Coated device and production method for same

A hydrophilic polymer coating with specific compounds and optimized ratios is applied to medical devices, addressing the limitations of conventional surface modification methods by achieving enhanced hydrophilicity, slipperiness, and adhesion inhibition, thereby improving biocompatibility and user comfort.

WO2024237064A1PCT designated stage expired Publication Date: 2024-11-21TORAY INDUSTRIES INC
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016431
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-04-26
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional methods for surface modification of medical devices, such as those using silicone rubber or metal, fail to impart sufficient hydrophilicity, slipperiness, and lipid and protein adhesion inhibiting properties, which are essential for improved biocompatibility and user comfort.

Method used

A coated device with a hydrophilic polymer coating comprising a compound represented by a specific general formula, including a compound with an amide group and multiple hydroxyl groups, is used, where the copolymerization ratio of these compounds is optimized to achieve the desired properties, and the device is treated with a solution at a controlled pH and temperature.

Benefits of technology

The coated device achieves sufficient hydrophilicity, slipperiness, and lipid and protein adhesion inhibition, enhancing biocompatibility and user comfort, while maintaining durability and ease of manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a coated device that has been given lipid and protein adhesion–suppressing characteristics in addition to substantial hydrophilicity and slipperiness; and a simple production method for the coated device. The present invention provides a coated device that comprises a device and a hydrophilic polymer that coats the surface of the device. The hydrophilic polymer includes a hydrophilic polymer A. The hydrophilic polymer A includes, as monomer units, a compound a1 that has a specific structure, a compound a2 that has an amide group, and a compound a3 that has a plurality of hydroxyl groups. The copolymerization proportions of the compound a1, the compound a2, and the compound a3 are 1–96 mass% for the compound a1, 1–96 mass% for the compound a2, and 8–61 mass% for the compound a3.
Need to check novelty before this filing date? Find Prior Art

Description

Coated device and method of manufacturing same

[0001] The present invention relates to a coated device and a method for manufacturing the same.

[0002] BACKGROUND ART Conventionally, devices using soft materials such as silicone rubber and hydrogel, or devices using hard materials such as metal and glass, have been used for a variety of purposes in various fields.

[0003] For example, when a medical device is inserted into a living body or attached to a living body surface, surface modification of the medical device is important to improve its biocompatibility. In addition to improving biocompatibility, surface modification can impart properties such as hydrophilicity, slipperiness, and lipid adhesion inhibition to the medical device, which can be expected to improve the user's experience, reduce discomfort, and alleviate symptoms.

[0004] Known methods for surface modification of medical devices include immersing the medical device in a solution of pH 6 to 9 containing a polymer made of a compound having an amide group, such as N,N-dimethylacrylamide or vinylpyrrolidone, at room temperature or by immersing the medical device in the solution and then heating the solution (Patent Documents 1 to 3).

[0005] International Publication No. 2017 / 018425 International Publication No. 2015 / 119256 Patent No. 5154231

[0006] However, none of the inventions disclosed in Patent Documents 1 to 3 are capable of imparting sufficient hydrophilicity, slipperiness, etc. to the surface of a medical device, and furthermore, they are not methods capable of imparting lipid adhesion inhibitory properties to a medical device.

[0007] Therefore, an object of the present invention is to provide a coated device that is endowed with sufficient hydrophilicity and lubricity as well as lipid and protein adhesion inhibitory properties, and a simple method for producing the same.

[0008] In order to achieve the above object, the present invention provides a coated device comprising a device and a hydrophilic polymer that coats the surface of the device, wherein the hydrophilic polymer includes a hydrophilic polymer A that includes, as monomer units, a compound a1 represented by the following general formula (I), a compound a2 having an amide group, and a compound a3 having multiple hydroxyl groups, and wherein the copolymerization ratios of compound a1, compound a2, and compound a3 are 1 to 96 mass % for compound a1, 1 to 96 mass % for compound a2, and 8 to 61 mass % for compound a3:

[0009]

[0010] In general formula (I), R 1 represents a hydrogen atom or a methyl group, and X represents an oxygen atom or NR 2 represents R 2 represents a hydrogen atom or an alkyl group, m represents an integer of 1 to 30, and Y represents a hydrogen atom or an alkyl group.

[0011] The present invention also provides a method for producing a coated device, comprising: (A) a contacting step of storing a device in a container and bringing the device into contact with a solution a containing a hydrophilic polymer A; and (C) a heating step of heating the container, wherein the hydrophilic polymer A contains, as monomer units, a compound a1 represented by general formula (I) above, a compound a2 having an amide group, and a compound a3 having multiple hydroxyl groups, the copolymerization ratios of compound a1, compound a2, and compound a3 being, in mass ratio, 1 to 96 mass % for compound a1, 1 to 96 mass % for compound a2, and 8 to 61 mass % for compound a3, and the pH of the solution a after the heating step is 6.1 to 8.0.

[0012] According to the present invention, it is possible to provide a coated device that has sufficient hydrophilicity and slipperiness, which are required particularly when the device is a medical device, as well as lipid and protein adhesion inhibitory properties. Furthermore, according to the manufacturing method of the present invention, the coated device can be obtained by a simple process.

[0013] The coated device of the present invention comprises a device and a hydrophilic polymer that coats the surface of the device. The hydrophilic polymer includes a hydrophilic polymer A, which includes, as monomer units, a compound a1 represented by the following general formula (I), a compound a2 having an amide group, and a compound a3 having multiple hydroxyl groups, and is characterized in that the copolymerization ratios of compound a1, compound a2, and compound a3 are 1 to 96 mass %, 1 to 96 mass %, and 8 to 61 mass %, respectively:

[0014]

[0015] [In general formula (I), R 1 represents a hydrogen atom or a methyl group, and X represents an oxygen atom or NR 2 represents R 2 represents a hydrogen atom or an alkyl group, m represents an integer of 1 to 30, and Y represents a hydrogen atom or an alkyl group.] Examples of devices included in the coated device of the present invention include ophthalmic lenses, skin dressings, wound dressings, skin protective materials, cutaneous drug carriers, infusion tubes, gas transport tubes, drainage tubes, blood circuits, coating tubes, catheters, stents, sheaths, biosensor chips, artificial heart-lung machines, and endoscope covering materials. Examples of ophthalmic lenses include contact lenses, intraocular lenses, artificial corneas, corneal inlays, corneal onlays, and spectacle lenses.

[0016] The material constituting the device may be either a hydrous material or a low-moisture-containing material. Examples of hydrous materials include hydrogels and silicone hydrogels. When the device is a contact lens, silicone hydrogels are preferred because they have high lipid and protein adhesion inhibition properties, can form a durable surface that exhibits excellent hydrophilicity and slipperiness, and are likely to maintain their effectiveness even when worn for long periods of time. Examples of low-moisture-containing materials include low-moisture-containing soft materials and low-moisture-containing hard materials. A low-moisture-containing material refers to a material with a water content of 10% by mass or less.

[0017] Hereinafter, the United States Adopted Names (USAN) may be used to represent the names of hydrogels or silicone hydrogels. In the USAN, a suffix such as A, B, or C may be added to indicate a material variant. In this specification, however, when no suffix is ​​added, all variants are represented. For example, the term "ocufilcon" refers to all variants of ocufilcon, such as "ocufilcon A," "ocufilcon B," "ocufilcon C," "ocufilcon D," "ocufilcon E," or "ocufilcon F."

[0018] Examples of hydrogels include tefilcon, tetrafilcon, hefilcon, mafilcon, polymacon, hioxifilcon, alfafilcon, omafilcon, hixoifilcon, and nelfilcon. , nesofilcon, hilafilcon, acofilcon, deltafilcon, etafilcon, focofilcon, ocufilcon, femfilcon, mesafilcon or vilfilcon.

[0019] When the device is a contact lens made of hydrogel, it belongs to Group 1 to Group 4 of the contact lens classification defined by the U.S. Food and Drug Administration (FDA), but Group 2 or Group 4, which show good hydrophilicity, is preferred, and Group 4 is more preferred.

[0020] Examples of non-ionic hydrogels belonging to Group 1 having a water content of less than 50% by mass include tefilcon, tetrafilcon, helifilcon, mafilcon, polymacon, and hioxifilcon.

[0021] Examples of non-ionic hydrogels belonging to Group 2 having a water content of 50% by mass or more include alfafilcon, omafilcon, hixoifilcon, nelfilcon, nesofilcon, hilafilcon, and acofilcon. ), of which omafilcon, hixoifilcon, nelfilcon or nesofilcon, which exhibit good hydrophilicity, are preferred, omafilcon or hixoifilcon are more preferred, and omafilcon is even more preferred.

[0022] An example of an ionic hydrogel having a water content of less than 50% by mass belonging to Group 3 is deltafilcon.

[0023] Examples of ionic hydrogels belonging to Group 4 having a water content of 50% by mass or more include etafilcon, focofilcon, ocfilcon, femfilcon, methafilcon, and vilfilcon. Of these, etafilcon, focofilcon, ocfilcon, and femfilcon are preferred, as they exhibit good hydrophilicity, with etafilcon and ocfilcon being more preferred, and etafilcon being even more preferred.

[0024] When the device is a contact lens made of silicone hydrogel, it preferably belongs to Group 5, a classification for contact lenses as defined by the US Food and Drug Administration (FDA).

[0025] Silicone hydrogels belonging to Group 5 are preferably polymers that have silicon atoms in the main chain and / or side chain and have hydrophilic properties, such as copolymers of a monomer containing a siloxane bond and a hydrophilic monomer.Such copolymers include, for example, lotrafilcon, gallyfilcon, narafilcon, senofilcon, comfilcon, enfilcon, balafilcon, efrofilcon, fanfilcon, somofilcon, samfilcon, and otrafilcon. Examples of such anti-lipid-adhesion agents include olifilcon, asmofilcon, formofilcon, stenfilcon, abafilcon, mangofilcon, liofilcon, sifilcon, larafilcon, kalifilcon, and delefilcon. and lotrafilcon, galifilcon, narafilcon, senofilcon, comfilcon, enfilcon, stenfilcon, somofilcon, delefilcon, balafilcon, kalifilcon, or samfilcon, which exhibit good hydrophilicity and antifouling properties. Samfilcon is preferred, with lotrafilcon, narafilcon, senofilcon, comfilcon, kalifilcon, or enfilcon being more preferred, and narafilcon, senofilcon, kalifilcon, or comfilcon being even more preferred.

[0026] When the device is a contact lens, the low water content soft material or low water content hard material is preferably a material containing silicon atoms, which exhibits high oxygen permeability that allows sufficient oxygen to be supplied to the cornea.

[0027] The low water content hard material is preferably a low water content hard material that falls under the category of contact lenses as defined by the US Food and Drug Administration (FDA).

[0028] Such low-water-absorbent hard materials are preferably polymers having silicon atoms such as siloxane bonds in the main chain and / or side chain, and more preferably homopolymers using highly oxygen-permeable tris(trimethylsiloxy)silylpropyl methacrylate, polydimethylsiloxane having double bonds at both ends, or silicone-containing acrylate or silicone-containing methacrylate, or copolymers of these with other monomers.

[0029] Specifically, the low water content hard material is preferably selected from the group consisting of neofocon, pasifoccon, telefocon, silafocon, paflufocon, petrafocon, and fluorofocon. Among them, because they exhibit good lipid adhesion inhibition and antifouling properties, neofocon, pasifoccon, telefocon, and silafocon are more preferred, neofocon, pasifoccon, and telefocon are even more preferred, and neofocon is particularly preferred.

[0030] When the device is other than a contact lens, the low water-absorbent hard material is preferably polyethylene, polypropylene, polysulfone, polyetherimide, polystyrene, polymethyl methacrylate, polyamide, polyester, epoxy resin, polyurethane, or polyvinyl chloride. Among these, polysulfone, polystyrene, polymethyl methacrylate, polyurethane, or polyamide is more preferred, and polymethyl methacrylate is even more preferred, as they exhibit good lipid adhesion inhibition and antifouling properties.

[0031] Examples of low-water-content soft materials include materials disclosed in WO 2013 / 024799 that have a water content of 10% by mass or less, an elastic modulus of 100 to 2,000 kPa, and a tensile elongation of 50 to 3,000%, and elastofilcon.

[0032] In the present invention, whether the device is hydrous or low in hydrous content, the surface of the device can be provided with an appropriate lipid and protein adhesion inhibitory property, but in order to provide an appropriate lipid adhesion inhibitory property, the water content of the device is preferably 0.0001% by mass or more, more preferably 0.001% by mass or more, and the water content of the device is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less.

[0033] When the device is a contact lens, the water content of the device is preferably 15% by mass or more, and more preferably 20% by mass or more, since this makes it easier to ensure the movement of the lens within the eye.

[0034] The hydrophilic polymer A has hydrophilicity. Here, "hydrophilic" means that the polymer is soluble in 100 parts by mass of water or a mixture of 100 parts by mass of water and 100 parts by mass of tert-butanol at room temperature (20 to 23°C) at a concentration of 0.0001 part by mass or more. The polymer is preferably soluble in 0.01 part by mass or more, more preferably soluble in 0.1 part by mass or more, and even more preferably soluble in 1 part by mass or more.

[0035] The hydrophilic polymer A contains, as monomer units, a compound a1 represented by the following general formula (I), a compound a2 having an amide group, and a compound a3 having multiple hydroxyl groups, and the copolymerization ratios of the compound a1, the compound a2, and the compound a3 are 1 to 96% by mass of the compound a1, 1 to 96% by mass of the compound a2, and 8 to 61% by mass of the compound a3. Here, the copolymerization ratios of the compound a1, the compound a2, and the compound a3 refer to the respective mass ratios of the compound a1, the compound a2, and the compound a3 when the total mass of the compound a1, the compound a2, and the compound a3 is taken as 100%.

[0036] As each of the compound a1, the compound a2 and the compound a3, a single monomer or a mixture of a plurality of monomers having different structures can be used.

[0037] From the viewpoint of high polymerizability, compound a1, compound a2 and compound a3 are preferably monomers having an allyl group, a vinyl group or a (meth)acryloyl group, and particularly preferably monomers having a (meth)acryloyl group.

[0038]

[0039] In general formula (I), R 1 represents a hydrogen atom or a methyl group, and X represents an oxygen atom or NR 2 represents R 2 represents a hydrogen atom or an alkyl group, m represents an integer of 1 to 30, and Y represents a hydrogen atom or an alkyl group.

[0040] R 2 When R is an alkyl group, it may be linear or branched, but is preferably an alkyl group having 1 to 10 carbon atoms. 2 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a 2-propyl group, a butyl group, a 2-butyl group, a tert-butyl group, a pentyl group, a 2-pentyl group, a 3-pentyl group, a hexyl group, a heptyl group, and an octyl group.

[0041] From the viewpoint of appropriate hydrophilicity and ease of polymerization, m is preferably 1 to 30. The lower limit of m is more preferably 1, further preferably 2, and particularly preferably 4. The upper limit of m is more preferably 25, further preferably 13, and particularly preferably 9.

[0042] From the viewpoint of ease of forming a coating, Y is preferably an alkyl group having 1 to 5 carbon atoms, more preferably a methyl group, an ethyl group, a propyl group, an isopropyl group, or a butyl group, particularly preferably a methyl group or an ethyl group, and most preferably a methyl group.

[0043] As the compound a2 having an amide group, a compound having an acrylamide group or a methacrylamide group, or an N-vinylcarboxylic acid amide (including cyclic ones) is preferred in terms of ease of polymerization.

[0044] Specific examples include N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylacetamide, N-methyl-N-vinylacetamide, N-vinylformamide, N,N-dimethylacrylamide, N-isopropylacrylamide, N-methylacrylamide, N-ethylacrylamide, N-butylacrylamide, N-tert-butylacrylamide, N-hydroxymethylacrylamide, N-methoxymethylacrylamide, N-ethoxymethylacrylamide, N-propoxymethylacrylamide, N-isopropoxymethylacrylamide, N-(2-hydroxyethyl)acrylamide, N-butoxymethylacrylamide, N-isobutoxymethylacrylamide, N-hydroxymethylmethacrylamide, N-methoxymethylmethacrylamide, N-ethoxymethylmethacrylamide, N-propoxymethylmethacrylamide, N-butoxymethylmethacrylamide, N-isobutoxymethylmethacrylamide, acryloylmorpholine, and acrylamide. To enhance lubricity, N-vinylpyrrolidone, N-isopropylacrylamide or N,N-dimethylacrylamide is preferred, N-isopropylacrylamide or N,N-dimethylacrylamide is more preferred, and N,N-dimethylacrylamide is even more preferred.

[0045] Examples of compounds a3 having multiple hydroxyl groups include glycerol acrylate, glycerol methacrylate, divalent phenyl(meth)acrylate, trivalent phenyl(meth)acrylate, a compound represented by the following structural formula (a), or a compound represented by the following structural formula (b). "Having multiple hydroxyl groups" means having two or more hydroxyl groups (OH groups). However, this does not include OH groups constituting a carboxyl group (COOH group) or hydroxyl groups directly bonded to atoms other than carbon.

[0046]

[0047]

[0048] In order to improve adsorption to the device, from the viewpoint of moderate hydrophilicity and ease of polymerization, glycerol acrylate, glycerol methacrylate, 2-methacryloyloxyethyl acid phosphate, a compound represented by the above structural formula (a), or a compound represented by the above structural formula (b), which are chain compounds having multiple hydroxyl groups, are preferred, with glycerol acrylate or glycerol methacrylate being more preferred. Furthermore, the term "chain compound" as used herein refers to a compound that does not have a cyclic structure. Chain compounds are also sometimes called acyclic compounds.

[0049] The hydrophilic polymer A may contain, as a monomer unit, one or more copolymerized compounds other than the compound a1 represented by the general formula (I), the compound a2 having an amide group, and the compound a3 having multiple hydroxyl groups. Examples of such other compounds include N-(4-hydroxyphenyl)maleimide, hydroxystyrene, vinyl alcohol (a vinyl carboxylic acid ester precursor), hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, caprolactone-modified 2-hydroxyethyl (meth)acrylate, (meth)acrylic acid, vinylbenzoic acid, thiophene-3-acetic acid, 4-styrenesulfonic acid, vinylsulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, or salts thereof. To improve the antifouling properties against body fluids, hydroxyethyl (meth)acrylate, vinyl alcohol, or (meth)acrylic acid is preferred, with hydroxyethyl (meth)acrylate being more preferred. In addition, compounds that exhibit functions such as hydrophilicity, antibacterial properties, antifouling properties, or medicinal properties can also be used as other compounds.

[0050] When the hydrophilic polymer A contains the compound a1 represented by the above general formula (I) as a monomer unit, the hydrophilic polymer A is easily soluble in water, exhibits hydrophilic properties, and can form a surface that is not only hydrophilic but also inhibits the adhesion of lipids and proteins.

[0051] When the hydrophilic polymer A contains the compound a2 having an amide group as a monomer unit, the hydrophilic polymer A exhibits an appropriate viscosity when dissolved in water, and can form a surface that is not only hydrophilic but also slippery.

[0052] When the hydrophilic polymer A contains the compound a3 having a plurality of hydroxyl groups as a monomer unit, the hydrophilic polymer A is easily adsorbed onto the device surface, and a durable hydrophilic surface can be formed.

[0053] The copolymerization ratio of the compound a1 is in the range of 1 to 96% by mass to facilitate the development of functions such as lipid and protein adhesion inhibition and durable hydrophilicity. In other words, when the total amount of monomers constituting the hydrophilic polymer A is taken as 100% by mass, the proportion of the compound a1 must be 1% by mass or more, preferably 5% by mass or more, and more preferably 10% by mass or more. Furthermore, from the viewpoint of ease of polymerization, the proportion of the compound a1 must be 96% by mass or less, preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 40% by mass or less.

[0054] When the total amount of the monomers constituting the hydrophilic polymer A is taken as 100% by mass, the proportion of the compound a2 is in the range of 1 to 96% in order to facilitate the development of functions such as durable hydrophilicity and easy slippage. The proportion of the compound a2 must be 1% by mass or more, preferably 10% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more. The proportion of the compound a2 must be 90% by mass or less, preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less.

[0055] When the total amount of the monomers constituting the hydrophilic polymer A is taken as 100% by mass, the proportion of the compound a3 is in the range of 8 to 61% because this facilitates ease of polymerization and facilitates adsorption to the device surface. The proportion of the compound a3 must be 8% by mass or more, preferably 9% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more. The proportion of the compound a3 must be 60% by mass or less, preferably 55% by mass or less, more preferably 50% by mass or less, and even more preferably 45% by mass or less.

[0056] When a compound other than the compound a1 represented by the general formula (I), the compound a2 having an amide group, and the compound a3 having multiple hydroxyl groups is copolymerized as the fourth monomer component, the copolymerization ratio of the fourth monomer component is preferably 2% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, from the viewpoint of ease of polymerization. Also, the copolymerization ratio of the fourth monomer component is preferably 90% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less.

[0057] When the copolymerization ratio of the compound a1 represented by the above general formula (I), the compound a2 having an amide group, the compound a3 having a plurality of hydroxyl groups, and the fourth monomer component is within the above range, functions such as easy lubricity and antifouling properties against body fluids are easily exhibited.

[0058] In order to improve durability in addition to hydrophilicity and slipperiness while suppressing deformation of the device, the detection depth of the hydrophilic polymer A from the outermost surface of the coated device is preferably 10.00 μm or less, more preferably 4.00 to 5.00 μm, even more preferably 3.00 to 4.00 μm, particularly preferably 2.00 to 3.00 μm, and most preferably 0.05 to 2.00 μm.

[0059] The detection depth of the hydrophilic polymer A can be confirmed by measuring the surface of the coated device by time-of-flight secondary ion mass spectrometry (hereinafter referred to as "TOF-SIMS").

[0060] The detection depth of hydrophilic polymer A is the length (depth) between the surface and the point where the detection intensity of the ion species corresponding to hydrophilic polymer A detected in the depth direction from the surface of the coated device coincides with the detection intensity (background) of the ion species corresponding to hydrophilic polymer A detected from the device itself (uncoated). If the device is not coated with a hydrophilic polymer containing hydrophilic polymer A, the detection depth of the hydrophilic polymer is 0 μm. The details of the TOF-SIMS measurement method will be described later.

[0061] In the obtained coated device, it is preferable that there is no covalent bond between the hydrophilic polymer A and the device. The absence of a covalent bond enables the coated device to be produced using a simpler process, regardless of whether the device is made of a water-containing material or a low-water-containing material. Here, the absence of a covalent bond means that there is no chemically reactive group or a group formed by reaction thereof between the hydrophilic polymer A and the device. The absence of a chemically reactive group or a group formed by reaction thereof can be confirmed by elemental analysis such as electron energy loss spectroscopy, energy dispersive X-ray spectroscopy, or time-of-flight secondary ion mass spectrometry, or by compositional analysis. Examples of chemically reactive groups include azetidinium groups, epoxy groups, isocyanate groups, aziridine groups, and azlactone groups.

[0062] In the obtained coated device, the hydrophilic polymer A may be present only on a part of the surface of the device, or on the entire surface of either the front or back side, or on the entire surface.

[0063] In the coated device of the present invention, in order to achieve a stronger coating, it is preferable that at least a portion of the hydrophilic polymer A is present in a mixed state with the device. Here, the mixed state of the hydrophilic polymer A and the device refers to a state in which elements derived from the hydrophilic polymer A and elements derived from the device are both detected in the same region, and this can be confirmed by observing a cross section of the coated device using elemental analysis such as scanning transmission electron microscopy, electron energy loss spectroscopy, energy dispersive X-ray spectroscopy, or time-of-flight secondary ion mass spectrometry, or a composition analysis means.

[0064] When the hydrophilic polymer A is dissolved in water, it exhibits an appropriate viscosity, enabling the formation of a surface that is not only hydrophilic but also slippery. Therefore, the viscosity of the aqueous solution of the hydrophilic polymer A is preferably 1 to 2000 mPa·s. The viscosity of the aqueous solution of the hydrophilic polymer A is more preferably 2 mPa·s or more, even more preferably 5 mPa·s or more, and particularly preferably 10 mPa·s or more. The viscosity is more preferably 1900 mPa·s or less, even more preferably 1000 mPa·s or less, and particularly preferably 500 mPa·s or less. The viscosity referred to here is the viscosity measured using a solution in which 2.0 to 3.5 mass% of the hydrophilic polymer A is dissolved in water. Details of the measurement method will be described later.

[0065] In order to increase the adsorption force of the hydrophilic polymer A onto the surface of the device and to impart sufficient lipid adhesion inhibition to the device, the weight-average molecular weight of the hydrophilic polymer A is preferably 2,000 to 1,500,000. The weight-average molecular weight is more preferably 5,000 or more, even more preferably 10,000 or more, and particularly preferably 100,000 or more. The weight-average molecular weight is more preferably 1,000,000 or less, even more preferably 800,000 or less, and particularly preferably 600,000 or less. The weight-average molecular weight referred to here is the weight-average molecular weight in terms of polyethylene glycol, measured by gel permeation chromatography using an aqueous solvent as the developing solvent. Details of the measurement method will be described below.

[0066] The filterability of the hydrophilic polymer A of the present invention is preferably such that the solution containing the hydrophilic polymer A can be continuously filtered, because of the ease of manufacturing the coated device and the high adsorption power of the hydrophilic polymer A to the surface of the device. The details of the measurement method will be described later.

[0067] Furthermore, since the hydrophilic polymer A has a high adsorption force on the surface of the device and can impart sufficient hydrophilicity and slipperiness to the device, it is preferable that the change in the average particle size of the hydrophilic polymer A is irreversible when the temperature is lowered again after heating. "Irreversible" means that when a solution containing the hydrophilic polymer A is heated from 25°C to 121°C and then cooled again to 25°C, the average particle size of the hydrophilic polymer A increases by 10 nm or more when cooled again to 25°C compared to before heating, and the hydrophilic polymer A aggregates. Since a stronger coating of the hydrophilic polymer A on the device is possible, the increase in the average particle size of the hydrophilic polymer A when cooled again to 25°C compared to before heating is preferably 40 nm or more, more preferably 70 nm or more, and particularly preferably 80 nm or more. Details of the measurement method will be described later.

[0068] The charge of the hydrophilic polymer A is preferably within ±5 mV, which means that the coated device has no charge, since the coated device has excellent lipid and protein adhesion suppression properties. The measurement method will be described in detail later.

[0069] Furthermore, the hydrophilic polymer A that coats the surface of the device of the present invention is preferably present non-uniformly in a frozen state. The term "non-uniformly present" means that when a cross-sectional image of the hydrophilic polymer A that coats the surface of the device in a frozen state is observed with a scanning transmission electron microscope, the hydrophilic polymer A is not uniformly present. 4 Stained area and RuO 4 This means that unstained areas are mixed in. 4 The unstained areas are areas where water is present, spaces, or where the hydrophilic polymer A is not RuO 4 This is a region that exists in an unstained structure, and when an ophthalmic lens is used as the device, for example, components in tears, such as lipids and proteins, can easily pass through, thereby suppressing adhesion of tear components and increasing the antifouling properties of the coated device. The region in which hydrophilic polymer A is unevenly present may be present only in a part of hydrophilic polymer A, or may be present throughout hydrophilic polymer A. The measurement method will be described in detail below.

[0070] The method for producing a coated device of the present invention includes: (A) a contacting step of storing a device in a container and bringing the device into contact with a solution a containing a hydrophilic polymer A; and (C) a heating step of heating the container, wherein the hydrophilic polymer A contains, as monomer units, a compound a1 represented by the following general formula (I), a compound a2 having an amide group, and a compound a3 having multiple hydroxyl groups, and the copolymerization ratios of the compound a1, the compound a2, and the compound a3 are 1 to 96 mass % for compound a1, 1 to 96 mass % for compound a2, and 8 to 61 mass % for compound a3; and the pH of the solution a after the heating step is 6.1 to 8.0.

[0071]

[0072] [In general formula (I), R 1 represents a hydrogen atom or a methyl group, and X represents an oxygen atom or NR 2 represents R 2 represents a hydrogen atom or an alkyl group, m represents an integer of 1 to 30, and Y represents a hydrogen atom or an alkyl group.] The concentration of hydrophilic polymer A in solution a containing hydrophilic polymer A is preferably in the range of 0.0001 to 30% by mass in order to ensure an appropriate viscosity of solution a. The concentration of hydrophilic polymer A is preferably 0.001% by mass or more, more preferably 0.005% by mass or more, and even more preferably 0.05% by mass or more. The concentration of hydrophilic polymer A is preferably 10.0% by mass or less, more preferably 5.0% by mass or less, even more preferably 1.0% by mass or less, and particularly preferably 0.5% by mass or less.

[0073] As the solvent for solution a containing hydrophilic polymer A, a water-soluble organic solvent or water, or a mixed solvent thereof is preferred from the viewpoint of ease of handling, a mixed solvent of water and a water-soluble organic solvent or water is more preferred, and water is even more preferred. As the water-soluble organic solvent, water-soluble alcohols are preferred, water-soluble alcohols having 6 or less carbon atoms are more preferred, and water-soluble alcohols having 5 or less carbon atoms are even more preferred. Solution a may further contain a buffer or other additives.

[0074] Examples of the buffer contained in solution a include boric acid, borate salts (e.g., sodium borate), citric acid, citrate salts (e.g., potassium citrate), bicarbonate (e.g., sodium bicarbonate), phosphate buffer (e.g., Na 2 HPO 4 , NaH 2 P.O. 4 or KH 2 P.O. 4 ), TRIS (tris(hydroxymethyl)aminomethane), 2-bis(2-hydroxyethyl)amino-2-(hydroxymethyl)-1,3-propanediol, bis-aminopolyols, triethanolamine, ACES (N-(2-acetamido)-2-aminoethanesulfonic acid), BES (N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid), HEPES (4-(2-hydroxyethyl)-1-piperazineethanesulfonic acid), MES (2-(N-morpholino)ethanesulfonic acid), MOPS (3-[N-morpholino]-propanol Examples of suitable buffering agents include piperazine-N,N'-bis(2-ethanesulfonic acid), PIPES (piperazine-N,N'-bis(2-ethanesulfonic acid), TES (N-[tris(hydroxymethyl)methyl]-2-aminoethanesulfonic acid), and salts thereof. The proportion of the buffering agent in solution a may be appropriately adjusted to achieve the desired pH, but is usually preferably 0.001 to 2.000% by mass. The proportion of the buffering agent is more preferably 0.010% by mass or more, and even more preferably 0.050% by mass or more. The proportion of the buffering agent is more preferably 1.000% by mass or less, and even more preferably 0.300% by mass or less.

[0075] The pH of the buffer solution used to prepare solution a is preferably within the physiologically acceptable range of 6.3 to 7.8. The pH of the buffer solution is more preferably 6.5 or higher, and even more preferably 6.8 or higher. The pH of the buffer solution is more preferably 7.6 or lower, and even more preferably 7.4 or lower.

[0076] The container for storing the device in the contacting step may be, for example, a vial or blister container used for packaging ophthalmic lenses when the device is an ophthalmic lens. A blister container usually consists of a plastic base surrounded by a flat flange that rises around the edge of the cavity, and a soft cover sheet that is adhered to the flat flange to seal the cavity.

[0077] Examples of materials for the plastic base include fluororesin, polyamide, polyacrylate, polyethylene, nylons, olefin copolymers (e.g., copolymer of polypropylene and polyethylene), polyethylene terephthalate, polyvinyl chloride, amorphous polyolefin, polycarbonate, polysulfone, polybutylene terephthalate, polypropylene, polymethylpentene, polyesters, rubbers, or urethane.

[0078] Flexible cover sheets include, for example, laminate materials such as aluminum foil coated polypropylene sheets.

[0079] The method for producing a coated device of the present invention includes a heating step (C) of heating the container.

[0080] Examples of the heating method include heating (hot air), high-pressure steam sterilization, dry heat sterilization, flame sterilization, boiling disinfection, circulating steam disinfection, electromagnetic wave (γ-ray, microwave, etc.) irradiation, ethylene oxide gas sterilization (EOG sterilization), and ultraviolet sterilization. High-pressure steam sterilization is preferred because it can impart sufficient lipid adhesion inhibitory properties to the device and has low production costs, and autoclave sterilization using an autoclave is more preferred.

[0081] The heating temperature is preferably 80 to 200°C so as to impart sufficient lipid and protein adhesion inhibition to the device while not affecting the strength of the resulting coated device itself. The heating temperature is more preferably 90°C or higher, even more preferably 105°C or higher, even more preferably 110°C or higher, still more preferably 115°C or higher, and particularly preferably 121°C or higher. The heating temperature is more preferably 180°C or lower, even more preferably 170°C or lower, and particularly preferably 150°C or lower.

[0082] For the same reasons as for the heating temperature, the heating time is preferably 1 to 600 minutes. The heating time is more preferably 2 minutes or more, even more preferably 5 minutes or more, and particularly preferably 10 minutes or more. The heating time is more preferably 400 minutes or less, even more preferably 300 minutes or less, and particularly preferably 100 minutes or less.

[0083] The method for producing a coated device of the present invention preferably further comprises (B) a sealing step of sealing the container containing the device after the contacting step and before the heating step. Performing the heating step after sealing the container containing the device makes it possible to impart lipid and protein adhesion inhibitory properties to the device surface while simultaneously sterilizing the resulting coated device and maintaining its sterility, which is industrially significant from the perspective of reducing the number of production steps. In other words, in the method for producing a coated device of the present invention, it is preferable to sterilize the device by the heating step in order to simplify the production process. Examples of means for sealing the container include a capped vial or blister container used to seal the container. Furthermore, when the device is a contact lens, another example of a means for sealing the container is to use a common lens case included with contact lens care products as the container to store the device.

[0084] After the heating step, the resulting coated device may be subjected to other treatments, such as a similar heating treatment using a buffer solution that does not contain a hydrophilic polymer, irradiation with ion beams, electron beams, positron beams, X-rays, gamma rays, or neutron beams, LbL treatment (Layer by Layer treatment; for example, the treatment described in International Publication No. 2013 / 024800) in which polymer materials having opposite charges are alternately coated one layer at a time, or crosslinking treatment with metal ions or chemical crosslinking treatment (for example, the treatment described in JP-A-2014-533381).

[0085] Before the contacting step and the heating step, the surface of the device may be pretreated, for example, by hydrolysis using an acid such as polyacrylic acid or an alkali such as sodium hydroxide (for example, the treatment described in Japanese Patent No. 6954490).

[0086] The method for producing a coated device of the present invention requires that the pH of solution a after the heating step be 6.1 to 8.0. Having a pH in this range eliminates the need to wash the coated device obtained after the heating step with a neutral solution, which is industrially important from the perspective of reducing the number of production steps. Note that if washing with a neutral solution is performed after the heating step, the resulting coated device may need to be sterilized again. The pH of solution a after the heating step is preferably 6.5 or higher, more preferably 6.6 or higher, even more preferably 6.7 or higher, and particularly preferably 6.8 or higher. The pH is also preferably 7.9 or lower, more preferably 7.8 or lower, and even more preferably 7.6 or lower.

[0087] The pH of solution a before the heating step is also preferably 6.1 to 8.0. Here, the pH of solution a before the heating step refers to the pH value measured after preparing solution a, stirring it with a rotor at room temperature (20 to 23°C) for 30 minutes to make the solution uniform.

[0088] The pH of the solution a can be measured using a pH meter (for example, pH meter Eutech pH2700 (manufactured by Eutech Instruments)). The pH value is rounded to one decimal place.

[0089] When the coated device is an ophthalmic lens or the like, it is preferable that the liquid film on the surface of the coated device be maintained for a long time, not only to prevent the lens from adhering to the wearer's cornea but also to reduce the feeling of dryness and maintain a good wearing sensation for a long period of time.

[0090] Here, the liquid film retention time on the surface of the coated device refers to the time during which the liquid film on the surface is maintained without breaking when the coated device is immersed in a solution at room temperature (20-23°C), removed from the solution, and held in the air with the longitudinal direction of the device aligned with gravity. In the case of a spherical crown-shaped test piece such as a contact lens, the test piece is held with the diameter of the circle formed by the edge of the spherical crown aligned with gravity. Note that "the liquid film breaks" refers to a state in which a portion of the solution covering the surface of the coated device is repelled, and the surface of the coated device is no longer completely covered with a liquid film. Note that if the liquid film retention time is too long, water evaporation from the surface of the coated device will proceed more easily, reducing the hydrophilic effect. Therefore, the liquid film retention time is preferably 300 seconds or less, and more preferably 200 seconds or less.

[0091] When the coated device is an ophthalmic lens or the like, it is preferable that the droplet contact angle on the surface of the coated device is small, not only to prevent the lens from adhering to the cornea of ​​the wearer but also to reduce the feeling of dryness and maintain a good wearing sensation for a long period of time. A method for measuring the droplet contact angle will be described later. When the device is made of a material containing silicon atoms, the droplet contact angle is preferably 80° or less, more preferably 70° or less, and even more preferably 65° or less.

[0092] Furthermore, when the device is made of a material that does not contain silicon atoms, the droplet contact angle is preferably 70° or less, more preferably 60° or less, and even more preferably 55° or less.

[0093] For example, when the coated device is a coated device to be inserted into a living body, it is preferable that the surface has excellent slipperiness. The friction coefficient, which is an index of slipperiness, is preferably 0.300 or less, more preferably 0.200 or less, even more preferably 0.100 or less, and even more preferably 0.080 or less. On the other hand, if the slipperiness is extremely high, the coated device may be difficult to handle, so the friction coefficient is preferably 0.001 or more, more preferably 0.002 or more. The method for measuring the friction coefficient will be described later.

[0094] When the coated device is a soft device such as an ophthalmic lens, in order to improve wearing comfort, the tensile modulus is preferably 10.00 MPa or less, more preferably 5.00 MPa or less, even more preferably 3.00 MPa or less, even more preferably 2.00 MPa or less, even more preferably 1.00 MPa or less, and particularly preferably 0.60 MPa or less. On the other hand, in order to facilitate handling, the tensile modulus of the coated device is preferably 0.01 MPa or more, more preferably 0.10 MPa or more, even more preferably 0.20 MPa or more, and particularly preferably 0.25 MPa or more. Furthermore, the rate of change in the tensile modulus of the device before and after the heating process, i.e., before and after coating, is preferably ±15.00% or less, more preferably ±13.00% or less, and even more preferably ±10.00% or less, in order to suppress the risk of deformation and poor usability. The method for measuring the tensile modulus will be described later.

[0095] The antifouling properties of the coated device of the present invention can be evaluated by the degree of mucin adhesion and lipid (methyl palmitate) adhesion. The less adhesion there is in these evaluations compared to the adhesion amount on the device itself before coating, the better the usability and the lower the risk of bacterial proliferation. The mucin adhesion amount is 10 μg / cm 2 Preferably, 8 μg / cm or less 2 More preferably, 6 μg / cm 2The following is particularly preferred. The measurement method will be described later. When the coated device is an ophthalmic lens, in order to prevent poor visibility and deformation caused by distortion of the refractive index due to an increase in water content, the change in water content of the device before and after coating is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 6% by mass or less. The method for measuring the water content will be described later.

[0096] When the coated device is an ophthalmic lens, in order to prevent corneal damage due to deformation, the size change rate of the device before and after coating is preferably ±5.00% or less, more preferably ±4.00% or less, and even more preferably ±3.00% or less.

[0097] The present invention will be specifically explained below with reference to examples, but the present invention is not limited to these. First, analytical and evaluation methods used in the examples will be described.

[0098] <Hydrophilicity (liquid film retention time)> After the heating step, the coated device (or devices) was allowed to cool to room temperature (20 to 23°C), and then lifted out of the solution in the container and held in the air with its longitudinal direction aligned with gravity. The time from the time the device began to be held in the air until part of the liquid film covering the device surface broke was visually observed, and the average of N=3 values ​​was evaluated according to the following criteria. The maximum measurement value was 120 seconds. A: The liquid film on the surface was held for 20 seconds or more. B: The liquid film on the surface broke in 15 to less than 20 seconds. C: The liquid film on the surface broke in 10 to less than 15 seconds. D: The liquid film on the surface broke in 1 to less than 10 seconds. E: The liquid film on the surface broke in less than 1 second.

[0099] <Hydrophilicity after immersion in fresh phosphate buffer solution for 26 hours (liquid film retention time after 26 hours)> In order to eliminate the influence of insufficiently adsorbed hydrophilic polymer on the device surface, the coated device or devices after the heating step were left to stand in 4 mL of fresh phosphate buffer solution in a glass vial at room temperature (20 to 23° C.) for 26 hours. The coated device or devices were then removed from the phosphate buffer solution in the glass vial as a sample (hereinafter referred to as "Sample S"), and evaluated in the same manner as for "hydrophilicity" above.

[0100] <Droplet Contact Angle (Droplet Contact Angle X) After Immersion in Fresh Phosphate Buffer Solution for 26 Hours> The above sample S was separately prepared and measured using a contact angle measurement device (droplet method) Drop Master DM500 (manufactured by Kyowa Interface Science Co., Ltd.). Specifically, after wiping off moisture from the surface of the coated device (or device), the device was placed on a hemispherical polypropylene plate with a diameter of 14.5 mm to prepare a sample. The sample was set in the contact angle measurement device, and phosphate buffer solution was dropped onto the sample to measure the droplet contact angle. The volume of the dropped droplet of phosphate buffer solution was 20 μL. The droplet contact angle was determined as the average of N=3 values ​​30 seconds after the drop.

[0101] <Moisture Content of Device and Coated Device> Before being subjected to the manufacturing method of the present invention, the device was immersed in a phosphate buffer solution and allowed to stand at room temperature (20 to 23°C) for 24 hours or more. The device was then removed from the phosphate buffer solution, and the surface moisture was wiped off with a wiping cloth "Kimwipe" (registered trademark) (manufactured by Nippon Paper Crecia Co., Ltd.). The mass (Ww) of the device was then measured. The device was then dried in a vacuum dryer at 40°C for 2 hours, and the mass (Wd) of the device was measured. The moisture content of the device was calculated from these masses using the following formula (1). The average value of N = 3 values ​​was taken as the moisture content. The moisture content of the coated device obtained after the heating step was also calculated in the same manner. Moisture content of device (mass%) = 100 × (Ww - Wd) / Ww ... Formula (1).

[0102] <Change in moisture content of device before and after coating> From the measurement results of the moisture content of the above device and the coated device, the change in moisture content (percentage points) was calculated using the following formula (2): Change in moisture content of device before and after coating (percentage points) = moisture content of coated device (mass %) - moisture content of device (mass %) Formula (2).

[0103] <Coefficient of Friction> The coefficient of friction of the surface of the coated device (or devices) wetted with phosphate buffer solution was measured with N=5 under the following conditions, and the average value of the N=5 values ​​was taken as the coefficient of friction. Apparatus: Friction Sensation Tester KES-SE (manufactured by Kato Tech Co., Ltd.) Friction SENS: H Measurement Speed: 2 × 1 mm / sec Friction Load: 44 g

[0104] <Friction Coefficient (Friction Coefficient X) After Immersion in Fresh Phosphate Buffer Solution for 26 Hours> The above sample S was prepared separately and evaluated in the same manner as in the above "friction coefficient."

[0105] <Friction coefficient (friction coefficient Y) after immersion in fresh phosphate buffer solution for 26 hours and subsequent scrubbing for 1 minute> The above sample S was separately prepared, held between the fingers (thumb and index finger) and scrubbed for 1 minute, and then evaluated in the same manner as the above "friction coefficient."

[0106] <Detection Depth of Hydrophilic Polymer> As a pretreatment, phosphate buffer solution was dropped onto the coated device (or devices) using a pipette, and the surface was lightly washed. Next, the coated device (or devices) was placed in 10 mL of phosphate buffer solution in a glass vial so that it was completely immersed, and left to stand at room temperature (20-23°C) for 24 hours. After that, it was air-dried on a clean Si wafer until the phosphate buffer solution droplets were no longer visible, and then it was introduced into an ultra-high vacuum chamber.

[0107] The pretreated sample was measured under the following conditions: Apparatus: TOF. SIMS 5 (manufactured by ION-TOF) Primary ion: Bi 3 ++ Secondary ion polarity: positive only Etching ions: Ar-GCIB (gas cluster ion beam).

[0108] <Non-uniformity of hydrophilic polymer> Cryosection images of the hydrophilic polymer coating the surface of the device were observed under the following conditions to evaluate the non-uniformity of the hydrophilic polymer. 4 Stained area and RuO 4 If both areas were unstained, the sample was judged to be heterogeneous. 4This was performed using stained frozen ultrathin sectioning. The coated device (or devices) was immersed in phosphate buffer for 24 hours to remove the effects of insufficiently adsorbed hydrophilic polymer on the device surface. Frozen ultrathin sections were then prepared and, while still frozen, were introduced into the apparatus using a cryotransfer holder. Observation area: Center of the coated device (or devices) Equipment: Atomic resolution analytical electron microscope JEM-ARM200F Dual-X (manufactured by JEOL) Measurement conditions: Accelerating voltage 200 kV.

[0109] <Amount of lipid deposition> 0.03 g of methyl palmitate, 10 g of pure water, and the coated device (or devices) were placed in a 20 cc screw tube. The screw tube was shaken for 3 hours at 37°C and 165 rpm. After shaking, the coated device (or devices) in the screw tube was scrubbed with 40°C tap water and household liquid detergent "Mama Lemon" (registered trademark) (manufactured by Lion Corporation). The washed sample was placed in a screw tube containing phosphate buffer and stored in a refrigerator at 4°C for 24 hours. The coated device (or devices) was then visually observed, and any cloudy areas were determined to indicate adhesion of methyl palmitate, and the area of ​​the methyl palmitate-adhered portion relative to the entire surface of the sample was observed.

[0110] <Mucin Adhesion Amount> A test piece measuring 5 mm wide (at the smallest part) and 14 mm long was cut from the coated device (or device) using a specified punching die. Calbiochem Mucin, Bovine Submaximal Grand (catalog number 499643) was used as the mucin. The test piece was immersed in a 0.1% aqueous mucin solution for 20 hours at 37°C, and the amount of mucin adhering to the sample was then quantified using a BCA (bicinchoninic acid) protein assay. The average value of N=3 was used as the mucin adhesion amount.

[0111] <Tensile modulus> A test piece measuring 5 mm in width (at the smallest part) and 14 mm in length was cut out from the coated device (or device) using a specified punching die. A tensile test was carried out using this test piece using a Tensilon RTG-1210 (manufactured by A&D Co., Ltd.). The tensile speed was 100 mm / min, and the distance between the grips (initial) was 5 mm. Measurements were carried out on both the device before the contacting step and the heating step, and the coated device after the contacting step and the heating step. Measurements were carried out with N=8, and the average of N=6 values ​​excluding the maximum and minimum values ​​was taken as the tensile modulus.

[0112] <Change in tensile modulus of device before and after coating> From the measurement results of the tensile modulus, the change in tensile modulus of the device before and after coating was calculated using the following formula (3): Change in tensile modulus of device before and after coating (%) = (tensile modulus of coated device after coating - tensile modulus of device before coating) / tensile modulus of device before coating × 100 Formula (3).

[0113] <Size> The longitudinal length of the coated device (or devices) (diameter in the case of a circular contact lens or the like) was measured N=3, and the average of the N=3 values ​​was taken as the size.

[0114] <Size Change Rate of Device Before and After Covering> From the size measurement results above, the size change rate before and after covering was calculated using the following formula (4).

[0115] Size change rate (%) before and after coating=(size of coated device after coating−size of device before coating) / size of device before coating×100 Equation (4).

[0116] <Measurement of Weight Average Molecular Weight> The weight average molecular weight (hereinafter referred to as "Mw") of the hydrophilic polymer was measured under the conditions shown below. Apparatus: Prominence GPC system (Shimadzu Corporation) Pump: LC-20AD Autosampler: SIL-20AV HT Column oven: CTO-20A Detector: RID-10A Column: GMPWXL (Tosoh Corporation, inner diameter 7.8 mm × 30 cm, particle size 13 μm) Solvent: water / methanol = 1 / 1 (0.1 N lithium nitrate added) Flow rate: 0.5 mL / min Measurement time: 60 minutes Sample concentration: 0.1 mass% Sample filtration: Filtration using a syringe filter with a pore size of 0.8 μm (Advantec Toyo Co., Ltd., DISMIC 25CS080AN) and a syringe filter with a pore size of 0.45 μm (Advantec Toyo Co., Ltd., DISMIC 13HP045AN) Sample injection volume: 10 to 20 μL Standard sample: polyethylene oxide standard sample (Agilent, 0.1 to 1258 kD).

[0117] <Viscosity Measurement> A 2 to 3.5 mass% aqueous solution of the hydrophilic polymer was measured using an SV-10H viscometer manufactured by A&D Corporation. <pH> The pH of the solution was measured using a Eutech pH2700 (manufactured by Eutech Instruments) as a pH meter. The "pH after heating step" of solution a was measured immediately after cooling solution a to room temperature (20 to 23°C) after the heating step.

[0118] <Phosphate Buffer Solution> The composition of the phosphate buffer solution used in the Examples and Comparative Examples is as follows: KCl 0.2 g / L KH 2 P.O. 4 0.2g / L NaCl 8.0g / L Na 2 HPO 4 1.19g / L EDTA 2 Na (disodium dihydrogen ethylenediaminetetraacetate) 0.5 g / L.

[0119] <Filterability of Hydrophilic Polymer> A hydrophilic polymer was dissolved in a phosphate buffer solution at 0.1% by mass. 50 g of this hydrophilic polymer solution was suction filtered through a 0.45 μm bottle-top filter (Thermo Fisher Scientific, model number 295-4545) and the filterability was evaluated based on the degree of clogging. A good result was obtained when the solution was continuously filtered, and a poor result was obtained when only one drop or less of the solution was filtered per 5 seconds.

[0120] <Copolymerization ratio of hydrophilic polymer> In order to calculate the copolymerization ratio of the hydrophilic polymer, the aqueous solution of the hydrophilic polymer was freeze-dried and extracted with acetonitrile to remove unreacted monomers, and then 1 H NMR measurement was carried out. 1 The copolymerization ratio of the constituent components was calculated from the peak area ratio of HNMR.

[0121] <Hydrophilic polymer concentration in aqueous hydrophilic polymer solution> The hydrophilic polymer concentration in the aqueous hydrophilic polymer solution after polymerization was calculated by measuring the mass of acetonitrile-insoluble matter obtained by freeze-drying the aqueous hydrophilic polymer solution and extracting it with acetonitrile to remove unreacted monomers, using the following formula (5): Hydrophilic polymer concentration (mass %) = Amount of acetonitrile-insoluble matter / Collected mass of aqueous hydrophilic polymer solution × 100 ... formula (5).

[0122] <Average particle size of hydrophilic polymer> A solution of hydrophilic polymer diluted with phosphate buffer to a concentration of 0.2% by mass was filtered through a 0.45 μm filter to prepare the measurement solution. Measurements were performed under the following conditions. Particle size distribution was confirmed at different temperatures using dynamic light scattering. Device name: Dynapro NanoStar, manufactured by Wyatt Technology. Light source: Semiconductor laser (wavelength: 658 nm). Measurement temperature: 25°C, 121°C* → Remeasurement after cooling to 25°C. Analysis method: Contin method. Number of measurements: 2 (measurement solution was reprepared and measured twice). *At 121°C, measurements were performed using the following procedure to prevent solvent evaporation. (1) Confirm that the measurement cell setting section has reached the target measurement temperature. (2) Place the measurement cell in the device and perform the measurement after 10 minutes. (3) After the measurement is completed, remove the measurement cell from the device.

[0123] <Charge of Hydrophilic Polymer> The zeta potential of a hydrophilic polymer solution under neutral conditions was measured by laser Doppler electrophoresis under the following conditions: Apparatus: Electrophoretic Light Scattering Photometer ELSZneo, manufactured by Otsuka Electronics Co., Ltd. Light source: Semiconductor laser (wavelength: 660 nm) Cell: Standard flow cell Voltage: 60 V Measurement temperature: 25°C Dispersion medium: 1 mM NaCl aqueous solution Number of measurements: 2 (measurement was performed twice with a different measurement solution (measurement was performed five times with the same measurement solution)) Charge: average value of 10 measurements Evaluation: a value within ±5 mV was determined to be no charge.

[0124] Synthesis Example 1 Into a 500 mL four-neck flask equipped with a stirrer, a thermometer, a condenser, and a three-way cock, 58.15 g of distilled water, 1.13 g of polyalkylene glycol monomethacrylate with methyl end chains (PME-100, manufactured by NOF Corporation, number of polyethylene glycol chains: 2 (m=2 (average value disclosed by the manufacturer), 6 mmol), 2.58 g of N,N-dimethylacrylamide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 26 mmol), and 1.28 g of glycerol methacrylate (GLM, manufactured by NOF Corporation, 8 mmol) were placed, and ultrasonic degassing and nitrogen substitution were performed five times. After completion of nitrogen substitution in the system, the mixture was stirred in an oil tank set at 85°C. The bottom of the flask was immersed in a bathtub. Once the internal temperature of the flask exceeded 70°C, 2.7 mg of polymerization initiator V-50 (Fujifilm Wako Pure Chemical Industries, Ltd., 0.01 mmol) dissolved in 20.00 g of distilled water was added in five divided doses at 5-minute intervals. After the entire amount of polymerization initiator was added, the internal temperature of the flask was maintained at 70 to 75°C for 4 hours to obtain an aqueous solution of a side chain-terminated methyl polyalkylene glycol monomethacrylate (PME-100) / N,N-dimethylacrylamide / glycerol methacrylate copolymer (molar ratio in copolymerization: 15 / 65 / 20, weight-average molecular weight: 200,000, viscosity of 2.3% by mass aqueous solution: 2.7 mPa s).

[0125] Synthesis Example 2 A 500 mL four-neck flask equipped with a stirrer, thermometer, condenser, and three-way stopcock was charged with 38.13 g of distilled water, 0.75 g of side chain terminal methyl polyalkylene glycol monomethacrylate (PME-100, 4 mmol), 2.38 g of N,N-dimethylacrylamide (Fujifilm Wako Pure Chemical Industries, Ltd., 24 mmol), and 1.92 g of glycerol methacrylate (GLM, 12 mmol), and ultrasonic degassing and nitrogen substitution were performed five times. After completion of nitrogen substitution in the system, the bottom of the flask was immersed in an oil bath set to 85°C while stirring. Once the temperature inside the flask exceeded 70°C, 2.7 mg of polymerization initiator V-50 dissolved in 20.00 g of distilled water was added in five divided doses at 5-minute intervals. After the entire amount of the polymerization initiator was added, the flask was kept at an internal temperature of 70 to 75°C for 4 hours to obtain an aqueous solution of a side chain terminal methyl polyalkylene glycol monomethacrylate / N,N-dimethylacrylamide / glycerol methacrylate copolymer (molar ratio in copolymerization: 10 / 60 / 30, weight average molecular weight: 210,000, viscosity of 2.3% by mass aqueous solution: 1.7 mPa s).

[0126] Synthesis Example 3 A 100 mL three-neck flask was charged with 3.20 g of methoxytetraethylene glycol methacrylate (NOF Corp., "Blenmer" (registered trademark) PME-200, 11.6 mmol), 50.1 mg of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] as a polymerization initiator (VA-061, Wako Pure Chemical Industries, Ltd., 0.200 mmol), and 28.23 g of distilled water (Fujifilm Wako Pure Chemical Industries, Ltd.), and the flask was equipped with a digital thermometer, a Dimroth condenser equipped with a three-way stopcock, and a sealer with a stirring blade. Under ultrasonic irradiation, a cycle of suction to 10 mmHg and nitrogen flushing was repeated five times to remove dissolved oxygen from the mixed solution. Subsequently, the mixture was reacted for 7 hours with stirring at 60°C in an oil bath, and then the reaction vessel was removed from the oil bath and air-cooled. 50 mL of methanol was added to the polymerization reaction solution and stirred to reduce the viscosity, then transferred to a 1 L Teflon (registered trademark) beaker and heated and dried at 40°C overnight in a vacuum dryer. After drying, 5 mL of isopropanol (IPA) was added to the resulting viscous solid to dissolve it, and the mixture was left standing overnight in a refrigerator. After cooling, the supernatant was removed by decantation, and the mixture was dried at 30°C for 2 hours in a vacuum dryer to obtain a white powder polymer. The weight-average molecular weight of the resulting methoxypolyethylene glycol methacrylate homopolymer (number of ethylene oxide repeating units: 4) was 250,000.

[0127] Synthesis Example 4 A 500 mL four-neck flask equipped with a stirrer, thermometer, condenser, and three-way stopcock was charged with 82.18 g of distilled water, 3.97 g of polyalkylene glycol monomethacrylate with methyl end chains (NOF Corporation, PME-400, polyethylene glycol chain number 9 (m = 9 in Formula (I) (average value disclosed by the manufacturer)), 8 mmol), 6.34 g of N,N-dimethylacrylamide (Fujifilm Wako Pure Chemical Industries, Ltd., 64 mmol), and 1.04 g of 2-hydroxyethyl methacrylate (Fujifilm Wako Pure Chemical Industries, Ltd., 8 mmol). Ultrasonic degassing and nitrogen substitution were performed five times. After completion of nitrogen substitution in the system, the bottom of the flask was immersed in an oil bath set to 85°C while stirring. Once the temperature inside the flask exceeded 70°C, 5.4 mg of polymerization initiator V-50 (0.02 mmol) dissolved in 20.00 g of distilled water was added in five divided doses at 5-minute intervals. After the entire amount of the polymerization initiator was added, the flask was kept at an internal temperature of 80 to 85°C for 4 hours, thereby obtaining an aqueous solution of a polyalkylene glycol monomethacrylate having a side chain terminated with methyl / N,N-dimethylacrylamide / 2-hydroxyethyl methacrylate copolymer (molar ratio in copolymerization: 10 / 80 / 10, weight average molecular weight: 300,000, viscosity of 3.4% by mass aqueous solution: 50 mPa s).

[0128] Synthesis Example 5 Into a 500 mL four-neck flask equipped with a stirrer, a thermometer, a condenser, and a three-way cock, 34.52 g of tert-amyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 9.22 g of polyalkylene glycol monomethacrylate with methyl end chains (PME-100, 49 mmol), 4.96 g of N,N-dimethylacrylamide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 50 mmol), and silicone monomer T represented by the following chemical formula (II) were added. 10.61 g (manufactured by Toray Industries, Inc., 1 mmol) and 0.0248 g of polymerization initiator 2,2-azobis(2,4-dimethylvaleronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 0.1 mmol) were added, and ultrasonic degassing and nitrogen substitution were performed five times. After completing the nitrogen substitution in the system, the bottom of the flask was immersed in an oil bath set to 85°C while stirring. The internal temperature of the flask was kept at 70 to 75°C for 4 hours, and the side chain terminal methyl polyalkylene glycol monomethacrylate / N,N-dimethylacrylamide / silicone monomer T 1 An aqueous copolymer solution was obtained. 43 mL of ethanol was added to the obtained aqueous copolymer solution and stirred to reduce the viscosity, and then the solution was dropped into 740 mL of hexane to precipitate the copolymer. The precipitated copolymer was heated and dried at 60°C for 4 hours in a vacuum dryer. The molar ratio of the copolymer obtained was 49 / 50 / 1. Since some of the copolymer remained undissolved and was not completely dissolved in the measurement solvent, the weight average molecular weight and viscosity could not be measured.

[0129]

[0130] Synthesis Example 6 Into a 500 mL four-neck flask equipped with a stirrer, a thermometer, a condenser, and a three-way cock, 34.07 g of tert-amyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 9.22 g of polyalkylene glycol monomethacrylate with methyl end chains (PME-100, 49 mmol), 4.96 g of N,N-dimethylacrylamide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 50 mmol), and silicone monomer T represented by the following chemical formula (III): 2 0.42 g (manufactured by Toray Industries, Inc., 1 mmol) and 0.0248 g of polymerization initiator 2,2-azobis(2,4-dimethylvaleronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 0.1 mmol) were added, and ultrasonic degassing and nitrogen substitution were performed five times. After completing the nitrogen substitution in the system, the bottom of the flask was immersed in an oil bath set to 85°C while stirring. The internal temperature of the flask was kept at 70 to 75°C for 4 hours, and the side chain terminal methyl polyalkylene glycol monomethacrylate / N,N-dimethylacrylamide / silicone monomer T 2An aqueous copolymer solution was obtained. 43 mL of ethanol was added to the obtained aqueous copolymer solution and stirred to reduce the viscosity, and then the solution was dropped into 740 mL of hexane to precipitate the copolymer. The precipitated polymer was heated and dried at 60°C for 4 hours in a vacuum dryer. The molar ratio of the copolymer obtained was 49 / 50 / 1. Since some of the copolymer remained undissolved and was not completely dissolved in the measurement solvent, the weight average molecular weight and viscosity could not be measured.

[0131]

[0132] Synthesis Example 7 A 500 mL four-neck flask equipped with a stirrer, thermometer, condenser, and three-way stopcock was charged with 45.15 g of distilled water, 0.75 g of side chain terminal methyl polyalkylene glycol monomethacrylate (PME-100, 4 mmol), 1.39 g of N,N-dimethylacrylamide (Fujifilm Wako Pure Chemical Industries, Ltd., 14 mmol), and 3.52 g of glycerol methacrylate (GLM, 22 mmol). Ultrasonic degassing and nitrogen substitution were performed five times. After completion of nitrogen substitution in the system, the bottom of the flask was immersed in an oil bath set at 85°C while stirring. Once the internal temperature of the flask exceeded 70°C, 2.7 mg of polymerization initiator V-50 (0.01 mmol) dissolved in 20.00 g of distilled water was added in five divided doses at 5-minute intervals. After the entire amount of the polymerization initiator was added, the flask was kept at an internal temperature of 70 to 75°C for 4 hours to obtain an aqueous solution of a side chain terminal methyl polyalkylene glycol monomethacrylate / N,N-dimethylacrylamide / glycerol methacrylate copolymer (molar ratio in copolymerization: 10 / 35 / 55, weight average molecular weight: 220,000, viscosity of 3.4% by mass aqueous solution: 50 mPa s).

[0133] Synthesis Example 8 A 500 mL four-neck flask equipped with a stirrer, thermometer, condenser, and three-way stopcock was charged with 33.15 g of distilled water, 1.13 g of polyalkylene glycol monomethacrylate with methyl end chains (PME-100, 6 mmol), 3.17 g of N,N-dimethylacrylamide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 32 mmol), and 0.32 g of glycerol methacrylate (GLM, 2 mmol). Ultrasonic degassing and nitrogen substitution were performed five times. After completion of nitrogen substitution in the system, the bottom of the flask was immersed in an oil bath set at 85°C while stirring. Once the internal temperature of the flask exceeded 70°C, 2.7 mg of polymerization initiator V-50 (0.01 mmol) dissolved in 20.00 g of distilled water was added in five divided doses at 5-minute intervals. After the entire amount of the polymerization initiator was added, the flask was kept at an internal temperature of 70 to 75°C for 4 hours to obtain an aqueous solution of a side chain terminal methyl polyalkylene glycol monomethacrylate / N,N-dimethylacrylamide / glycerol methacrylate copolymer (molar ratio in copolymerization: 15 / 80 / 5, weight average molecular weight: 230,000, viscosity of 2.3% by mass aqueous solution: 15 mPa s).

[0134] Synthesis Example 9 A 500 mL four-neck flask equipped with a stirrer, a thermometer, a condenser, and a three-way cock was charged with 46.17 g of distilled water, 2.07 g of polyalkylene glycol monomethacrylate with methyl end chains (PME-200, manufactured by NOF Corporation, polyethylene glycol chain number 4 (m = 4 (average value disclosed by the manufacturer), 7.5 mmol), 2.48 g of N,N-dimethylacrylamide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 25 mmol), and 2.80 g of glycerol methacrylate (GLM-EX, manufactured by NOF Corporation, 17.5 mmol), and ultrasonic degassing and nitrogen substitution were performed five times. After completion of nitrogen substitution in the system, the temperature was set to 85°C with stirring. The bottom of the flask was immersed in an oil bath. Once the internal temperature of the flask exceeded 70°C, 3.4 mg of polymerization initiator V-50 (Fujifilm Wako Pure Chemical Industries, Ltd., 0.0125 mmol) dissolved in 20.00 g of distilled water was added in five divided doses at 5-minute intervals. After the entire polymerization initiator was added, the internal temperature of the flask was maintained at 70 to 75°C for 4 hours to obtain an aqueous solution of a side chain-terminated methyl polyalkylene glycol monomethacrylate (PME-200) / N,N-dimethylacrylamide / glycerol methacrylate copolymer (molar ratio in copolymerization: 15 / 50 / 35, weight average molecular weight: 290,000, viscosity of 3.5% by mass aqueous solution: 1040 mPa s).

[0135] Synthesis Example 10 Into a 500 mL four-neck flask equipped with a stirrer, a thermometer, a condenser, and a three-way cock, 44.34 g of distilled water, 1.13 g of polyalkylene glycol monomethacrylate with methyl end chains (PME-100, manufactured by NOF Corporation, polyethylene glycol chain number 2 (m=2 in formula (I) (average value disclosed by the manufacturer), 6 mmol), 2.22 g of N-vinylpyrrolidone (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 20 mmol), and 2.24 g of glycerol methacrylate (GLM-EX, manufactured by NOF Corporation, 14 mmol) were placed, and ultrasonic degassing and nitrogen substitution were performed five times. After completion of nitrogen substitution in the system, the temperature was set at 85° C. while stirring. The bottom of the flask was immersed in an oil bath. Once the internal temperature of the flask exceeded 70°C, 2.7 mg of polymerization initiator V-50 (Fujifilm Wako Pure Chemical Industries, Ltd., 0.01 mmol) dissolved in 20.00 g of distilled water was added in five divided doses at 5-minute intervals. After the entire polymerization initiator was added, the internal temperature of the flask was maintained at 70 to 75°C for 4 hours to obtain an aqueous solution of a side chain-terminated methyl polyalkylene glycol monomethacrylate (PME-100) / N-vinylpyrrolidone / glycerol methacrylate copolymer (molar ratio in copolymerization: 15 / 50 / 35, weight average molecular weight: 300,000, viscosity of 2.3% by mass aqueous solution: 10.6 mPa s).

[0136] Synthesis Example 11 Into a 500 mL four-neck flask equipped with a stirrer, a thermometer, a condenser, and a three-way cock, 32.14 g of distilled water, 0.85 g of polyalkylene glycol monomethacrylate with methyl end chains (PME-100, manufactured by NOF Corporation, polyethylene glycol chain number 2 (m = 2 (average value disclosed by the manufacturer), 4.5 mmol), 1.64 g of N,N-dimethylacrylamide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 16.5 mmol), and 1.44 g of glycerol methacrylate (GLM, manufactured by NOF Corporation, 9 mmol) were placed, and ultrasonic degassing and nitrogen substitution were performed five times. After completion of nitrogen substitution in the system, the mixture was stirred in an oven set at 85°C. The bottom of the flask was immersed in a water bath. Once the internal temperature of the flask exceeded 70°C, 2.0 mg of polymerization initiator V-50 (Fujifilm Wako Pure Chemical Industries, Ltd., 0.0075 mmol) dissolved in 20.00 g of distilled water was added in five divided doses at 5-minute intervals. After the entire amount of polymerization initiator was added, the internal temperature of the flask was maintained at 70 to 75°C for 4 hours to obtain an aqueous solution of a side chain-terminated methyl polyalkylene glycol monomethacrylate (PME-100) / N,N-dimethylacrylamide / glycerol methacrylate copolymer (molar ratio in copolymerization: 15 / 55 / 30, weight average molecular weight: 370,000, viscosity of 2.3% by mass aqueous solution: 10.4 mPa s).

[0137] Example 1 The "device" used was a commercially available silicone hydrogel lens "Ultra 1day" (registered trademark) (Kalifilcon A, manufactured by Bausch & Lomb), which is primarily composed of silicone. The "container" was a glass vial. The "solution a" used was 3 mL of a solution containing 0.2% by mass of PME-100 / N,N-dimethylacrylamide / glycerol methacrylate copolymer, the hydrophilic polymer A obtained in Synthesis Example 1, in a phosphate buffer solution. The device was immersed in the solution a ((A) contacting step), the glass vial was sealed with a cap ((B) sealing step), and then heated at 121°C for 10 minutes in an autoclave ((C) heating step). The results of evaluating the obtained coated device using the above method are shown in Tables 1 to 3.

[0138] [Example 2] The same procedure as in Example 1 was carried out, except that a commercially available silicone hydrogel lens "Acuvue Oasys" (registered trademark) (senofilcon A, manufactured by Johnson & Johnson) containing polyvinylpyrrolidone and silicone as its main components was used as the device. The results of evaluation of the obtained coated device by the above-mentioned method are shown in Tables 1 to 3.

[0139] [Example 3] The same procedure as in Example 1 was carried out, except that a commercially available hydrogel lens "Medalist 1day Plus" (registered trademark) (manufactured by Bausch & Lomb, hilafilcon B) containing 2-hydroxyethyl methacrylate as the main component was used as the device. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 1 to 3.

[0140] Example 4 The same operations as in Example 1 were carried out, except that a solution containing 0.3% by mass of PME-100 / N,N-dimethylacrylamide / glycerol methacrylate copolymer, which is the hydrophilic polymer A obtained in Synthesis Example 2 above, in a phosphate buffer solution was used instead of solution a, and heating was carried out in an autoclave at 121° C. for 30 minutes. The results of evaluating the obtained coated device by the above-mentioned method are shown in Tables 1 to 3.

[0141] Example 5 The same procedure as in Example 4 was carried out, except that a commercially available silicone hydrogel lens "Acuvue Oasys" (registered trademark) was used as the device. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 1 to 3.

[0142] [Example 6] The same procedure as in Example 4 was carried out, except that a commercially available hydrogel lens "Medalist One Day Plus" (registered trademark) was used as the device. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 1 to 3.

[0143] Example 7 The same operations as in Example 1 were carried out, except that the device used was a commercially available silicone hydrogel lens "1day Acuvue TruEye" (registered trademark) (manufactured by Johnson & Johnson, Narafilcon A) containing polyvinylpyrrolidone and silicone as the main components, and a solution containing 0.2% by mass of PME-200 / N,N-dimethylacrylamide / glycerol methacrylate copolymer, which is the hydrophilic polymer A obtained in Synthesis Example 9 above, in a phosphate buffer solution was used instead of solution a, and the device was heated in an autoclave at 121°C for 30 minutes. The results of evaluating the obtained coated device by the above-mentioned method are shown in Tables 1 to 3.

[0144] Example 8 The same procedure as in Example 7 was carried out, except that a commercially available silicone hydrogel lens "Acuvue Oasys" (registered trademark) was used as the device. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 1 to 3.

[0145] Example 9 The same procedure as in Example 7 was carried out, except that a solution containing 0.3% by mass of PME-100 / N-vinylpyrrolidone / glycerol methacrylate copolymer (hydrophilic polymer A obtained in Synthesis Example 10) in a phosphate buffer solution was used instead of solution a. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 1 to 3.

[0146] Example 10 The same procedure as in Example 9 was carried out, except that a commercially available silicone hydrogel lens "Acuvue Oasys" (registered trademark) was used as the device. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 1 to 3.

[0147] Example 11 The same procedure as in Example 1 was carried out, except that the commercially available silicone hydrogel lens "1day Acuvue TruEye" (registered trademark) was used as the device, and PME-100 / N,N-dimethylacrylamide / glycerol methacrylate copolymer, which is the hydrophilic polymer A obtained in Synthesis Example 11 above, was used instead of solution a. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 1 to 3.

[0148] Example 12 The same procedures as in Example 1 were carried out, except that the device used was a commercially available silicone hydrogel lens "1day Acuvue Oasys" (registered trademark) (senofilcon A, manufactured by Johnson & Johnson) containing polyvinylpyrrolidone and silicone as the main components, and a solution containing 0.07% by mass of a PME-100 / N,N-dimethylacrylamide / glycerol methacrylate copolymer aqueous solution (molar ratio in copolymerization: 24 / 27 / 49, weight-average molecular weight: 180,000, viscosity of 2.3% by mass aqueous solution: 10.7 mPa s), a hydrophilic polymer A manufactured by Osaka Organic Chemical Industry Ltd., was used instead of solution a, and the device was heated in an autoclave at 121°C for 14 minutes. The results of evaluating the obtained coated device by the above-mentioned method are shown in Tables 1 to 3.

[0149] Example 13 The same procedure as in Example 12 was carried out, except that a commercially available silicone hydrogel lens "1day Acuvue TruEye" (registered trademark) was used as the device. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 1 to 3.

[0150] Example 14 The same procedure as in Example 12 was carried out, except that solution a was replaced with an aqueous solution of PME-100 / N,N-dimethylacrylamide / glycerol methacrylate copolymer (hydrophilic polymer A manufactured by Osaka Organic Chemical Industry Co., Ltd., molar ratio in copolymerization: 24 / 27 / 49, weight average molecular weight: 510,000, viscosity of 2.3% by mass aqueous solution: 10.9 mPa s). The coated devices obtained were evaluated by the above-mentioned methods, and the results are shown in Tables 1 to 3.

[0151] Example 15 The same procedure as in Example 14 was carried out, except that a commercially available silicone hydrogel lens "1day Acuvue TruEye" (registered trademark) was used as the device. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 1 to 3.

[0152]

[0153]

[0154]

[0155]

[0156] Comparative Example 1 The same procedures as in Example 1 were carried out, except that a commercially available silicone hydrogel lens "Acuvue Oasys" (registered trademark) was used as a device, and a solution containing 0.2% by mass of acrylic acid / vinylpyrrolidone / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization: 1 / 1 / 2, Mw: 550,000, manufactured by Osaka Organic Chemical Industry Ltd.) in a phosphate buffer solution was used instead of solution a, and the device was heated in an autoclave at 121°C for 30 minutes. The results of evaluating the obtained coated device by the above-mentioned method are shown in Tables 4 to 6.

[0157] Comparative Example 2 The same procedure as in Comparative Example 1 was carried out, except that a solution containing 0.1% by mass of acrylic acid / vinylpyrrolidone / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization: 1 / 1 / 2, Mw: 330,000, manufactured by Osaka Organic Chemical Industry Ltd.) in a phosphate buffer solution was used instead of solution a. The obtained coated devices were evaluated by the above-mentioned methods, and the results are shown in Tables 4 to 6.

[0158] Comparative Example 3 The same procedure as in Comparative Example 1 was carried out, except that a solution containing 0.1% by mass of acrylic acid / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization: 1 / 9, Mw: 300,000, manufactured by Osaka Organic Chemical Industry Ltd.) in a phosphate buffer solution was used instead of solution a. The results of evaluation of the obtained coated device by the above-mentioned method are shown in Tables 4 to 6.

[0159] Comparative Example 4 The same procedure as in Comparative Example 1 was carried out, except that a commercially available hydrogel lens "Medalist One Day Plus" (registered trademark) was used as the device, and a solution containing 0.3% by mass of polyethylene glycol (Mw: 500,000, manufactured by Wako Pure Chemical Industries, Ltd.) in a phosphate buffer solution was used instead of solution a. The results of evaluation of the obtained coated device by the above-mentioned method are shown in Tables 4 to 6.

[0160] Comparative Example 5 The same procedure as in Comparative Example 1 was carried out, except that a solution containing 0.1% by mass of an acrylic acid / vinylpyrrolidone copolymer (molar ratio in copolymerization: 1 / 4, Mw: 590,000, manufactured by Osaka Organic Chemical Industry Ltd.) in a phosphate buffer solution was used instead of solution a. The results of evaluation of the obtained coated device by the above-mentioned method are shown in Tables 4 to 6.

[0161] Comparative Example 6 The same procedure as in Comparative Example 1 was carried out, except that a solution containing 0.1% by mass of an acrylic acid / vinylpyrrolidone copolymer (molar ratio in copolymerization: 1 / 9, Mw: 390,000, manufactured by Osaka Organic Chemical Industry Ltd.) in a phosphate buffer solution was used instead of solution a. The results of evaluation of the obtained coated devices by the above-mentioned methods are shown in Tables 4 to 6.

[0162] Comparative Example 7 The same procedure as in Comparative Example 1 was carried out, except that a solution containing 0.2 mass % of acrylic acid / 2-hydroxyethyl methacrylate / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization: 1 / 1 / 2, Mw: 430,000, manufactured by Osaka Organic Chemical Industry Ltd.) in a phosphate buffer solution was used instead of solution a. The obtained coated devices were evaluated by the above-mentioned methods, and the results are shown in Tables 4 to 6.

[0163] Comparative Example 8 The same procedure as in Comparative Example 1 was carried out, except that a solution containing 0.2 mass % of acrylic acid / 2-hydroxyethyl methacrylate / N,N-dimethylacrylamide copolymer (molar ratio in copolymerization: 1 / 1 / 8, Mw: 480,000, manufactured by Osaka Organic Chemical Industry Ltd.) in a phosphate buffer solution was used instead of solution a. The obtained coated devices were evaluated by the above-mentioned methods, and the results are shown in Tables 4 to 6.

[0164] Comparative Example 9 The same procedure as in Comparative Example 1 was carried out, except that a solution containing 0.3% by mass of polyvinylpyrrolidone (Mw: 500,000, manufactured by Osaka Organic Chemical Industry Ltd.) in a phosphate buffer solution was used instead of solution a. The results of evaluation of the obtained coated device (by the above-mentioned method) are shown in Tables 4 to 6.

[0165] Comparative Example 10 The same procedure as in Comparative Example 1 was carried out, except that a solution containing 0.3% by mass of poly-N,N-dimethylacrylamide (Mw: 700,000, manufactured by Wako Pure Chemical Industries, Ltd.) in a phosphate buffer solution was used instead of solution a. The results of evaluation of the obtained coated device by the above-mentioned method are shown in Tables 4 to 6.

[0166] Comparative Example 11 The same procedure as in Example 1 was carried out, except that a phosphate buffer solution was used instead of solution a and heating was carried out in an autoclave at 121° C. for 30 minutes. The obtained device was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.

[0167] Comparative Example 12 The same procedure as in Comparative Example 11 was carried out, except that a commercially available silicone hydrogel lens "Acuvue Oasys" (registered trademark) was used as the device. The obtained device was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.

[0168] Comparative Example 13 The same procedure as in Comparative Example 11 was carried out, except that a commercially available hydrogel lens, "Medalist One Day Plus" (registered trademark), was used as the device. The obtained device was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.

[0169] Comparative Example 14 The same procedure as in Comparative Example 10 was carried out, except that a commercially available hydrogel lens, "Medalist One Day Plus" (registered trademark), was used as the device. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.

[0170] Comparative Example 15 The same procedure as in Comparative Example 14 was carried out, except that a solution containing 0.2% by mass of the methoxypolyethylene glycol methacrylate homopolymer (number of polyethylene glycol chains: 4, Mw: 250,000, manufactured by Toray Industries, Inc.) obtained in Synthesis Example 3 above was used instead of solution a. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.

[0171] Comparative Example 16 The same procedure as in Comparative Example 15 was carried out, except that a commercially available silicone hydrogel lens "Ultra 1day" (registered trademark) (Kalifilcon A, manufactured by Bausch & Lomb) was used. The results of evaluation of the obtained coated device by the above-mentioned method are shown in Tables 4 to 6.

[0172] Comparative Example 17 The same procedure as in Comparative Example 15 was carried out, except that a commercially available silicone hydrogel lens "Acuvue Oasys" (registered trademark) was used as the device. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.

[0173] Comparative Example 18 The same procedure as in Comparative Example 11 was carried out, except that a commercially available hydrogel lens "1dayAcuvue" (registered trademark) (manufactured by Johnson & Johnson, etafilcon A) containing 2-hydroxyethyl methacrylate as the main component was used as the device. The obtained device was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.

[0174] Comparative Example 19 The same operations as in Comparative Example 11 were carried out, except that a commercially available hydrogel lens "Proclear 1day" (registered trademark) (Omafilcon A, manufactured by Cooper Vision) containing, as the main component, 2-hydroxyethyl methacrylate copolymerized with MPC monomer (2-methacryloyloxyethyl phosphorylcholine) was used as the device. The obtained device was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.

[0175] [Comparative Example 20] The same operation as in Comparative Example 11 was carried out, except that a commercially available hydrogel color lens "1day Acuvue Define Moist" (registered trademark) containing 2-hydroxyethyl methacrylate as the main component was used as the device. The obtained device was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.

[0176] Comparative Example 21 The same procedure as in Comparative Example 11 was carried out, except that a commercially available silicone hydrogel lens "1day Acuvue Trueye" (registered trademark), whose main components are polyvinylpyrrolidone and silicone, was used as the device. The obtained device was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.

[0177] Comparative Example 22 The same procedure as in Comparative Example 11 was carried out, except that a commercially available silicone hydrogel lens "Air Optics Aqua" (registered trademark) (manufactured by Alcon Japan Co., Ltd., Lotrafilcon A), whose main component is silicone and whose lens surface has been plasma-treated, was used as the device. The obtained device was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.

[0178] Comparative Example 23 The same operations as in Example 1 were carried out, except that a solution containing 0.3% by mass of the PME-400 / N,N-dimethylacrylamide / 2-hydroxyethyl methacrylate copolymer obtained in Synthesis Example 4 above in a phosphate buffer solution was used instead of solution a, and the solution was heated in an autoclave at 121° C. for 30 minutes. The results of evaluating the obtained coated device by the above-mentioned method are shown in Tables 4 to 6.

[0179] Comparative Example 24: Instead of solution a, PME-100 / N,N-dimethylacrylamide / silicone monomer T obtained in Synthesis Example 5 was used. 1 The same procedure as in Comparative Example 23 was carried out, except that a solution containing 0.3% by mass of the copolymer in phosphate buffer was used. The results of evaluation of the obtained coated devices by the above-mentioned methods are shown in Tables 4 to 6.

[0180] Comparative Example 25: Instead of solution a, PME-100 / N,N-dimethylacrylamide / silicone monomer T obtained in Synthesis Example 6 was used. 2 The same operation as in Comparative Example 23 was carried out, except that a solution containing 0.3% by mass of the above in a phosphate buffer solution was used. The results of evaluation of the obtained coated device by the above-mentioned method are shown in Tables 4 to 6.

[0181] Comparative Example 26 The same procedure as in Comparative Example 23 was carried out, except that a solution containing 0.3% by mass of the PME-100 / N,N-dimethylacrylamide / hydroxyl group-containing monomethacrylate copolymer obtained in Synthesis Example 7 above in a phosphate buffer solution was used instead of solution a. The coated devices obtained were evaluated by the above-mentioned methods, and the results are shown in Tables 4 to 6.

[0182] Comparative Example 27 The same procedure as in Example 2 was carried out, except that a solution containing 0.3% by mass of PME-100 / N,N-dimethylacrylamide / hydroxyl group-containing monomethacrylate obtained in Synthesis Example 8 above in phosphate buffer was used instead of solution a. The obtained coated device was evaluated by the above-mentioned method, and the results are shown in Tables 4 to 6.

[0183]

[0184]

[0185]

[0186]

[0187] From a comparison of the results of the Examples and Comparative Examples, it is clear that the present invention can impart sufficient hydrophilicity and lubricity to a device, as well as excellent lipid adhesion inhibitory properties and mucin adhesion inhibitory properties.

[0188] Furthermore, when focusing on the change in the coefficient of friction before and after immersion in phosphate buffer for 26 hours, i.e., the difference between the above-mentioned coefficient of friction and the above-mentioned coefficient of friction X, systems in which the amount of change is small can be said to have a device surface coated with a highly slippery hydrophilic polymer that has higher adsorptive power and superior durability. The results of Examples 1 to 15 correspond to this. Furthermore, when focusing on scrubbing resistance, systems in which the value of the above-mentioned coefficient of friction Y is smaller than the value for a device containing no hydrophilic polymer can be said to have a device surface coated with a hydrophilic polymer that has particularly excellent adsorptive power. The results of Examples 1, 2, 4, 5 and 7 to 15 for silicone hydrogel-based devices correspond to this.

Claims

1. A coated device comprising: a device; and a hydrophilic polymer coating a surface of the device, the hydrophilic polymer including a hydrophilic polymer A, the hydrophilic polymer A including, as monomer units, a compound a1 represented by the following general formula (I), a compound a2 having an amide group, and a compound a3 having a plurality of hydroxyl groups, the copolymerization ratios of the compound a1, the compound a2, and the compound a3 being 1 to 96% by mass, 1 to 96% by mass, and 8 to 61% by mass of the compound a3. [In general formula (I), R 1 represents a hydrogen atom or a methyl group, and X represents an oxygen atom or NR 2 represents R 2 represents a hydrogen atom or an alkyl group, m represents an integer of 1 to 30, and Y represents a hydrogen atom or an alkyl group.

2. The coated device according to claim 1, wherein said compound a3 is glycerol (meth)acrylate.

3. The coated device according to claim 1 or 2, wherein the change in the average particle size of the hydrophilic polymer A is irreversible when the temperature is lowered after heating.

4. The coated device according to claim 1 or 2, wherein the detection depth of the hydrophilic polymer A is 10 μm or less.

5. The coated device according to claim 1 or 2, wherein the hydrophilic polymer A coating the surface of the device is present non-uniformly in a frozen state.

6. The coated device of claim 1 or 2, wherein the device is a medical device.

7. The coated device of claim 6, wherein said device comprises a material selected from the group consisting of hydrogels, silicone hydrogels, low water content soft materials and low water content hard materials.

8. The coated device of claim 7, wherein the hydrogel is selected from the group consisting of tefilcon, tetrafilcon, helfilcon, mafilcon, polymacon, hioxifilcon, alfafilcon, omafilcon, nelfilcon, nesofilcon, hilafilcon, acofilcon, deltafilcon, etafilcon, focofilcon, ocufilcon, phemfilcon, methafilcon and vilfilcon.

9. The coated device of claim 7, wherein said silicone hydrogel is selected from the group consisting of lotrafilcon, galyfilcon, narafilcon, senofilcon, comfilcon, enfilcon, balafilcon, efrofilcon, fanfilcon, somofilcon, samfilcon, olifilcon, asmofilcon, formofilcon, stenfilcon, abafilcon, mangofilcon, riofilcon, sifilcon, larafilcon, kalifilcon and delefilcon.

10. The coated device of claim 7, wherein said low water content soft material or said low water content hard material is selected from the group consisting of polysulfone, polystyrene, polymethyl methacrylate, polyurethane and polyamide.

11. The coated device of claim 6, wherein the device is selected from the group consisting of ophthalmic lenses, skin coverings, wound coverings, skin protective materials, dermal drug carriers, infusion tubes, gas transport tubes, drainage tubes, blood circuits, covering tubes, catheters, stents, sheaths, biosensor chips, heart-lung machines, and covering materials for endoscopes.

12. A method for producing a coated device according to claim 1 or 2, comprising: (A) a contacting step of storing a device in a container and bringing the device into contact with a solution a containing a hydrophilic polymer A; and (C) a heating step of heating the container, wherein the hydrophilic polymer A contains, as monomer units, a compound a1 represented by the following general formula (I), a compound a2 having an amide group, and a compound a3 having a plurality of hydroxyl groups, and the copolymerization ratios of the compound a1, the compound a2, and the compound a3 are 1 to 96% by mass of the compound a1, 1 to 96% by mass of the compound a2, and 8 to 61% by mass of the compound a3, [In general formula (I), R 1 represents a hydrogen atom or a methyl group, and X represents an oxygen atom or NR 2 represents R 2 represents a hydrogen atom or an alkyl group, m represents an integer of 1 to 30, and Y represents a hydrogen atom or an alkyl group.] The method for producing a coated device, wherein the pH of solution a after the heating step is 6.1 to 8.

0.

13. The method for producing a coated device according to claim 12, further comprising a sealing step (B) of sealing the container containing the device.

14. The method of claim 12, wherein the heating step sterilizes the device.

Citation Information

Patent Citations

  • Cross-linked hydrophilic coated silicone hydrogel lens

    JP2014533381A

  • Comfortable ophthalmic devices and their manufacturing methods

    JP5154231B2

  • Medical treatment device, composition for coating solution, and method for manufacturing medical treatment device

    WO2013024799A1

  • Low-moisture-content soft device and method for producing same

    WO2013024800A1

  • Lens solution, contact lens, and production method therefor

    WO2015119256A1