Vinyl-based polymer, method for producing same, polishing liquid, and vinyl-based monomer

A stable vinyl polymer with specific structural units is used in semiconductor polishing liquids to address the hydrolysis issues of (meth)acrylic acid ester polymers, enhancing storage stability and processing accuracy in CMP processes.

WO2024237174A1PCT designated stage expired Publication Date: 2024-11-21TOAGOSEI CO LTD

Patent Information

Application Number
PCT/JP2024/017333
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-05-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing polishing liquids for semiconductor devices, particularly those containing (meth)acrylic acid ester polymers, face issues with hydrolyzability of ester bonds, leading to unstable performance and potential loss of processing accuracy due to hydrolysis during storage.

Method used

Development of a vinyl polymer with specific structural units derived from vinyl monomers, exhibiting excellent storage stability, used as an additive in polishing liquids, along with a method for producing such polymers through radical polymerization, and a polishing liquid configuration including ceria and silica abrasive grains.

Benefits of technology

The vinyl polymer maintains stability and processing accuracy over time, ensuring consistent performance in CMP processes and reducing dishing and polishing rate variations, while being responsive to polishing pressure changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017333_21112024_PF_FP_ABST
    Figure JP2024017333_21112024_PF_FP_ABST
Patent Text Reader

Abstract

This vinyl-based polymer includes a structural unit (A) derived from a vinyl-based monomer (A) represented by structural formula (1). In structural formula (1), R represents a hydrogen atom or a methyl group, W represents a divalent hydrocarbon group having not more than 6 carbon atoms, X represents a divalent functional group having not more than one carbon atom and including a hetero atom, Y represents a divalent hydrocarbon group having not more than 6 carbon atoms, Z represents a hydrogen atom or an alkyl group having 1-4 carbon atoms, and n represents an integer of 4 or more. The vinyl-based polymer is obtained by, for example, polymerizing one or more vinyl-based monomers including the vinyl-based monomer (A) through living radical polymerization.
Need to check novelty before this filing date? Find Prior Art

Description

Vinyl polymer, its manufacturing method, polishing liquid and vinyl monomer

[0001] The present invention relates to a vinyl polymer, a method for producing the same, a polishing liquid, and a vinyl monomer.

[0002] Semiconductor devices are used in almost all familiar electronic devices, such as information and communication devices and home appliances, and are indispensable to modern life. In recent years, the role played by semiconductor devices has become even greater due to the spread of IoT and the use of cloud computing. To date, the high integration and capacity of semiconductor chips have been achieved at a remarkable speed, but the demand for higher performance continues, and the importance of microfabrication technology is increasing.

[0003] To achieve high performance in semiconductor devices, polishing processes for polishing the surface of a silicon wafer to a desired quality are extremely important, such as a polishing process for polishing the surface of a silicon substrate to a high-quality surface, and a chemical mechanical polishing (CMP) process for polishing an insulating layer or a wiring layer formed on a silicon substrate. Therefore, polishing solutions containing various water-soluble polymers are used to improve the processing accuracy in these polishing processes.

[0004] For example, in the CMP process, a polishing composition containing a (meth)acrylic acid ester polymer (see Patent Document 1) is used.

[0005] JP 2017-17177 A

[0006] However, (meth)acrylic acid ester polymers contain ester bonds in their molecular structure, which are hydrolyzable. If the ester bonds are hydrolyzed during storage of the polishing liquid, the properties of the polishing liquid may change, potentially making it impossible to achieve the desired processing accuracy.

[0007] The present invention has been made in view of the above background, and aims to provide a vinyl polymer that can be used as an additive to a polishing liquid and has excellent storage stability, a method for producing the same, a polishing liquid containing the vinyl polymer, and a vinyl monomer that is a raw material for the vinyl polymer.

[0008] A first aspect of the present invention resides in a vinyl polymer according to the following items [1] to

[10] : [1] A vinyl polymer comprising a structural unit (A) derived from a vinyl monomer (A) represented by the following structural formula (1):

[0009]

[0010] In the structural formula (1), R is a hydrogen atom or a methyl group, W is a divalent hydrocarbon group having 6 or less carbon atoms, X is a divalent functional group having 1 or less carbon atoms and containing a hetero atom, Y is a divalent hydrocarbon group having 6 or less carbon atoms, Z is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and n is an integer of 4 or more.

[0011] [2] The vinyl polymer according to [1], wherein the vinyl polymer is composed of the structural unit (A), and the structural unit (A) is derived from a vinyl monomer (A') represented by the following structural formula (1'):

[0012]

[0013] In the structural formula (1'), R is a hydrogen atom or a methyl group, W is a divalent hydrocarbon group having 6 or less carbon atoms, X is a divalent functional group having 1 or less carbon atoms and containing a hetero atom, Y is a divalent hydrocarbon group having 6 or less carbon atoms, Z is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and n is an integer of 6 or more.

[0014] [3] The vinyl polymer according to [1], which contains the structural unit (A) and a structural unit (B) derived from a vinyl monomer (B) different from the vinyl monomer (A). [4] The vinyl polymer has an SP value calculated by the Fedors estimation method of 17 (J / cm 3 ) 0.5 More than 25 (J / cm 3 ) 0.5 The vinyl polymer according to [3], which contains the structural unit (B) which is: [5] The vinyl polymer according to [3] or [4], wherein the vinyl monomer (B) contains a (meth)acrylamide monomer.

[0015] [6] The vinyl polymer according to any one of [3] to [5], which is a block copolymer having a polymer block (A) containing the structural unit (A) and a polymer block (B) containing the structural unit (B). [7] The polymer block (B) has an SP value of 17 (J / cm) calculated by the Fedors estimation method. 3 ) 0.5 More than 25 (J / cm 3 ) 0.5 The vinyl polymer according to [6], which is constituted by the structural unit (B) below:

[0016] [8] The vinyl polymer according to [6] or [7], wherein the vinyl polymer is a diblock copolymer having the polymer block (A) and the polymer block (B), and the ratio of the polymer block (A) to the total of the polymer block (A) and the polymer block (B) is 0.1% by mass or more and 99.9% by mass or less. [9] The vinyl polymer according to any one of [1] to [8], wherein the number average molecular weight Mn of the vinyl polymer is 1,000 or more and 1,000,000 or less.

[10] The vinyl polymer according to any one of [1] to [9], wherein the polydispersity index PDI of the vinyl polymer, represented by the following formula (I), is 2.0 or less: PDI = weight average molecular weight Mw / number average molecular weight Mn (I)

[0017] A second aspect of the present invention resides in a method for producing a vinyl polymer according to the following items

[11] and

[12] .

[0018]

[11] A method for producing a vinyl polymer according to any one of [1] to

[10] , wherein the vinyl polymer is obtained by polymerizing one or more monomers including the vinyl monomer (A) by a living radical polymerization method.

[12] The method for producing a vinyl polymer according to

[11] , wherein the living radical polymerization method is a reversible addition-fragmentation chain transfer polymerization method.

[0019] A third aspect of the present invention resides in the polishing liquid according to the following items

[13] to

[16] .

[0020]

[13] A polishing liquid containing the vinyl polymer according to any one of [1] to

[10] .

[14] The polishing liquid according to

[13] , which is configured to be used for chemical mechanical polishing.

[15] The polishing liquid according to

[13] or

[14] , which is configured to be used for planarizing the surface of at least one of an insulating layer and a wiring layer in a semiconductor device.

[16] The polishing liquid according to any one of

[13] to

[15] , which contains one or two types of abrasive grains selected from the group consisting of ceria and silica.

[0021] A fourth aspect of the present invention is a vinyl monomer according to the following item

[17] .

[0022]

[17] A vinyl monomer represented by the following structural formula (1'):

[0023]

[0024] In the structural formula (1'), R is a hydrogen atom or a methyl group, W is a hydrocarbon group having 6 or less carbon atoms, X is a divalent functional group having 1 or less carbon atoms and containing a hetero atom, Y is a divalent hydrocarbon group having 6 or less carbon atoms, Z is an alkyl group having 1 to 4 carbon atoms, and n is an integer of 6 or more.

[0025] According to the above-described aspect, it is possible to provide a vinyl polymer that can be used as an additive to a polishing liquid and has excellent storage stability, a method for producing the same, a polishing liquid containing the vinyl polymer, and a vinyl monomer that is a raw material for the vinyl polymer.

[0026] (Vinyl Polymer) The vinyl polymer (hereinafter referred to as "polymer") contains a structural unit (A) derived from a vinyl monomer (A). The vinyl polymer may, for example, be composed of only the structural unit (A). Alternatively, the vinyl polymer may, for example, contain the structural unit (A) and a structural unit (B) derived from a vinyl monomer (B) different from the vinyl monomer (A). Each structural unit contained in the polymer will be described below.

[0027] [Structural Unit (A)] The structural unit (A) contained in the polymer is a structural unit derived from a vinyl monomer (A) represented by the following structural formula (1). All of the structural units (A) contained in the polymer may have the same structure. Furthermore, the polymer may contain two or more types of structural units (A) having different structures. More specifically, the polymer may contain only structural units (A) in which R, W, X, Y, Z, and n in the following structural formula (1) are the same, or may contain multiple types of structural units (A) in which at least one of R, W, X, Y, Z, and n is different.

[0028]

[0029] R in the structural formula (1) is a hydrogen atom or a methyl group. W in the structural formula (1) is a divalent hydrocarbon group having 6 or less carbon atoms. Examples of W in the structural formula (1) include a methylene group, an ethylene group, and —CH(CH 3 )-group, -C(CH 3 ) 2 Examples of alkylene groups include alkylene groups such as - group and n-propylene group.

[0030] X in the structural formula (1) is a divalent functional group containing a heteroatom and having one or less carbon atoms. Examples of X in the structural formula (1) include an ether group (—O—), a urea bond (—NHC(═O)NH—), and a urethane bond (—NHC(═O)O—).

[0031] X in the structural formula (1) is preferably a functional group not containing an ester bond, and more preferably an ether group. In this case, the storage stability of the polymer can be further improved. Furthermore, when X in the structural formula (1) is an ether group, W in the structural formula (1) is preferably a methylene group.

[0032] Y in the structural formula (1) is a divalent hydrocarbon group having 6 or less carbon atoms. Examples of Y in the structural formula (1) include a methylene group, an ethylene group, a -CHMe- group, an n-propylene group, a -CHEt- group, and a -CHMeCH 2 - group, -CH 2CHMe- group, n-butylene group, -CH(n-Pr)- group, -CH(i-Pr)- group, -CHEtCH 2 - group, -CH 2 CHEt- group, -CHMeCH 2 CH 2 - group, -CH 2 CHMeCH 2 - group, -CH 2 CH 2 Examples include saturated hydrocarbon groups such as a CHMe- group. Multiple Ys in the structural formula (1) may have the same structure. Furthermore, the structural formula (1) may contain two or more types of Ys having different structures.

[0033] In consideration of the ease of industrially obtaining raw materials and the solubility of the polymer in water, Y in the structural formula (1) is preferably a saturated hydrocarbon group, and is preferably an ethylene group, -CHMeCH 2 - group and -CH 2 More preferably, it is one or more saturated hydrocarbon groups selected from the group consisting of CHMe- groups, and even more preferably, it is an ethylene group.

[0034] In the structural formula (1), n ​​is an integer of 4 or greater. Preferably, n in the structural formula (1) is an integer of 6 or greater. In this case, the water solubility of the polymer can be easily adjusted to a range suitable for the polishing liquid. From the viewpoint of storage stability, the upper limit of n in the structural formula (1) is not particularly limited. However, if the value of n is excessively large, a decrease in the polishing rate may occur when the polymer is used as an additive to the polishing liquid. To more easily avoid such problems, the value of n in the structural formula (1) is preferably 150 or less, more preferably 100 or less, even more preferably 50 or less, and particularly preferably 30 or less.

[0035] When constituting a preferred range of the value of n in the structural formula (1), the above-mentioned upper and lower limits of the value of n can be arbitrarily combined. For example, the preferred range of the value of n in the structural formula (1) may be 4 to 150, 4 to 100, 4 to 50, or 4 to 30. Furthermore, the preferred range of the value of n in the structural formula (1) may be 6 to 150, 6 to 100, 6 to 50, or 6 to 30. In particular, when the polymer is composed only of the structural unit (A), n in the structural formula (1) is preferably 6 or more, more preferably 6 to 150, even more preferably 6 to 100, even more preferably 6 to 50, and most preferably 6 to 30.

[0036] Note that n in the structural formula (1) is the total number of repeating units -(Y-O)- present between X and Z in the structural formula (1). Therefore, for example, when all of Y in the structural formula (1) have the same structure, n in the structural formula (1) is equal to the number of Y. Furthermore, for example, when the structural formula (1) contains two or more types of Y having mutually different structures, n in the structural formula (1) is equal to the total number of these Ys.

[0037] Z in the structural formula (1) is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. For example, when Z in the structural formula (1) is an alkyl group, Z may be a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, a tert-butyl group, or the like. In consideration of the availability of industrial raw materials and the solubility of the polymer in water, Z in the polymer is preferably a methyl group.

[0038] When the polymer contains the structural unit (A) and the structural unit (B), the content of the structural unit (A) in the polymer is preferably 0.1% by mass or more and 99.9% by mass or less, more preferably 30% by mass or more and 99% by mass or less, even more preferably 50% by mass or more and 98% by mass or less, particularly preferably 80% by mass or more and 97% by mass or less, and most preferably 91% by mass or more and 97% by mass or less, based on the total content of the structural unit (A) and the structural unit (B).

[0039] When used as an additive for polishing liquid, the polymer in which the ratio of structural unit (A) to structural unit (B) is within the above-mentioned specific range tends to adsorb to oxide film and exhibit protective effect.In addition, such polymer has high responsiveness to changes in polishing pressure, and when the oxide film is convex (high polishing pressure), it does not adsorb, thereby suppressing the decrease in polishing rate, and when polishing progresses and the nitride film is exposed and the polishing target becomes concave (low polishing pressure), it tends to adsorb to the oxide film interface and suppress over-polishing.Therefore, by making the ratio of structural unit (A) to structural unit (B) within the above-mentioned specific range, it is thought that it is easy to obtain a good polished surface with reduced dishing without decreasing the polishing rate.Therefore, the polymer in which the ratio of structural unit (A) to structural unit (B) is within the above-mentioned specific range is suitable as an additive for polishing liquid.

[0040] [Structural Unit (B)] The polymer may contain a structural unit (B). The structural unit (B) contained in the polymer is a structural unit derived from a vinyl monomer (B) having a structure different from that of the vinyl monomer (A). The polymer may contain only a structural unit (B) derived from one type of vinyl monomer (B), or may contain structural units (B) derived from two or more types of vinyl monomers (B).

[0041] As the vinyl-based monomer (B), any monomer having a vinyl group other than the vinyl-based monomer (A) can be used. The vinyl-based monomer (B) preferably has a structure that is relatively resistant to hydrolysis. Examples of monomers having such a structure include (meth)acrylamide-based monomers, vinyl ether-based monomers, and styrene-based monomers. By using these monomers as the vinyl-based monomer (B), deterioration of the storage stability of the polymer can be avoided. Among these, polymers containing a structural unit (B) derived from a (meth)acrylamide-based monomer can easily adjust the balance between hydrophilicity and hydrophobicity within an appropriate range when used as an additive in a polishing liquid. Therefore, the polymer can be appropriately adsorbed to the oxide film interface, thereby suppressing overpolishing.

[0042] Examples of the (meth)acrylamide-based monomer that can be used include (meth)acrylamide, (meth)acryloylmorpholine, and alkyl(meth)acrylamides. Examples of the alkyl(meth)acrylamides include tert-butyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, and N-(2-hydroxyethyl)acrylamide. As the (meth)acrylamide-based monomer, tert-butylacrylamide and / or N-isopropyl(meth)acrylamide are preferred, and N-isopropyl(meth)acrylamide is more preferred.

[0043] Examples of the vinyl ether monomer that can be used include alkyl vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, t-butyl vinyl ether, n-hexyl vinyl ether, 2-ethylhexyl vinyl ether, n-octyl vinyl ether, n-nonyl vinyl ether, and n-decyl vinyl ether.

[0044] As the styrene-based monomer, for example, aromatic vinyl compounds such as styrene, vinyltoluene, and vinylxylene can be used.

[0045] The aforementioned "(meth)acrylamide monomer" is a concept that encompasses amides of acrylic acid and its derivatives, and amides of methacrylic acid and its derivatives. For example, "(meth)acrylamide" is a concept that encompasses acrylamide and methacrylamide, "alkyl(meth)acrylamide" is a concept that encompasses alkylacrylamides and alkylmethacrylamides, and "(meth)acryloylmorpholine" is a concept that encompasses acryloylmorpholine and methacryloylmorpholine.

[0046] The content of the structural unit derived from the (meth)acrylamide monomer in the polymer is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 2% by mass or more, and particularly preferably 3% by mass or more, based on the total content of the structural unit (A) and the structural unit (B). Furthermore, the content of the structural unit derived from the (meth)acrylamide monomer in the polymer is preferably 99.9% by mass or less, more preferably 70% by mass or less, even more preferably 50% by mass or less, particularly preferably 20% by mass or less, and most preferably 7% by mass or less, based on the total content of the structural unit (A) and the structural unit (B). In this case, when the polymer is used as an additive to a polishing liquid, a good polished surface with reduced dishing is easily obtained.

[0047] In determining a preferred range of the content of the structural units derived from the (meth)acrylamide-based monomer in the polymer, the upper and lower limits of the content of the structural units derived from the (meth)acrylamide-based monomer described above can be combined arbitrarily. For example, a preferred range of the content of the structural units derived from the (meth)acrylamide-based monomer in the polymer may be 0.1% by mass or more and 99.9% by mass or less, 1% by mass or more and 70% by mass or less, 2% by mass or more and 50% by mass or less, 3% by mass or more and 20% by mass or less, or 3% by mass or more and 7% by mass or less.

[0048] Furthermore, examples of the vinyl monomer (B) that can be used include (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, and t-butyl (meth)acrylate; vinyl alcohols such as vinyl alcohol, 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, and 4-hydroxybutyl vinyl ether; and α-olefins such as ethylene, propylene, and butylene.

[0049] The content of structural units derived from vinyl monomers (B) other than (meth)acrylamide monomers in the polymer is preferably 10% by mass or less, more preferably 8% by mass or less, even more preferably 5% by mass or less, still more preferably 3% by mass or less, particularly preferably 1% by mass or less, and most preferably 0% by mass, i.e., all structural units (B) in the polymer are structural units derived from (meth)acrylamide monomers.

[0050] The polymer has an SP value of 17 (J / cm) calculated by the Fedors estimation method (see Polymer Engineering & Science, Vol. 14, No. 2, pp. 147-154, 1974). 3 ) 0.5 More than 25 (J / cm 3 ) 0.5 It is preferable that the structural unit (B) is 18 (J / cm3 ) 0.5 21.8 (J / cm 3 ) 0.5 It is more preferable that the polymer contains a structural unit (B) having an SP value of 17 (J / cm) or less, as calculated by the Fedors estimation method, of all the structural units (B) in the polymer. When the polymer contains such a structural unit (B) as an additive to a polishing liquid, the processing precision can be further improved. From the same viewpoint, it is preferable that the SP value of all the structural units (B) in the polymer is 17 (J / cm) or less, as calculated by the Fedors estimation method. 3 ) 0.5 More than 25 (J / cm 3 ) 0.5 More preferably, it is 18 (J / cm 3 ) 0.5 21.8 (J / cm 3 ) 0.5 It is particularly preferred that:

[0051] As the structural unit (B) having an SP value within the specific range, for example, a structural unit derived from tert-butylacrylamide and a structural unit derived from N-isopropylacrylamide can be preferably used.

[0052] [Molecular Weight of Polymer] The number-average molecular weight Mn of the polymer can be appropriately set in the range of 1,000 or more and 1,000,000 or less. When the polymer is used as an additive to a polishing liquid, the number-average molecular weight of the polymer is preferably 1,500 or more, more preferably 2,000 or more, even more preferably 3,000 or more, and particularly preferably 4,000 or more. In this case, it is possible to suppress a decrease in the polishing rate while ensuring sufficient wettability of the surface of the object to be polished.

[0053] Furthermore, when the polymer is used as an additive to a polishing liquid, the number average molecular weight of the polymer is preferably 100,000 or less, more preferably 60,000 or less, even more preferably 30,000 or less, and particularly preferably 10,000 or less. In this case, aggregation of abrasive grains due to shear force can be sufficiently suppressed, and the occurrence of defects such as scratches during polishing can be sufficiently suppressed.

[0054] In determining a preferred range of the number-average molecular weight Mn of the polymer, the upper and lower limits of the number-average molecular weight Mn of the polymer can be combined in any manner. For example, the preferred range of the number-average molecular weight Mn of the polymer may be 1,000 or more and 60,000 or less, 1,500 or more and 30,000 or less, 2,000 or more and 30,000 or less, 2,500 or more and 10,000 or less, or 4,000 or more and 10,000 or less.

[0055] The polydispersity index (PDI) of the vinyl polymer represented by the following formula (I) is preferably 2.0 or less, more preferably 1.8 or less, even more preferably 1.5 or less, particularly preferably 1.3 or less, and most preferably 1.2 or less. The lower limit of the polydispersity index (PDI) is usually 1.0. PDI=weight average molecular weight (Mw) / number average molecular weight (Mn) (I)

[0056] Polymers having a polydispersity PDI within the above-mentioned specific range have suitable properties as additives to polishing liquids. The reasons for this are thought to be, for example, as follows: For polymers with abrasive particle dispersion properties, the molecular weight is thought to affect the rate of adsorption / desorption to the polishing target, and generally, the smaller the molecular weight of the polymer, the higher the rate of adsorption / desorption to the polishing target. Furthermore, polymers with large molecular weights are thought to be more likely to form abrasive particle aggregation structures due to shear force. Therefore, for polymers with abrasive particle dispersion properties, a narrow molecular weight distribution is preferred.

[0057] In this specification, the number-average molecular weight Mn and weight-average molecular weight Mw of the polymer are values ​​calculated as polymethyl methacrylate, which are obtained by converting the retention time measured by gel permeation chromatography (GPC) into molecular weight using standard polymethyl methacrylate. More specific measurement conditions for molecular weight measurement will be described in the examples.

[0058] [Block Copolymer] When the polymer contains the structural unit (A) and the structural unit (B), the polymer may be a random copolymer containing the structural unit (A) and the structural unit (B). However, the polymer is preferably a block copolymer having a polymer block (A) containing the structural unit (A) and a polymer block (B) containing the structural unit (B). In a random copolymer, functional groups that adsorb to the surface of a polishing object, such as a silicon wafer, are uniformly distributed throughout the molecular chain. On the other hand, a block copolymer has regions on the molecular chain where functional groups that adsorb to the surface of a polishing object are arranged in clusters. Therefore, when the block copolymer is used as an additive to a polishing liquid, the block copolymer is easily adsorbed to the surface of the polishing object, thereby more easily protecting the surface of the polishing object. As a result, over-polishing of the polishing object can be more easily avoided.

[0059] When the polymer is a block copolymer, it is sufficient that the polymer has at least one polymer block (A) and at least one polymer block (B). More specifically, the polymer may be, for example, an AB diblock copolymer having one or more repeating units each consisting of polymer block (A) and polymer block (B). The polymer may also be, for example, an ABA triblock copolymer having one or more repeating units each consisting of polymer block (A), polymer block (B), and polymer block (A), or a BAB triblock copolymer having one or more repeating units each consisting of polymer block (B), polymer block (A), and polymer block (B). The block copolymer may also be a multiblock copolymer having four or more polymer blocks.

[0060] Furthermore, the polymer may contain a polymer block (C) different from the polymer block (A) and the polymer block (B). In this case, the polymer may have a structure such as an ABC triblock copolymer having one or more repeating units each consisting of the polymer block (A), the polymer block (B), and the polymer block (C), or an ABCA multiblock copolymer having one or more repeating units each consisting of the polymer block (A), the polymer block (B), the polymer block (C), and the polymer block (A).

[0061] Among these, the polymer is preferably a diblock copolymer (i.e., an AB diblock copolymer) having repeating units composed of the polymer block (A) and the polymer block (B). The diblock copolymer has a simple production process, which reduces the possibility of contamination with various impurities, making it easier to obtain a high-purity polymer.

[0062] The ratio of the polymer block (A) to the total of the polymer block (A) and the polymer block (B) is preferably 0.1% by mass or more and 99.9% by mass or less, more preferably 30% by mass or more and 99% by mass or less, even more preferably 50% by mass or more and 98% by mass or less, particularly preferably 80% by mass or more and 97% by mass or less, and most preferably 93% by mass or more and 97% by mass or less. When used as an additive to a polishing liquid, such a polymer tends to adsorb to an oxide film and exhibit a protective effect. Furthermore, such a polymer is highly responsive to changes in polishing pressure, and does not adsorb and do not reduce the polishing rate when the oxide film is convex (high polishing pressure). However, when polishing progresses and the nitride film is exposed and the polished object becomes concave (low polishing pressure), it tends to adsorb to the oxide film interface and suppress over-polishing. Therefore, it is believed that using the polymer as an additive to a polishing liquid makes it easier to obtain a good polished surface with reduced dishing without reducing the polishing rate.

[0063] Furthermore, when the polymer contains polymer block (A), polymer block (B), and polymer block (C), the total content of polymer block (A) and polymer block (B) in the polymer is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, and particularly preferably 99% by mass or more.

[0064] Polymer Block (A) The polymer block (A) is mainly composed of structural units (A) derived from a vinyl-based monomer (A). The polymer block (A) may contain one type of structural unit (A), or may contain two or more types of structural units (A). The polymer block (A) may also contain structural units other than the structural unit (A) as long as the above-mentioned effects are not impaired. Examples of structural units other than the structural unit (A) that can be contained in the polymer block (A) include structural units derived from (meth)acrylamide-based monomers, structural units derived from (meth)acrylic acid esters, structural units derived from alkyl vinyl ethers, structural units derived from vinyl alcohols, structural units derived from aromatic vinyl compounds, and structural units derived from α-olefins.

[0065] The content of the structural unit (A) in the polymer block (A) is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 97% by mass or more, particularly preferably 99% by mass or more, and most preferably 100% by mass, i.e., the polymer block (A) is composed solely of the structural unit (A). The use of such a polymer as an additive to the polishing liquid provides high responsiveness to changes in polishing pressure, and prevents the decrease in polishing rate when the oxide film is convex (high polishing pressure). Furthermore, when polishing progresses and the nitride film is exposed, making the polished object concave (low polishing pressure), the polymer adsorbs to the oxide film interface, thereby preventing over-polishing. Therefore, the use of such a polymer as an additive to the polishing liquid makes it easier to obtain a good polished surface with reduced dishing without reducing the polishing rate.

[0066] The weight-average molecular weight of the polymer block (A) is preferably 500 or more, more preferably 900 or more, even more preferably 1,500 or more, particularly preferably 2,100 or more, and most preferably 2,700 or more. The weight-average molecular weight of the polymer block (A) is preferably 100,000 or less, more preferably 60,000 or less, even more preferably 30,000 or less, particularly preferably 10,000 or less, and most preferably 6,000 or less. By using a polymer having a weight-average molecular weight of the polymer block (A) within the above-mentioned range as an additive to the polishing liquid, it is possible to suppress a decrease in the polishing rate while ensuring sufficient wettability of the surface of the object to be polished. Furthermore, it is possible to sufficiently suppress aggregation of abrasive grains due to shear force, and to sufficiently suppress the occurrence of defects such as scratches during polishing.

[0067] In determining a preferred range of the weight-average molecular weight of the polymer block (A), the lower and upper limits of the weight-average molecular weight of the polymer block (A) can be combined arbitrarily. For example, the preferred range of the weight-average molecular weight of the polymer block (A) may be 500 to 100,000, 900 to 60,000, 1,500 to 30,000, 2,100 to 10,000, or 2,700 to 6,000.

[0068] Polymer Block (B) The polymer block (B) is mainly composed of structural units (B) derived from a vinyl-based monomer (B). The polymer block (B) may contain one type of structural unit (B), or may contain two or more types of structural units (B). Furthermore, the polymer block (B) may contain structural units other than the structural unit (B) as long as the above-mentioned effects are not impaired. Examples of structural units other than the structural unit (B) that can be contained in the polymer block (B) include structural units derived from a vinyl-based monomer represented by the structural formula (1) above.

[0069] The content of the structural unit (B) in the polymer block (B) is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, still more preferably 97% by mass or more, and particularly preferably 99% by mass or more.

[0070] Furthermore, from the viewpoint of more reliably obtaining a polymer having properties suitable as an additive for a polishing liquid, the content of structural units derived from a (meth)acrylamide-based monomer in the polymer block (B) is preferably 90% by mass or more, more preferably 92% by mass or more, even more preferably 95% by mass or more, still more preferably 97% by mass or more, and particularly preferably 99% by mass or more.

[0071] The weight average molecular weight of the polymer block (B) is preferably 100 or more, more preferably 120 or more, even more preferably 130 or more, particularly preferably 140 or more, and most preferably 150 or more. The weight average molecular weight of the polymer block (B) is preferably 50,000 or less, more preferably 10,000 or less, even more preferably 5,000 or less, particularly preferably 1,000 or less, and most preferably 500 or less.

[0072] In determining a preferred range of the weight-average molecular weight of the polymer block (B), the lower and upper limits of the weight-average molecular weight of the polymer block (B) can be combined arbitrarily. For example, the preferred range of the weight-average molecular weight of the polymer block (B) may be 100 or more and 50,000 or less, 120 or more and 10,000 or less, 130 or more and 5,000 or less, 140 or more and 1,000 or less, or 150 or more and 500 or less.

[0073] The polymer block (B) has an SP value calculated by the Fedors estimation method of 17 (J / cm 3 ) 0.5 More than 25 (J / cm 3 ) 0.5It is preferable that the structural unit (B) is 18 (J / cm 3 ) 0.5 21.8 (J / cm 3 ) 0.5 It is more preferable that the polymer is composed of the following structural unit (B): When a polymer containing such a structural unit is used as an additive to a polishing liquid, it can further improve processing accuracy.

[0074] (Method for producing vinyl polymer) The method for producing the polymer is not particularly limited as long as it does not impair the effects of the present invention. For example, the polymer can be produced by polymerizing one or more monomers including the vinyl monomer (A) represented by the structural formula (1) using a known radical polymerization method such as solution polymerization or bulk polymerization. When synthesizing a vinyl polymer by solution polymerization, for example, a solvent and monomers are charged into a reactor, a polymerization initiator is added, and the mixture is heated to polymerize the monomers, thereby obtaining the target polymer.

[0075] Furthermore, the polymer obtained by the above-mentioned method may be purified as necessary in order to adjust the molecular weight distribution of the polymer, etc. As a method for purifying the polymer, for example, a known polymer purification method such as a reprecipitation method or a method using a porous material can be used.

[0076] Suitable methods for producing the polymer include various controlled polymerization methods such as living radical polymerization and living anionic polymerization.Among these, it is preferable to obtain the vinyl polymer by polymerizing one or more monomers including the vinyl monomer (A) by living radical polymerization, because it has high controllability of the polydispersity index (PDI) and can produce a polymer with excellent dispersion stability of abrasive grains, and it is easy to operate and can be applied to a wide range of monomers.When using living radical polymerization, the polymerization method is not particularly limited, and polymerization can be carried out in various modes such as bulk polymerization, solution polymerization, emulsion polymerization, mini-emulsion polymerization, and suspension polymerization.

[0077] For example, when the polymer is produced by solution polymerization using a living radical polymerization method, the polymer can be obtained by charging a solvent and a monomer into a reactor, adding a radical polymerization initiator, and polymerizing, preferably by heating. In the polymerization, any process such as a batch process, a semi-batch process, a dry continuous polymerization process, or a continuous stirred tank process (CSTR) may be used.

[0078] In producing the polymer, a polymerization method utilizing a known polymerization mechanism can be employed as the living radical polymerization method. Examples of living radical polymerization methods that can be employed include a living radical polymerization method utilizing an exchange chain mechanism, a living radical polymerization method utilizing a bond-dissociation mechanism, and a living radical polymerization method utilizing an atom transfer mechanism. More specifically, examples of living radical polymerization methods utilizing an exchange chain mechanism include reversible addition-fragmentation chain transfer polymerization (RAFT method), iodine transfer polymerization, a polymerization method using an organotellurium compound (TERP method), a polymerization method using an organoantimony compound (SBRP method), and a polymerization method using an organobismuth compound (BIRP method). Examples of living radical polymerization methods utilizing a bond-dissociation mechanism include the nitroxy radical method (NMP method). Examples of living radical polymerization methods utilizing an atom transfer mechanism include atom transfer radical polymerization (ATRP method). Among these, it is preferable to employ a living radical polymerization method utilizing an exchange chain mechanism, as it can be applied to the widest range of monomers and has excellent controllability over polymerization. In addition, the RAFT method or the NMP method is preferred in that contamination of the polishing object due to the inclusion of metal or semi-metallic compounds can be avoided, and the RAFT method is particularly preferred in that synthesis is easy in an aqueous system that does not require high temperatures.

[0079] In the RAFT method, polymerization proceeds via a reversible chain transfer reaction in the presence of a polymerization control agent (RAFT agent) and a radical polymerization initiator. Various known RAFT agents can be used as the RAFT agent, such as dithioester compounds, xanthate compounds, trithiocarbonate compounds, and dithiocarbamate compounds. Among these, trithiocarbonate compounds and dithiocarbamate compounds are preferred because they can produce polymers with a smaller molecular weight dispersity. Furthermore, as the RAFT agent, a monofunctional compound having only one active site may be used, or a polyfunctional compound having two or more active sites may be used. The amount of the RAFT agent used is appropriately adjusted depending on the type of monomer and RAFT agent used, etc.

[0080] The radical polymerization initiator used in polymerization by the RAFT method can be any known radical polymerization initiator, such as an azo compound, an organic peroxide, or a persulfate. Among these, an azo compound is preferred because it is easy to handle safely and is less likely to cause side reactions during radical polymerization. Specific examples of azo compounds include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), dimethyl-2,2'-azobis(2-methylpropionate), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide], and 2,2'-azobis(N-butyl-2-methylpropionamide). These radical polymerization initiators may be used alone or in combination of two or more.

[0081] The amount of radical polymerization initiator used is preferably 0.5 mol or less, and more preferably 0.2 mol or less, per mol of the RAFT agent, from the viewpoint of further reducing the polydispersity index (PDI) of the molecular weight of the polymer. Furthermore, from the viewpoint of stably carrying out the polymerization reaction, the amount of radical polymerization initiator used is preferably 0.01 mol or more, and more preferably 0.05 mol or more, per mol of the RAFT agent. The amount of radical polymerization initiator used is preferably 0.01 mol or more and 0.5 mol or less, and more preferably 0.05 mol or more and 0.2 mol or less, per mol of the RAFT agent.

[0082] When a solvent is used in living radical polymerization, examples of the polymerization solvent include aromatic compounds such as benzene, toluene, xylene, and anisole; ester compounds such as methyl acetate, ethyl acetate, propyl acetate, and butyl acetate; ketone compounds such as acetone and methyl ethyl ketone; dimethylformamide, acetonitrile, dimethyl sulfoxide, alcohol, water, etc. These polymerization solvents may be used alone, or two or more of them may be used in combination.

[0083] The reaction temperature in the polymerization reaction using the RAFT method is preferably 40°C or higher and 100°C or lower, more preferably 45°C or higher and 90°C or lower, and even more preferably 50°C or higher and 80°C or lower. A reaction temperature of 40°C or higher is preferred because it allows the polymerization reaction to proceed smoothly, while a reaction temperature of 100°C or lower is preferred because it can suppress side reactions and alleviate restrictions on the initiators and solvents that can be used. The reaction time can be appropriately set depending on the monomers used, etc., but is preferably 1 hour or higher and 48 hours or lower, more preferably 3 hours or higher and 24 hours or lower. If necessary, the polymerization may be carried out in the presence of a chain transfer agent (e.g., an alkylthiol compound having 2 to 20 carbon atoms, etc.). In the production process, particularly when a monomer having an acidic group is used, if there is a concern about metal contamination due to corrosion of the reactor, etc., it is preferable to produce the product using equipment whose surface is coated with a fluororesin or the like. In this case, it is preferable to use a corrosion-resistant resin container or the like for storing the product. When a resin container is used, the container is preferably made of a material that prevents metal contamination due to dissolution of filler or the like.

[0084] (Vinyl Monomer) In the method for producing the polymer, it is preferable to use a vinyl monomer (A') having a molecular structure represented by the following structural formula (1').

[0085]

[0086] In the structural formula (1'), R is a hydrogen atom or a methyl group, W is a hydrocarbon group having 6 or less carbon atoms, X is a divalent functional group having 1 or less carbon atoms and containing a hetero atom, Y is a divalent hydrocarbon group having 6 or less carbon atoms, Z is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and n is an integer of 6 or more.

[0087] In addition, R, W, X, Y, Z, and n in the structural formula (1') representing the molecular structure of the vinyl monomer (A') are the same as R, W, X, Y, Z, and n in the structural unit of the polymer described above. Therefore, for the explanation of R, W, X, Y, Z, and n in the vinyl monomer (A'), the explanation of R, W, X, Y, Z, and n in the structural unit of the polymer described above can be appropriately referred to.

[0088] The polymer can be easily obtained by using the vinyl monomer (A') represented by the structural formula (1'). The polymer obtained by polymerizing the vinyl monomer (A') has suitable properties as an additive for a polishing liquid and can be used for various purposes.

[0089] In addition, it is preferable that W in the structural formula (1') is a methylene group, X is an ether group, and Y is an ethylene group. That is, it is preferable that the vinyl monomer has a structure represented by the following structural formula (2).

[0090]

[0091] (Polishing Liquid) The polymer is suitable, for example, as a component of a polishing liquid. A polishing liquid containing the polymer can be used, for example, to polish the surface of a silicon wafer. More specifically, the polishing liquid containing the polymer can be used in a polishing step in the manufacturing process of a semiconductor device, in which the surface of a silicon substrate is polished to a high-quality mirror finish, in a step of chemically and mechanically polishing a silicon wafer, and in a polishing step for planarizing the surface of at least one of an insulating layer and a wiring layer in a semiconductor device.

[0092] The polishing liquid may contain abrasive grains in addition to the polymer. The abrasive grains may be at least one type of grains selected from the group consisting of known inorganic particles, organic particles, and organic-inorganic composite particles.

[0093] Examples of inorganic particles that can be used include cerium oxide (ceria), fumed silica, fumed alumina, fumed titania, and colloidal silica. Examples of organic particles that can be used include (meth)acrylic copolymers such as polymethyl methacrylate, polystyrene, polystyrene copolymers, polyacetal, polyamide, polycarbonate, polyolefin, polyolefin copolymers, and phenoxy resins. Examples of organic-inorganic composite particles that can be used include organic-inorganic composite particles that are bonded or composited to an extent that they do not decompose under the conditions used in the polishing composition, such as composite particles in which functional groups of an organic component and functional groups of an inorganic component are chemically bonded.

[0094] The polishing liquid preferably contains one or two types of abrasive grains selected from the group consisting of ceria and silica. These abrasive grains have the advantage of being lower in hardness than alumina and the like and being able to suppress the occurrence of defects on the polished surface, so by using these abrasive grains, processing accuracy can be further improved. Furthermore, from the viewpoint of further improving the polishing rate, it is more preferable that the polishing liquid contains abrasive grains made of ceria.

[0095] The average particle size of the abrasive grains is not particularly limited, but may be, for example, in the range of 1 nm to 500 nm. From the viewpoint of ensuring a high polishing rate, the average particle size of the abrasive grains is preferably 2 nm or more, more preferably 3 nm or more. From the viewpoint of suppressing the occurrence of scratches on the surface of the object to be polished, the upper limit of the average particle size of the abrasive grains is preferably 300 nm or less, more preferably 100 nm or less. In this specification, the average particle size of the abrasive grains refers to the volume-based median diameter (i.e., d50) of primary particles measured by dynamic light scattering (DLS).

[0096] From the viewpoint of realizing a high polishing rate, the content of the abrasive grains in the polishing liquid is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more. On the other hand, from the viewpoint of improving the smoothness of the object to be polished, the content of the abrasive grains in the polishing liquid is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less.

[0097] The preferred range of the content of abrasive grains in the polishing liquid can be determined by any combination of the above-mentioned lower and upper limits of the content of abrasive grains. For example, the preferred range of the content of abrasive grains in the polishing liquid may be 0.1% by mass to 20% by mass, 1% by mass to 10% by mass, or 2% by mass to 5% by mass.

[0098] The polishing liquid may contain a solvent. The solvent is preferably an aqueous solvent. Examples of aqueous solvents include water and mixed solvents of water and other solvents. The other solvents are preferably solvents that are compatible with water. Examples of such solvents include alcohols such as ethanol. The polishing liquid may further contain known additives such as polishing accelerators, pH adjusters, surfactants, chelating agents, and anticorrosive agents, as long as the effects of the polymer are not impaired.

[0099] The concentration of the polymer in the polishing liquid is preferably 0.001% by mass or more, more preferably 0.05% by mass or more. Furthermore, the concentration of the polymer in the polishing liquid is preferably 10% by mass or less, more preferably 5% by mass or less. When determining the preferred range of the polymer concentration in the polishing liquid, the upper and lower limits of the polymer concentration described above can be arbitrarily combined. For example, the preferred range of the polymer concentration in the polishing liquid may be 0.001% by mass or more and 10% by mass or less, or 0.05% by mass or more and 5% by mass or less.

[0100] The polishing liquid is usually prepared as a slurry mixture by mixing the components by a known method. The viscosity of the polishing liquid at 25°C can be appropriately selected depending on the object to be polished, the shear rate during polishing, etc., but is preferably in the range of 0.1 mPa s to 10 mPa s, and more preferably in the range of 0.5 mPa s to 5 mPa s.

[0101] When preparing the polishing liquid, the polymer may be added alone to the polishing liquid, or may be added to the polishing liquid in the form of a mixture with other components. Examples of components to be mixed with the polymer include water, organic solvents, and mixed solvents of water and organic solvents. The solvent is preferably one that can dissolve the polymer, more preferably water or a mixed solvent of water and a water-soluble organic solvent, and particularly preferably water. Examples of organic solvents that can be used together with water include alcohols such as methanol, ethanol, propanol, and butanol; ketones such as acetone and methyl ethyl ketone; alkylene glycols such as ethylene glycol and propylene glycol; ethers such as ethylene glycol monomethyl ether, propylene glycol monomethyl ether, ethylene glycol dimethyl ether, and tetrahydrofuran; esters such as ethylene glycol monomethyl ether acetate and ethyl acetate; amide-based solvents such as N,N-dimethylformamide and N,N-dimethylacetamide; and nitrile-based solvents such as acetonitrile. These organic solvents may be used alone, or two or more organic solvents may be used in combination.

[0102] When a mixture of the polymer and the solvent is used to prepare the polishing liquid, from the viewpoint of ensuring sufficient contact between the polymer and the surface of the polishing object and the polishing pad, the content of the polymer in the mixture relative to the total mass of the polymer and the solvent is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.05% by mass or more. Furthermore, from the viewpoint of preventing the viscosity from becoming too high and reducing handleability, the content of the polymer in the mixture is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less, relative to the total mass of the polymer and the solvent. When determining the preferred range of the polymer content in the mixture, the lower and upper limits of the polymer content described above can be arbitrarily combined. For example, the preferred range of the polymer content in the mixture may be 0.001% by mass or more to 70% by mass or less, 0.01% by mass or more to 60% by mass or less, or 0.05% by mass or more to 50% by mass or less, relative to the total mass of the polymer and the solvent.

[0103] Examples of the vinyl polymers are described below. The materials used in these examples are as follows:

[0104] [Vinyl Monomer (A)] StPEO-550: vinylbenzyl methoxypoly(oxyethylene) ether (average number of moles added: 13 moles) StPEO-1000: vinylbenzyl methoxypoly(oxyethylene) ether (average number of moles added: 23 moles)

[0105] The synthesis methods for StPEO-550 and StPEO-1000 are as follows.

[0106] Synthetic Method of StPEO-550 143 g of polyoxyethylene monomethyl ether having an average molecular weight of 550 ("UNIOX (registered trademark) M-550" manufactured by NOF Corporation) was added to a reaction vessel containing 1500 mL of tetrahydrofuran. While the reaction vessel was cooled in an ice bath, the contents of the reaction vessel were subjected to nitrogen bubbling and stirring. Next, 10 g of sodium hydride was added to the reaction vessel, and a tetrahydrofuran solution of p-chloromethylstyrene (manufactured by AGC Seimi Chemical Co., Ltd.) was slowly added dropwise, followed by stirring for 24 hours under a nitrogen atmosphere. Thereafter, water and methylene chloride were added to the reaction vessel, and reprecipitation purification was performed to obtain StPEO-550. The purity of the obtained StPEO-550 was confirmed by liquid chromatography, and the purity of the purified StPEO-550 was 97%.

[0107] Synthesis of StPEO-1000 The synthesis of StPEO-1000 was the same as that of StPEO-550, except that polyoxyethylene monomethyl ether having an average molecular weight of 1000 ("UNIOX M-1000" manufactured by NOF Corporation) was used instead of polyoxyethylene monomethyl ether having an average molecular weight of 550.

[0108] [Vinyl Monomer (B)] AME-400: methoxypolyethylene glycol monoacrylate (n=9) (NOF Corporation, "BLEMMER (registered trademark) AME-400") TBAM: N-tert-butylacrylamide NIPAM: N-isopropylacrylamide BA: n-butyl acrylate

[0109] [Radical polymerization initiator] V-501: 4,4-azobis(4-cyanovaleric acid) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) [Chain transfer agent] 3-MPA: 5% aqueous solution of 3-mercaptopropionic acid [RAFT agent] BM1429: 3-((((1-carboxyethyl)thio)carbonothioyl)thio)propanoic acid ("BM1429" manufactured by BORON MOLECULAR)

[0110] The synthesis methods and analytical methods for the polymers used in the examples and comparative examples are as follows.

[0111] (Synthesis of Polymer) [Polymer P1-1] 9.60 g of pure water, 6.00 g of StPEO-550, 0.08 g of V-501, and 2.55 g of 3-MPE were placed in a test tube containing a stirrer, and the inside of the test tube was thoroughly degassed by bubbling with nitrogen. Thereafter, the test tube was heated to 85°C to initiate polymerization. Three hours after the start of heating, the test tube was cooled with water to terminate the polymerization. In this manner, polymer P1-1 was obtained.

[0112] [Polymer P1-2] The synthesis method of polymer P1-2 was the same as the synthesis method of polymer P1-1, except that the type of vinyl monomer was changed as shown in Table 1.

[0113] [Polymers P1-3 to P1-4] The synthesis method for polymers P1-3 to P1-4 was the same as the synthesis method for polymers P1-1 to P1-2, except that a RAFT agent (specifically, BM1429) was used instead of the chain transfer agent.

[0114] [Polymer CP1-1] 50.00 g of pure water, 75.00 g of AME-400, 0.60 g of V-501, and 4.50 g of 3-MPA were placed in a 500 mL four-necked eggplant-shaped flask equipped with a stirrer, a thermometer, and a nitrogen inlet tube, and the flask was thoroughly degassed by nitrogen bubbling. Thereafter, the flask was heated in a thermostatic bath set at a temperature of 70°C to initiate polymerization. Three hours after the start of heating, the flask was water-cooled to terminate the polymerization. In this manner, polymer CP1-1 was obtained.

[0115] [Polymer CP1-2] The synthesis method of polymer CP1-2 was the same as the production method of polymer CP1-1, except that the amounts of pure water and radical polymerization initiator added were changed as shown in Table 2, and a RAFT agent (specifically, BM1429) was used instead of the chain transfer agent.

[0116] [Polymer P2-1] 12.00 g of pure water, 6.00 g of StPEO-550 as a first monomer, 0.08 g of V-501, and 0.31 g of BM1429 were placed in a test tube containing a stirrer, and the test tube was thoroughly degassed by nitrogen bubbling. The test tube was then heated to 85°C to initiate the first-stage polymerization. Three hours after the start of heating, the test tube was water-cooled to terminate the first-stage polymerization. Next, 0.30 g of BA as a second monomer was added to the test tube, and the test tube was thoroughly degassed by nitrogen bubbling. The test tube was then heated to 90°C to initiate the second-stage polymerization. Three hours after the start of heating, the test tube was water-cooled to terminate the second-stage polymerization. In this manner, polymer P2-1 was obtained.

[0117] [Polymers P2-2 to P2-4] The synthesis method for polymers P2-2 to P2-4 was the same as the synthesis method for polymer P2-1, except that the type and amount of the second monomer were changed as shown in Table 3.

[0118] [Polymers P2-5 to P2-8] The synthesis method for polymers P2-5 to P2-8 was the same as the synthesis method for polymer P2-1, except that StPEO-1000 was used as the first monomer and the type and amount of the second monomer were changed as shown in Table 4.

[0119] [Polymers CP2-1 to P2-3] The synthesis method of polymers CP2-1 to CP2-3 was the same as the production method of polymer P2-1, except that AME-400 was used instead of StPEO-550 as the first monomer and the type of the second monomer was changed as shown in Table 5.

[0120] (Analytical Methods) [Molecular Weight Measurement] For polymers P1-1 to 1-4, CP1-1 to 1-2, P2-1 to P2-8, and CP2-1 to CP2-3, the number average molecular weight Mn and weight average molecular weight Mw, calculated in terms of polymethyl methacrylate, were measured using a gel permeation chromatograph (model name "HLC-8320", manufactured by Tosoh Corporation) under the following conditions. Furthermore, the molecular weight dispersity PDI, i.e., the ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn, was calculated from the obtained values. The number average molecular weight Mn, weight average molecular weight Mw, and dispersity PDI for each polymer were as shown in Tables 1 to 5.

[0121] Measurement conditions Column: TSKgel Super HM-M (manufactured by Tosoh Corporation) x 3 Column temperature: 40°C Eluent: N,N-dimethylformamide Standard substance: polymethyl methacrylate Flow rate: 0.3 mL / min

[0122] Next, the polymers P1-1 to P1-4, CP1-1 to CP1-2, P2-1 to P2-8, and polymers CP2-1 to CP2-3 were used to prepare polishing solutions of Examples and Comparative Examples.

[0123] (Examples 1-1 to 1-4, Examples 2-1 to 2-8, Comparative Examples 1-2 to 1-3, and Comparative Examples 2-1 to 2-3) An aqueous dispersion of colloidal ceria (Nyacol Ce80 / 10 manufactured by Nyacol, particle concentration 10%, average particle diameter 80 nm) was diluted with water to a predetermined abrasive concentration, and then polymers P1-1 to P1-4, P2-1 to P2-8, CP1-1 to 1-2, and CP2-1 to CP2-3 obtained by the above-mentioned methods were added to the diluted dispersion to a predetermined polymer concentration. In this way, the polishing solutions of Examples 1-1 to 1-4, Examples 2-1 to 2-8, Comparative Examples 1-2 to 1-3, and Comparative Examples 2-1 to 2-3 were obtained.

[0124] (Comparative Example 1-1) An aqueous dispersion of colloidal ceria (Nyacol Ce80 / 10 manufactured by Nyacol, particle concentration 10%, average particle diameter 80 nm) was diluted with water to a predetermined abrasive concentration, thereby obtaining a polishing liquid of Comparative Example 1-1.

[0125] (Polishing test) As the object to be polished, a 1,000 nm thick SiO 2 A blanket wafer on which a film was formed was prepared. Then, the object to be polished was polished for 4 minutes using the polishing solutions of the examples and comparative examples under the following conditions. 2 From the thickness of the film, the SiO 2 The polishing amount (RA) (unit: nm) was calculated by subtracting the thickness of the film. 2 The thickness of the film was measured using an optical interference film thickness meter.

[0126] [Polishing conditions] Polishing tester: Engis Japan, trade name EJ-380IN-CH-Y-D Polishing pad: Nitta DuPont, trade name IC-1000 Platen rotation speed: 60 rpm Carrier rotation speed: 40 rpm Polishing liquid supply rate: 30 g / min Polishing load: 3 kgf, 7 kgf or 12 kgf

[0127] [Evaluation of Polishing Rate] In the evaluation of the polishing rate, the ratio RAb / RAa was calculated, where RAb was the polishing amount when polishing was performed using the polishing liquid of Examples 1-1 to 1-4, Examples 2-1 to 2-8, Comparative Examples 1-2 to 1-3, and Comparative Examples 2-1 to 2-3 and a polishing load of 12 kgf, relative to RAa when polishing was performed using the polishing liquid of Comparative Example 1-1 and a polishing load of 12 kgf.The polishing rate was then evaluated based on the value of the ratio RAb / RAa.The larger the value of the ratio RAb / RAa, the faster the polishing rate, which is preferable.

[0128] The evaluation results of the RA3 value, RA7 value, RA12 value, ratio RAb / RAa value, and polishing rate for the polishing liquids of the Examples and Comparative Examples are shown in Tables 6 to 10. The symbols shown in the "polishing rate" column in Tables 6 to 10 have the following meanings:

[0129] A: RAb / RAa≧0.60 B: 0.60>RAb / RAa≧0.50 C: 0.50>RAb / RAa

[0130] [Evaluation of dishing reduction performance] In the evaluation of dishing reduction performance, for each polishing liquid, the ratio RA7 / RA3 of the polishing amount RA7 when polishing is performed under a polishing load of 7 kgf to the polishing amount RA3 when polishing is performed under a polishing load of 3 kgf, and the ratio RA12 / RA3 of the polishing amount RA12 when polishing is performed under a polishing load of 12 kgf to the polishing amount RA3 when polishing is performed under a polishing load of 3 kgf were calculated. Then, the dishing reduction performance was evaluated based on the values ​​of the ratio RA7 / RA3 and the ratio RA12 / RA3.

[0131] When no vinyl polymer is added to the polishing liquid, the polishing rate usually increases in proportion to the polishing pressure.On the other hand, when a vinyl polymer is added to the polishing liquid, the polishing rate may be lower when polishing at a low polishing pressure, and higher when polishing at a high polishing pressure, compared to a polishing liquid that does not contain a vinyl polymer.A polishing liquid with such polishing properties can obtain a good polished surface with reduced dishing of the patterned wafer without reducing the polishing rate.Therefore, the larger the ratio RA12 / RA3 value and the ratio RA7 / RA3 value, the more dishing can be suppressed, which is preferable.

[0132] The ratio RA7 / RA3, the ratio RA12 / RA3, and the evaluation results of dishing reduction performance for the polishing solutions of the Examples and Comparative Examples are shown in Tables 6 to 10. The symbols shown in the "Dishing reduction performance" column in Tables 6 to 10 have the following meanings:

[0133] A: RA7 / RA3≧4.0 and RA12 / RA3≧11.5 B: When A above is not satisfied, and at least one of 4.0>RA7 / RA3>3.8 and 11.5>RA12 / RA3>10.0 is satisfied C: When A and B above are not satisfied, and at least one of 3.8≧RA7 / RA3>3.0 and 10.0≧RA12 / RA3>9.0 is satisfied D: When A to C above are not satisfied, and at least one of 3.0≧RA7 / RA3 and 9.0≧RA12 / RA3 is satisfied

[0134] (Evaluation of storage stability) Of the polishing solutions of the Examples and Comparative Examples, the polishing solutions containing a polymer were dissolved in ion-exchanged water to prepare sample solutions with a concentration of 5%. Using these sample solutions, the storage stability in an acidic environment and an alkaline environment was evaluated by the following method.

[0135] [Storage stability in an acidic environment] First, the initial pH and acid value of the sample solution were measured. Then, the sample solution was left standing at a temperature of 60°C for one week. The pH and acid value of the sample solution after standing were measured, and the change in pH after standing, ΔpH, relative to the initial pH, and the change in acid value after standing, ΔAV, relative to the initial acid value, were calculated.

[0136] [Storage Stability in an Alkaline Environment] First, the initial pH and acid value of the sample solution were measured. Then, the pH of the sample solution was adjusted to 10.0 using potassium hydroxide. The sample solution after pH adjustment was allowed to stand at a temperature of 60°C for one week. After standing, hydrochloric acid was added to the sample solution in a number of moles equal to the number of moles of potassium hydroxide added during the pH adjustment, and the pH and acid value of the sample solution were then measured. Then, the change in pH after standing, ΔpH, relative to the initial pH, and the change in acid value after standing, ΔAV, relative to the initial acid value, were calculated.

[0137] The pH was measured using a pH measuring instrument ("D-51" manufactured by Horiba Ltd.). The temperature of the sample solution used for the pH measurement was 25°C. In measuring the acid value, first, an appropriate amount of the sample solution was dissolved in 50 mL of tetrahydrofuran, and a small amount of water was added to prepare a titration sample. This titration sample was titrated with a 0.1 mol / L KOH-EtOH solution, and the acid value was calculated by measuring the neutralization point. The titration was performed using an automatic titrator ("COM-A19" manufactured by HIRANUMA Corporation).

[0138] Based on the ΔpH and ΔAV in an acidic environment and the ΔpH and ΔAV in an alkaline environment obtained as described above, the storage stability in each environment was evaluated. Tables 6 to 10 show the evaluation results of the ΔpH and ΔAV values ​​and storage stability of the polishing liquid containing the polymer in each environment. The symbols shown in the "Evaluation" column in Tables 6 to 10 have the following meanings.

[0139] A: ΔpH<0.22 and ΔAV≦1.0 B: When the above A is not satisfied, and at least one of 0.22≦ΔpH≦0.25 and 1.0<ΔAV≦1.9 is satisfied C: When the above A and B are not satisfied, and at least one of 0.25<ΔpH≦0.35 and 1.9<ΔAV≦2.5 is satisfied D: When the above A to C are not satisfied, and at least one of 0.35<ΔpH and 2.5<ΔAV is satisfied

[0140]

[0141]

[0142]

[0143]

[0144]

[0145]

[0146]

[0147]

[0148]

[0149]

[0150] The vinyl polymers P1-1 to P1-4 contained in the polishing liquids of Examples 1-1 to 1-4 are composed of structural units (A) derived from the vinyl monomer (A) (more specifically, StPEO-550 or StPEO-1000) represented by the structural formula (1), as shown in Table 1. Therefore, as shown in Table 6, these polishing liquids showed little change in pH and acid value when stored in either an acidic environment or an alkaline environment, and exhibited excellent storage stability.

[0151] Similarly, the vinyl polymers P2-1 to P2-8 contained in the polishing liquids of Examples 2-1 to 2-8 are composed of structural units derived from the vinyl monomer (A) (more specifically, StPEO-550 or StPEO-1000) represented by the structural formula (1) and structural units derived from a vinyl monomer (B) different from the vinyl polymer (A), as shown in Tables 3 and 4. Therefore, as shown in Tables 8 and 9, these polishing liquids showed little change in pH and acid value when stored in an acidic environment and when stored in an alkaline environment, and exhibited excellent storage stability.

[0152] On the other hand, the vinyl polymers CP1-1 and CP1-2 contained in the polishing solutions of Comparative Examples 1-2 and 1-3 are composed of structural units derived from vinyl monomers other than the vinyl monomer (A), as shown in Table 2. Therefore, as shown in Table 7, these polishing solutions were inferior in storage stability to the polishing solutions of the Examples.

[0153] Similarly, the vinyl polymers CP2-1 and CP2-2 contained in the polishing solutions of Comparative Examples 2-1 to 2-3 do not contain a structural unit (A) derived from a vinyl monomer other than the vinyl monomer (A), as shown in Table 5. Therefore, as shown in Table 10, these polishing solutions were inferior in storage stability to the polishing solutions of the Examples.

[0154] The above has described the vinyl polymer, its manufacturing method, polishing liquid, and vinyl monomer based on the examples. However, the specific aspects of the vinyl polymer, its manufacturing method, polishing liquid, and vinyl monomer according to the present invention are not limited to those in the examples, and the configurations can be changed as appropriate within the scope of the present invention.

Claims

1. A vinyl polymer comprising a structural unit (A) derived from a vinyl monomer (A) represented by the following structural formula (1): (In the structural formula (1), R is a hydrogen atom or a methyl group, W is a divalent hydrocarbon group having 6 or less carbon atoms, X is a divalent functional group having 1 or less carbon atoms and containing a hetero atom, Y is a divalent hydrocarbon group having 6 or less carbon atoms, Z is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and n is an integer of 4 or more.) 2. The vinyl polymer according to claim 1, wherein the vinyl polymer is composed of the structural unit (A), and the structural unit (A) is derived from a vinyl monomer (A') represented by the following structural formula (1'): (In the structural formula (1'), R is a hydrogen atom or a methyl group, W is a divalent hydrocarbon group having 6 or less carbon atoms, X is a divalent functional group having 1 or less carbon atoms and containing a hetero atom, Y is a divalent hydrocarbon group having 6 or less carbon atoms, Z is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and n is an integer of 6 or more.) 3. The vinyl polymer according to claim 1, comprising the structural unit (A) and a structural unit (B) derived from a vinyl monomer (B) different from the vinyl monomer (A).

4. The vinyl polymer has an SP value of 17 (J / cm) calculated by the Fedors estimation method. 3 ) 0.5 More than 25 (J / cm 3 ) 0.5 The vinyl polymer according to claim 3 , comprising the structural unit (B) which is:

5. The vinyl polymer according to claim 3, wherein the vinyl monomer (B) comprises a (meth)acrylamide monomer.

6. The vinyl polymer according to claim 3, which is a block copolymer having a polymer block (A) containing the structural unit (A) and a polymer block (B) containing the structural unit (B).

7. The polymer block (B) has an SP value of 17 (J / cm) calculated by the Fedors estimation method. 3 ) 0.5 More than 25 (J / cm3 ) 0.5 The vinyl polymer according to claim 6 , which is constituted by the structural unit (B) having the following structure:

8. The vinyl polymer according to claim 6, wherein the vinyl polymer is a diblock copolymer having the polymer block (A) and the polymer block (B), and a ratio of the polymer block (A) to the total of the polymer block (A) and the polymer block (B) is 0.1 mass % or more and 99.9 mass % or less.

9. The vinyl polymer according to claim 1, wherein the number average molecular weight Mn of the vinyl polymer is 1,000 or more and 1,000,000 or less.

10. The vinyl polymer according to claim 1, wherein the polydispersity index (PDI) of the vinyl polymer represented by the following formula (I) is 2.0 or less. PDI=weight average molecular weight (Mw) / number average molecular weight (Mn) (I) 11. A method for producing a vinyl polymer according to any one of claims 1 to 10, comprising polymerizing one or more monomers including the vinyl monomer (A) by living radical polymerization to obtain the vinyl polymer.

12. The method for producing a vinyl polymer according to claim 11, wherein the living radical polymerization is a reversible addition-fragmentation chain transfer polymerization.

13. A polishing liquid containing the vinyl polymer according to any one of claims 1 to 10.

14. The polishing fluid of claim 13, wherein the polishing fluid is configured for use in chemical mechanical polishing.

15. The polishing liquid according to claim 14, wherein the polishing liquid is configured to be used for planarizing the surface of at least one of an insulating layer and a wiring layer in a semiconductor device.

16. The polishing liquid according to claim 15, wherein the polishing liquid contains one or two types of abrasive grains selected from the group consisting of ceria and silica.

17. A vinyl monomer represented by the following structural formula (1'): (In the structural formula (1'), R is a hydrogen atom or a methyl group, W is a hydrocarbon group having 6 or less carbon atoms, X is a divalent functional group having 1 or less carbon atoms and containing a heteroatom, Y is a divalent hydrocarbon group having 6 or less carbon atoms, Z is an alkyl group having 1 to 4 carbon atoms, and n is an integer of 6 or more.)

Citation Information

Patent Citations

  • Method for producing water soluble polymer for polishing liquid composition

    JP2017017177A

  • Novel polymer

    JP1978079983A

  • Styrene oligomer and its production

    JP1999140133A

  • Hair cosmetic

    JP2001064123A

  • Agent for prevention or treatment of hypercholesterolemia

    JP2005213438A

Cited By

  • Vinyl copolymer, method for producing same, and cleaning agent for semiconductor component

    WO2026088871A1