Rubber composition and tire
The rubber composition for heavy-duty tires addresses high-temperature rupture and heat generation issues by combining diene rubber with a specific polyolefin and fillers, ensuring improved breaking strength and handling stability while meeting environmental standards for reduced rolling resistance.
Patent Information
- Application Number
- PCT/JP2024/015399
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-16
- Filing Date
- 2024-04-18
- Publication Date
- 2024-11-21
AI Technical Summary
Heavy-duty tires face challenges with high-temperature rupture and heat generation, which affects their breaking strength and handling stability, while there is a need for reduced rolling resistance to comply with stricter environmental regulations, but existing solutions compromise on heat generation and stability.
A rubber composition with a diene rubber component and a polyolefin having a specific melting point and melt mass flow rate, combined with carbon black or silica fillers, to enhance breaking strength, reduce heat generation, and improve handling stability, specifically designed for tire treads and undertreads.
The rubber composition maintains high breaking strength at elevated temperatures, reduces heat generation, and enhances handling stability, making it suitable for heavy-duty tire applications while meeting environmental standards.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Rubber composition and tire
[0001] The present invention relates to a rubber composition and a tire using the same.
[0002] Heavy-duty tires such as truck and bus tires can be exposed to temperatures of 100°C or higher depending on road surface conditions, and their breaking properties tend to deteriorate under such high temperatures, so improvements are needed. Meanwhile, there is an increasing demand for lower fuel consumption in automobiles from the perspective of global environmental conservation, and the development of tires with good rolling resistance is desired.
[0003] As a conventional technique for providing a tire with good break properties and low heat generation, for example, Patent Document 1 below discloses a rubber composition containing a diene rubber, a filler, and an acid-modified polypropylene polymer, wherein the acid-modified polypropylene polymer has a melting point of 136 to 155°C and the amount of the acid-modified polypropylene polymer is 1 to 30 parts by mass per 100 parts by mass of the diene rubber. The diene rubber contains a natural rubber, a butadiene rubber, and an aromatic vinyl-conjugated diene copolymer rubber, and the amount of the natural rubber is 15 to 80% by mass per 100 parts by mass of the diene rubber. Furthermore, Patent Document 2 below discloses a rubber composition obtained by blending 2 to 75 parts by weight of high-density polyethylene (including 35 to 70% by weight of high-density polyethylene having a crosslinkable portion) per 100 parts by weight of the rubber component, and kneading the blended resins at a temperature higher than the melting point of the blended resins. Furthermore, Patent Document 3 listed below discloses a rubber composition characterized by blending 1 to 100 parts by mass of a resin material (B) containing an olefin random copolymer (C1) with 100 parts by mass of a diene rubber (A). However, none of Patent Documents 1 to 3 listed below discloses any technical idea of using a polyolefin having the specific melting point and melt mass flow rate of the present invention described below to provide a rubber composition that is excellent in breaking strength at high temperatures and low heat buildup, or a rubber composition for tire undertreads that is low in heat buildup and excellent in steering stability.
[0004] Meanwhile, due to the strengthening of international standards such as R-117 by the United Nations Economic Commission for Europe (UN / ECE) and the strengthening of greenhouse gas (GHG) regulations by the U.S. Environmental Protection Agency (EPA), tires are required to have low rolling resistance, and therefore it is desirable to make the undertread of heavy-duty tires used as truck and bus tires low heat buildup. However, when the undertread is made low heat buildup, the hardness and elastic modulus tend to decrease, which poses the problem of not being able to ensure sufficient handling stability.
[0005] Japanese Patent No. 6350509 Japanese Patent No. 3657389 Japanese Patent Application Laid-Open No. 2017-75236
[0006] Therefore, a first object of the present invention is to provide a rubber composition having excellent breaking strength at high temperatures and low heat buildup, and a tire using the same. A second object of the present invention is to provide a rubber composition for tire undertreads having low heat buildup and excellent steering stability.
[0007] To achieve the first object, the present invention provides a rubber composition (1) characterized by containing, per 100 parts by mass of (A) a rubber component containing 50 parts by mass or more of a diene rubber, 1 to 200 parts by mass of (B) a polyolefin having a melting point of 110°C or more and 155°C or less, and having a melt mass flow rate (MFR) measured at a temperature of 230°C under a load of 2.16 kg of more than 6 g / 10 min, or a melt mass flow rate (MFR) measured at a temperature of 190°C under a load of 2.16 kg of 10 g / 10 min or more. To achieve the second object, the present invention provides (A2) a rubber component comprising an isoprene rubber and a butadiene rubber, wherein, when the total amount of the rubber component is 100 parts by mass, the proportion of the butadiene rubber is 15 parts by mass or less, and (D) a nitrogen adsorption specific surface area (N 2 SA) is 40 to 130 m 2and (C) 0.1 to 20 parts by mass of a high-flow random polypropylene having a melting point of 110°C or higher and 155°C or lower and a melt mass-flow rate (MFR) of more than 6 g / 10 min measured at a temperature of 230°C under a load of 2.16 kg.
[0008] The rubber composition (1) of the present invention is a compound in which 1 to 200 parts by mass of the polyolefin (B) is blended with 100 parts by mass of the rubber component (A). Therefore, it is possible to provide a rubber composition that has excellent breaking strength at high temperatures and low heat buildup, and a tire using the same.
[0009] The (B) polyolefin used in the present invention has high fluidity, which promotes wettability with the (A) rubber component and molecular entanglement, resulting in good dispersion in the matrix (A) rubber component. Furthermore, the (B) polyolefin has a melting point set to 110°C or higher and 155°C or lower, which prevents a decrease in breaking strength even when the tire is heated during running. It can be melted and dispersed at an economical rubber mixing temperature. Furthermore, the melt mass flow rate (MFR) measured at 230°C or 190°C is set within a specific range, which promotes wettability and molecular entanglement, inhibits the (B) polyolefin from becoming foreign matter, and effectively improves breaking properties and reduces heat buildup. Furthermore, the (B) polyolefin also improves the wear resistance of the rubber composition.
[0010] Furthermore, the rubber composition (2) for heavy-duty tire undertreads of the present invention can provide a rubber composition for tire undertreads that exhibits low heat buildup and excellent steering stability. The high-fluidity random polypropylene (C) used in the rubber composition (2) for heavy-duty tire undertreads of the present invention has high fluidity and low crystallinity, which promotes wettability with the rubber component (A) and molecular entanglement, resulting in good dispersion in the matrix rubber component (A2). Furthermore, the high-fluidity random polypropylene (C) has a melt mass-flow rate (MFR) measured at 230°C within a specific range, which promotes the wettability and molecular entanglement, suppresses the formation of foreign matter in the high-fluidity random polypropylene (C), provides excellent heat buildup (low heat buildup), and increases hardness, thereby providing excellent steering stability.
[0011] The present invention will be described in more detail below. First, the rubber composition (1) will be described.
[0012] (A) Rubber Component The rubber component used in the rubber composition (1) of the present invention contains 50 parts by mass or more of a diene rubber, based on 100 parts by mass of the entire rubber composition. The diene rubber is not particularly limited, but examples thereof include natural rubber (NR), synthetic isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), and acrylonitrile-butadiene copolymer rubber (NBR). Among these, a combination of NR and / or IR with BR is preferred from the viewpoint of improving the effects of the present invention. The molecular weight and microstructure of the rubber component are not particularly limited, and the rubber may be terminally modified with amine, amide, silyl, alkoxysilyl, carboxyl, hydroxyl, or the like, or may be epoxidized. In a preferred embodiment of the present invention, the rubber component (A) is preferably composed of a diene rubber.
[0013] (B) Polyolefin The (B) polyolefin used in the rubber composition (1) of the present invention is a high-fluidity polyolefin having a melting point of 110°C or higher and 155°C or lower, and a melt mass-flow rate (MFR) measured at a temperature of 230°C under a load of 2.16 kg of more than 6 g / 10 min, or a melt mass-flow rate (MFR) measured at a temperature of 190°C under a load of 2.16 kg of 10 g / 10 min or higher.
[0014] Furthermore, from the viewpoint of improving the effects of the present invention, the melting point of the (B) polyolefin is preferably 130°C or higher and 150°C or lower. Furthermore, from the viewpoint of improving the effects of the present invention, the melt mass flow rate (MFR) of the (B) polyolefin, measured at a temperature of 230°C and a load of 2.16 kg, is preferably more than 6 g / 10 min and 8 g / 10 min or higher. The upper limit of the MFR is, for example, preferably 5000 g / 10 min or lower, more preferably 1000 g / 10 min or lower, even more preferably 500 g / 10 min or lower, and still more preferably less than 100 g / 10 min. Furthermore, from the viewpoint of improving the effects of the present invention, the melt mass flow rate (MFR) of the (B) polyolefin, measured at a temperature of 190°C and a load of 2.16 kg, is preferably 10 g / 10 min or higher, more preferably 20 g / 10 min or higher. The upper limit of the MFR is, for example, preferably 5,000 g / 10 min or less, more preferably 1,000 g / 10 min or less, and particularly preferably 500 g / 10 min or less. In the description herein, the melting point is measured by differential scanning calorimetry (DSC) in accordance with ASTM D3418 at a heating rate of 10°C / min, and the melt mass flow rate (MFR) is measured in accordance with JIS K7210:1999 "Test method for melt mass flow rate (MFR) of plastics - thermoplastics" under the conditions of a temperature of 190°C or 230°C and a load of 2.16 kg, as described above. Among the above MFR measurement conditions, the temperature of 230°C applies to random polypropylene, and the temperature of 190°C applies to other polyolefins.
[0015] Examples of the type of polyolefin (B) include polyethylenes such as high-density polyethylene (HDPE), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and ultra-low-density polyethylene (ULDPE); random polypropylenes such as propylene-ethylene random copolymers, propylene-1-butene random copolymers, and propylene-ethylene-1-butene random copolymers; ethylene-α-olefin copolymers such as ethylene-propylene copolymers (EPR), ethylene-butene copolymers (EBR), ethylene-pentene copolymers, ethylene-hexene copolymers, and ethylene-octene copolymers; ethylene-(meth)acrylate copolymers, ethylene-vinyl acetate copolymers (EVA), propylene-ethylene block copolymers, and propylene-butene block copolymers. Of these, from the viewpoint of improving the effects of the present invention, at least one selected from the group consisting of propylene-ethylene random copolymers, propylene-1-butene random copolymers, propylene-ethylene-1-butene random copolymers, LDPE, LLDPE, and HDPE is preferred. In the case of ethylene-(meth)acrylic acid ester copolymers and ethylene-vinyl acetate copolymers (EVA), the amount of polar monomer contained therein is preferably 1 to 60 mass %. In addition, the polyolefin (B) used in the present invention can optionally employ a comonomer other than those mentioned above, as long as the above melting point and MFR conditions of the present invention are satisfied.
[0016] In addition, from the viewpoint of improving the effects of the present invention, it is also preferable that the (B) polyolefin used in the rubber composition (1) of the present invention is a high-fluidity polyolefin having a hydrolytically condensable silyl group (hereinafter, sometimes referred to as a silyl group-containing polyolefin) or an acid-modified high-fluidity polyolefin.
[0017] Silyl group-containing polyolefins or acid-modified high-flow polyolefins can be obtained, for example, by grafting a hydrolytically condensable silane compound or an unsaturated carboxylic acid (or its derivative) onto a polyolefin base resin. Specifically, the polyolefin and a free radical generator are coexisted and heated to decompose the free radical generator. The generated free radicals abstract hydrogen from the polyolefin, generating polymer radicals to which the hydrolytically condensable silane compound or unsaturated carboxylic acid (or its derivative) is added.
[0018] Examples of the hydrolytic condensable silane compound include vinyl silane compounds such as vinyl trimethoxysilane, vinyl triethoxysilane, and vinyl tris(β-methoxyethoxy)silane; amino silane compounds such as γ-aminopropyl trimethoxysilane, γ-aminopropyl triethoxysilane, N-β-(aminoethyl)γ-aminopropyl trimethoxysilane, β-(aminoethyl)γ-aminopropylmethyl dimethoxysilane, and N-phenyl-γ-aminopropyl trimethoxysilane; and β-(3,4-epoxycyclohexyl)ethyl trimethylsilane. Examples of compounds that can be used include epoxy silane compounds such as trimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-glycidoxypropylmethyldiethoxysilane; acryl silane compounds such as γ-methacryloxypropyltrimethoxysilane; polysulfide silane compounds such as bis(3-(triethoxysilyl)propyl)disulfide and bis(3-(triethoxysilyl)propyl)tetrasulfide; and mercaptosilane compounds such as 3-mercaptopropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane.
[0019] Examples of unsaturated carboxylic acids include (meth)acrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, and isocrotonic acid. Among these, maleic acid is preferred. One or more unsaturated carboxylic acids can be used. Examples of derivatives of unsaturated carboxylic acids include acid anhydrides, acid halides, amides, imides, esters, and salts of unsaturated carboxylic acids. Among these, acid anhydrides of unsaturated carboxylic acids are preferred, and maleic anhydride is more preferred.
[0020] Examples of the free radical generator include known organic peroxides, such as dicumyl peroxide, benzoyl peroxide, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, t-butylperoxyisopropyl carbonate, t-butylperoxybenzoate, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, methyl ethyl ketone peroxide, 2,2-bis(t-butylperoxy)butane, and cumene hydroperoxide.
[0021] Conditions for the reaction process in which the polyolefin base resin is graft-copolymerized with a hydrolytically condensable silane compound or an unsaturated carboxylic acid (or a derivative thereof) include, for example, blending 0.1 to 10 parts by mass of the hydrolytically condensable silane compound per 100 parts by mass of the polyolefin base resin, and mixing the resulting blend at a temperature above the melting point of the polyolefin. The amount of free radical generator added is, for example, approximately 0.01 to 0.5 parts by mass per 100 parts by mass of the polyolefin. The reaction conditions for the graft copolymerization are known and are disclosed, for example, in Japanese Patent No. 5768696. During the reaction process, known additives such as antioxidants can also be added to the reaction system. The same known reaction conditions can also be used to obtain acid-modified high-fluidity polyolefins.
[0022] From the viewpoint of improving the effects of the present invention, the density of the polyolefin (B) is, for example, 0.860 g / cm 3 1.000g / cm or more 3Preferably, it is 0.880 g / cm or less. 3 0.980g / cm or more 3 More preferably, it is 0.890 g / cm or less. 3 0.970g / cm or more 3 It is particularly preferable that the density is below 100%. In the present invention, the density can be measured by the method described in JIS K7112. When the (B) polyolefin is a silyl group-containing polyolefin, the density of the (B) polyolefin refers to the density of the unmodified polyolefin that is the base resin before it has hydrolytically condensable silyl groups. In addition, the morphology and / or dispersion state of the (B) polyolefin in the rubber composition (1) may be in any form.
[0023] (Carbon Black) Carbon black can be compounded in the rubber composition (1) of the present invention. From the viewpoint of improving the effects of the present invention, the carbon black used in the present invention has a nitrogen adsorption specific surface area (N 2 SA) is 20 to 300m 2 / g, and 40 to 150m 2 / g. It is more preferable that the nitrogen adsorption specific surface area (N 2 SA) is a value determined in accordance with JIS K6217-2.
[0024] (Silica) Silica can be compounded in the rubber composition (1) of the present invention. From the viewpoint of improving the effects of the present invention, the silica used in the present invention has a nitrogen adsorption specific surface area N 2 SA is 20 to 300m 2 / g, and 80 to 250m 2 It is more preferable that the SiO2 content is 1 / g.
[0025] (Ratio of Compounding of Rubber Composition (1)) The rubber composition (1) of the present invention is characterized in that it is compounded with 1 to 200 parts by mass of (B) polyolefin per 100 parts by mass of (A) rubber component. If the compounding amount of the (B) polyolefin is less than 1 part by mass, the compounding amount is too small to achieve the effects of the present invention, and conversely, if it exceeds 200 parts by mass, the rubber elasticity decreases. In the rubber composition of the present invention, the compounding amount of the (B) polyolefin per 100 parts by mass of the rubber component is preferably 1 to 150 parts by mass, more preferably 2 to 100 parts by mass, and particularly preferably 5 to 50 parts by mass.
[0026] In the rubber composition (1) of the present invention, the blending amount of carbon black and / or silica is preferably 20 to 200 parts by mass per 100 parts by mass of the rubber component. Specifically, in the rubber composition (1) of the present invention, the blending amount of carbon black is preferably 5 to 200 parts by mass per 100 parts by mass of the rubber component, and the blending amount of silica is preferably 0 to 195 parts by mass per 100 parts by mass of the rubber component, more preferably 5 parts by mass or more, and particularly preferably 5 to 100 parts by mass.
[0027] When the rubber composition (1) of the present invention is used in a tire tread, the rubber component (A) is preferably composed of an isoprene rubber, and / or a butadiene rubber, and / or a styrene-butadiene rubber, and the proportion of the filler consisting of carbon black and / or silica is preferably 40 to 80 parts by mass per 100 parts by mass of the rubber component (A). When carbon black is used, its nitrogen adsorption specific surface area (N 2 SA) is 90 to 130 m 2 / g.
[0028] When the rubber composition (1) of the present invention is used for a sidewall, the rubber component (A) is preferably composed of an isoprene rubber and a butadiene rubber, and the proportion of the filler consisting of carbon black and / or silica is preferably 30 to 50 parts by mass per 100 parts by mass of the rubber component (A). When carbon black is used, its nitrogen adsorption specific surface area (N2 SA) is 40 to 90 m 2 / g.
[0029] When the rubber composition (1) of the present invention is used for a rim cushion, the rubber component (A) is preferably composed of an isoprene rubber and / or a butadiene rubber, and the proportion of the filler composed of carbon black and / or silica is preferably 40 to 80 parts by mass per 100 parts by mass of the rubber component (A). When carbon black is used, its nitrogen adsorption specific surface area (N 2 SA) is 40 to 120 m 2 / g.
[0030] When the rubber composition (1) of the present invention is used for a bead filler, the rubber component (A) is preferably composed of an isoprene rubber and / or a styrene-butadiene rubber, and the proportion of the filler composed of carbon black and / or silica is preferably 30 to 80 parts by mass per 100 parts by mass of the rubber component (A). When carbon black is used, its nitrogen adsorption specific surface area (N 2 SA) is 40 to 120 m 2 / g.
[0031] (Other Components) In addition to the above-mentioned components, the rubber composition (1) of the present invention may contain various additives that are generally compounded in rubber compositions, such as vulcanization or crosslinking agents; vulcanization or crosslinking accelerators; various fillers such as clay, talc, calcium carbonate, and aluminum hydroxide; antioxidants; plasticizers; resins; curing agents; silane coupling agents; and processing aids. These additives can be kneaded by a general method to form a composition, which can then be used for vulcanization or crosslinking. The amounts of these additives that can be compounded may be conventional amounts, as long as they do not contradict the object of the present invention.
[0032] The method for producing the rubber composition (1) of the present invention includes a compounding step of compounding 1 to 200 parts by mass of (B) polyolefin with 100 parts by mass of (A) rubber component, and a kneading step of kneading the resulting compound under conditions equal to or higher than the melting point of the (B) polyolefin. After the kneading step, a vulcanization step may be carried out under conditions equal to or higher than the melting point of the (B) polyolefin. The kneading and vulcanization may be carried out under known conditions using known equipment.
[0033] The rubber composition (1) of the present invention has excellent breaking strength at high temperatures and low heat buildup, and is therefore preferably used for tire treads, and more preferably for heavy-duty tire treads, heavy-duty tire sidewalls, heavy-duty tire rim cushions, and heavy-duty tire bead fillers. The tire of the present invention is preferably a pneumatic tire, which can be filled with air, an inert gas such as nitrogen, or other gases.
[0034] Next, the rubber composition (2) for the undertread of a tire for heavy loads of the present invention will be described. The rubber composition (2) for the undertread of a tire for heavy loads of the present invention (hereinafter sometimes simply referred to as rubber composition (2)) comprises (A2) a rubber component comprising an isoprene-based rubber and a butadiene rubber, and when the total amount of the rubber components is taken as 100 parts by mass, the ratio of the butadiene rubber is 15 parts by mass or less, and (D) a nitrogen adsorption specific surface area (N 2 SA) is 40 to 130 m 2 / g, and / or (C) 0.1 to 20 parts by mass of a high-fluidity random polypropylene having a melting point of 110°C or higher and 155°C or lower and a melt mass-flow rate (MFR) of more than 6 g / 10 min measured at a temperature of 230°C under a load of 2.16 kg.
[0035] In the rubber composition (2) of the present invention, the rubber component (A2) preferably comprises an isoprene-based rubber and a butadiene rubber (BR), and the proportion of the butadiene rubber is preferably 15 parts by mass or less when the total amount of the rubber component (A) is 100 parts by mass. Examples of isoprene-based rubber include natural rubber (NR) and synthetic isoprene rubber (IR). Furthermore, in the rubber component (A2), the proportion of the BR is preferably 5 to 15 parts by mass when the total amount of the rubber component (A2) is 100 parts by mass.
[0036] (D) Filler The rubber composition (2) of the present invention contains a filler made of carbon black and / or silica. From the viewpoint of improving the effects of the present invention, the (D) carbon black used in the rubber composition (2) of the present invention has a nitrogen adsorption specific surface area (N 2 SA) is 40 to 130 m 2 / g, and 40m 2 / g or more 100m 2 On the other hand, from the viewpoint of improving the effects of the present invention, it is more preferable that the silica has a nitrogen adsorption specific surface area (N 2 SA) is 80 to 160 m 2 / g, and 80 to 100m 2 It is more preferable that the SiO2 content is 1 / g.
[0037] (C) High-fluidity random polypropylene The (C) high-fluidity random polypropylene used in the rubber composition (2) of the present invention is characterized by having a melting point of 110°C or higher and 155°C or lower, and a melt mass-flow rate (MFR) measured at 230°C under a load of 2.16 kg of more than 6 g / 10 min. From the viewpoint of improving the effects of the present invention, the melt mass-flow rate (MFR) of the (C) high-fluidity random polypropylene measured at 230°C under a load of 2.16 kg is preferably 8 g / 10 min or higher, and the upper limit of the melt mass-flow rate (MFR) is preferably less than 12 g / 10 min. Furthermore, from the viewpoint of improving the effects of the present invention, the melting point of the (C) high-fluidity random polypropylene is preferably 130°C or higher and 160°C or lower, more preferably 130°C or higher and 150°C or lower.
[0038] Examples of the high fluidity random polypropylene (C) used in the rubber composition (2) of the present invention include propylene-ethylene random copolymers, propylene-1-butene random copolymers, propylene-ethylene-1-butene random copolymers, etc., which are preferred from the viewpoint of the effects of the present invention. Note that the high fluidity random polypropylene (C) used in the present invention can optionally employ a comonomer other than those mentioned above, as long as it satisfies the MFR requirement of the present invention.
[0039] The high-flow random polypropylene (C) used in the rubber composition (2) of the present invention may have a hydrolytically condensable silyl group in the molecule. The conditions for introducing the hydrolytically condensable silyl group into the molecule of the high-flow random polypropylene (C) are the same as those for the silyl group-containing polyolefin described in the rubber composition (1) of the present invention.
[0040] (Rubber composition (2) blending ratio) The rubber composition (2) of the present invention has a ratio of (D) nitrogen adsorption specific surface area (N 2 SA) is 40 to 130 m 2 The composition is characterized by containing 45 parts by mass or less of a filler consisting of carbon black and / or silica having a melting point of 110°C or higher and 155°C or lower, and 0.1 to 20 parts by mass of (C) a high-fluidity random polypropylene having a melting point of 110°C or higher and a melt mass-flow rate (MFR) of more than 6 g / 10 min measured at 230°C under a load of 2.16 kg. If the amount of the (D) filler exceeds 45 parts by mass, heat buildup deteriorates. If the amount of the (C) high-fluidity random polypropylene is less than 0.1 parts by mass, the amount is too small to achieve the effects of the present invention, while if it exceeds 20 parts by mass, heat buildup and handling stability deteriorate.
[0041] In the (D) filler, the blending amount of carbon black is preferably 30 to 45 parts by mass, more preferably 30 to 40 parts by mass, per 100 parts by mass of the (A2) rubber component, and the blending amount of silica is preferably 5 to 15 parts by mass, more preferably 5 to 10 parts by mass, per 100 parts by mass of the (A) rubber component.
[0042] In the rubber composition (2) of the present invention, the blending amount of the high fluidity random polypropylene (C) is preferably 3 to 8 parts by mass per 100 parts by mass of the rubber component (A).
[0043] (Other Components) The rubber composition (2) of the present invention may contain other components similar to those described in the rubber composition (1). The method for producing the rubber composition (2) of the present invention is also the same as the method for producing the rubber composition (1).
[0044] The rubber composition (2) of the present invention has excellent heat buildup (low heat buildup) and also increases hardness to impart excellent steering stability, and is therefore preferably used for the undertread of a heavy-duty tire. The tire of the present invention is preferably a pneumatic tire, which can be filled with air, an inert gas such as nitrogen, or other gases.
[0045] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples. First, examples and comparative examples relating to the rubber composition (1) of the present invention will be described.
[0046] (Preparation of Various Polyolefins) The following materials were used as random polypropylenes. Random polypropylene A: Novatec PP MG05ES manufactured by Japan Polypropylene Corporation Random polypropylene B: SunAllomer PM731V manufactured by SunAllomer Co., Ltd. Random polypropylene C: SunAllomer PM931M manufactured by SunAllomer Co., Ltd. Random polypropylene D: SunAllomer PM940M manufactured by SunAllomer Co., Ltd. Random polypropylene E: SunAllomer PMA20V manufactured by SunAllomer Co., Ltd. Random polypropylene F: Prime Polypropylene E-333GV manufactured by Prime Polymer Co., Ltd. The melting points and melt mass flow rates (MFR) of the various random polypropylenes measured at a temperature of 230°C and a load of 2.16 kg are shown in Table 1 below.
[0047]
[0048] The following materials were used as polyolefins other than random polypropylene: Polyolefin G (HDPE): Novatec HD HJ590N manufactured by Japan Polyethylene Co., Ltd. Polyolefin H (HDPE): Novatec HD HJ580N manufactured by Japan Polyethylene Co., Ltd. Polyolefin I (HDPE): Novatec HD HJ362N manufactured by Japan Polyethylene Co., Ltd. Polyolefin J (LDPE): Novatec LD LJ902 manufactured by Japan Polyethylene Co., Ltd. The melting points and melt mass-flow rates (MFR) measured at a temperature of 190°C and a load of 2.16 kg for the various polyolefins are shown in Table 2 below.
[0049]
[0050] Standard Example 1, Examples 1 to 6, and Comparative Example 1 Sample Preparation In the formulation (parts by mass) shown in Table 3, the components excluding the vulcanization system (vulcanization accelerator, sulfur) were mixed for 5 minutes in a Banbury mixer at 80°C. The temperature reached at this time was 150°C. Next, the vulcanization system was added and mixed using a roll to obtain a rubber composition. Each obtained rubber composition (unvulcanized) was press-vulcanized at 170°C for 10 minutes in a mold (15 cm x 15 cm x 0.2 cm) to prepare vulcanized rubber test pieces, which were then evaluated as follows.
[0051] <Breaking Strength and Breaking Elongation> From the vulcanized rubber test pieces prepared as described above, JIS No. 3 dumbbell-shaped test pieces (thickness: 2 mm) were punched out in accordance with JIS K6251, and tests were conducted at a pulling rate of 500 mm / min in an atmosphere of 20°C or 100°C to measure the tensile breaking strength and breaking elongation. The results obtained are shown in the columns for "Breaking Strength" and "Breaking Elongation" as indexes, with the value for Standard Example 1 being 100. Larger indexes indicate greater tensile breaking strength and breaking elongation, and more excellent mechanical properties.
[0052] <Heat buildup: tan δ (60°C) index> For the vulcanized rubber test pieces prepared as described above, the loss tangent tan δ (60°C) at a temperature of 60°C was measured using a viscoelasticity spectrometer (manufactured by Toyo Seiki Seisakusho, Ltd.) under conditions of an initial strain of 10%, an amplitude of ±2%, and a frequency of 20 Hz, to evaluate heat buildup. The reciprocal of the obtained tan δ (60°C) was calculated, and the results are shown in the "Heat buildup" column as an index, with the value for Reference Example 1 set to 100. The larger these indices, the lower the heat buildup, and the more preferable it is.
[0053] The results are shown in Table 3.
[0054]
[0055] *1: NR (SIR20) *2: BR (Nipol BR1220 manufactured by Nippon Zeon Co., Ltd., number average molecular weight = 1.8 × 10 5 *3: Silica (ULTRASIL VN3GR manufactured by Evonik, nitrogen adsorption specific surface area (N 2 SA) = 177m 2 / g, CTAB specific surface area = 166 m 2 / g) *4: Carbon black (trade name: Show Black N339, manufactured by Cabot Japan Co., Ltd., CTAB specific surface area = 90 m 2 / g) *5: Silane coupling agent (Si69 manufactured by Evonik Degussa, bis(3-triethoxysilylpropyl)tetrasulfide) *6: Zinc oxide (3 types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd.) *7: Stearic acid (Stearic acid YR manufactured by NOF Corporation) *8: Antiaging agent (SANTOFLEX 6PPD manufactured by Flexis) *9: Sulfur (refinery processed sulfur from Karuizawa Refinery Co., Ltd.) *10: Vulcanization accelerator NS (Suncerer NS-G manufactured by Sanshin Chemical Industry Co., Ltd.) *11: Vulcanization accelerator D (Noccelaer D manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)
[0056] Standard Example 2, Examples 7-8, Comparative Examples 2-3 The procedures for Standard Example 1, Examples 1-6, and Comparative Example 1 were repeated, except that the polyolefin (B) shown in Table 4 was used, and various physical properties were measured. The results for the various physical properties of Examples 7-8 and Comparative Examples 2-3 were expressed as an index, with the value for Standard Example 2 set at 100. The results are shown in Table 4.
[0057]
[0058] Standard Example 3, Examples 9 to 11, Comparative Example 4 The random polypropylene A, the random polypropylene D, the polyolefin G, or the following random polypropylene K, the following hydrolytically condensable silane compound, the free radical generator, and the antioxidant were grafted through the following extruder according to the formulations (parts by mass) shown in Table 5 below, to obtain silyl group-containing polyolefins of Synthesis Examples 1 to 3. An extruder with an L / D ratio of 28 and a screw outer diameter of 65 mm was used, and the temperature conditions for each zone were as follows: First Zone: 160°C, Second Zone: 180°C, Third Zone: 200°C, Fourth Zone: 230°C, Head Zone: 230°C, Die Zone: 230°C. The strands were extruded under the above conditions, cooled with water, and pelletized using a pelletizer.
[0059]
[0060] Hydrolytic condensation silane compound: vinyltriethoxysilane (KBE1003 manufactured by Shin-Etsu Chemical Co., Ltd.) Free radical generator: dicumyl peroxide Antioxidant: Irganox 1010 manufactured by BASF Japan Ltd. Random polypropylene K (Linkron PM700N manufactured by Mitsubishi Chemical Corporation)
[0061] The procedures for "Standard Example 1, Examples 1 to 6, and Comparative Example 1" were repeated, except that the (B) polyolefins shown in Table 6 were used, and various physical properties were measured. The results are shown in Table 6, with the value for Standard Example 3 set as an index of 100, and the various physical properties for Examples 9 to 11 and Comparative Example 4.
[0062]
[0063] Standard Example 4, Examples 12-13, Comparative Example 5 The random polypropylene A, the random polypropylene D, or the random polypropylene F, maleic anhydride, a free radical generator, and an antioxidant were graft-reacted in the formulations (parts by mass) shown in Table 7 below through the following extruder to obtain polyolefin (B) of Synthesis Examples 4-6. An extruder with an L / D ratio of 28 and a screw outer diameter of 65 mm was used, and the temperature conditions for each zone were as follows: First Zone: 160°C, Second Zone: 180°C, Third Zone: 200°C, Fourth Zone: 230°C, Head Zone: 230°C, Die Zone: 230°C. The strands were extruded under the above conditions, cooled with water, and pelletized using a pelletizer.
[0064]
[0065] Maleic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd.) Free radical generator: dicumyl peroxide Antioxidant: Irganox 1010 manufactured by BASF Japan Ltd.
[0066] The procedures for "Standard Example 1, Examples 1 to 6, and Comparative Example 1" were repeated, except that the (B) polyolefins shown in Table 8 were used, and various physical properties were measured. The results are shown in Table 8, with the value for Standard Example 4 set as an index of 100, and the various physical properties for Examples 12 to 13 and Comparative Example 5.
[0067]
[0068] *12: SBR (Nipol 1502 manufactured by Nippon Zeon Co., Ltd.)
[0069] From the results in each table, each example of the rubber composition (1) of the present invention is characterized by containing, per 100 parts by mass of a rubber component containing at least 50 parts by mass of (A) diene rubber, 1 to 200 parts by mass of a polyolefin having a melting point of 110°C or higher and 155°C or lower, and a melt mass flow rate (MFR) measured at 230°C and a load of 2.16 kg of greater than 6 g / 10 min, or a melt mass flow rate (MFR) measured at 190°C and a load of 2.16 kg of greater than 10 g / 10 min, thereby providing a rubber composition with excellent break strength at high temperatures and low heat buildup. In contrast, in Comparative Example 1, the melt mass flow rate (MFR) of the random polypropylene measured at 230°C and a load of 2.16 kg was less than the lower limit specified in the present invention, resulting in poor elongation at break at 20°C and 100°C. In Comparative Example 2, the polyolefin had a melt mass flow rate (MFR) of less than 10 g / 10 min measured at 190°C under a load of 2.16 kg, resulting in poor strength at break at 20°C and 100°C and poor elongation at break at both 20°C and 100°C. In Comparative Example 3, the polyolefin had a melting point of less than 110°C, resulting in poor strength at break and elongation at break at 100°C. In Comparative Example 4, the random polypropylene had a melting point of less than 110°C, resulting in poor strength at break at 20°C and poor strength at break and elongation at break at both 100°C and 20°C. In Comparative Example 5, the polyolefin had a melt mass flow rate (MFR) of less than 5 g / 10 min measured at 230°C under a load of 2.16 kg, resulting in poor strength at break at 20°C and 100°C and poor elongation at break at both 20°C and 100°C.
[0070] Next, examples and comparative examples relating to the rubber composition (2) of the present invention are described. Reference Example 5, Examples 14-21, and Comparative Examples 6-9: In the formulations (parts by mass) shown in Table 9, the components excluding the vulcanization system (vulcanization accelerator, sulfur) were mixed for 5 minutes in a Banbury mixer at 80°C. The temperature reached at this time was 150°C. Next, the vulcanization system was added and mixed using a roll to obtain a rubber composition. Each of the obtained rubber compositions (unvulcanized) was press-vulcanized in a mold (15 cm x 15 cm x 0.2 cm) at 170°C for 10 minutes to prepare vulcanized rubber test pieces, which were then evaluated as follows.
[0071] <Heat buildup: tan δ (60°C) index> For the vulcanized rubber test pieces prepared as described above, the loss tangent tan δ (60°C) at a temperature of 60°C was measured using a viscoelasticity spectrometer (manufactured by Toyo Seiki Seisakusho, Ltd.) under conditions of an initial strain of 10%, an amplitude of ±2%, and a frequency of 20 Hz, to evaluate heat buildup. The reciprocal of the obtained tan δ (60°C) was calculated, and the results are shown in the "Heat buildup" column as an index, with the value for Reference Example 5 being set at 100. The larger these indices, the lower the heat buildup, and the more preferable it is.
[0072] <Handling stability: hardness> The hardness of the vulcanized rubber test pieces prepared as described above was measured at 20°C in accordance with JIS K6253. The results were expressed as an index, with the value of Standard Example 5 being 100. A larger index indicates higher hardness and better handling stability.
[0073] The results are shown in Table 9.
[0074]
[0075] * 13: Carbon black A (product name Show Black N339, manufactured by Cabot Japan Co., Ltd.), nitrogen adsorption specific surface area (N 2 SA) = 88m 2 / g) *14: Carbon black B (trade name Show Black N550, manufactured by Cabot Japan Co., Ltd., nitrogen adsorption specific surface area (N 2 SA) = 40 m 2 / g) *15: Carbon black C (product name Show Black S118, manufactured by Cabot Japan Co., Ltd., nitrogen adsorption specific surface area (N 2 SA) = 148 m 2 / g) * 16: Vulcanization accelerator NS (Noccela CZ-G manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)
[0076] Standard Example 6, Examples 22-25 Using the silyl group-containing polyolefins obtained in Synthesis Examples 1 and 2, rubber compositions were obtained in the same manner as in Standard Example 5, Examples 14-21, and Comparative Examples 6-9, based on the compounding formulations (parts by mass) in Table 10, and the heat buildup: tan δ (60°C) index and steering stability: hardness were measured. The results are expressed as an index, with the value of Standard Example 6 being 100. The results are shown in Table 10.
[0077]
[0078] As shown in Tables 9 and 10, the rubber composition (2) in each example is (A2) a rubber component comprising an isoprene-based rubber and a butadiene rubber, and when the total amount of the rubber components is 100 parts by mass, the ratio of the butadiene rubber is 15 parts by mass or less. 2 SA) is 40 to 130 m 2 The composition is characterized by containing 45 parts by mass or less of a filler consisting of carbon black and / or silica having a melting point of 110°C or more and 155°C or less, and (C) 0.1 to 20 parts by mass of a high-fluidity random polypropylene having a melting point of 110°C or more and a melt mass-flow rate (MFR) of more than 6 g / 10 min measured at 230°C under a load of 2.16 kg, and therefore exhibits low heat buildup and excellent handling stability. On the other hand, in Comparative Example 6, the random polypropylene had a melt mass-flow rate (MFR) of 6 g / 10 min or less measured at 230°C under a load of 2.16 kg, so no improvement in handling stability was observed compared to Control Example 5. In Comparative Example 7, the amount of butadiene rubber blended exceeded the upper limit specified in the present invention, so no improvement in heat buildup was observed compared to Control Example 5. In Comparative Example 8, the nitrogen adsorption specific surface area (N 2 In Comparative Example 9, the amount of filler blended exceeded the upper limit specified in the present invention, and therefore the heat buildup was worse than in Control Example 5. In Comparative Example 9, the amount of filler blended exceeded the upper limit specified in the present invention, and therefore the heat buildup was worse than in Control Example 5.
[0079] Examples 26 to 27: Rubber compositions were prepared in the same manner as in "Standard Example 5, Examples 14 to 21, and Comparative Examples 6 to 9," except that (C) the high-fluidity random polypropylene shown in Table 11 was used, and various physical properties were measured. The results are expressed as an index, with the value of Standard Example 5 being 100. The results are shown in Table 11.
[0080]
[0081] The present disclosure includes the following inventions. Invention [1]: A rubber composition comprising, per 100 parts by mass of a rubber component containing (A) 50 parts by mass or more of a diene-based rubber, (B) 1 to 200 parts by mass of a polyolefin having a melting point of 110°C or higher and 155°C or lower, and having a melt mass flow rate (MFR) measured at a temperature of 230°C under a load of 2.16 kg of more than 6 g / 10 min, or a melt mass flow rate (MFR) measured at a temperature of 190°C under a load of 2.16 kg of 10 g / 10 min or higher. Invention [2]: The rubber composition according to Invention 1, wherein the diene-based rubber is at least one selected from the group consisting of natural rubber, synthetic isoprene rubber, butadiene rubber, styrene-butadiene copolymer rubber, and acrylonitrile-butadiene copolymer rubber. Invention [3]: The rubber composition according to Inventions 1 or 2, further comprising 20 to 200 parts by mass of carbon black and / or silica per 100 parts by mass of the (A) rubber component. Invention [4]: The rubber composition according to any one of Inventions 1 to 3, wherein the (B) polyolefin is at least one selected from the group consisting of a propylene-ethylene random copolymer, a propylene-1-butene random copolymer, a propylene-ethylene-1-butene random copolymer, a low-density polyethylene (LDPE), a linear low-density polyethylene (LLDPE), and a high-density polyethylene (HDPE). Invention [5]: The rubber composition according to any one of Inventions 1 to 4, wherein the (B) polyolefin has a melting point of 130°C or higher and 150°C or lower. Invention [6]: A rubber composition according to any one of Inventions 1 to 5, wherein the (B) polyolefin has a melt mass flow rate (MFR) of 8 g / 10 min or more measured at a temperature of 230° C. and a load of 2.16 kg, or a melt mass flow rate (MFR) of 20 g / 10 min or more measured at a temperature of 190° C. and a load of 2.16 kg. Invention [7]: A rubber composition according to any one of Inventions 1 to 6, wherein the (B) polyolefin is selected from a propylene-ethylene random copolymer, a propylene-1-butene random copolymer, and a propylene-ethylene-1-butene random copolymer.Invention [8]: A method for producing a rubber composition, comprising: a blending step of blending 100 parts by mass of a rubber component containing (A) 50 parts by mass or more of a diene-based rubber with 1 to 200 parts by mass of (B) a polyolefin having a melting point of 110°C or more and 155°C or less, and having a melt mass flow rate (MFR) measured at a temperature of 230°C under a load of 2.16 kg of more than 6 g / 10 min, or a melt mass flow rate (MFR) measured at a temperature of 190°C under a load of 2.16 kg of 10 g / 10 min or more, and a kneading step of kneading the resulting blend at a temperature equal to or higher than the melting point of the (B) polyolefin. Invention [9]: (A2) A rubber component comprising an isoprene-based rubber and a butadiene rubber, wherein, when the total amount of the rubber component is 100 parts by mass, the proportion of the butadiene rubber is 15 parts by mass or less, and (D) a nitrogen adsorption specific surface area (N 2 SA) is 40 to 130 m 2A rubber composition for a heavy-duty tire undertread, comprising 45 parts by mass or less of a filler consisting of carbon black and / or silica having a viscosity of 1000 psi / g, and 0.1 to 20 parts by mass of (C) a high-flow random polypropylene having a melting point of 110°C or more and 155°C or less and a melt mass-flow rate (MFR) of more than 6 g / 10 min measured at a temperature of 230°C under a load of 2.16 kg. Invention
[10] : The rubber composition for a heavy-duty tire undertread according to Invention 9, wherein the (C) high-flow random polypropylene has a hydrolytic condensation silyl group in its molecule and contains 5 parts by mass or more of the silica per 100 parts by mass of the (A) rubber component. Invention
[11] : The rubber composition for a heavy-duty tire undertread according to Invention 9 or 10, wherein the (C) high-flow random polypropylene is selected from a propylene-ethylene random copolymer, a propylene-1-butene random copolymer, and a propylene-ethylene-1-butene random copolymer. Invention
[12] : A rubber composition according to any one of Inventions 9 to 11, characterized in that the melting point of the (C) high fluidity random polypropylene is 130°C or higher and 150°C or lower. Invention
[13] : A rubber composition according to any one of Inventions 9 to 12, characterized in that the (C) high fluidity random polypropylene has a melt mass flow rate (MFR) of 8 g / 10 min or higher, measured at a temperature of 230°C and a load of 2.16 kg. Invention
[14] : A tire using the rubber composition according to any one of Inventions 1 to 7. Invention
[15] : A heavy-duty tire using the rubber composition according to any one of Inventions 9 to 13.
Claims
1. A rubber composition comprising, for every 100 parts by mass of rubber component (A) containing 50 parts by mass or more of diene rubber, (B) 1 to 200 parts by mass of a polyolefin having a melting point of 110°C or higher and 155°C or lower, and a melt mass flow rate (MFR) measured at 230°C under a load of 2.16 kg that exceeds 6 g / 10 min, or a melt mass flow rate (MFR) measured at 190°C under a load of 2.16 kg that is 10 g / 10 min or higher.
2. The rubber composition according to claim 1, wherein the diene rubber is at least one selected from the group consisting of natural rubber, synthetic isoprene rubber, butadiene rubber, styrene-butadiene copolymer rubber and acrylonitrile-butadiene copolymer rubber.
3. The rubber composition according to claim 1, further comprising 20 to 200 parts by mass of carbon black and / or silica per 100 parts by mass of the rubber component (A).
4. The rubber composition according to claim 1, characterized in that the polyolefin (B) is at least one selected from the group consisting of propylene-ethylene random copolymers, propylene-1-butene random copolymers, propylene-ethylene-1-butene random copolymers, low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and high-density polyethylene (HDPE).
5. The rubber composition according to claim 1, characterized in that the melting point of the polyolefin (B) is 130°C or higher and 150°C or lower.
6. The rubber composition according to claim 1, characterized in that the (B) polyolefin has a melt mass flow rate (MFR) of 8 g / 10 min or more measured at a temperature of 230°C and a load of 2.16 kg, or a melt mass flow rate (MFR) of 20 g / 10 min or more measured at a temperature of 190°C and a load of 2.16 kg.
7. The rubber composition according to claim 1, wherein the polyolefin (B) is selected from the group consisting of propylene-ethylene random copolymers, propylene-1-butene random copolymers and propylene-ethylene-1-butene random copolymers.
8. A method for producing a rubber composition, comprising: a compounding step of compounding 1 to 200 parts by mass of (B) a polyolefin having a melting point of 110°C or higher and 155°C or lower, and having a melt mass flow rate (MFR) measured at a temperature of 230°C under a load of 2.16 kg that exceeds 6 g / 10 min, or a melt mass flow rate (MFR) measured at a temperature of 190°C under a load of 2.16 kg that is 10 g / 10 min or higher, with respect to 100 parts by mass of a rubber component containing 50 parts by mass or more of (A) a diene rubber; and a kneading step of kneading the resulting compound under conditions at or above the melting point of said (B) polyolefin.
9. (A2) A rubber component consisting of an isoprene-based rubber and a butadiene rubber, in which the ratio of the butadiene rubber is 15 parts by mass or less when the total amount of the rubber components is 100 parts by mass, (D) a nitrogen adsorption specific surface area (N 2 SA) is 40 to 130m 2 and (C) 0.1 to 20 parts by mass of a high-flow random polypropylene having a melting point of 110°C or more and 155°C or less and a melt mass-flow rate (MFR) of more than 6 g / 10 min measured at a temperature of 230°C and a load of 2.16 kg.
10. A rubber composition for the undertread of a heavy-load tire as described in claim 9, characterized in that the (C) high-fluidity random polypropylene has a hydrolytic condensable silyl group in its molecule and contains 5 parts by mass or more of the silica per 100 parts by mass of the (A2) rubber component.
11. The rubber composition for undertread of a tire for heavy loads according to claim 9, wherein the high flow random polypropylene (C) is selected from the group consisting of propylene-ethylene random copolymers, propylene-1-butene random copolymers and propylene-ethylene-1-butene random copolymers.
12. The rubber composition according to claim 9, characterized in that the melting point of the (C) high fluidity random polypropylene is 130°C or higher and 150°C or lower.
13. The rubber composition according to claim 9, characterized in that the melt mass flow rate (MFR) of the (C) high fluidity random polypropylene measured at a temperature of 230°C and a load of 2.16 kg is 8 g / 10 min or more.
14. A tire using the rubber composition according to claim 1.
15. A heavy duty tire using the rubber composition according to claim 9.
Citation Information
Patent Citations
Rubber composition, method for producing the same, and pneumatic tire
JP2017115029A
Rubber composition and tire prepared therewith
JP2018178034A
Rubber-reinforcing fiber, rubber-fiber composite, and pneumatic tire using same
WO2017065305A1