Near-infrared absorbing composition, near-infrared absorbing cured film, and optical member
The near-infrared absorbing composition, featuring a copper phosphonate complex and specific additives, addresses stability and resistance issues in solid-state image sensors by enhancing storage stability and heat and humidity resistance, resulting in durable and reliable near-infrared absorbing films and optical members.
Patent Information
- Application Number
- PCT/JP2024/015694
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2024-04-22
- Publication Date
- 2024-11-21
AI Technical Summary
Existing near-infrared absorbing compositions for solid-state image sensors face challenges with storage stability and heat and humidity resistance, particularly in forming cured films that maintain performance over time.
A near-infrared absorbing composition comprising a copper phosphonate complex, a specific phosphoric acid ester, a titanium compound, and a silicon compound, along with a solvent, which balances dispersibility and crosslinking effects to enhance storage stability and heat and humidity resistance.
The composition forms a cured film with improved storage stability and heat and humidity resistance, ensuring consistent performance and longevity of the near-infrared absorbing films and optical members.
Smart Images

Figure JP2024015694_21112024_PF_FP_ABST
Abstract
Description
Near-infrared absorbing composition, near-infrared absorbing cured film, and optical component
[0001] The present invention relates to a near-infrared absorbing composition, a near-infrared absorbing cured film, and an optical component.
[0002] In recent years, solid-state imaging devices for color imaging have been used in video cameras, digital still cameras, mobile phones with camera functions, and the like. Examples of solid-state imaging devices include CCD (Charge Coupled Device) and CMOS (Complementary Metal Oxide Semiconductor) image sensors. These solid-state imaging devices use silicon photodiodes in their light-receiving sections that are sensitive to light in the near-infrared wavelength region. Therefore, solid-state imaging devices require luminosity correction. For luminosity correction, a near-infrared cut filter, which is an optical filter, is often used.
[0003] These near-infrared cut filters can be broadly divided into absorption and reflection types. Conventionally, reflection types have been used, which utilize light reflection by a dielectric multilayer film to block infrared or ultraviolet rays.
[0004] However, the reflective layer used in reflective types is susceptible to dependence on the angle of incidence. For this reason, total absorption types have been mainly considered in recent years. In recent years, optical filters using films containing light-absorbing agents have been attracting attention.
[0005] Optical filters using a film containing a light absorber are also advantageous in terms of miniaturizing and thinning imaging devices. When light is incident on the optical filter, the transmittance characteristics of the optical filter are less affected by the angle of incidence. Therefore, by using the optical filter, good images with little change in color can be obtained during shooting, even when light is incident at an oblique angle.
[0006] In recent years, near-infrared absorbing compositions using copper phosphonate complexes have been disclosed as materials for producing such near-infrared cut filters.
[0007] For example, Patent Document 1 discloses a near-infrared absorbing composition containing a near-infrared absorber containing a phosphonic acid compound and copper ions, and a Ti compound. However, the composition disclosed in Patent Document 1 leaves room for improvement in terms of storage stability and moist heat resistance of the cured film.
[0008] Patent Document 2 discloses an infrared absorbing composition containing a light absorber and an alkoxysilane monomer. The light absorber is formed from a phosphonic acid having a phenyl group or a halogenated phenyl group and copper ions. However, the composition disclosed in Patent Document 2 has problems with storage stability and the moist heat resistance of the cured film.
[0009] International Publication No. 2019-221061 International Publication No. 2018-173386
[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a near-infrared absorbing composition capable of forming a cured film having excellent storage stability and excellent moist heat resistance, and a near-infrared absorbing cured film and an optical component using the same.
[0011] The present inventors have investigated the causes of the above problems in order to solve them. As a result, the present inventors have found that the above problems can be solved by incorporating a specific copper phosphonate complex, a specific phosphate ester, a specific Ti compound, a specific Si compound, and a specific solvent, and have arrived at the present invention. That is, the above problems of the present invention are solved by the following means.
[0012] 1. A near-infrared absorbing composition comprising the following components (A) to (E):
[0013] Component (A): A copper complex coordinated with a compound having a structure represented by the following general formula (I):
[0014]
[0015] [In general formula (I), R 1 is an alkyl group having 1 to 20 carbon atoms, which may further have a substituent.
[0016] Component (B): A compound having a structure represented by the following general formula (II):
[0017]
[0018] [In general formula (II), R 2 is an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, and may further have a substituent. 21 ~R 24 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 21 ~R 24 represents the average number of partial structural units added, each of which is a hydrogen atom, and is in the range of 0 to 19. 21 ~R 24 represents the average number of partial structural units added, at least one of which is an alkyl group having 1 to 4 carbon atoms, and is within the range of 0 to 19. m+n represents the total number of m and n, and is within the range of 1 to 20. Z represents a structural unit selected from the following formulae (Z-1) and (Z-2).
[0019]
[0020] Component (C): A compound having a structure represented by the following general formula (III) or (IV): General formula (III) (R 3 O) 4-m Ti(O-R 4 -OH) m General formula (IV) (R 3 O) 4-m Ti(OCOR 5 ) m [In general formulas (III) and (IV), m is an integer of 1 to 4. 4 is an alkylene group having 1 to 30 carbon atoms, which may further have a substituent. 3 and R 5 are each independently an alkyl group having 1 to 30 carbon atoms, and may further have a substituent.
[0021] Component (D): A compound having a structure represented by the following general formula (V): General formula (V) R 6 - (CH 2 ) m -Si(CH 3 ) n - (OR 7 )3-n [In general formula (V), R 6 R is a vinyl group, a styryl group, an acryloxy group, a methacryloxy group, a mercapto group, an epoxy group, an epoxycyclohexyl group, or a glycidoxy group, and may further have a substituent. 7 is an alkyl group having 1 to 3 carbon atoms, m is an integer of 0 to 8, and n is 0 or 1.
[0022] Component (E): polar term δ of Hansen solubility parameter P The value of is in the range of 3 to 6, and the hydrogen bond term δ H A solvent having a value in the range of 3 to 6.
[0023] 2. The compound having the structure represented by the general formula (II) has at least one partial structure satisfying the following condition (i) and at least one partial structure satisfying the following condition (ii), and the condition (i): R 21 ~R 24 are all hydrogen atoms. Condition (ii): R 21 ~R 24 2. The near-infrared absorbing composition according to item 1, wherein at least one of the groups represented by the general formula (II) is an alkyl group having a carbon number of 1 to 4. 3. The near-infrared absorbing composition according to item 1, wherein m and n in the general formula (II) are each within the range of 1 to 19.
[0024] 3. The near-infrared absorbing composition according to item 1, wherein the content of the component (C) is within a range of 1 to 30 mass % relative to the component (A).
[0025] 4. The near-infrared absorbing composition according to item 1, wherein the content of the component (D) is within a range of 1 to 30 mass % relative to the component (A).
[0026] 5. R in the general formula (V) 6 is an acryloxy group or a methacryloxy group.
[0027] 6. The near-infrared absorbing composition according to item 1, wherein the component (E) is cyclopentyl methyl ether or 4-methyltetrahydropyran.
[0028] 7. A near-infrared absorbing cured film comprising a cured product of the near-infrared absorbing composition according to any one of items 1 to 6.
[0029] 8. An optical member comprising a cured product of the near-infrared absorbing composition according to any one of items 1 to 6.
[0030] The above-described means of the present invention can provide a near-infrared absorbing composition capable of forming a cured film having excellent storage stability and excellent resistance to moist heat, as well as a near-infrared absorbing cured film and an optical component using the same.
[0031] The mechanism by which the effects of the present invention are manifested or the mechanism of action is not clear, but is presumed to be as follows.
[0032] In a composition containing a copper phosphonate complex and a phosphate ester, the phosphate ester acts as a dispersant for the copper phosphonate complex. If a Ti compound is simply added to this, the storage stability of the near-infrared absorbing composition deteriorates. This is presumably due to the crosslinking action of the Ti compound.
[0033] The near-infrared absorbing composition of the present invention further contains a Si compound and a specific solvent. This suppresses the crosslinking action of the Ti compound, improving the storage stability of the near-infrared absorbing composition. Furthermore, when a cured film is formed, the solvent is removed, thereby allowing the suppressed crosslinking action of the Ti compound to be expressed. Furthermore, at this time, a synergistic effect of the crosslinking action between the Ti compound and the Si compound is also expressed. These effects improve the moist heat resistance of the cured film.
[0034] Schematic cross-sectional view showing an example of the configuration of a near-infrared cut filter. Schematic cross-sectional view showing an example of the configuration of an image sensor for a solid-state imaging device. Schematic cross-sectional view showing an example of the configuration of a camera module.
[0035] The near-infrared absorbing composition of the present invention is characterized by containing the above-mentioned components (A) to (E). This characteristic is a technical characteristic common to or corresponding to the following embodiments.
[0036] In an embodiment of the present invention, it is preferable that the compound having the structure represented by the general formula (II) has at least one partial structure that satisfies the following condition (i) and at least one partial structure that satisfies the following condition (ii), and that m and n in the general formula (II) are each within the range of 1 to 19. This further enhances the effect of the component (B) as a dispersant. Condition (i): R 21 ~R 24 are all hydrogen atoms. Condition (ii): R 21 ~R 24 At least one of the groups is an alkyl group having 1 to 4 carbon atoms.
[0037] In an embodiment of the present invention, the content of the component (C) is preferably within a range of 1 to 30 mass % relative to the component (A), thereby achieving a good balance between the storage stability of the near-infrared absorbing composition and the moist heat resistance of the near-infrared absorbing cured film.
[0038] In an embodiment of the present invention, the content of the component (D) is preferably within a range of 1 to 30 mass % relative to the component (A), thereby achieving a good balance between the storage stability of the near-infrared absorbing composition and the moist heat resistance of the near-infrared absorbing cured film.
[0039] In an embodiment of the present invention, R 6 is preferably an acryloxy group or a methacryloxy group, which further improves the storage stability of the near-infrared absorbing composition and the moist heat resistance of the cured film.
[0040] In an embodiment of the present invention, the component (E) is preferably cyclopentyl methyl ether or 4-methyltetrahydropyran. These can disperse the near-infrared absorbing composition in an appropriate state. This further improves the storage stability of the near-infrared absorbing composition.
[0041] The near-infrared absorbing cured film of the present invention is characterized by containing a cured product of the near-infrared absorbing composition of the present invention.
[0042] The optical member of the present invention is characterized by containing a cured product of the near-infrared absorbing composition of the present invention.
[0043] The present invention, its components, and modes and aspects for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values before and after it are included as lower and upper limits.
[0044] [Outline of Near-Infrared Absorbing Composition of the Present Invention] The near-infrared absorbing composition of the present invention is characterized by containing the following components (A) to (E):
[0045] [Component (A)] The component (A) is a copper complex coordinated with a compound having a structure represented by the following general formula (I). The compound having the structure represented by the following general formula (I) is a phosphonic acid compound. That is, the component (A) is a phosphonic acid copper complex. The component (A) is a near-infrared absorber.
[0046]
[0047] [In general formula (I), R 1 is an alkyl group having 1 to 20 carbon atoms, which may further have a substituent.
[0048] R 1 Examples of the substituent that may be possessed by include the following: alkyl groups (for example, methyl groups, ethyl groups, trifluoromethyl groups, isopropyl groups, etc.), alkoxy groups (for example, methoxy groups, ethoxy groups, etc.), halogen atoms (for example, fluorine atoms, etc.), cyano groups, nitro groups, dialkylamino groups (for example, dimethylamino groups, etc.), and trialkylsilyl groups (for example, trimethylsilyl groups, etc.).
[0049] R 1 is preferably an alkyl group having 1 to 20 carbon atoms, in terms of good resistance to humidity and heat and near-infrared absorbing properties. 1 It is more preferable that the alkyl group has 1 to 4 carbon atoms, since this can achieve both near-infrared absorption and visible light transmittance.
[0050] R 1Examples of phosphonic acids in which is an alkyl group having 1 to 20 carbon atoms include the following: methylphosphonic acid, ethylphosphonic acid, propylphosphonic acid, butylphosphonic acid, pentylphosphonic acid, hexylphosphonic acid, heptylphosphonic acid, octylphosphonic acid, nonylphosphonic acid, and decylphosphonic acid.
[0051] As the compound having the structure represented by general formula (I) in component (A), propylphosphonic acid and butylphosphonic acid are particularly preferred.
[0052] The near-infrared absorbing composition may contain, as the component (A), a plurality of copper complexes in which phosphonic acids with different alkyl groups are coordinated.
[0053] As the compound having the structure represented by general formula (I), commercially available products can be used.
[0054] The copper complex coordinated with a compound having a structure represented by general formula (I) may be a copper complex coordinated with at least one compound having a structure represented by general formula (I). The copper complex may also be a copper complex coordinated with a compound other than the compound having a structure represented by general formula (I).
[0055] The structure of a copper complex coordinated with a compound having a structure represented by general formula (I) is represented, for example, by the following general formula (IC).
[0056]
[0057] R in the following general formula (IC) 1 represents R in general formula (I). 1 is the same as
[0058] Among the hydroxy groups possessed by phosphonic acid, the hydroxy group directly bonded to the phosphorus atom is called a "reactive hydroxy group." In general formula (IC), two reactive hydroxy groups of one phosphonic acid react with the same copper ion to form a copper complex. However, the form of the phosphonic acid copper complex is not limited to this.
[0059] The near-infrared absorbing composition may contain one or more types of component (A).
[0060] Phosphonic acid can be synthesized by referring to known methods described in, for example, JP-A-2016-94512 and JP-A-2016-124903.
[0061] In the near-infrared absorbing composition, the phosphonic acid copper complex is mainly in the form of fine particles.
[0062] The content of component (A) in the near-infrared absorbing composition is preferably in the range of 3 to 40% by mass, more preferably in the range of 10 to 30% by mass. When the content is 3% by mass or more, a thick cured film is easily formed. When the content is 10% by mass or more, a thick cured film is more easily formed. When the content is 40% by mass or less, particle aggregation and an increase in viscosity of the composition can be suppressed, and the storage stability of the composition is improved. When the content is 30% by mass or less, the storage stability of the composition is further improved.
[0063] From the viewpoint of spectral characteristics, it is preferable that the copper complex fine particles are uniformly dispersed when a cured film is formed. To this end, it is preferable that the particle size of the copper complex fine particles in the near-infrared absorbing composition (dispersion liquid) is small. The average particle size of the copper complex fine particles in the near-infrared absorbing composition is preferably 200 nm or less, more preferably 100 nm or less, and even more preferably 80 nm or less. The average particle size can be measured by a dynamic light scattering method using an ELSZ-1000ZS manufactured by Otsuka Electronics Co., Ltd.
[0064] [Component (B)] Component (B) is a phosphate ester compound having a structure represented by the following general formula (II). Component (B) exerts the effect of forming nano-sized small particle diameters when a copper phosphonate complex is formed. Component (B) also contributes to maintaining the dispersibility of the copper phosphonate complex particles in a medium.
[0065]
[0066] [In general formula (II), R 2 is an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, and may further have a substituent. 21 ~R 24each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 21 ~R 24 represents the average number of partial structural units added, each of which is a hydrogen atom, and is in the range of 0 to 19. 21 ~R 24 represents the average number of partial structural units added, at least one of which is an alkyl group having 1 to 4 carbon atoms, and is within the range of 0 to 19. m+n represents the total number of m and n, and is within the range of 1 to 20. Z represents a structural unit selected from the following formulae (Z-1) and (Z-2).
[0067]
[0068] R 21 ~R 24 When all of are hydrogen atoms, the partial structure in the parentheses in the formula is called an "ethylene oxide structure." In the formula, m is the average number of ethylene oxide structures added.
[0069] R 21 ~R 24 The partial structure in the parentheses in the formula, in which at least one of the above is an alkyl group having 1 to 4 carbon atoms and the others are hydrogen atoms, is called an "alkyl-substituted ethylene oxide structure." In the formula, n is the average number of alkyl-substituted ethylene oxide structures added.
[0070] In the compound having the structure represented by general formula (II), either m or n is equal to or greater than 1. This gives the compound a high ability to form a complex with copper, and a high effect as a dispersant.
[0071] The compound having the structure represented by general formula (II) preferably has at least one partial structure that satisfies the following condition (i) and at least one partial structure that satisfies the following condition (ii). This enhances the effect of the component (B) as a dispersant. Condition (i): R 21 ~R 24 are all hydrogen atoms. Condition (ii): R 21 ~R 24 At least one of the groups is an alkyl group having 1 to 4 carbon atoms.
[0072] In general formula (II), m and n are preferably each within the range of 1 to 19. This compound has a large number of isomers due to the combination of an ethylene oxide structure and an alkyl-substituted ethylene oxide structure. This increases the entropy, making this compound highly effective as a dispersant. In addition, this compound has a substituent (R 21 ~R 24 The effect of steric hindrance of the ethylene oxide structure and the alkyl-substituted ethylene oxide structure is suppressed, and the copper complex can be finely dispersed. Therefore, the effects of the ethylene oxide structure and the alkyl-substituted ethylene oxide structure are exerted in a well-balanced manner. Therefore, the compound can improve the dispersibility and dispersion stability of the near-infrared absorbing composition.
[0073] In general formula (II), R 21 ~R 24 It is more preferable that at least one of the groups is a methyl group from the viewpoint of dispersibility of the copper complex.
[0074] In general formula (II), R 2 is preferably an alkyl group having 6 to 16 carbon atoms from the viewpoint of dispersibility of the copper complex and resistance to humidity and heat.
[0075] The compound having the structure represented by general formula (II) is a diester when Z is formula (Z-1), and a monoester when Z is formula (Z-2).
[0076] The mixing ratio of the diester and the monoester is preferably such that the molar ratio of the monoester to the total amount of the diester and the monoester is within the range of 20 to 95%.
[0077] Specific examples of compounds having a structure represented by general formula (II) are shown in the following Tables 1 to 5. The compounds having a structure represented by general formula (II) according to the present invention are not limited to these.
[0078] In Tables IV, there are exemplary compounds in which both (Z-1) and (Z-2) are listed in the "Structure" column for "Z." Such exemplary compounds are mixtures of compounds in which Z is represented by formula (Z-1) and compounds in which Z is represented by formula (Z-2).
[0079]
[0080]
[0081]
[0082]
[0083]
[0084] Exemplary Compound II-1 will be specifically described. Exemplary Compound II-1 is a mixture of a compound (diester) in which Z is represented by formula (Z-1) and a compound (monoester) in which Z is represented by formula (Z-2).
[0085] A compound (monoester) in which Z is formula (Z-2) is represented, for example, by the structure of the following exemplary compound II-1-1. A compound (diester) in which Z is formula (Z-1) is represented, for example, by the structure of the following exemplary compound II-1-2.
[0086]
[0087] In Exemplary Compound II-1, the molar ratio of the compound (monoester) in which Z is represented by Formula (Z-2) is 50%. That is, Exemplary Compound II-1 contains Exemplary Compound II-1-1 and Exemplary Compound II-1-2 in equimolar amounts.
[0088] m and n are the average addition numbers. Therefore, even in the case of Exemplified Compound 1 in which m is 5 and n is 5, the number of ethylene oxide structures in one molecule is not necessarily 5, and the number of alkyl-substituted ethylene oxide structures is not necessarily 5.
[0089] In the general formula (II), the order of the ethylene oxide structure and the alkyl-substituted ethylene oxide structure is not particularly limited. Compounds in which the respective structures are randomly arranged are also included in the compounds having the structure represented by the general formula (II). The order of the ethylene oxide structure and the alkyl-substituted ethylene oxide structure can be arbitrarily changed depending on the synthesis method.
[0090] Compounds having a structure represented by general formula (II) can be synthesized by referring to the methods described in the following documents, for example: JP 2005-255608 A JP 2015-000396 A JP 2015-000970 A JP 2015-178072 A JP 2015-178073 A Japanese Patent No. 4422866 A International Publication No. 2019-221061
[0091] The near-infrared absorbing composition may contain one or more types of component (B).
[0092] The content of the component (B) is preferably within a range of 40 to 80 mass % relative to the mass of the component (A), and more preferably within a range of 50 to 70 mass %, which allows for a better balance between the storage stability of the dispersible near-infrared absorbing composition of the near-infrared absorbing composition and the moist heat resistance of the cured film.
[0093] When the proportion of component (B) is low, the proportion of component (A), which is effective in absorbing near-infrared rays, becomes large, resulting in good near-infrared absorption. Furthermore, it has been found that the phosphate ester compound of component (B) causes cloudiness in high-temperature, high-humidity environments. Therefore, by reducing the proportion of component (B), the moist heat resistance of the cured film improves. However, a certain amount of the phosphate ester compound is necessary to maintain the dispersibility of the copper complex microparticles.
[0094] [Component (C)] Component (C) is a compound having a structure represented by the following general formula (III) or (IV), and is a Ti compound.
[0095] General formula (III) (R 3 O) 4-m Ti(O-R 4 -OH) m General formula (IV) (R 3 O) 4-m Ti(OCOR 5 ) m
[0096] [In general formulas (III) and (IV), m is an integer of 1 to 4. 4 is an alkylene group having 1 to 30 carbon atoms, which may further have a substituent. 3 and R5 are each independently an alkyl group having 1 to 30 carbon atoms, and may further have a substituent.
[0097] R 3 and R 5 The alkyl group having 1 to 30 carbon atoms represented by the formula (I) may be linear or branched.
[0098] Examples of alkyl groups having 1 to 30 carbon atoms include the following: methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, tert-butyl group, n-hexyl group, 2-ethylhexyl group, n-octyl group, 2-butyloctyl group, 2-hexyloctyl group, n-decyl group, 2-hexyldecyl group, n-dodecyl group, n-stearyl group, and isostearyl group.
[0099] R 3 and R 5 is preferably an alkyl group having 6 to 20 carbon atoms.
[0100] R 4 The alkylene group having 1 to 30 carbon atoms represented by the formula (I) may be linear or branched.
[0101] Examples of alkylene groups having 1 to 30 carbon atoms include the following: methylene group, ethylene group, n-propylene group, isopropylene group, n-butylene group, tert-butylene group, n-hexylene group, 2-ethylhexylene group, n-octylene group, 2-butyloctylene group, 2-hexyloctylene group, n-decylene group, 2-hexyldecylene group, n-dodecylene group, n-stearylene group, and isostearylene group.
[0102] R 4 Preferably, it is an alkylene group having 6 to 20 carbon atoms.
[0103] R 3 and R 5Examples of the substituents that each of may have include the following: alkyl groups (for example, methyl groups, ethyl groups, trifluoromethyl groups, isopropyl groups, etc.) alkoxy groups (for example, methoxy groups, ethoxy groups, etc.) halogen atoms (for example, fluorine atoms, etc.) cyano groups nitro groups dialkylamino groups (for example, dimethylamino groups, etc.) trialkylsilyl groups (for example, trimethylsilyl groups, etc.) triarylsilyl groups (for example, triphenylsilyl groups, etc.) triheteroarylsilyl groups (for example, tripyridylsilyl groups, etc.) benzyl groups aryl groups (for example, phenyl groups, etc.) heteroaryl groups (for example, pyridyl groups, carbazolyl groups, etc.) fused ring groups (for example, 9,9'-dimethylfluorene, carbazole, dibenzofuran, etc.)
[0104] The compound having the structure represented by general formula (III) is preferably a compound that forms a chelate structure. Examples of such compounds include the following titanium chelate compounds: titanium ethylene dioleate titanium propylene dioleate titanium butylene dioleate titanium pentylene dioleate titanium hexylene dioleate titanium-2-ethyl-1,3-hexylene dioleate titanium octylene dioleate
[0105] Specific examples of the compound having the structure represented by general formula (III) are shown below: The compound having the structure represented by general formula (III) according to the present invention is not limited to these.
[0106]
[0107]
[0108] Compounds having the structure represented by general formula (III) are also available as commercially available products, such as "Orgatix TC245" (manufactured by Matsumoto Fine Chemical Co., Ltd.).
[0109] The compound having the structure represented by general formula (IV) is preferably a compound that forms an acylate structure. Examples of such compounds include the following titanium acylate compounds: titanium caprylate, titanium caprate, titanium laurate, titanium myristylates, titanium palmitates, titanium stearate, and titanium isostearate.
[0110] Specific examples of the compound having the structure represented by general formula (IV) are shown below: The compound having the structure represented by general formula (IV) according to the present invention is not limited to these.
[0111]
[0112] Compounds having the structure represented by general formula (IV) are also available as commercially available products, such as "Orgatix TC-800" (manufactured by Matsumoto Fine Chemical Co., Ltd.).
[0113] The compound having the structure represented by general formula (III) or general formula (IV) can be obtained by referring to the synthesis method described in, for example, JP-A-2011-219704.
[0114] The near-infrared absorbing composition may contain one or more types of component (C).
[0115] The content of the component (C) is preferably in the range of 1 to 30% by mass, more preferably in the range of 3 to 20% by mass, relative to the component (A). This results in a good balance between the storage stability of the near-infrared absorbing composition and the moist heat resistance of the near-infrared absorbing cured film. When the content of the component (C) is a certain amount or more, the moist heat resistance of the cured film tends to be good. When the content of the component (C) is a certain amount or less, the storage stability of the near-infrared absorbing composition tends to be good.
[0116] [Component (D)] Component (D) is a compound having a structure represented by the following general formula (V), and is a Si compound. The compound having a structure represented by general formula (V) suppresses the crosslinking action of the Ti compound in the near-infrared absorbing composition, improving the storage stability of the near-infrared absorbing composition. Furthermore, when a cured film is formed, a synergistic effect of the crosslinking action between the Ti compound and the Si compound is exhibited. Therefore, when a Ti compound and a Si compound are used in combination, the moist heat resistance of the cured film is improved compared to when a Ti compound is used alone.
[0117] General formula (V) R 6 - (CH 2 ) m -Si(CH 3 ) n - (OR 7 ) 3-n
[0118] [In general formula (V), R 6 R is a vinyl group, a styryl group, an acryloxy group, a methacryloxy group, a mercapto group, an epoxy group, an epoxycyclohexyl group, or a glycidoxy group, and may further have a substituent. 7 is an alkyl group having 1 to 3 carbon atoms, m is an integer of 0 to 8, and n is 0 or 1.
[0119] R 6 is preferably an acryloxy group or a methacryloxy group, which further improves the storage stability of the near-infrared absorbing composition and the moist heat resistance of the cured film.
[0120] Specific examples of the compound having the structure represented by general formula (V) are shown below: The compound having the structure represented by general formula (V) according to the present invention is not limited to these.
[0121]
[0122]
[0123] Compounds having a structure represented by general formula (V) are also available as commercially available products. Examples of commercially available products include the following: KBM-1003, KBE-1003, KBM-1083, KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-4803, KBM-1403, KBM-502, KBM-503, KBE-502, KBE-503, KBM-5803, KBM-5103, KBM-802, and KBM-803 (all manufactured by Shin-Etsu Chemical Co., Ltd.).
[0124] The near-infrared absorbing composition may contain one or more types of component (D).
[0125] The compound having the structure represented by general formula (V) can be obtained by referring to the synthesis method described in, for example, JP-A-9-157280.
[0126] The content of the component (D) is preferably in the range of 1 to 30% by mass, more preferably in the range of 3 to 20% by mass, relative to the component (A). This results in a good balance between the storage stability of the near-infrared absorbing composition and the moist heat resistance of the near-infrared absorbing cured film. When the content of the component (D) is a certain amount or less, the moist heat resistance of the cured film tends to be good. When the content of the component (D) is a certain amount or more, the storage stability of the near-infrared absorbing composition tends to be good.
[0127] [Component (E)] Component (E) is a component having a polarity term δ of the Hansen solubility parameter. P The value of is in the range of 3 to 6, and the hydrogen bond term δ H The solvent has a value of 3 to 6.
[0128] The Hansen solubility parameter (HSP) is a value that indicates the solubility of a substance. The HSP is a solubility parameter introduced by Hildebrand, expressed as a function of the dispersion term δ D , polarity term δ P , hydrogen bond term δ H It is divided into three components and represented in three-dimensional space.
[0129] Dispersion term δ Drepresents the energy derived from dispersion forces. P represents the energy derived from polar forces. The hydrogen bond term δ H represents the energy derived from hydrogen bonding forces.
[0130] In the present invention, δ D , δ P and δ H The unit is MPa 1/2 is.
[0131] The definition and calculation method of HSP are described in the following literature: "Hansen Solubility Parameters: A User's Handbook" by Charles M. Hansen (CRC Press, 2007).
[0132] Compounds with similar HSP vectors can be judged to have high solubility. The similarity of the vectors can be determined by the HSP distance.
[0133] HSP can be an indicator not only of solubility but also of the degree to which a substance is likely to exist in another substance, i.e., dispersibility.
[0134] The HSP of the various solvents used in the present invention is a value determined using the following commercially available computer software: "Hansen Solubility Parameters in Practice (HSPiP)"
[0135] There are no particular limitations on component (E) other than the requirements for HSP described above, but it is preferably an ether solvent.
[0136] From the viewpoint of dispersibility, the solvent (E) preferably has a cycloalkyl group or a cycloether group.
[0137] From the viewpoint of dispersibility, the cycloalkyl group is preferably a cyclopentyl group or a cyclohexyl group, and the cycloether group is preferably a tetrahydrofuran group or a tetrahydropyran group.
[0138] The term "dispersibility" refers to the performance or function as a dispersion medium that disperses components constituting the near-infrared absorbing composition in an appropriate state in the near-infrared absorbing composition.
[0139] The term "storage stability" refers to the performance or function of maintaining the dispersion state of various components constituting the near-infrared absorbing composition in an appropriate state without or with little change due to the passage of time, changes in environmental conditions, etc.
[0140] The component (E) is more preferably cyclopentyl methyl ether or 4-methyltetrahydropyran, and particularly preferably cyclopentyl methyl ether. These can disperse the near-infrared absorbing composition in an appropriate state. This further improves the storage stability of the near-infrared absorbing composition.
[0141] Specific examples and comparative examples of the solvent (E) are shown in Table VI, but the solvent according to the present invention is not limited to these.
[0142]
[0143] The boiling point of the solvent (E) is preferably within the range of 80 to 150°C from the viewpoint of preventing cracks during the formation of a cured film.
[0144] The near-infrared absorbing composition may contain one or more types of component (E).
[0145] From the viewpoints of dispersibility and storage stability, the content of the component (E) is more preferably within a range of 50 to 95 mass % based on the total amount of the near-infrared absorbing composition.
[0146] Other solvents may be used in combination as long as they do not impair the effects of the present invention. Preferred examples of other solvents include aliphatic hydrocarbon solvents and ether solvents.
[0147] [Near-infrared absorbing cured film] The near-infrared absorbing cured film of the present invention is characterized by containing a cured product of a near-infrared absorbing composition.
[0148] The near-infrared absorbing cured film of the present invention is suitable for use in, for example, CCDs, CMOSs, or other light-receiving elements, as constituting the following: - Visibility correction members - Photometric members - Heat ray absorbing members - Composite optical filters - Lens members (eyeglasses, sunglasses, goggles, optical systems, optical waveguides) - Fiber members (optical fibers) - Noise-cutting members - Display covers or display filters such as plasma display front panels - Projector front panels - Light source heat ray-cutting members - Color tone correction members - Illumination brightness adjustment members - Optical elements (light amplifiers, wavelength conversion elements, etc.) - Faraday elements - Optical communication functional devices such as isolators - Optical disc elements
[0149] The near-infrared absorbing cured film can be produced, for example, by the following procedure. First, a resin material is dissolved in the near-infrared absorbing composition (dispersion) of the present invention to prepare a coating liquid for forming the near-infrared absorbing cured film. The coating liquid is applied onto a substrate by a wet coating method. The coating film is cured by performing a predetermined heat treatment or the like.
[0150] Examples of wet coating methods include the following: Drop casting method Dispenser method Spin coater method Slit spin coater method Slit coater method Screen printing method Applicator method
[0151] The thickness of the near-infrared absorbing cured film is preferably in the range of 10 to 500 μm, more preferably in the range of 10 to 300 μm.
[0152] The resin material preferably has optical transparency to visible light and near-infrared light, and is capable of dispersing fine particles of the near-infrared absorbing composition.
[0153] The component (A), which is a copper phosphonate complex, is a substance with relatively low polarity and disperses well in hydrophobic materials. Therefore, the resin material for forming the near-infrared absorbing film is preferably a resin material having a polysiloxane structure, or a resin material having an acrylic group, an epoxy group, or a phenyl group. Among these, resins having a polysiloxane structure are particularly preferred because they are resistant to thermal decomposition, have high optical transparency for visible light and near-infrared light, and are also highly heat-resistant.
[0154] Examples of resin materials having a polysiloxane structure include the following: KR-255, KR-300, KR-2621-1, KR-211, KR-311, KR-216, KR-212, and KR-251 (all manufactured by Shin-Etsu Chemical Co., Ltd.).
[0155] Examples of resin materials having epoxy groups include the following: KJC-X5 (manufactured by Shin-Etsu Chemical Co., Ltd.) EpiFine series (manufactured by KISCO Co., Ltd.)
[0156] As the resin material having an acrylic group, a (meth)acrylic acid ester monomer is preferred. Examples of the (meth)acrylic acid ester monomer include the following: - Alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate - Modified (meth)acrylates such as phenoxy (meth)acrylate - Polyfunctional (meth)acrylates such as trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate
[0157] A polymer (resin polymer) may be used as the resin material for forming the near-infrared absorbing film. Examples of the polymer (resin polymer) include the following: Polymers of (meth)acrylic acid ester compounds Polymers of aromatic vinyl compounds such as styrene, α-methylstyrene, methoxystyrene, and divinylbenzene Cycloolefin polymers (COP)
[0158] In this specification, the term "(meth)acrylic group" means both a "methacrylic group" and an "acrylic group."
[0159] The coating liquid for forming a near-infrared absorbing cured film may contain other additives to the extent that the intended effects of the present invention are not impaired. Examples of other additives include sensitizers, crosslinking agents, curing accelerators, polymerization initiators, fillers, thermal curing accelerators, thermal polymerization inhibitors, and plasticizers. The coating liquid may further contain other components such as auxiliary agents. Examples of auxiliary agents include conductive particles, fillers, antifoaming agents, flame retardants, leveling agents, release accelerators, antioxidants, fragrances, surface tension modifiers, chain transfer agents, and surface treatment agents. By appropriately adding these components to the coating liquid, the stability, film properties, and other properties of the near-infrared absorbing cured film can be adjusted.
[0160] [Spectral Properties of Near-Infrared Absorbing Composition (Dispersion)] The near-infrared absorbing composition preferably has an average spectral transmittance of 70% or more in the wavelength region of 450 to 600 nm, more preferably 80% or more, and even more preferably 90% or more. This is the value measured after diluting the near-infrared absorbing composition with a solvent so that the maximum spectral transmittance in the wavelength region of 850 to 1000 nm is 10%. This results in a good visible light transmittance of the cured film.
[0161] As a device for measuring the spectral transmittance, for example, a spectrophotometer V-570 manufactured by JASCO Corporation can be used.
[0162] [Spectral Properties of Near-Infrared Absorptive Cured Film] From the viewpoint of visible light transmittance, it is preferable that the near-infrared absorptive cured film has an average spectral transmittance of 80% or more in the wavelength region of 450 to 600 nm.
[0163] From the viewpoint of near-infrared absorbing properties, it is preferable that the average spectral transmittance of the near-infrared absorbing cured film in the wavelength region of 850 to 1000 nm is 10% or less.
[0164] From the viewpoint of near-infrared absorbing properties, it is preferable that the near-infrared absorbing cured film has an average spectral transmittance of 1% or less in the wavelength region of 850 to 1080 nm.
[0165] The cutoff wavelength is the wavelength at which the spectral transmittance decreases with increasing wavelength from 600 to 700 nm, and the wavelength at which the spectral transmittance is 50% from 600 to 800 nm. The cutoff wavelength of the near-infrared absorbing cured film for light incident on the surface at an incident angle of 0° is preferably within the range of 600 to 750 nm. This improves the near-infrared absorbing properties of the cured film.
[0166] [Optical Member] The optical member of the present invention is characterized by containing a cured product of the near-infrared absorbing composition.
[0167] The near-infrared absorbing cured film of the present invention can be used as various optical members or parts.
[0168] Hereinafter, examples of application of the near-infrared absorbing composition or the near-infrared absorbing cured film as an optical member or part will be described.
[0169] (Near-infrared cut filter) The optical member of the present invention is, for example, a near-infrared cut filter. The near-infrared cut filter includes, for example, a transparent dielectric substrate and a near-infrared absorbing layer on at least one surface thereof. The near-infrared absorbing layer is a cured product of the near-infrared absorbing composition of the present invention.
[0170] It is preferable to further provide a dielectric multilayer film on at least one surface of the transparent dielectric substrate, since this allows more flexible adjustment of the spectral characteristics of the near-infrared cut filter.
[0171] The near-infrared absorbing layer and the dielectric multilayer film may be provided in contact with the transparent dielectric substrate, or may be provided via an intermediate layer.
[0172] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a near-infrared cut filter.
[0173] 1 includes a near-infrared absorbing layer 22 on one surface of a transparent dielectric substrate 21. The near-infrared absorbing filter 9 further includes a dielectric multilayer film 23 on the other surface of the transparent dielectric substrate 21.
[0174] The material of the transparent dielectric substrate is not particularly limited as long as the object of the present invention is achieved. The transparent dielectric substrate may be made of, for example, glass or optical resin. Examples of optical resin include polycarbonate (PC), polymethyl methacrylate (PMMA), cycloolefin polymer (COP), and silicone.
[0175] The thickness of the transparent dielectric substrate is preferably 0.01 to 1 mm.
[0176] The transparent dielectric substrate is required to transmit visible light, and therefore preferably has an average spectral transmittance of 80% or more in the wavelength range of 450 to 600 nm.
[0177] The near-infrared absorbing cured film of the present invention can be used as the near-infrared absorbing layer.
[0178] A near-infrared cut filter can be produced by forming a near-infrared absorbing cured film directly on a transparent dielectric substrate as a near-infrared absorbing layer.
[0179] A dielectric multilayer film is a film formed by laminating multiple layers made of materials with different refractive indices, and is used to control the transmittance of each wavelength of light. By combining a dielectric multilayer film with a near-infrared absorbing layer, the spectral characteristics of the near-infrared cut filter can be adjusted more freely.
[0180] The spectral characteristics of the dielectric multilayer film can be adjusted by the thickness and material of each layer. For example, the following dielectrics can be used as the material for each layer of the dielectric multilayer film: Titanium oxide, Silicon oxide, Aluminum oxide, Zirconium oxide, Tantalum pentoxide, Niobium pentoxide, Lanthanum oxide, Yttrium oxide, Zinc oxide, Zinc sulfide, Indium oxide, Silica, Alumina, Lanthanum fluoride, Magnesium fluoride, Sodium aluminum hexafluoride
[0181] A near-infrared cut filter having a dielectric multilayer film can be produced by laminating each dielectric layer on a transparent dielectric substrate by, for example, vacuum deposition, chemical vapor deposition, sputtering, etc.
[0182] A near-infrared cut filter having a dielectric multilayer film can also be produced by laminating a separately prepared dielectric multilayer film to a transparent dielectric substrate with an adhesive.
[0183] (Image Sensor for Solid-State Imaging Device) The near-infrared cut filter can be provided in an image sensor for a solid-state imaging device. The image sensor for a solid-state imaging device is a component mainly composed of a solid-state imaging device substrate equipped with a light receiving element. The image sensor for a solid-state imaging device may also include a planarizing layer, a glass substrate, etc. in addition to the near-infrared cut filter.
[0184] The image sensor for a solid-state imaging device may include a planarizing layer, a glass substrate, and the like in addition to the near-infrared cut filter.
[0185] FIG. 2 is a schematic cross-sectional view showing an example of the configuration of an image sensor for a solid-state imaging device.
[0186] 2 includes a solid-state imaging element substrate 10 having a light-receiving element on the light-receiving surface of a silicone substrate, a planarization layer 8 provided on the solid-state imaging element substrate 10, a near-infrared cut filter 9 provided on the planarization layer 8, and a glass substrate 3 (light-transmitting substrate) arranged above the near-infrared cut filter 9. Each member is bonded with an adhesive 2.
[0187] (Camera Module) The image sensor for a solid-state imaging device can be provided in a camera module. The camera module may be composed of an imaging lens, a lens holder, a light-shielding and electromagnetic shield, etc. in addition to the image sensor for a solid-state imaging device.
[0188] FIG. 3 is a schematic cross-sectional view showing an example of the configuration of a camera module.
[0189] The camera module 1 shown in Fig. 3 includes a solid-state imaging element image sensor similar to that shown in Fig. 2, a lens holder 5, an imaging lens 4, and a light-shielding and electromagnetic shield 6. As in Fig. 2, the solid-state imaging element image sensor is composed of a solid-state imaging element substrate 10, a planarizing layer 8, a near-infrared cut filter 9, and a glass substrate 3. The light-shielding and electromagnetic shield 6 is disposed so as to surround the periphery of the solid-state imaging element image sensor. Each component is bonded with an adhesive 7.
[0190] Furthermore, the camera module 1 is connected to a circuit board 12, which is a mounting board, via solder balls 11 (connecting material), which are connecting members.
[0191] In the camera module 1, incident light L from the outside passes through the imaging lens 4, the glass substrate 3, the near-infrared cut filter 9, and the planarization layer 8 in this order. Thereafter, the incident light L reaches the light receiving element of the solid-state imaging element substrate 10.
[0192] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the following examples, unless otherwise specified, operations were carried out at room temperature (25°C). In the following examples, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.
[0193] <Preparation of Near-Infrared Absorbing Composition> Near-infrared absorbing composition No. 1 was prepared according to the following method.
[0194] The following compounds and solvents were mixed in the amounts shown below, stirred for 3 hours, and filtered to remove insoluble matter, to prepare solution A: Copper (II) acetate monohydrate 18 g Tetrahydrofuran 800 g
[0195] A solution was prepared by dissolving a compound having a structure represented by the following general formula (II) in the following solvent in the following amounts. Solution A was added to this and stirred at room temperature for 30 minutes to prepare solution B. Exemplary compound II-66 10 g Tetrahydrofuran 70 g
[0196] A compound having a structure represented by the following general formula (I) was dissolved in the following solvent in the following amounts to prepare solution C: butylphosphonic acid 12 g tetrahydrofuran 70 g
[0197] Solution C was added to solution B while stirring, and the mixture was stirred at room temperature for 16 hours. The resulting solution was designated solution D.
[0198] The entire amount of Solution D and 300 g of methylcyclohexane were placed in a flask. This was heated to 50 to 100°C and subjected to a solvent removal and acetic acid removal treatment using a rotary evaporator. 300 g of cyclopentyl methyl ether was then added to this. The solvent removal operation was repeated three times using the rotary evaporator. In this way, the solvent was replaced with cyclopentyl methyl ether, and the concentration of component (A) was adjusted to 10% by mass. The solution obtained in this manner is designated Solution E.
[0199] A compound having a structure represented by the following general formula (III) and a compound having a structure represented by the following general formula (V) were dissolved in the following solvent in the following amounts. This was added to 100 g of Solution E and stirred at room temperature for 30 minutes to obtain near-infrared absorbing composition No. 1. Exemplary compound III-2 1.0 g Exemplary compound V-10 1.0 g Cyclopentyl methyl ether 10 g
[0200] Near infrared absorbing compositions Nos. 2 to 36 were prepared in the same manner as in the preparation of near infrared absorbing composition No. 1, except for changing the following points as shown in Tables VII and VIII: - Type of compound having a structure represented by general formula (I) - Type of compound having a structure represented by general formula (II) - Type and added amount of compound having a structure represented by general formula (III) or (IV) - Type and added amount of compound having a structure represented by general formula (V) - Type of solvent
[0201] <Evaluation of Dispersibility> The dispersibility of the near-infrared absorbing composition was evaluated by measuring the average particle size of particles in the near-infrared absorbing composition. The near-infrared absorbing composition was diluted with toluene to a solid content concentration of 0.5% by mass. The average particle size was measured by dynamic light scattering using an ELSZ-1000ZS manufactured by Otsuka Electronics Co., Ltd. The dispersibility was evaluated according to the following evaluation criteria, which was used as a measure of dispersibility. The evaluation results are shown in the table below.
[0202] A: The average particle size is 100 nm or less. B: The average particle size is more than 100 nm and not more than 150 nm. C: The average particle size is more than 150 nm and not more than 200 nm. D: The average particle size is more than 200 nm.
[0203] <Evaluation of Storage Stability> The storage stability of the near-infrared absorbing composition was evaluated by measuring the change in particle size and viscosity of the near-infrared absorbing composition over time.
[0204] (Change in particle size) The near-infrared absorbing composition was left to stand at room temperature for 7 days. Thereafter, the average particle size of the particles in the near-infrared absorbing composition was measured using the same method as described above. The average particle size variation rate [%] was calculated from the average particle size before and after standing. The average particle size variation rate [%] was evaluated according to the following criteria. The evaluation results are shown in the table below.
[0205] A: The average particle size fluctuation rate is less than 10%. B: The average particle size fluctuation rate is 10% or more and less than 30%. C: The average particle size fluctuation rate is 30% or more and less than 50%. D: The average particle size fluctuation rate is 50% or more.
[0206] (Change in Viscosity) The viscosity of the near-infrared absorbing composition was measured. Thereafter, the near-infrared absorbing composition was heated at 45°C for 2 days. After heating, the viscosity of the near-infrared absorbing composition was measured again. The viscosity change rate [%] was calculated from the viscosity before and after heating. The viscosity change rate [%] was evaluated according to the following criteria. The evaluation results are shown in the table below.
[0207] A: The viscosity fluctuation rate is less than 10%. B: The viscosity fluctuation rate is 10% or more and less than 30%. C: The viscosity fluctuation rate is 30% or more and less than 50%. D: The viscosity fluctuation rate is 50% or more.
[0208]
[0209]
[0210] The results shown in Table VIII show that the near-infrared absorbing composition of the present invention is excellent in dispersibility and storage stability.
[0211] <Preparation of near-infrared absorbing cured film> The near-infrared absorbing composition and the following resin material were mixed in the combinations shown in Tables IX and X so that the solid content ratio of the resin material was 70 mass %. In this way, coating solutions for forming near-infrared absorbing cured films No. 1 to 60 were prepared, respectively.
[0212] Details of the resin materials used are as follows: (Resin material No. 1) A solution obtained by mixing 80% by mass of 2-ethylhexyl methacrylate, 19% by mass of trimethylolpropane triacrylate, and 1.0% by mass of a polymerization initiator, Perbutyl ND (manufactured by NOF Corporation); (Resin material No. 2) Silicone resin KR311 (manufactured by Shin-Etsu Chemical Co., Ltd.); (Resin material No. 3) A solution obtained by dissolving 20% by mass of Dianal BR-87 (manufactured by Mitsubishi Chemical Corporation) in cyclopentyl methyl ether.
[0213] The coating liquid for forming a near-infrared absorbing cured film was cast onto a glass substrate. The coating amount was adjusted so that the thickness would result in a maximum spectral transmittance of 10% in the wavelength range of 850 to 1000 nm after curing. The glass substrate coated with the coating liquid was pre-baked on a hot plate at 110°C for 2 minutes.
[0214] The composition was then cured by heat treatment on a hot plate. When resin material 1 was used, the heating temperature was 120°C and the heating time was 1 hour. When resin material 2 was used, the heating temperature was 180°C and the heating time was 1 hour. When resin material 3 was used, the heating temperature was 120°C and the heating time was 15 minutes.
[0215] In this way, near-infrared absorbing cured films Nos. 1 to 60 were prepared.
[0216] <Evaluation of moist heat resistance of near-infrared absorbing cured film> The average transmittance T of the near-infrared absorbing cured film in the wavelength region of 700 to 1200 nm immediately after preparation was ave1 The near-infrared absorbing cured film was then left to stand for 1000 hours in an environment of 85°C and 85% RH. The average transmittance T ave2 asked for.
[0217] T ave1 T for ave2 The decrease in visible light transmittance (T ave1 -T ave2 The extent of decrease in visible light transmittance was evaluated according to the following criteria, and this was used as a measure of moist heat resistance. The evaluation results are shown in the table below.
[0218] A: The decrease in average transmittance is less than 3%. B: The decrease in average transmittance is 3% or more and less than 5%. C: The decrease in average transmittance is 5% or more and less than 10%. D: The decrease in average transmittance is 10% or more.
[0219]
[0220]
[0221] The results shown in Tables IX and X show that the near-infrared absorbing cured film of the present invention has excellent resistance to moist heat.
[0222] From the above results, it can be confirmed that the near-infrared absorbing composition of the present invention can form a cured film that has excellent storage stability and excellent resistance to moist heat.
[0223] The present invention can be used in near-infrared absorbing compositions, near-infrared absorbing cured films, and optical components.
[0224] REFERENCE SIGNS LIST 1 camera module 2 adhesive 3 glass substrate 4 imaging lens 5 lens holder 6 light-shielding and electromagnetic shield 7 adhesive 8 planarizing layer 9 near-infrared cut filter 10 solid-state imaging element substrate 11 solder ball 12 circuit board 14 image sensor for solid-state imaging element 21 transparent dielectric substrate 22 near-infrared absorbing layer 23 dielectric multilayer film
Claims
1. A near infrared absorbing composition comprising the following components (A) to (E): Component (A): a copper complex coordinated with a compound having a structure represented by the following general formula (I). [In general formula (I), R 1 is an alkyl group having 1 to 20 carbon atoms, which may further have a substituent.] Component (B): a compound having a structure represented by the following general formula (II). [In general formula (II), R 2 R is an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, and may further have a substituent. 21 ~R 24 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 21 ~R 24 represents the average number of partial structural units added that are all hydrogen atoms, and is in the range of 0 to 19. 21 ~R 24 represents the average number of partial structural units added, at least one of which is an alkyl group having 1 to 4 carbon atoms, and is within the range of 0 to 19. m+n represents the total number of m and n, and is within the range of 1 to 20. Z represents a structural unit selected from the following formulae (Z-1) and (Z-2). Component (C): A compound having a structure represented by the following general formula (III) or (IV). General formula (III) (R 3 O) 4-m Ti(O-R 4 -OH) m General formula (IV) (R 3 O) 4-m Ti(OCOR 5 ) m In general formulas (III) and (IV), m is an integer of 1 to 4. 4 is an alkylene group having 1 to 30 carbon atoms, which may further have a substituent. 3 and R 5 are each independently an alkyl group having 1 to 30 carbon atoms, which may further have a substituent.] Component (D): a compound having a structure represented by the following general formula (V). General formula (V) R 6 - (CH 2 ) m -Si(CH 3 ) n - (OR 7 ) 3-n [In general formula (V), R 6 R is a vinyl group, a styryl group, an acryloxy group, a methacryloxy group, a mercapto group, an epoxy group, an epoxycyclohexyl group, or a glycidoxy group, and may further have a substituent. 7 is an alkyl group having 1 to 3 carbon atoms. m is an integer of 0 to 8. n is 0 or 1.] Component (E): polar term δ of Hansen solubility parameter P is in the range of 3 to 6, and the hydrogen bond term δ H A solvent having a value in the range of 3 to 6.
2. The compound having the structure represented by the general formula (II) has at least one partial structure that satisfies the following condition (i) and at least one partial structure that satisfies the following condition (ii), and Condition (i): R 21 ~R 24 are all hydrogen atoms. 21 ~R 24 The near infrared absorbing composition according to claim 1, wherein at least one of the above is an alkyl group having a carbon number of 1 to 4. The near infrared absorbing composition according to claim 1, wherein m and n in the general formula (II) are each within a range of 1 to 19.
3. The near infrared absorbing composition according to claim 1, wherein the content of said component (C) is within the range of 1 to 30 mass % relative to said component (A).
4. The near infrared absorbing composition according to claim 1, wherein the content of said component (D) is within the range of 1 to 30 mass % relative to said component (A).
5. R in the general formula (V) 6 The near infrared absorbing composition according to claim 1 , wherein is an acryloxy group or a methacryloxy group.
6. The near infrared absorbing composition according to claim 1, wherein the component (E) is cyclopentyl methyl ether or 4-methyltetrahydropyran.
7. A near infrared absorbing cured film comprising a cured product of the near infrared absorbing composition according to any one of claims 1 to 6.
8. An optical component comprising a cured product of the near infrared absorbing composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Curable resin composition, infrared cut filter, and solid imaging device using infrared cut filter
JP2014142629A
Thermosetting resin composition comprising phosphonium salt as resin curing accelerator, and near-infrared cut filter
JP2017137401A
Housing member
JP2022116998A
Near-infrared absorbing composition, near-infrared blocking filter, method for producing near-infrared blocking filter, camera module and method for manufacturing camera module
WO2014129366A1
Near-infrared absorbing composition, near-infrared absorbing film, and image sensor for solid-state imaging element
WO2019221061A1
Cited By
Near-infrared absorbing composition, near-infrared absorbing cured film, and optical member