Thermally conductive silicone composition and cured product

The thermally conductive silicone composition, featuring phenyl-modified organopolysiloxane and thermally conductive fillers, addresses the limitations of existing materials by providing excellent heat and chemical resistance with enhanced thermal conductivity for efficient heat dissipation in ATF environments.

WO2024237187A1PCT designated stage expired Publication Date: 2024-11-21SHIN ETSU CHEMICAL CO LTD

Patent Information

Application Number
PCT/JP2024/017373
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-05-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Current thermally conductive silicone materials, such as dimethyl silicone, are susceptible to swelling and deterioration in organic solvents like ATF, and fluororubber alternatives have low thermal conductivity and high viscosity issues, making them unsuitable for high-temperature automotive applications.

Method used

A thermally conductive silicone composition comprising phenyl-modified organopolysiloxane, organohydrogenpolysiloxane, hydrolyzable organopolysiloxane, thermally conductive fillers, a platinum group metal catalyst, and a hydrosilylation reaction control agent, which provides excellent heat and chemical resistance with improved thermal conductivity.

Benefits of technology

The composition achieves high thermal conductivity (1.0 W/m·K or more) and chemical resistance, enabling effective heat dissipation in organic solvent environments like ATF, while maintaining workability and processability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017373_21112024_PF_FP_ABST
    Figure JP2024017373_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to: a thermally conductive silicone composition obtained by adding a hydrolyzable organopolysiloxane represented by general formula (1) to a component (C); and a cured product. Therefore, provided are a thermally conductive silicone composition and a cured product. (In the formula, R1 is independently a C6-10 aromatic hydrocarbon group, R 2 is independently a C1-10 alkyl group, and R 3 is a C1-4 alkyl group. a is 2 or 3, and n is an integer satisfying 2 ≤ n ≤ 60.)
Need to check novelty before this filing date? Find Prior Art

Description

Thermally conductive silicone composition and cured product

[0001] The present invention relates to a thermally conductive silicone composition and a cured product thereof.

[0002] The performance of electronic components, such as highly integrated circuits like CPUs, is significantly degraded by heat generation during use. To solve this problem, heat-dissipating materials are used, which improve heat transfer efficiency when introduced into the air gap between the heat-generating and cooling components. Silicone heat-dissipating materials, in particular, are used in a wide range of fields due to their high heat resistance, weather resistance, and electrical insulation properties inherent to silicone. In addition, as electronic devices have become increasingly miniaturized and highly integrated in recent years, it is important to more efficiently cool the generated heat, which has led to a demand for heat-dissipating materials with high thermal conductivity.

[0003] In recent years, there has been an increasing use of automotive heat-dissipating materials in oils containing chemicals, such as automatic transmission fluid (ATF), which is a lubricant for engine gears. Therefore, heat-dissipating materials are required to have chemical resistance. However, general-purpose silicone (dimethyl silicone) heat-dissipating materials have the problem of being prone to swelling and degradation in organic solvent environments such as ATF. Furthermore, ATF is often heated to high temperatures, so heat resistance as well as ATF resistance is required.

[0004] As a chemical-resistant heat-dissipating material, a heat-dissipating material using fluororubber, which has a perfluoropolyether structure in the main chain and is a mixture of thermally conductive fillers, has been proposed (Patent Documents 1 to 3). However, this fluororubber has a lower thermal conductivity than dimethyl silicone. When an attempt is made to compensate for this by increasing the thermally conductive filler loading, the composition does not become grease-like or becomes highly viscous, resulting in poor workability and processability. Furthermore, this heat-dissipating material has a high specific gravity and is expensive, so there is a need to develop a new heat-dissipating material that can replace it and has chemical resistance.

[0005] Compared to dimethylsilicone, phenylsilicone has a greater affinity for aromatic solvents such as benzene and toluene, but a lower affinity for saturated hydrocarbons such as automatic transmission fluid (ATF). Phenylsilicone also has a thermal conductivity comparable to that of dimethylsilicone. Furthermore, phenylsilicone is known to have higher heat resistance because it is less susceptible to oxidative degradation than dimethylsilicone (Patent Documents 4 and 5). Therefore, by incorporating phenylsilicone into a heat-dissipating material, it is possible to provide a heat-dissipating material that also has chemical resistance.

[0006] However, a dispersant (wetter) for phenylsilicone and thermally conductive filler has not yet been developed, and there has been little research into compositions using phenylsilicone and their cured products.

[0007] JP 2015-67736 A JP 2015-67737 A JP 2017-082090 A JP 2007-039621 A JP 2004-262919 A

[0008] An object of the present invention is to provide a thermally conductive silicone composition and cured product that exhibit excellent heat resistance and chemical resistance.

[0009] The present invention has been made to solve the above problems, and provides the following thermally conductive silicone composition and cured product.

[0010] That is, the present invention provides the following (A) to (F): (A) a viscoelastic composition having two or more alkenyl groups in one molecule and having a kinematic viscosity at 25°C of 100 to 100,000 mm 2 / s: 100 parts by mass; (B) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the number of moles of hydrosilyl groups in component (B) is 0.1 to 3 moles per mole of alkenyl groups in component (A); (C) a compound represented by the following general formula (1): (In the formula, R 1 are independently aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, and n is an integer satisfying the formula: (A) a hydrolyzable organopolysiloxane represented by the formula: 10 to 300 parts by mass; (D) one or more thermally conductive fillers selected from the group consisting of metals, metal oxides, metal hydroxides, and metal nitrides: in an amount that provides 10 to 97% by mass of the entire composition; (E) a platinum group metal catalyst: 0.1 to 500 ppm by mass, calculated as platinum group metal atoms, relative to the mass of component (A); and (F) a hydrosilylation reaction inhibitor: 0.05 to 5 parts by mass.

[0011] Such a thermally conductive silicone composition can yield a cured product that has excellent heat resistance and chemical resistance.

[0012] R shown in the above general formula (1) 1 is a phenyl group, and R 2 is preferably a methyl group.

[0013] From the viewpoint of synthesis of hydrolyzable organopolysiloxane, these groups are preferred.

[0014] The viscosity of the thermally conductive silicone composition at 23°C is preferably 1 to 1,000 Pa·s.

[0015] If the viscosity of the thermally conductive silicone composition at 23°C is within the above range, it will be excellent in terms of workability and processability.

[0016] The present invention also provides a thermally conductive silicone cured product obtained by curing the above thermally conductive silicone composition.

[0017] Such thermally conductive silicone cured products are excellent in terms of heat resistance and chemical resistance.

[0018] In this case, the thermally conductive silicone cured product is characterized by having a thermal conductivity of 1.0 W / m·K or higher.

[0019] A thermally conductive silicone cured product that has heat resistance, chemical resistance, and good thermal conductivity can be used as a heat dissipation material in an organic solvent environment such as ATF.

[0020] The thermally conductive silicone composition and cured product of the present invention can be highly thermally conductive with excellent heat resistance and chemical resistance. In particular, the cured product of the thermally conductive silicone composition of the present invention can be used in environments containing organic solvents such as ATF.

[0021] The present invention is described in detail below, but is not limited to these. As a result of extensive research conducted by the present inventors to achieve the above-mentioned object, they have completed a thermally conductive silicone composition and a cured product thereof that combines heat resistance and chemical resistance by adding a hydrolyzable organopolysiloxane having a specific structure to a thermally conductive silicone composition, which acts as a dispersant (wetter) for the phenylsilicone and thermally conductive filler.

[0022] That is, the present invention provides the following (A) to (F): (A) a viscoelastic composition having two or more alkenyl groups in one molecule and having a kinematic viscosity at 25°C of 100 to 100,000 mm 2 / s: 100 parts by mass; (B) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the number of moles of hydrosilyl groups in component (B) is 0.1 to 3 moles per mole of alkenyl groups in component (A); (C) a compound represented by the following general formula (1): (In the formula, R 1 are independently aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3 is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, and n is an integer satisfying the formula: (A) a hydrolyzable organopolysiloxane represented by the formula: 10 to 300 parts by mass; (D) one or more thermally conductive fillers selected from the group consisting of metals, metal oxides, metal hydroxides, and metal nitrides: in an amount that provides 10 to 97% by mass of the entire composition; (E) a platinum group metal catalyst: 0.1 to 500 ppm by mass, calculated as platinum group metal atoms, relative to the mass of component (A); and (F) a hydrosilylation reaction inhibitor: 0.05 to 5 parts by mass.

[0023] The present invention will be described in detail below.

[0024] [(A) Phenyl-modified organopolysiloxane] Component (A) has two or more, preferably 2 to 10, and more preferably 2 to 5 alkenyl groups in the molecule, and has a kinematic viscosity at 25°C of 100 to 100,000 mm 2 The phenyl-modified organopolysiloxane is a phenyl-modified organopolysiloxane having the formula:

[0025] The main chain is generally composed of diorganosiloxane units, but may also have a partially branched structure or may be a cyclic organopolysiloxane. From the viewpoint of the physical properties of the cured product, however, a linear organopolysiloxane is preferred.

[0026] The alkenyl group is preferably an alkenyl group having 2 to 8 carbon atoms, more preferably 2 to 6 carbon atoms. Examples include vinyl, allyl, propenyl, isopropenyl, butenyl, hexenyl, cyclohexenyl, and octenyl groups. Vinyl groups are particularly preferred. The alkenyl group may be bonded to a silicon atom at the terminal of the molecular chain, a silicon atom in the middle of the molecular chain, or both.

[0027] The phenyl-modified organopolysiloxane of component (A) preferably has 0.00001 to 0.01 mol / g, and especially 0.0001 to 0.01 mol / g, of alkenyl groups per molecule.

[0028] Component (A) is also characterized by having phenyl groups. The amount of phenyl groups in one molecule is preferably 10 to 80%, more preferably 20 to 60%, of the number of siloxane units containing phenyl groups per total siloxane units. If the amount of phenyl groups in one molecule is 10% or more of the total siloxane units, compatibility with component (C) will not be significantly reduced. Furthermore, if the amount of phenyl groups in one molecule is 80% or less of the total siloxane units, the viscosity of the composition will not increase more than necessary.

[0029] Furthermore, from the viewpoint of viscosity, it is preferable that the groups other than the alkenyl group and the phenyl group contained in the phenyl-modified organopolysiloxane of component (A) are alkyl groups having 1 to 18 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 8 carbon atoms. Examples include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, nonyl, and decyl groups. These alkyl groups in which some of the hydrogen atoms have been substituted with halogen atoms may also be used. As the alkyl group, a methyl group is particularly preferable.

[0030] The phenyl-modified organopolysiloxane of component (A) has a kinematic viscosity at 25°C of 100 to 100,000 mm 2 In the present invention, the kinematic viscosity is a value measured by an Ostwald viscometer described in JIS Z8803:2011. The kinematic viscosity is preferably 300 to 20,000 mm 2 / s, and more preferably 500 to 10,000 mm 2 / s. The kinematic viscosity is 100 mm 2 If the kinematic viscosity is less than 100,000 mm / s, the phenyl modification rate becomes too small, which is not preferable. 2 If the ratio exceeds 1 / s, the composition becomes difficult to handle, which is not preferred. The phenyl-modified organopolysiloxane may be used alone or in combination of two or more kinds.

[0031] [(B) Organohydrogenpolysiloxane] Component (B) is an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule, preferably 2 to 50, more preferably 2 to 20, and even more preferably 2 to 10 hydrosilyl groups.

[0032] Any compound that can undergo an addition reaction with the alkenyl group of the component (A) in the presence of the platinum group metal catalyst (E) described below to form a crosslinked structure can be used.

[0033] The molecular structure of the organohydrogenpolysiloxane is not particularly limited as long as it has the above properties, and examples thereof include a linear structure, a branched structure, a cyclic structure, and a linear structure having a partially branched or cyclic structure, with linear structures and cyclic structures being preferred.

[0034] The organohydrogenpolysiloxane preferably has a kinematic viscosity at 25°C of 1 to 1,000 mm 2 / s, more preferably 10 to 100 mm 2 / s. The kinematic viscosity is 1 mm 2 / s or more, there is no risk of the physical properties of the silicone composition being reduced, and 2 If the viscosity is 1 / s or less, there is no risk of the silicone composition having poor extensibility.

[0035] The organic group bonded to the silicon atom of the organohydrogenpolysiloxane preferably contains a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms, and preferably does not contain a hydrosilylation-reactive group such as an alkenyl group or an alkynyl group. Furthermore, the group other than the monovalent aromatic hydrocarbon group is preferably an alkyl group, preferably an alkyl group having 1 to 12 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms. Examples include methyl, ethyl, propyl, butyl, hexyl, and dodecyl groups. These alkyl groups in which some of the hydrogen atoms have been substituted with halogen atoms may also be used. Among these, methyl groups are preferred. The organohydrogenpolysiloxane may be used alone or in combination of two or more types.

[0036] The amount of organohydrogenpolysiloxane in component (B) is such that the ratio of the number of hydrosilyl groups in component (B) to the total number of alkenyl groups in component (A) is 0.1 to 3, preferably 0.7 to 3, and more preferably 1 to 2. If the amount of component (B) is less than the above-mentioned lower limit, the addition reaction will not proceed sufficiently, resulting in insufficient crosslinking. If the amount exceeds the above-mentioned upper limit, the crosslinked structure may become non-uniform and the stability of the composition over time may deteriorate.

[0037] [(C) Hydrolyzable Organopolysiloxane] Component (C) acts as a dispersant (wetter) for the phenyl silicone and thermally conductive filler, and is a hydrolyzable organopolysiloxane represented by the following general formula (1). (In the formula, R 1 are independently aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3 is an alkyl group having 1 to 4 carbon atoms; a is 2 or 3, and n is an integer satisfying the condition 2≦n≦60.

[0038] In the above general formula (1), R 1 are independently monovalent aromatic hydrocarbon groups having 6 to 10 carbon atoms. 1 Specific examples of include aryl groups such as phenyl, tolyl, xylyl, and mesityl groups, and among these, phenyl is preferred from the viewpoint of ease of synthesis.

[0039] In the above general formula (1), R 2 is an alkyl group having 1 to 10 carbon atoms, more preferably 1 to 5, and even more preferably 1 to 3 carbon atoms. 2 Examples of the alkyl group include methyl, ethyl, propyl, isopropyl, butyl, tert-butyl, pentyl, hexyl, octyl, nonyl, and decyl groups, with methyl and ethyl groups being particularly preferred.

[0040] In the above general formula (1), R 3 is an alkyl group having 1 to 4 carbon atoms, preferably a methyl group or an ethyl group. 3 Examples of the alkyl group include methyl, ethyl, propyl, isopropyl, butyl, and tert-butyl. Of these, methyl and ethyl groups are particularly preferred from the viewpoint of the hydrolysis property of the present organopolysiloxane compound. In addition, in the above general formula (1), a is an integer of 2 or 3, preferably 3.

[0041] In the general formula (1), n ​​is an integer satisfying 2≦n≦60, more preferably 9≦n≦30, and even more preferably 12≦n≦18. If n is outside this range, compatibility with the phenyl-modified silicone, which is components (A) and (B), will be significantly reduced, which is not preferred.

[0042] The blend amount of component (C) is 10 to 300 parts by mass, preferably 15 to 200 parts by mass, and more preferably 20 to 100 parts by mass per 100 parts by mass of component (A). An amount of component (C) less than 10 parts is not preferred because it becomes difficult to highly fill the thermally conductive silicone cured product with the thermally conductive filler. An amount exceeding 300 parts by mass is also not preferred because the hardness of the cured product of the thermally conductive silicone composition does not increase or a cured product cannot be obtained.

[0043] [(D) Thermally conductive filler] Component (D) is one or more thermally conductive fillers selected from the group consisting of metals, metal oxides, metal hydroxides, and metal nitrides. Examples include alumina, zinc oxide, magnesium oxide, aluminum oxide, silicon dioxide, cerium oxide, iron oxide, aluminum hydroxide, cerium hydroxide, aluminum nitride, and boron nitride. These may be used alone or in appropriate combinations of two or more, and a combination of a large particle component and a small particle component is preferred.

[0044] If the average particle size of the large particle component is 0.1 μm or more, the viscosity of the resulting composition will not be too high and the processability will not be reduced.If the average particle size of the large particle component is 100 μm or less, the resulting composition will not be non-uniform and there will be no risk of oil bleeding.Therefore, the range of 0.1 to 100 μm, preferably 10 to 75 μm, is preferred.

[0045] Furthermore, if the average particle size of the small particle component is 0.01 μm or more, the viscosity of the resulting composition will not be too high and the processability will not be impaired. On the other hand, if it is less than 10 μm, the resulting composition will not be non-uniform, so it is preferable that the average particle size is in the range of 0.01 μm or more and less than 10 μm, preferably in the range of 1 to 4 μm.

[0046] The ratio of the large particle component to the small particle component is not particularly limited, and is preferably in the range of 9:1 to 1:9 (mass ratio). The shapes of the large particle component and the small particle component are not particularly limited, and may be spherical, irregular, acicular, or the like. The average particle size can be determined, for example, as the volume-based average value (or median diameter) in particle size distribution measurement by laser diffraction.

[0047] The blending amount of component (D) is 10 to 97% by mass, preferably 20 to 95% by mass, more preferably 30 to 95% by mass, and even more preferably 50 to 95% by mass, based on the total mass of the composition. If it is more than 97% by mass, the viscosity of the composition increases and processability decreases. If it is less than 10% by mass, thermal conductivity decreases.

[0048] [(E) Platinum Group Metal Catalyst] Component (E) is a platinum group metal catalyst that functions to promote the addition reaction between the above-mentioned components (A) and (B). Any conventionally known platinum group metal catalyst used in addition reactions can be used. Examples include platinum-based, palladium-based, and rhodium-based catalysts, with platinum or platinum compounds being preferred, as they are relatively readily available. Examples include platinum itself, platinum black, chloroplatinic acid, platinum-olefin complexes, platinum-alcohol complexes, and platinum coordination compounds. Platinum group metal catalysts may be used singly or in combination of two or more.

[0049] The amount of component (E) to be blended is 0.1 to 500 ppm, preferably 1 to 200 ppm, by mass, calculated as platinum group metal atoms relative to the mass of component (A). If the amount of catalyst is less than the lower limit, the catalytic effect may not be obtained. On the other hand, if the amount exceeds the upper limit, the catalytic effect will not increase and it is uneconomical, so it is not preferred.

[0050] [(F) Hydrosilylation Reaction Inhibitor] Component (F) is a reaction inhibitor that suppresses the progress of the hydrosilylation reaction at room temperature and is added to extend shelf life and pot life. This reaction inhibitor can be any known inhibitor used in addition-curable silicone compositions. Examples of such reaction inhibitors include acetylene compounds such as acetylene alcohols (e.g., 3-methyl-1-tridecyn-3-ol, 1-ethynyl-1-cyclohexanol, 3,5-dimethyl-1-hexyn-3-ol), various nitrogen compounds such as tributylamine, tetramethylethylenediamine, and benzotriazole, organophosphorus compounds such as triphenylphosphine, oxime compounds, and organochloro compounds.

[0051] The amount of component (F) blended is 0.05 to 5 parts by mass, and preferably 0.1 to 1 part by mass. If the amount of reaction retarder is less than 0.05 parts by mass, the desired shelf life and pot life may not be achieved, while if it is more than 5 parts by mass, the curability of the silicone composition may decrease.

[0052] Manufacturing Process for Thermally Conductive Silicone Composition A manufacturing method for the thermally conductive silicone composition of the present invention will now be described. There are no particular limitations on the manufacturing method for the thermally conductive silicone composition of the present invention. Examples of methods include mixing the above-mentioned components (A) to (F) using a mixer such as a rotation-revolution type mixer (product name: Awatori Rentaro, manufactured by THINKYO Corporation), Trimix, Twinmix, or Planetary Mixer (all manufactured by Inoue Seisakusho Co., Ltd.), Ultramixer (Mizuho Kogyo Co., Ltd.), or Hivis Dispermix (Tokushu Kika Kogyo Co., Ltd.). All of the components to be mixed may be mixed at once, or one or more components may be mixed in several stages.

[0053] In the present invention, it is preferable to first mix components (A), (C), and (D) at room temperature, and then mix components (E), (B), and (F). The viscosity of the phenyl silicone composition of the present invention, measured at 23°C, is preferably 1 to 1,000 Pa·s, more preferably 20 to 700 Pa·s, and even more preferably 50 to 500 Pa·s. If the viscosity is 1 Pa·s or higher, there is no risk of poor workability, such as difficulty in maintaining shape. Furthermore, if the viscosity is 1,000 Pa·s or lower, there is no risk of poor processability. The above viscosity can be obtained by adjusting the blending amounts of each of the above-mentioned components. Note that in the present invention, the viscosity is a value measured using a viscosity / viscoelasticity measuring device.

[0054] Process for Producing Cured Thermally Conductive Silicone Products The thermally conductive silicone composition of the present invention can be cured by heating at a temperature generally between 50 and 180°C, preferably between 80 and 150°C, and more preferably between 100 and 120°C.

[0055] Thermal Conductivity of Cured Thermally Conductive Silicone Product The thermal conductivity of the cured thermally conductive silicone product of the present invention is 1.0 W / m K or more, and preferably 2.0 W / m K or more. There is no particular upper limit to the thermal conductivity, but it can be, for example, 20 W / m K or less. In the present invention, the thermal conductivity is a value measured by the hot disc method.

[0056] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these.

[0057] Preparation of Thermally Conductive Silicone Composition Components (A) to (F) used in the following examples are shown below, where Me represents a methyl group and Ph represents a phenyl group.

[0058] (A) Component A-1: ​​A component represented by the following formula, having a kinematic viscosity of 700 mm at 25°C 2 s-1 phenyl-modified organopolysiloxane

[0059] A-2: A viscosity expressed by the following formula, having a kinematic viscosity of 600 mm at 25°C 2 Organopolysiloxane s-1

[0060] (B) Component B-1: A component having a kinematic viscosity of 20 mm at 25°C, as represented by the following formula: 2 ・s-1 phenyl-modified organohydrogenpolysiloxane

[0061] B-2: A kinematic viscosity at 25 ° C. represented by the following formula is 19 mm 2 ・s-1 phenyl-modified organohydrogenpolysiloxane

[0062] B-3: A viscosity of 5 mm at 25 ° C., as expressed by the following formula: 2 s-1 organohydrogenpolysiloxane

[0063] Component (C) C-1: Hydrolyzable organosiloxane represented by the following formula:

[0064] C-2: Hydrolyzable organosiloxane represented by the following formula:

[0065] C-3: Decyltrimethoxysilane represented by the following formula

[0066] C-4: Phenyltrimethoxysilane represented by the following formula

[0067] C-5: Hydrolyzable organosiloxane represented by the following formula:

[0068] Component (D) The filler particle size of component (D) was measured using a particle size distribution measuring device MT3000II (manufactured by Microtrac Bell Co., Ltd.). D-1: Spherical alumina powder (median diameter: 70 μm) D-2: Spherical alumina powder (median diameter: 45 μm) D-3: Spherical alumina powder (median diameter: 10 μm) D-4: Irregular alumina powder (median diameter: 2 μm)

[0069] Component (E): 5% chloroplatinic acid solution in 2-ethylhexanol

[0070] Component (F): 3-methyl-1-tridecyn-3-ol

[0071] [Manufacturing Method] Components (A), (C), and (D) were mixed as follows to obtain compositions of Examples and Comparative Examples. The plastic containers containing components (A), (C), and (D) were placed in a rotation-revolution mixer (trade name: Awatori Rentaro, manufactured by THINKY Corporation) in the composition ratios (parts by mass) shown in Tables 1 and 2, and mixed at room temperature at 2,000 rpm for 1 minute twice. The resulting mixture was then cooled to room temperature. Component (E) was then added, and the mixture was mixed at 2,000 rpm for 30 seconds twice. The resulting mixture was then cooled to room temperature. A mixture of components (B) and (F) was then added, and the mixture was mixed at 2,000 rpm for 10 seconds twice. The mixture was then cooled to room temperature and degassed using a vacuum pump.

[0072] [Molding method] The prepared thermally conductive silicone composition was poured into a mold measuring 60 mm × 60 mm × 6 mm or 190 mm × 140 mm × 2 mm, the mold opening was sandwiched between two sheets of fluorine-treated PET film, and then the composition was cured in a press molding machine at 110°C for 10 minutes to obtain a cured thermally conductive silicone product.

[0073] [Evaluation Method] [Viscosity] The viscosity of the obtained composition was measured at a rotation speed of 10 s using a viscosity / viscoelasticity measuring device (trade name: MARS40 (Thermo Fisher Scientific Co., Ltd.)). The measurement conditions were 23°C, parallel plates, and a gap of 0.5 mm.

[0074] [Thermal Conductivity] Using two 6 mm thick sheets molded in Examples 1 to 3 and Comparative Examples 1 to 5 below, the thermal conductivity of the cured product was measured with a thermal conductivity meter (TPS 2500S, manufactured by Kyoto Electronics Manufacturing Co., Ltd.).

[0075] [Hardness] The hardness of the cured thermally conductive silicone was measured using a durometer (TYPE A) hardness tester specified in JIS K6253-3: 2012. For products with measured values ​​of less than 20, the hardness was measured using a durometer (ASKER C) hardness tester measured in accordance with the method described in JIS K7312: 1996, Appendix 2.

[0076] [Heat Resistance Test] A 6 mm thick sheet was aged at 180° C. After aging for 90 hours, the sheet was returned to room temperature, and the hardness before and after aging was measured.

[0077] [Chemical Resistance Test] A 2 mm thick, 40 × 40 mm sheet was immersed in a genuine TOYOTA ATF and aged at 150° C. After aging for 250 hours, the sheet was removed from the ATF, and the volume change rate was calculated from the changes in mass and density before and after aging.

[0078]

[0079]

[0080] The thermally conductive silicone cured product obtained by using a phenyl-modified hydrolyzable organosiloxane corresponding to the general formula (1) as the component (C) used in Example 1 had a thermal conductivity of 2.0 W / m·K or higher, and showed almost no change in hardness in a heat resistance test at 180°C. Furthermore, the cured product was found to have a very low hardness. Furthermore, despite the high thermally conductive filler loading in Examples 2 and 3, the inclusion of the component (C) of the present invention suppressed increases in the viscosity of the composition and the hardness of the cured product, achieving high thermal conductivity. On the other hand, when a hydrolyzable dimethylorganosiloxane (C-2) was used as the component (C), as in Comparative Example 1, it was found that a stable cured product could not be obtained. This is thought to be due to the low compatibility between the phenyl-modified organopolysiloxane of component (A) and the dimethylorganosiloxane (C-2), which resulted in separation of (C-2) in the composition. Furthermore, even when a long-chain compound (C-5) was used in a hydrolyzable organosiloxane containing a triphenyl group, a stable cured product could not be obtained (Comparative Example 5). As mentioned above, this is believed to be due to low compatibility with the phenyl-modified organosiloxane (A). Furthermore, when decyltrimethoxysilane (C-3) or phenyltrimethoxysilane (C-4) was used as component (C), as in Comparative Examples 2 and 3, hardness after heat resistance testing increased significantly. This is believed to be due to the low molecular weight and high volatility of (C-3) and (C-4). Furthermore, the phenyl-modified silicone cured product in Example 1 showed a volume change of approximately -4% after a 250-hour ATF resistance test. This differs from the results of a 2.6% swelling under the same conditions for a cured product of a dimethylsilicone elastomer, as in Comparative Example 4. Furthermore, the volume change of the cured product using the phenyl-modified silicone composition after the ATF resistance test showed almost no difference depending on the component (C), which is believed to be a property unique to the phenyl-modified silicone composition. The above results show that the thermally conductive silicone cured product of the present invention exhibits relatively high ATF resistance and can also achieve a thermal conductivity of 4.0 W / m K or higher. Therefore, the thermally conductive silicone composition and cured product of the present invention have the potential to become new heat-dissipating materials with chemical resistance.

[0081] This specification includes the following aspects: [1]: (A) A composition having two or more alkenyl groups in one molecule and a kinematic viscosity at 25°C of 100 to 100,000 mm 2 / s: 100 parts by mass; (B) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the number of moles of hydrosilyl groups in component (B) is 0.1 to 3 moles per mole of alkenyl groups in component (A); (C) a compound represented by the following general formula (1): (In the formula, R 1 are independently aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3 is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, and n is an integer satisfying the condition 2≦n≦60.) A thermally conductive silicone composition comprising: 10 to 300 parts by mass of a hydrolyzable organopolysiloxane represented by the formula (I); (D) one or more thermally conductive fillers selected from the group consisting of metals, metal oxides, metal hydroxides, and metal nitrides; (E) a platinum group metal catalyst in an amount of 0.1 to 500 ppm, calculated as platinum group metal atoms, relative to the mass of component (A); and (F) a hydrosilylation reaction inhibitor in an amount of 0.05 to 5 parts by mass. [2]: The R 1 is a phenyl group, and the R 2 is a methyl group. [3]: The thermally conductive silicone composition according to [1] or [2], characterized in that the viscosity of the thermally conductive silicone composition at 23°C is 1 to 1,000 Pa s. [4]: ​​A thermally conductive silicone cured product obtained by curing the thermally conductive silicone composition according to any one of [1] to [3]. [5]: The thermally conductive silicone cured product according to [4], characterized in that the thermal conductivity is 1.0 W / m K or more.

[0082] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.

Claims

1. The following (A) to (F): (A) A viscoelastic composition having two or more alkenyl groups in one molecule and a kinetic viscosity at 25°C of 100 to 100,000 mm 2 (B) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the number of moles of hydrosilyl groups in component (B) is 0.1 to 3 moles per mole of alkenyl groups in component (A); and (C) a phenyl-modified organopolysiloxane represented by the following general formula (1): (In the formula, R 1 are each independently an aromatic hydrocarbon group having 6 to 10 carbon atoms; R 2 are independently an alkyl group having 1 to 10 carbon atoms; R 3 is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, and n is an integer satisfying 2≦n≦60.) a hydrolyzable organopolysiloxane represented by the formula: 10 to 300 parts by mass, (D) one or more thermally conductive fillers selected from the group consisting of metals, metal oxides, metal hydroxides, and metal nitrides: in an amount of 10 to 97% by mass based on the entire composition, (E) a platinum group metal catalyst: 0.1 to 500 ppm by mass calculated as platinum group metal atoms, based on the mass of component (A), and (F) a hydrosilylation reaction inhibitor: 0.05 to 5 parts by mass.

2. The R in the general formula (1) 1 is a phenyl group, and the R 2 2. The thermally conductive silicone composition according to claim 1, wherein: is a methyl group.

3. The thermally conductive silicone composition according to claim 1, characterized in that the viscosity of said thermally conductive silicone composition at 23° C. is 1 to 1,000 Pa·s.

4. A thermally conductive silicone cured product obtained by curing the thermally conductive silicone composition according to any one of claims 1 to 3.

5. The thermally conductive cured silicone product according to claim 4, characterized in that it has a thermal conductivity of 1.0 W / m·K or more.

Citation Information

Patent Citations

  • Cosmetic composition containing hydrocarbon oil and silicone oil

    JP2004262919A

  • Heat-conductive silicone oil composition, heat-dissipation agent and electronic device

    JP2007039621A

  • Method for thermoconductive rubber sheet and thermoconductive rubber sheet

    JP2015067736A

  • Thermoconductive resin composition and thermoconductive sheet using the same

    JP2015067737A

  • Heat-conductive fluorine-containing curable composition, cured product of the same, and electric and electronic component

    JP2017082090A

Cited By

  • Thermosoftening thermally conductive composition

    WO2025239281A1