboxy group generated by hydrolysis of an amide group. Examples of hydrophilic groups that the compound 22 may have include an amino group, a carboxy group, a carboxylate group, a hydroxy group, a phosphate group, a thiol group, a thioether group, an aldehyde group, a functional group containing sulfonic acid, and a functional group containing sulfonate. Using this hydrophilic group, a group containing a functional functional group (e.g., a photosensitizing group) for imparting various functions to the microparticle 30 can also be bonded to the compound 22. The compound 22 may have a functional functional group (e.g., a photosensitizing group) derived from the linking group 21. The microparticle 30 does not necessarily contain the compound 22.
[0044] The average particle size of the microparticles 30 may be, for example, 1 nm or more and 500 nm or less. The average particle size of the microparticles 30 may be 400 nm or less, 300 nm or less, 200 nm or less, 150 nm or less, or 100 nm or less, or may be 10 nm or more, 20 nm or more, 30 nm or more, 40 nm or more, or 50 nm or more. According to the method of the present disclosure, microparticles having average particle sizes within these ranges can be easily produced.
[0045] According to the method of the present disclosure, it is also possible to easily produce microparticles 30 having a particle size distribution that is substantially monodisperse or close to monodisperse. For example, the polydispersity index of the microparticles 30 may be 0.4 or less, 0.3 or less, 0.2 or less, 0.1 or less, 0.09 or less, 0.08 or less, or 0.07 or less. The lower limit of the polydispersity index is not particularly limited, but is typically about 0.02. The polydispersity index may be a value determined by dynamic light scattering.
[0046] In the microparticles 30, the core 1, the compound 22, or both may contain a photosensitizing group. The microparticles 30 containing photosensitizing groups can efficiently generate reactive oxygen species such as singlet oxygen upon light irradiation, for example. When the core 1 contains quantum dots, reactive oxygen species such as singlet oxygen can be generated even more effectively. While the reason for this is not entirely clear, it is believed that efficient energy transfer from the quantum dots to the photosensitizing groups and suppression of the association of the photosensitizing groups in the compound 22 are factors. Therefore, microparticles containing photosensitizing groups can be used as singlet oxygen generators. This singlet oxygen generator may be used, for example, as a photosensitizer for photodynamic therapy of cancer. A singlet oxygen generator containing microparticles 30 corresponding to mesoscopic particles can efficiently accumulate in tumor tissue.
[0047] When the core 1 contains a photosensitizing group, the microparticle 30 can have a light absorption band similar to that of the photosensitizing group. Furthermore, the microparticle 30 can maintain the light absorption band even under pH conditions where the core 1 alone would lose its light absorption. This effect of maintaining the light absorption band can be significantly achieved when the microparticle 30 contains a large amount of compound 22 relative to the core 1.
[0048] When the core portion 1 contains quantum dots, the microparticles 30 can be used as a temperature sensor material. Quantum dots have the property that their fluorescence intensity changes with temperature changes in a system such as a cell. Therefore, by measuring the fluorescence intensity of the microparticles 30 containing quantum dots, it is possible to observe temperature changes in a small region in the system. Furthermore, by coexisting a luminescent material, whose fluorescence intensity does not change with temperature changes, as a probe with the microparticles 30, quantitative temperature measurement can be easily performed.
[0049] In the microparticles 30, the core 1, the compound 22, or both of them may contain a functional group that functions as a ligand that forms a coordinate bond with a metal ion. The microparticles 30 that contain a functional group that functions as a ligand can be used as a metal ion detector, for example, based on a change in absorption spectrum, fluorescence spectrum, or both of them that accompanies the formation of a coordinate bond with a metal ion.
[0050] The microparticles 30 may have swelling properties. The swellable microparticles 30 can encapsulate water-soluble drugs and can be used as carriers in drug delivery systems. For example, when the microparticles 30 are produced using hyaluronic acid as a linking agent, the microparticles 30 have swelling properties.
[0051] The hydrolysis reaction in the reaction solution typically forms a dispersion containing a water-containing solvent and microparticles 30 dispersed in the solvent. The microparticles may be recovered from the dispersion, or the microparticles in the dispersion may be purified as needed, and the solvent may be replaced as needed to obtain a microparticle dispersion for various applications. The recovered microparticles may also be dispersed again to obtain a microparticle dispersion. The solvent for the microparticle dispersion can be selected from those that allow the microparticles to be appropriately dispersed.
[0052] The present invention is not limited to the following examples.
[0053] The particle size of the microparticles was measured by dynamic light scattering using a nanoSAQLA multi-analyte nanoparticle size measurement system (Otsuka Electronics Co., Ltd.) equipped with a high-power semiconductor laser (660 nm, 70 mW). From the measurement results, the polydispersity index was determined by the cumulant method, and the average particle size was determined by the histogram method.
[0054] Amount of singlet oxygen generated The microparticles were added to a 10 mM HEPES buffer solution to prepare a test solution for measuring the amount of singlet oxygen generated. A singlet oxygen generation detection reagent (manufactured by Fisher Scientific, Invitrogen (registered trademark) Singlet Oxygen Sensor Green: SOSG) was added to the test solution to a concentration of 5 μM. Next, 730 nm LED light was applied to the test solution under atmospheric pressure at 500 mW / cm. 2 The amount of singlet oxygen generated was evaluated based on the increase in the peak intensity of the fluorescence of SOSG when excited by 450 nm light compared to the peak intensity when not irradiated with light.
[0055] Example 1: Microparticles containing a core containing semiconductor quantum dots Microparticles containing semiconductor quantum dots were prepared by the method shown in FIG. 2. Semiconductor quantum dots (core 1, CdSe / CdS / ZnS, average particle size 5 nm) were synthesized according to the method described in K. Boldt et al., Chem. Mater. 25 (2013) 4731. 1 mg of the obtained semiconductor quantum dots was dispersed in chloroform. 8000 molar equivalents of PEG were added to the obtained dispersion. 2000 -SH (polyethylene glycol having a thiol group at the end, molecular weight 2000) and 2000 molar equivalents of COOH-PEG 3500 -SH (polyethylene glycol having a thiol group and a carboxyl group at the end, molecular weight 3500) was added, and this was reacted with the semiconductor quantum dots by heating at 70°C for 2 hours. Next, hexane was added to this reaction solution to precipitate semiconductor quantum dots (hydrophobic core 1) and QD-COOH (modified core 1A, average particle size: approximately 27 nm) having polyoxyethylene chains (PEG) with a carboxyl group or a hydroxyl group at the end and bound to the semiconductor quantum dots. The precipitated QD-COOH was recovered from the dispersion.
[0056] The QD-COOH recovered from the dispersion was added to ethanol. To the resulting dispersion, 50 equivalents of trilysine (linking agent, Fujifilm Wako Pure Chemical Industries, Ltd.) relative to the carboxy groups of the QD-COOH and 60 equivalents of 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium tetrafluoroborate (DMT-MM) relative to the carboxy groups of the QD-COOH were added to prepare a reaction solution. The reaction solution was heated to 40°C and shaken for 2 hours to allow a linking reaction, including the reaction of the carboxy groups with the trilysine and the polymerization of the trilysine, to proceed. As the linking reaction progressed, a precipitate containing intermediate particles 10, primarily composed of trilysine polymer chains and containing linking groups with amide groups, was formed. Pure water was added to the dispersion containing the precipitate, and the precipitate was redispersed by ultrasonication, followed by centrifugation, three times to purify the intermediate particles. To the reaction solution containing the purified intermediate particles (precipitate), 0.5 w / v% trypsin (5.3 mmol / L EDTA 4Na solution, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added. The dispersion was heated to 40°C and shaken for 12 hours to hydrolyze the amide groups contained in the linking groups of the intermediate particles. As a result, the precipitate disappeared, and a microparticle dispersion was obtained containing microparticles 30 containing semiconductor quantum dots (cores) and compounds having amino and / or carboxyl groups generated by hydrolysis of the amide groups.
[0057] The particle size of the microparticles contained in the obtained microparticle dispersion was measured. Fig. 3 is a graph showing the particle size distribution (volume distribution) of the microparticles. The average particle size of the microparticles was 78.3 nm, and the polydispersity index was 0.175.
[0058] Example 2: Microparticles containing a core containing a porphyrin skeleton (photosensitizing group) Microparticles containing a core containing a porphyrin skeleton were prepared using the method shown in FIG. 4. rTPA (modified core 1A), a compound having a porphyrin skeleton (core 1) and a carboxylate group forming a potassium salt, was synthesized according to the method described in Satrialdi et al., Chem. Commun. 56 (2020) 1145. Three molar equivalents of trilysine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and four molar equivalents of DMT-MM were added to a reaction solution containing 1 mg of rTPA and ethanol. The reaction solution was then shaken at 40°C for 2 hours to allow a linkage reaction, including the reaction of the carboxylate group of rTPA with trilysine and the polymerization of trilysine, to proceed. As the linkage reaction progressed, a precipitate was formed containing intermediate particles 10 containing linking chains with amide groups, mainly composed of polymerized chains of trilysine. The intermediate particles were purified by adding pure water to the dispersion containing the precipitate, redispersing the precipitate using ultrasonic treatment, and then centrifuging the mixture three times. 0.5 w / v% trypsin (5.3 mmol / L EDTA 4Na solution, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the reaction solution containing the intermediate particles (precipitate), and the reaction solution was shaken at 40°C for 12 hours to hydrolyze the amide groups contained in the linking groups of the intermediate particles. As a result, the precipitate disappeared, and a microparticle dispersion containing microparticles 30 with core portions containing porphyrin skeletons was obtained.
[0059] The particle size of the microparticles contained in the obtained microparticle dispersion was measured. Fig. 5 is a graph showing the particle size distribution (volume distribution) of the microparticles. The average particle size of the microparticles was 100.7 nm, and the polydispersity index was 0.061.
[0060] The amount of singlet oxygen generated by the obtained microparticles was measured. Fig. 6 is a graph showing the relationship between the increase in peak intensity of SOSG excitation light and the light irradiation time. It was confirmed that the microparticles of Example 2 have the function of generating singlet oxygen under light irradiation.
[0061] Example 3: Microparticles containing a core containing semiconductor quantum dots and a compound containing a porphyrin skeleton Microparticles containing a core 1 containing semiconductor quantum dots and a compound containing a porphyrin skeleton were prepared by the method shown in FIG. 7. Semiconductor quantum dots coated with silica (average particle size: approximately 30 nm) were prepared. Amino groups were introduced onto the silica coating by reacting the silica coating containing the semiconductor quantum dots with aminopropyltriethoxysilane in ethanol. 3 mg of semiconductor quantum dots (siQD-NH) with a silica coating into which amino groups had been introduced were prepared. 2 To a reaction solution containing 0.1 mg of rTPA, modified core 1A, and ethanol, 0.24 mg of trilysine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added. An excess amount of DMT-MM was then added, and the reaction solution was shaken at 40°C for 2 hours to allow a linkage reaction to proceed, including the reaction between the semiconductor quantum dots and rTPA, the reaction between rTPA and trilysine, and the polymerization of trilysine. As the linkage reaction progressed, a precipitate of intermediate particles 10 containing a linking group comprising a porphyrin skeleton derived from rTPA and a trilysine polymer chain was formed. Pure water was added to the dispersion containing the precipitate, and the intermediate particles were redispersed by ultrasonic treatment, followed by centrifugation three times to purify the intermediate particles. A trypsin solution under Condition 1 or Condition 2 below was added to the reaction solution containing the intermediate particles (precipitate), and the reaction solution was shaken at 40°C for 12 hours to hydrolyze the amide group contained in the linking group of the intermediate particles. Condition 1: 0.5 w / v % trypsin (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., solvent: aqueous solution containing 0.5 mmol / L EDTA-4Na) Condition 2: 0.5 w / v % trypsin (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., solvent: aqueous solution containing 0.2 mmol / L EDTA-4Na and 10 mM HEPES) As a result, whether the trypsin solution was added under condition 1 or condition 2, the precipitate disappeared, and a microparticle dispersion was obtained containing microparticles including silica-coated semiconductor quantum dots (core 1) and a compound having a porphyrin skeleton and a structural unit derived from trilysine.
[0062] The particle size of the microparticles contained in the microparticle dispersion was measured. Figure 8 is a graph showing the particle size distribution (volume distribution) of the microparticles obtained using the trypsin solution under condition 1. The average particle size of the microparticles obtained using the trypsin solution under condition 1 was 77.1 nm, and the polydispersity index was 0.196. Figure 9 is a graph showing the particle size distribution (volume distribution) of the microparticles obtained using the trypsin solution under condition 2. The average particle size of the microparticles obtained using the trypsin solution under condition 2 was 187.5 nm, and the polydispersity index was 0.183.
[0063] The amount of singlet oxygen generated by the microparticles obtained using the trypsin solution under condition 1 of Example 3 was measured. Figure 6 also shows the measurement results of the amount of singlet oxygen generated by the microparticles obtained using the trypsin solution under condition 1 of Example 3. It was confirmed that the microparticles of Example 3 also have the function of generating singlet oxygen under light irradiation.
[0064] Example 4: Microparticles containing semiconductor quantum dots and a porphyrin skeleton rTPA and DMT-MM were added in an amount of 10% by mass relative to the amount of semiconductor quantum dots to the microparticle dispersion obtained in Example 1. The dispersion was then shaken at 40°C for 2 hours, whereby the carboxylate group and amino group of rTPA reacted to obtain microparticles of Example 4 containing a compound into which a porphyrin skeleton derived from rTPA had been introduced.
[0065] Comparative single particles containing semiconductor quantum dots and a porphyrin skeleton were prepared. To the dispersion containing the QD-COOH and ethanol obtained in Example 1, 1 equivalent of trilysine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) relative to the carboxyl groups of the QD-COOH and 1 equivalent of 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium tetrafluoroborate (DMT-MM) relative to the carboxyl groups of the QC-COOH were added. The dispersion was heated to 40°C and shaken for 2 hours to allow the reaction between the carboxyl groups and the trilysine to proceed. This reaction resulted in the formation of particles containing single semiconductor quantum dot particles and trilysine bound to each single particle. 10% by mass of rTPA and DMT-MM relative to the amount of semiconductor quantum dots were then added. The resulting solution was shaken at 40°C for 6 hours to allow the reaction between the carboxylate groups of the rTPA and the amino groups of the trilysine to proceed. As a result, single particles for comparison were obtained, each of which had a single particle of semiconductor quantum dot and a porphyrin skeleton introduced onto the single particle.
[0066] The amounts of singlet oxygen generated by the resulting microparticles of Example 4, the comparative single particles, and rTPA alone were measured. The concentrations of the particles and rTPA were adjusted so that the peak areas of light absorption derived from rTPA were similar for the microparticles of Example 4, the comparative single particles, and rTPA. Figure 10 is a graph showing the relationship between the increase in peak intensity of SOSG excitation light and light irradiation time. It was confirmed that the microparticles of Example 4 generated singlet oxygen approximately 1.5 times more efficiently than the comparative single particles containing a porphyrin skeleton and approximately 3.8 times more efficiently than rTPA after 10 minutes of LED light irradiation.
[0067] Example 5: Microparticles containing a bipyridine skeleton Microparticles of Example 5 containing a bipyridine skeleton (core portion 1) were prepared using the method shown in Figure 11. 1.1 mg of trilysine (Fujifilm Wako Pure Chemical Industries, Ltd.) and 3.8 mg of DMT-MM were added to a reaction solution containing 1.4 mg of 2,2'-bipyridyl-4-4'-dicarboxylic acid (Tokyo Chemical Industry Co., Ltd.) and ethanol. The reaction solution was shaken at 40°C for 2 hours to allow a linking reaction, including a reaction between the carboxyl group and the trilysine and a polymerization reaction of the trilysine, to proceed. As the linking reaction progressed, a precipitate was formed containing intermediate particles 10, which were primarily composed of trilysine polymer chains and contained linking groups with amide groups. The precipitate-containing dispersion was redispersed by adding pure water and ultrasonication, followed by centrifugation three times to purify the intermediate particles. To the reaction solution containing the intermediate particles (precipitates), 0.5 w / v % trypsin (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 5.3 mmol / L EDTA 4Na solution) was added, and the reaction solution was shaken at 40° C. for 12 hours to hydrolyze the amide groups contained in the linking groups of the intermediate particles. As a result, the precipitates disappeared, and a microparticle dispersion containing microparticles 30 having a bipyridine skeleton was obtained.
[0068] The particle size of the microparticles in the obtained microparticle dispersion was measured. Fig. 12 is a graph showing the particle size distribution (volume distribution) of the microparticles. The average particle size of the microparticles was 101.9 nm, and the polydispersity index was 0.093.
[0069] An aqueous solution containing zinc acetate (II) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the nanoparticle dispersion to prepare Zn at concentrations of 50 μM, 500 μM, or 5000 μM. 2+ Water not containing zinc acetate was added to the fine particle dispersion to obtain a test solution containing Zn. 2+ A test solution containing 0 μM of Zn was also prepared. Figure 13 shows the absorption spectrum of each test solution. 2+ In the presence of Zn, a change in the absorption peak around 300 nm due to the bipyridine skeleton was observed. Based on this change, it was confirmed that the nanoparticles could be used to detect metal ions. In addition, Zn at concentrations of 500 μM and 5000 μM was 2+In the presence of 500 μM, no change was observed in the absorption peak around 300 nm derived from the bipyridine skeleton. In Fig. 13, the solid line representing 500 μM and the dashed line representing 5000 μM overlap.
[0070] Example 6: Microparticles containing a core portion containing a porphyrin skeleton (photosensitizing group) Microparticles containing a core portion containing a porphyrin skeleton were prepared using the method shown in FIG. 14. TAPP (modified core portion 1A), a compound having a porphyrin skeleton (core portion 1) and an amino group, was synthesized according to the method described in Alexander B. Rudine et al. J. Org. Chem. 2013, 78, 12, 6040. To a reaction solution containing 40 nmol of TAPP and ethanol, 4.0 molar equivalents (Example 6-1), 16.0 molar equivalents (Example 6-2), or 64.0 molar equivalents (Example 6-3) of tetraglutamic acid (manufactured by GenScript) relative to the amino group of TAPP, and an excess amount of DMT-MM, were added. The reaction solution was then shaken at 60°C for 3 hours to allow a linkage reaction, including a reaction between the amino group of TAPP and tetraglutamic acid and a polymerization reaction of tetraglutamic acid, to proceed. As the linkage reaction progressed, a precipitate was formed containing intermediate particles 10 (average particle size: 5000 nm or greater) composed primarily of polymerized chains of tetraglutamic acid and including linking chains with amide groups. After the shaking was completed, glycine was added to the reaction solution to inactivate DMT-MM. The intermediate particles were purified by adding pure water to the dispersion containing the precipitate, redispersing the precipitate through ultrasonic treatment, and then centrifuging three times. 0.8 w / v% proteinase K (manufactured by Fujifilm Wako Co., Ltd.) was added to the reaction solution containing the intermediate particles (precipitates), and the reaction solution was shaken at 45°C for 15 hours to hydrolyze the amide groups contained in the linking groups of the intermediate particles. As a result, the precipitate disappeared, and a microparticle dispersion containing microparticles 30 with core portions containing porphyrin skeletons was obtained.
[0071] The particle diameters of the microparticles contained in the microparticle dispersions obtained in Examples 6-1 to 6-3 were measured. In Examples 6-1 to 6-3, the average particle diameter of the microparticles was 130 nm or less, and the polydispersity index was 0.20.
[0072] The amount of singlet oxygen generated by the microparticles obtained in Examples 6-1 to 6-3 was measured. Figure 15 is a graph showing the relationship between the increase in peak intensity of SOSG fluorescence and the light irradiation time. It was confirmed that the microparticles of Examples 6-1 to 6-3 have the function of generating singlet oxygen under light irradiation. The amount of singlet oxygen generated was greatest in Example 6-1, in which the molar equivalent of tetraglutamic acid to the amino group of TAPP was 4.0.
[0073] 16 shows the absorption spectra of the test solutions obtained by adding water to the microparticle dispersions obtained in Examples 6-1 to 6-3. The pH of all test solutions was 6.5 or less. An absorption peak at around 400 nm due to the porphyrin skeleton was observed in all test solutions. The absorption peak was largest in Example 6-1, and was comparable in Examples 6-2 and 6-3.
[0074] An aqueous solution containing sodium hydroxide (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) and glycine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was added to the microparticle dispersion or TAPP-containing solution obtained in Examples 6-1 to 6-3 to obtain a test solution containing glycine at a concentration of 0.1 mol / L and having a pH of 7.5 to 8.4. Figure 17 shows the absorption spectra of each test solution. Furthermore, while TAPP lost its absorption at wavelengths of 700 nm or more under pH conditions of 7.5 to 8.4, the microparticles of Examples 6-2 and 6-3 exhibited absorption at wavelengths of 700 nm or more, even under such pH conditions, similar to when the pH was 6.5 or less (Figure 16). Thus, it was confirmed that the microparticles of Examples 6-2 and 6-3 may be used as microparticles that do not change the performance of the modified core portion 1A even when the solution pH is increased.
[0075] Example 7: Microparticles containing graphene nanoparticles Microparticles containing graphene nanoparticles modified with amino groups (modified core 1A) were prepared using the method shown in Figure 18. An excess of 2,2'-(ethylenedioxy)bis(ethylamine) (Merck) and an excess of DMT-MM were added to a 16 mg / mL aqueous dispersion of carboxylic acid-modified nanographene (Merck). The reaction solution was then sonicated at 40°C for 1 hour, purified water was added, and the precipitate was redispersed by sonication. This process was then repeated three times to synthesize graphene nanoparticles modified with amino groups (modified core 1A, average particle size: approximately 200 nm). To a reaction solution containing amino-modified graphene nanoparticles (average particle size: approximately 200 nm) and pure water (concentration of amino-modified graphene nanoparticles: 8 mg / ml), 1 part by mass (Example 7-1), 3 parts by mass (Example 7-2), or 19 parts by mass (Example 7-3) of an aqueous solution (2.5 mg / ml) of sodium hyaluronate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., weight-average molecular weight: 500 kDa or more) was added per 1 part by mass of the reaction solution, and an excess amount of DMT-MM was further added to prepare a stock mixture. The stock mixture was then shaken at 50°C for 4 hours to allow a linkage reaction, including a reaction between the amino groups and hyaluronic acid and a polymerization reaction of hyaluronic acid, to proceed. As the linkage reaction progressed, a precipitate was formed containing intermediate particles 10 (average particle size: 5000 nm or more) composed primarily of polymer chains of hyaluronic acid and containing linking groups with amide groups. The precipitate-containing dispersion was redispersed by adding pure water and ultrasonic treatment, followed by centrifugation three times to purify the intermediate particles. 0.5 w / v% hyaluronidase (Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the reaction solution containing the intermediate particles (precipitate), and the reaction solution was shaken at 40°C for 22 hours to hydrolyze the amide groups contained in the linking groups of the intermediate particles. As a result, the precipitate disappeared, and a microparticle dispersion containing microparticles 30 containing graphene nanoparticles was obtained.
[0076] The particle size of the microparticles in the microparticle dispersion obtained in Example 7-2 was measured. Figure 19 is a graph showing the particle size distribution (number distribution) of the microparticles. In Example 7-2, the average particle size of the microparticles was 299 nm, and the polydispersity index was 0.20.
[0077] Figure 20 shows photographs of the stock solution mixture, after intermediate particle formation, after the third centrifugation, and after the action of hyaluronidase. After intermediate particle formation, visible particles were observed in Examples 7-1 to 7-3. After the third centrifugation, the swelling ratio in water was determined by weighing the black substance remaining after removing the supernatant liquid. The results showed that the swelling ratio of the microparticles in Example 7-1 was the highest, and the swelling ratio of the microparticles in Example 7-3 was the lowest.
[0078] The nanoparticles 30 (1 mg) of Examples 7-1 to 7-3 were dispersed in pure water (1 mL) to obtain a dispersion, and 0.5 mg of the anticancer drug doxorubicin was added to the dispersion to obtain a mixture, which was then shaken at 40 ° C. for 2 hours to obtain a reaction mixture. Pure water was added to the reaction mixture, which was then redispersed by ultrasonic treatment, and centrifuged three times to obtain a microquantum dispersion (Example 7-1D, Example 7-2D, Example 7-3D, respectively).
[0079] 21 shows the absorption spectra of test solutions prepared by adding water to the microparticle dispersions obtained in Examples 7-1 to 7-3 and Examples 7-1D to 7-3D. By comparing the absorption spectra of Examples 7-1 and 7-1D, absorption near 500 nm, characteristic of doxorubicin, was confirmed in Example 7-1D. Therefore, it was suggested that at least the microparticles obtained in Example 7-1 can encapsulate doxorubicin and thus can be used as a carrier in a drug delivery system.
[0080] Example 8: Microparticles Comprising a Core Portion Containing a Porphyrin Skeleton (Photosensitizing Group) Microparticles comprising a core portion containing a porphyrin skeleton were prepared using the method shown in FIG. 22. TAPP (modified core portion 1A), a compound having a porphyrin skeleton (core portion 1) and an amino group, was synthesized according to the method described in Alexander B. Rudine et al. J. Org. Chem. 2013, 78, 12, 6040. To a reaction solution containing 80 nmol of TAPP (modified core portion 1A) and dimethyl sulfoxide, 16 molar equivalents of sodium hyaluronate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) relative to the amino groups of TAPP and an excess amount of DMT-MM were added. The reaction solution was then shaken at 45°C for 5 hours to allow a linkage reaction, including a reaction between the amino groups of TAPP and hyaluronic acid and a polymerization reaction of hyaluronic acid, to proceed. As the linking reaction progressed, a precipitate was formed containing intermediate particles 10 (average particle size: 5000 nm or more) composed mainly of hyaluronic acid polymer chains and containing linking chains with amide groups. The precipitate-containing dispersion was added with pure water, redispersed by ultrasonication, and then centrifuged three times to purify the intermediate particles. 0.5 w / v% hyaluronidase (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the reaction solution containing the intermediate particles (precipitates), and the reaction solution was shaken at 40°C for 22 hours to hydrolyze the amide groups contained in the linking groups of the intermediate particles. As a result, the precipitate disappeared, and a microparticle dispersion containing microparticles 30 containing cores containing porphyrin skeletons was obtained.
[0081] The particle size of the microparticles in the obtained microparticle dispersion was measured. Fig. 23 is a graph showing the particle size distribution (number distribution) of the microparticles. The average particle size of the microparticles was 200 nm, and the polydispersity index was 0.24.
[0082] 24 shows the absorption spectra of a test solution obtained by adding 10 mM HEPES buffer solution to the microparticle dispersion obtained in Example 8, and a solution obtained by adding 10 mM HEPES buffer solution to the intermediate particle precipitate obtained in Example 8 and dispersing the precipitate by ultrasonic treatment. These absorption spectra retained the absorption band characteristic of porphyrin. Furthermore, the absorption spectrum of the former had a lower absorbance near 900 nm than the absorption spectrum of the latter. Therefore, it is thought that the former test solution scattered less light than the latter solution, suggesting that the microparticles were smaller in size than the intermediate particles.
[0083] The microparticles according to the present disclosure can be used as various functional materials and sensor materials such as luminescent materials, magnetic materials, photoelectric conversion materials, materials that exhibit chemical reaction catalyst functions (including materials that exhibit photocatalytic activity), and photosensitive substances.
[0084] 1...core portion, 1A...modified core portion, 2...modifying group, 10...intermediate particle, 21...linking group, 22...compound, 30...fine particle.
Claims
1. A method for producing microparticles, comprising: intermediate particles having two or more hydrophobic core portions and linking groups connecting the two or more core portions, the linking groups having a hydrolyzable group; hydrolytic enzyme; and a solvent containing water, thereby forming microparticles having an average particle size smaller than the average particle size of the intermediate particles and including one or more of the core portions by hydrolyzing the hydrolyzable group in a reaction solution containing the intermediate particles; 2. The method of claim 1, wherein said microparticles comprise two or more of said core portions.
3. The method according to claim 1 or 2, further comprising forming the intermediate particle comprising the linking group having a partial structure derived from the linking agent by a linking reaction including a reaction of bonding the core portion with a linking agent having a reactive group, wherein the linking agent may have a hydrolyzable group, and the linking reaction may include a reaction of bonding the linking agents together, and wherein the hydrolyzable group contained in the linking group is one or more types selected from the group consisting of a group formed by a reaction of bonding the linking agent with the core portion, the hydrolyzable group possessed by the linking agent before bonding with the core portion, and a group formed by bonding the linking agents together.
4. The method according to claim 1 or 2, wherein the microparticles have an average particle size of 500 nm or less.
5. The method of claim 1 or 2, wherein the hydrolase is a protease and the hydrolyzable group is an amide group; the hydrolase is an esterase or lipase and the hydrolyzable group is a carboxylic ester group; the hydrolase is an amylase and the hydrolyzable group is a group that includes a glycosidic bond; the hydrolase is a phosphodiesterase or nuclease and the hydrolyzable group is a group that includes a phosphodiester bond; or the hydrolase is a phosphotriesterase and the hydrolyzable group is a group that includes a phosphotriester bond.
6. Microparticles comprising one or more hydrophobic core portions and a compound having a hydrophilic group formed by hydrolysis of a hydrolyzable group, the compound optionally being covalently bonded to the core portion, and having an average particle size of 500 nm or less.
7. The microparticle according to claim 6, comprising an aggregate containing two or more of said core portions.
8. The microparticles according to claim 6, having a polydispersity index of 0.4 or less.
9. The microparticle of claim 6, wherein the core portion comprises a luminescent material.
10. The microparticle of claim 6, wherein the core portion comprises a metallic material.
11. The microparticle of claim 6, wherein said core comprises a magnetic material.
12. The microparticle according to claim 6, wherein the core portion contains a photosensitizing group.
13. The microparticle of claim 6, wherein the compound comprises a photosensitizing group.
14. A singlet oxygen generator comprising the microparticles according to claim 12 or 13.
15. A temperature sensor material comprising the microparticles according to claim 9, 12 or 13.
16. A microparticle dispersion comprising the microparticles according to any one of claims 6 to 13 and a solvent, the microparticles being dispersed in the solvent.
17. A composite particle comprising two or more hydrophobic core portions and a linking group linking the two or more core portions, the linking group having a hydrolyzable group.
Citation Information
Patent Citations
particle
JP2009517452A